Laminated, retort or boiling pouches
The laminate structure with a polypropylene resin layer, high-melting-point surface resin layer, adhesive resin layer, and polyolefin sealant layer addresses recyclability and gas barrier issues in retort or boil pouches, providing improved adhesion and heat resistance.
Patent Information
- Application Number
- JP2023027637
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-19
- Filing Date
- 2023-02-24
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2041-01-29
AI Technical Summary
Conventional polyester-based laminates for retort or boil pouches face challenges in recyclability due to poor interlayer adhesion and gas barrier properties, making them unsuitable for recycling.
A laminate structure comprising a polypropylene resin layer with a surface resin layer having a melting point of 180°C or higher, an adhesive resin layer, a vapor-deposited inorganic oxide film, and a sealant layer made of polyolefin with a melting point of 110°C or higher, enhancing adhesion and gas barrier properties.
The laminate improves interlayer adhesion and gas barrier properties, enabling recyclable monomaterial packaging containers with heat resistance, suitable for retort or boil pouch applications.
Smart Images

Figure 0007594742000010 
Figure 0007594742000011 
Figure 0007594742000012
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate, a retort or boiling pouch. [Background technology]
[0002] Conventionally, films made of polyesters such as polyethylene terephthalate (hereinafter also referred to as polyester films) have been used as substrates constituting laminates used in the manufacture of packaging containers such as retort or boiling pouches because they are excellent in mechanical properties, chemical stability, heat resistance, and transparency, and are inexpensive.
[0003] The polyester film is usually laminated with a sealant layer, which is a polyolefin film such as a polypropylene film, and then molded into a packaging container.
[0004] In the packaging container obtained by forming a laminate of the above-mentioned different resin films, i.e., a polyester film and a polypropylene film, it is difficult to separate the resin films from each other. Therefore, the packaging container collected after use is not suitable for recycling and is not actively recycled at present.
[0005] In light of this current situation, in order to improve the recyclability of packaging containers, studies are being conducted on the production of packaging containers using laminates made of the same material (mono-material packaging containers) by using stretched polypropylene film (stretched polypropylene film) as the base material instead of polyester film. Summary of the Invention [Problem to be solved by the invention]
[0006] In this study, the inventors formed a vapor-deposited film on the surface of a stretched polypropylene film in order to compensate for the reduced gas barrier property caused by replacing the polyester film with a stretched polypropylene film. However, the adhesion between the stretched polypropylene film and the vapor-deposited film was insufficient, and the desired gas barrier property was not achieved. Thus, the inventors found this new problem.
[0007] The inventors have discovered that, rather than forming a vapor-deposited film on the surface of a stretched polypropylene film, by providing a surface resin layer containing a resin material having a melting point of 180°C or higher on the surface of a stretched polypropylene film and then forming a vapor-deposited film on the surface resin layer, adhesion is improved and gas barrier properties are also improved.
[0008] The inventors also discovered that, rather than forming a vapor-deposited film on the surface of a stretched polypropylene film, by providing a surface coating layer containing a resin material having a polar group on the surface of the stretched polypropylene film and then forming a vapor-deposited film on the surface coating layer, adhesion can be improved and gas barrier properties can also be improved.
[0009] Furthermore, packaging containers are sometimes required to have heat resistance. The present inventors have found that by forming a laminate having a sealant layer containing a polyolefin having a melting point of 110° C. or more, a packaging container produced using the laminate has heat resistance.
[0010] The present invention has been made based on such findings, and the problem to be solved by the present invention is to provide a laminate that can be suitably used for mono-material packaging containers, can significantly improve the interlayer adhesion between the substrate and the vapor-deposited film, can achieve favorable gas barrier properties, and has heat resistance.
[0011] Another problem to be solved by the present invention is to provide a pouch for retort or boiling which is formed from the laminate. [Means for solving the problem]
[0012] In a first aspect, the present invention provides a laminate comprising: At least a first substrate, a vapor deposition film, a barrier coat layer, and a sealant layer are included, the first base material is a biaxially stretched resin film including a polypropylene resin layer, a surface resin layer provided on one surface of the polypropylene resin layer, and an adhesive resin layer between the polypropylene resin layer and the surface resin layer; the adhesive resin layer is provided on the polypropylene resin layer, the surface resin layer is provided on the adhesive resin layer, the vapor-deposited film is provided on a surface resin layer of the first substrate, The surface resin layer contains a resin material having a melting point of 180° C. or more, the resin material is vinyl resin, nylon 6, nylon 6,6, MXD nylon or polyester, The vapor-deposited film is composed of an inorganic oxide, The sealant layer is a laminate comprising a polyolefin having a melting point of 110° C. or higher.
[0013] In one embodiment, the surface resin layer includes a resin material having a melting point of 180° C. or more and 265° C. or less.
[0014] In one embodiment, the resin material of the surface resin layer has a melting point TA, The polypropylene of the polypropylene resin layer has a melting point TB, The difference between the melting point TA and the melting point TB is 20°C or more and 80°C or less.
[0015] In one embodiment, the resin material of the surface resin layer is made of a polymer having a polar group.
[0016] In one embodiment, the ratio of a thickness of the surface resin layer to a total thickness of the first base material is 1% or more and 10% or less.
[0017] In one embodiment, the sealant layer comprises a sealant material having a melting point of 150° C. or greater.
[0018] In one embodiment, the sealant layer comprises polypropylene having a melting point of 150° C. or greater.
[0019] In one embodiment, the laminate further comprises a second substrate.
[0020] In one embodiment, the second substrate comprises polypropylene.
[0021] In one embodiment, the first substrate and the deposited film are located between the second substrate and the sealant layer.
[0022] In one embodiment, the laminate further comprises an intermediate layer between the deposition film and the sealant layer, The intermediate layer is the second substrate.
[0023] In one embodiment, the intermediate layer is made of a polypropylene resin film that has been subjected to a stretching treatment.
[0024] In one embodiment, the barrier coat layer is provided between the vapor deposition film and the sealant layer.
[0025] In one embodiment, the barrier coat layer is a gas barrier coating film of a mixture of a metal alkoxide and a water-soluble polymer, or a gas barrier coating film of a mixture of a metal alkoxide, a water-soluble polymer, and a silane coupling agent.
[0026] In one embodiment, the laminate is used in a packaging container.
[0027] The present invention is a pouch for retort or boiling, comprising the laminate.
[0028] In one embodiment, the retort or boiling pouch includes a notch.
[0029] In one embodiment, the retort or boiling pouch includes a half-cut line. Effect of the Invention
[0030] According to the present invention, it is possible to provide a laminate which can be suitably used for mono-material packaging containers, can significantly improve the interlayer adhesion between the substrate and the vapor-deposited film, can achieve favorable gas barrier properties, and has heat resistance. Furthermore, according to the present invention, a pouch for retort or boiling comprising the laminate can be provided. [Brief description of the drawings]
[0031] [Figure 1] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Diagram 3] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Figure 4] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Diagram 5] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Figure 6] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Figure 7] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Figure 8] FIG. 2 is a plan view showing an example of a loop stiffness measuring device. [Figure 9] FIG. 9 is a cross-sectional view taken along line VV of the loop stiffness measuring device of FIG. 8. [Figure 10] FIG. 1 is a diagram for explaining a process of attaching a test piece to a loop stiffness measuring device. [Figure 11] FIG. 13 is a diagram for explaining a step of forming a loop portion in a test piece. [Figure 12] FIG. 13 is a diagram for explaining a process of applying a load to a loop portion of a test piece. [Figure 13]FIG. 13 is a diagram for explaining a process of applying a load to a loop portion of a test piece. [Figure 14] FIG. 13 is a diagram for explaining a process of applying a load to a loop portion of a test piece. [Figure 15] FIG. 1 is a schematic cross-sectional view illustrating one embodiment of a deposition apparatus. [Figure 16] FIG. 1 is a schematic cross-sectional view illustrating one embodiment of a deposition apparatus. [Figure 17] FIG. 11 is a schematic cross-sectional view illustrating another embodiment of a deposition apparatus. [Figure 18] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Figure 19] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Figure 20] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Figure 21] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Figure 22] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. [Figure 23] FIG. 1 is a front view showing one embodiment of a retort or boiling pouch of the present invention. [Figure 24] FIG. 1 is a perspective view showing one embodiment of a retort or boiling pouch of the present invention. [Diagram 25] FIG. 2 is a schematic diagram showing an example of a method for measuring laminate strength. [Figure 26] FIG. 2 is a schematic diagram showing an example of a method for measuring laminate strength. [Figure 27] FIG. 13 is a graph showing the change in tensile stress with respect to the distance between a pair of grippers that pull the substrate side and the sealant layer side to measure the laminate strength. [Figure 28] FIG. 1 is a diagram showing an example of a method for measuring puncture strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] [Laminate in the first embodiment] As shown in FIG. 1, a laminate 10A of the present invention includes a first substrate 11A, a vapor-deposited film 12A, and a sealant layer 13A, and the first substrate 11A includes at least a polypropylene resin layer 14A and a surface resin layer 15A. In one embodiment of the present invention, the laminate 10A may further include a barrier coat layer 16A between the vapor-deposited film 12A and the sealant layer 13A, as shown in FIG. In one embodiment of the present invention, the first base material 11A may include an adhesive resin layer 17A between the polypropylene resin layer 14A and the surface resin layer 15A, as shown in FIG. In one embodiment of the present invention, the laminate 10A may include a first base material 11A, a vapor-deposited film 12A, a barrier coat layer 16A provided on the vapor-deposited film 12A, and a sealant layer 13A, as shown in Fig. 4. The first base material 11A may include a polypropylene resin layer 14A, an adhesive resin layer 17A, and a surface resin layer 15A, and the adhesive resin layer 17A may be provided between the polypropylene resin layer 14A and the surface resin layer 15A. In one embodiment of the present invention, the laminate may further include a second substrate. When the laminate includes a second substrate, the laminate 10A may include a second substrate 18A, a deposition film 12A, a first substrate 11A, and a sealant layer 13A in this order, as shown in FIG. 5, or may include a second substrate 18A, a first substrate 11A, a deposition film 12A, and a sealant layer 13A in this order, as shown in FIG. 6, or may include a first substrate 11A, a deposition film 12A, a second substrate 18A, and a sealant layer 13A in this order, as shown in FIG. 7. The second substrate 18A in the laminate 10A of FIG. 5 and FIG. 6, and the first substrate 11A in the laminate 10A of FIG. 7 may be located in the outermost layer of the laminate 10A. In one embodiment of the present invention, the laminate 10A may include an adhesive layer (not shown) between any of the vapor-deposited film, the sealant layer, the first substrate, and the second substrate. In another embodiment, the laminate of the present invention may include an intermediate layer between the vapor-deposited film and the sealant layer, and the intermediate layer may be the second substrate.
[0033] The haze value of the laminate is preferably 20% or less, and more preferably 5% or less, which can improve the transparency of the laminate. In this specification, the haze value of the laminate is measured in accordance with JIS K 7105:1981 using a haze meter (Murakami Color Research Laboratory Co., Ltd.).
[0034] In the laminate of the first aspect, the laminate strength between the first substrate and the vapor-deposited film is preferably 3 N or more, more preferably 4 N or more, and even more preferably 5.5 N or more, per 15 mm width. The upper limit of the laminate strength of the laminate may be 20 N or less. The method for measuring the laminate strength of the laminate will be described later in the Examples.
[0035] The tensile strength of the laminate in one direction may be 30 MPa or more, or 35 MPa or more. The tensile strength of the laminate in one direction may be 70 MPa or less, or 50 MPa or less. The one direction of the laminate may be the machine direction (MD direction). The tensile strength of the laminate in a direction perpendicular to the one direction may be 40 MPa or more, or 60 MPa or more. The tensile strength of the laminate in a direction perpendicular to the one direction may be 150 MPa or less, or 100 MPa or less. The direction perpendicular to the one direction may be the transverse direction (TD) of the laminate. In this specification, the tensile strength of the laminate is measured in accordance with JIS K7127: 1999. As a measuring device, a tensile tester STA-1150 manufactured by Orientec Co., Ltd. can be used. The test piece may be a rectangular laminate cut out from the laminate with a width of 10 mm and a length of 150 mm. The distance between the pair of chucks holding the test piece at the start of the measurement is 50 mm, and the tensile speed is 300 mm / min. In this specification, unless otherwise specified, the environment during the measurement of the tensile strength is a temperature of 23°C and a relative humidity of 50%.
[0036] The loop stiffness in one direction of the laminate may be 30 mN or more, 50 mN or more, or 70 mN or more. The loop stiffness in one direction of the laminate may be 200 mN or less, 150 mN or less, or 120 mN or less. The one direction of the laminate may be the machine direction (MD direction). The loop stiffness of the laminate in a direction perpendicular to the one direction may be 30 mN or more, 50 mN or more, or 70 mN or more. The loop stiffness of the laminate in a direction perpendicular to the one direction may be 200 mN or less, 150 mN or less, or 130 mN or less. The direction perpendicular to the one direction may be the transverse direction (TD) of the laminate.
[0037] The loop stiffness is a parameter that indicates the stiffness of a laminate. A method for measuring the loop stiffness will be described below with reference to Figs.
[0038] FIG. 8 is a plan view showing the test piece 20 and the loop stiffness measuring instrument 25, and FIG. 9 is a cross-sectional view of the test piece 20 and the loop stiffness measuring instrument 25 of FIG. 8 taken along the line VV. The test piece 20 is a rectangular laminate having long and short sides. In this specification, the length X1 of the long side of the test piece 20 is set to 150 mm, and the length X2 of the short side is set to 15 mm. As the loop stiffness measuring instrument 25, a No. 581 Loop Stiffness Tester (registered trademark) LOOP STIFFNESS TESTER DA type manufactured by Toyo Seiki Seisakusho Co., Ltd. can be used. The length X1 of the long side of the test piece 20 can be adjusted as long as the test piece 20 can be held by a pair of chuck parts 26 described later.
[0039] The loop stiffness measuring device 25 has a pair of chuck portions 26 for gripping a pair of ends in the long side direction of the test piece 20, and a support member 27 for supporting the chuck portions 26. The chuck portions 26 include a first chuck 26A and a second chuck 26B. In the state shown in FIG. 8 and FIG. 9, the test piece 20 is placed on the pair of first chucks 26A, and the second chuck 26B does not yet grip the test piece 20 between the first chuck 26A and the second chuck 26B. As described later, during measurement, the test piece 20 is gripped between the first chuck 26A and the second chuck 26B of the chuck portions 26. The second chuck 26B may be connected to the first chuck 26A via a hinge mechanism.
[0040] A method for measuring the loop stiffness of the test piece 20 using the loop stiffness measuring device 25 will be described. First, as shown in FIG. 8 and FIG. 9, the test piece 20 is placed on the first chuck 26A of a pair of chuck parts 26 arranged with a gap X3 therebetween. In this specification, the gap X3 is set so that the length of the loop part 21 (hereinafter also referred to as the loop length) described later is 60 mm. The test piece 20 includes an inner surface 20x located on the first chuck 26A side and an outer surface 20y located on the opposite side of the inner surface 20x. When the loop part 21 described later is formed on the test piece 20, the inner surface 20x is located inside the loop part 21, and the outer surface 20y is located outside the loop part 21. Next, as shown in FIG. 10, the second chuck 26B is placed on the test piece 20 so as to grip the end of the long side direction of the test piece 20 between the first chuck 26A and the second chuck 26B.
[0041] Next, as shown in FIG. 11, at least one of the pair of chucks 26 is slid on the support member 27 in a direction in which the distance between the pair of chucks 26 is reduced. This allows the loop portion 21 to be formed in the test piece 20. The test piece 20 shown in FIG. 11 has the loop portion 21, a pair of intermediate portions 22, and a pair of fixing portions 23. The pair of fixing portions 23 are portions of the test piece 20 that are gripped by the pair of chucks 26. The pair of intermediate portions 22 are portions of the test piece 20 that are located between the loop portion 21 and the pair of intermediate portions 22. As shown in FIG. 11, the chuck portion 26 is slid on the support member 27 until the inner surfaces 20x of the pair of intermediate portions 22 come into contact with each other. This allows the loop portion 21 to be formed with a loop length of 60 mm. The loop length of the loop portion 21 is the length of the test piece 20 between position P1 where the surface of one second chuck 26B on the loop portion 21 side intersects with the test piece 20, and position P2 where the surface of the other second chuck 26B on the loop portion 21 side intersects with the test piece 20. When the thickness of the test piece 20 is ignored, the above-mentioned interval X3 is a value obtained by adding 2×t to the length of the loop portion 21, where t is the thickness of the second chuck 26B of the chuck portion 26.
[0042] 12, the posture of the chuck portion 26 is adjusted so that the protruding direction Y of the loop portion 21 relative to the chuck portion 26 is horizontal. For example, the posture of the chuck portion 26 supported by the support member 27 is adjusted by moving the support member 27 so that the normal direction of the support member 27 is horizontal. In the example shown in FIG. 12, the protruding direction Y of the loop portion 21 coincides with the thickness direction of the chuck portion. Also, a load cell 28 is prepared at a position separated by a distance Z1 from the second chuck 26B in the protruding direction Y of the loop portion 21.
[0043] 13, the load cell 28 is moved toward the loop portion 21, and the load cell 28 is brought into contact with the loop portion 12. The distance Z1 is the distance between the load cell 28 and the second chuck 26B of the chuck portion 26.
[0044] 14, the loop portion 21 is pressed toward the chuck portion 26 by a distance Z2 using the load cell 28. In this specification, the distance Z2 is set to 15 mm. 14, the load cell 28 is moved by a distance Z2 toward the chuck portion 26, and in a state in which the load cell 28 presses the loop portion 21 of the test piece 20, the value of the load applied to the load cell 28 from the loop portion 21 becomes stable, and then the value of the load is recorded. The value of the load thus obtained is regarded as the loop stiffness of the laminate constituting the test piece 20. In this specification, unless otherwise specified, the environment during the measurement of the loop stiffness is a temperature of 23°C and a relative humidity of 50%.
[0045] The piercing strength of the laminate may be 10N or more, or 15N or more. The puncture strength of the laminate is measured in accordance with JIS Z1707 7.4. A specific measurement method will be described in the examples below.
[0046] Conventionally, a laminate in which a substrate and a sealant layer are made of different resin materials has been used for a packaging container. However, since it is difficult to separate the substrate and the sealant layer after collecting used packaging containers, the current situation is that the packaging container is not actively recycled. In the present invention, a stretched polypropylene resin film is used as the first substrate, and the sealant layer is a layer containing polypropylene having a melting point of 110°C or higher, and both are constructed from the same material, thereby improving the recyclability of the laminate when used as a packaging container.
[0047] From the viewpoint of recyclability, the higher the proportion of polypropylene contained in the sealant layer, the more preferable, as will be described later. When the sealant layer is made of polypropylene, the content of polypropylene in the total amount of resin materials contained in the laminate of the present invention is preferably 80% by mass or more, and more preferably 95% by mass or more, which can further improve the recyclability of packaging containers produced using the laminate of the present invention.
[0048] Each layer of the laminate of the present invention will be described below.
[0049] (1st base material) The first base material comprises at least a polypropylene resin layer and a surface resin layer, and if desired, an adhesive resin layer may be provided between the polypropylene resin layer and the surface resin layer.
[0050] (Polypropylene resin layer) The polypropylene resin layer is made of polypropylene and may have a single-layer structure or a multi-layer structure. By providing the first base material with a polypropylene resin layer, the heat resistance and oil resistance of a packaging container produced using the first base material can be improved.
[0051] The polypropylene resin layer is a film that has been subjected to a stretching treatment. The stretching treatment may be uniaxial stretching or biaxial stretching. The stretching ratio in the machine direction (MD direction) and the transverse direction (TD direction) of the polypropylene resin layer is preferably 2 times or more and 15 times or less, and more preferably 5 times or more and 13 times or less. By setting the stretching ratio at 2 times or more, the strength and heat resistance of the polypropylene resin layer can be further improved, and the printability of the polypropylene resin layer can also be improved. From the viewpoint of the breaking limit of the polypropylene resin layer, the stretching ratio is preferably 15 times or less.
[0052] The polypropylene contained in the polypropylene resin layer may be any of a homopolymer, a random copolymer, and a block copolymer. A polypropylene homopolymer is a polymer of propylene alone, a polypropylene random copolymer is a random copolymer of propylene and an α-olefin other than propylene (e.g., ethylene, butene-1, 4-methyl-1-pentene, etc.), and a polypropylene block copolymer is a copolymer having a polymer block of propylene and a polymer block of the above-mentioned α-olefin other than propylene. Among these polypropylenes, it is preferable to use homopolymers or random copolymers from the viewpoint of transparency. When the rigidity and heat resistance of the packaging bag are important, it is preferable to use homopolymers, and when the impact resistance and the like are important, it is preferable to use random copolymers. It is also possible to use biomass-derived polypropylene and mechanically or chemically recycled polypropylene.
[0053] The polypropylene content in the polypropylene resin layer is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.
[0054] The polypropylene resin layer may contain a heat seal modifier, which can improve the heat sealability of the polypropylene resin layer and make it easier to produce a packaging container by sealing with an envelope. The heat seal modifier is not particularly limited as long as it has excellent compatibility with the polypropylene constituting the heat seal layer, and examples thereof include olefin copolymers. Furthermore, a conventionally known heat sealing agent may be applied to the surface of the polypropylene resin layer and then dried.
[0055] As long as the characteristics of the present invention are not impaired, the polypropylene resin layer may contain a resin material other than polypropylene, such as polyolefins such as polyethylene, (meth)acrylic resins, vinyl resins, cellulose resins, polyamide resins, polyesters, and ionomer resins. The polypropylene resin layer may contain additives, such as crosslinking agents, antioxidants, antiblocking agents, slip agents, UV absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, and modifying resins, as long as the additives do not impair the properties of the present invention.
[0056] The thickness of the polypropylene resin layer is preferably 10 μm or more, more preferably 10 μm or more, and is preferably 50 μm or less, more preferably 40 μm or less. By setting the thickness of the polypropylene resin layer to 10 μm or more, the strength and heat resistance of the first base material can be further improved. By setting the thickness of the polypropylene resin layer to 50 μm or less, the film-forming property and processability of the first base material can be further improved.
[0057] The polypropylene resin layer may have a printed layer on its surface. The image formed on the printed layer is not particularly limited, and may be a character, a pattern, a symbol, or a combination thereof. The printing layer on the first substrate can be formed using ink derived from biomass, which can further reduce the environmental impact. The method for forming the printed layer is not particularly limited, and examples of the method include conventionally known printing methods such as gravure printing, offset printing, and flexographic printing.
[0058] The polypropylene resin layer may be subjected to a surface treatment, which can improve the adhesion with the surface coating layer. The method of surface treatment is not particularly limited, and examples thereof include physical treatments such as corona discharge treatment, ozone treatment, low-temperature plasma treatment using oxygen gas and / or nitrogen gas, and glow discharge treatment, as well as chemical treatments such as oxidation treatment using chemicals.
[0059] (Surface resin layer) The first base material has a surface resin layer containing a resin material having a melting point of 180° C. or higher (hereinafter, also referred to as a high-melting-point resin material), which allows a highly adhesive vapor-deposited film to be formed on the surface resin layer, thereby improving the gas barrier property. In addition, as described below, a packaging container produced using a laminate having the surface resin layer has high laminate strength. In one embodiment, the surface resin layer may be provided on the polypropylene resin layer, that is, the surface resin layer may be adjacent to the polypropylene resin layer. In one embodiment, when the first substrate includes an adhesive resin layer between the polypropylene resin layer and the surface resin layer, the adhesive resin layer may be provided on the polypropylene resin layer, and the surface resin layer may be provided on the adhesive resin layer, i.e., the adhesive resin layer may be adjacent to the polypropylene resin layer, and the surface resin layer may be adjacent to the adhesive resin layer.
[0060] The melting point of the high melting point resin material is more preferably 185° C. or higher, further preferably 190° C. or higher, and particularly preferably 205° C. or higher. By setting the melting point of the high melting point resin material to 185° C. or higher, the adhesiveness of the evaporated film can be improved, the gas barrier properties can be improved, and the laminate strength of the packaging container can be improved. From the viewpoint of film-forming properties of the first substrate, the melting point of the high-melting-point resin material is preferably 265° C. or lower, more preferably 260° C. or lower, and even more preferably 250° C. or lower. In this specification, the melting point can be measured in accordance with JIS K7121:2012 (Method for measuring transition temperature of plastics). Specifically, the melting point can be determined by measuring a DSC curve at a temperature rise rate of 10° C. / min using a differential scanning calorimetry (DSC) device.
[0061] The high melting point resin material contained in the surface resin layer has a melting point TA, and the polypropylene contained in the polypropylene resin layer has a melting point TB, and the difference between the melting points TA and TB is preferably 20° C. or more. The difference between the melting points TA and TB is preferably 80° C. or less, and more preferably 60° C. or less. By making the difference between the melting point TA and the melting point TB 20° C. or more, the adhesiveness of the vapor-deposited film can be improved, the gas barrier property can be improved, and the laminate strength of the packaging container can be improved. In addition, by making the difference between the melting point TA and the melting point TB 80° C. or less, the film-forming properties of the first substrate can be further improved.
[0062] The high melting point resin material preferably has a polar group. In the present invention, the polar group refers to a group containing one or more heteroatoms. Examples of the polar group include an ester group, an epoxy group, a hydroxyl group, an amino group, an amide group, a carboxyl group, a carbonyl group, a carboxylic anhydride group, a sulfone group, a thiol group, and a halogen group. Among these, from the viewpoint of the laminate strength of the packaging container, a hydroxyl group, an ester group, an amino group, an amide group, a carboxyl group, and a carbonyl group are preferred, and an amide group is more preferred.
[0063] There are no particular limitations on the high melting point resin material that can be used as long as it has a melting point of 180° C. or higher. Examples of high melting point resin materials include vinyl resins, polyamides, polyimides, polyesters, (meth)acrylic resins, cellulose resins, polyolefins, and ionomer resins.
[0064] The high melting point resin material is particularly preferably a resin material having a melting point of 180° C. or higher and having a polar group, and is preferably polyester or a polyamide such as nylon 6, nylon 6,6, MXD nylon, or amorphous nylon. By using such a resin material, the adhesion of the evaporated film formed on the surface resin layer can be significantly improved, and the gas barrier properties can be effectively improved.
[0065] In one embodiment, the high melting point resin material is preferably polyamide. By using polyamide as the high melting point resin material, the deterioration of gas barrier property can be suppressed even after bending the laminate, and the heat resistance of the laminate can be improved. In addition, the deterioration of gas barrier property can be suppressed even after the laminate is subjected to retort treatment and boiling treatment described later. The high melting point resin material is more preferably nylon 6.
[0066] The content of the high melting point resin material in the surface resin layer is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.
[0067] The surface resin layer may contain a resin material other than the high melting point resin material as long as the characteristics of the present invention are not impaired. The surface resin layer may contain additives, such as crosslinking agents, antioxidants, antiblocking agents, slip agents, UV absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, and modifying resins, as long as the additives do not impair the properties of the present invention.
[0068] The ratio of the thickness of the surface resin layer to the total thickness of the first base material is preferably 1% or more, and more preferably 10% or less, and more preferably 5% or less. By setting the ratio of the thickness of the surface resin layer to the total thickness of the first base material to be 1% or more, the adhesion of the vapor-deposited film can be improved, the gas barrier property can be improved, and the laminate strength of the packaging container can be improved. By setting the ratio of the thickness of the surface resin layer to the total thickness of the first substrate to 10% or less, the film-forming property and processability of the first substrate can be further improved. In addition, as described later, the recyclability of a packaging container produced using the laminate of the present invention and a sealant layer made of polypropylene can be improved.
[0069] The thickness of the surface resin layer is preferably 0.1 μm or more, and more preferably 5 μm or less, and more preferably 4 μm or less. By making the thickness of the surface resin layer 0.1 μm or more, the adhesion of the evaporated film can be improved, the gas barrier property can be improved, and the laminate strength of the packaging container can be improved. In addition, by making the thickness of the surface resin layer 5 μm or less, the film-forming property and processability of the first base material can be further improved. In addition, as described later, the recyclability of a packaging container produced using the laminate of the present invention and a sealant layer made of polypropylene can be improved.
[0070] (adhesive resin layer) In one embodiment of the present invention, the first base material may include an adhesive resin layer between the polypropylene resin layer and the surface resin layer, which can improve the interlayer adhesion between the polypropylene resin layer and the surface resin layer.
[0071] The adhesive resin layer can be formed from adhesive resins such as polyether, polyester, silicone resin, epoxy resin, polyurethane, vinyl resin, phenol resin, polyolefin, and acid-modified polyolefin. Among these, from the viewpoint of recyclability, polyolefin and its acid-modified polyolefin are preferred, and polypropylene and its acid-modified polyolefin are particularly preferred. As the adhesive polypropylene, commercially available products can be used, for example, the Admer series manufactured by Mitsui Chemicals, Inc. can be used.
[0072] The thickness of the adhesive resin layer is not particularly limited, but can be, for example, 1 μm or more and 15 μm or less. By making the thickness of the adhesive resin layer 1 μm or more, the adhesion between the polypropylene resin layer and the surface resin layer can be further improved. By making the thickness of the adhesive resin layer 15 μm or less, the processability of the first base material can be improved.
[0073] The first base material composed of the above-mentioned layers is stretched. The stretching improves the mechanical strength. The stretching may be uniaxial or biaxial.
[0074] In one embodiment, the first substrate is a co-extruded film. The co-extruded film can be produced by forming a film using a T-die method or an inflation method, forming a laminated film, and then stretching the laminated film. The inflation method is preferable from the viewpoint of productivity because it allows film formation and stretching to be performed continuously in one step.
[0075] The stretching ratio of the first substrate in the longitudinal direction (MD direction) and transverse direction (TD direction) is preferably 2 times or more, more preferably 5 times or more. The stretching ratio of the first substrate in the longitudinal direction (MD direction) and transverse direction (TD direction) is preferably 15 times or less, more preferably 13 times or less. By setting the stretching ratio at 2 times or more, the strength of the first substrate can be further improved. In addition, the printability of the first substrate can be improved. On the other hand, from the viewpoint of the breaking limit of the first substrate, the stretching ratio is preferably 15 times or less. When the polypropylene resin layer of the first substrate is given heat sealability and used for a packaging container (for example, a tube, etc.) produced by enveloping, the stretching ratio is more preferably 2 times or more and 10 times or less, particularly preferably 2.5 times or more and 7 times or less.
[0076] In one embodiment, the first substrate is preferably stretched so that the tensile strength in the machine direction (MD) is greater than the tensile strength in the transverse direction (TD). By adopting such a configuration, it is possible to impart high tearability in one direction to the packaging container produced from the laminate of the present invention. The tensile strength of the first substrate in the machine direction (MD) is preferably 1.05 times or more, more preferably 1.10 times or more, and even more preferably 1.2 times or more, the tensile strength in the cross direction (TD). The tensile strength in the machine direction (MD direction) can be, for example, 200 MPa or more and 300 MPa or less. In this specification, the tensile strength of the first substrate is measured in accordance with JIS K7127: 1999. As a measuring device, a tensile tester STA-1150 manufactured by Orientec Co., Ltd. can be used. The test piece may be a rectangular film cut from the first substrate with a width of 15 mm and a length of 150 mm. The distance between the pair of chucks holding the test piece at the start of the measurement is 100 mm, and the tensile speed is 300 mm / min. In this specification, unless otherwise specified, the environment during the measurement of the tensile strength is a temperature of 23°C and a relative humidity of 50%.
[0077] The surface resin layer constituting the first base material may be subjected to a surface treatment, which can improve adhesion to the adjacent layer (vapor-deposited film). The method of surface treatment is not particularly limited, and examples thereof include physical treatments such as corona discharge treatment, ozone treatment, low-temperature plasma treatment using oxygen gas and / or nitrogen gas, and glow discharge treatment, as well as chemical treatments such as oxidation treatment using chemicals.
[0078] (evaporated film) The laminate of the present invention has a vapor-deposited film made of an inorganic oxide on the surface resin layer. That is, the vapor-deposited film is adjacent to the surface resin layer. This can impart gas barrier properties, specifically oxygen barrier properties and water vapor barrier properties, to the laminate. In addition, it can suppress the weight loss of the contents filled in a packaging container made using the laminate of the present invention.
[0079] Examples of inorganic oxides include aluminum oxide (alumina), silicon oxide (silica), magnesium oxide, calcium oxide, zirconium oxide, titanium oxide, boron oxide, hafnium oxide, barium oxide, silicon carbide oxide (carbon-containing silicon oxide), etc. Among these, silica, silicon carbide oxide, and alumina are preferred, and silica is particularly preferred from the viewpoint of not requiring aging treatment after the deposition film is formed.
[0080] In one embodiment, the inorganic oxide is more preferably carbon-containing silicon oxide, from the viewpoint of suppressing a decrease in gas barrier property even after the laminate is bent.
[0081] The thickness of the vapor-deposited film is preferably 1 nm or more, more preferably 5 nm or more, and even more preferably 10 nm or more. The thickness of the vapor-deposited film is preferably 150 nm or less, more preferably 60 nm or less, and even more preferably 40 nm or less. By making the thickness of the vapor-deposited film 1 nm or more, the oxygen barrier property and water vapor barrier property of the laminate can be further improved. On the other hand, by making the thickness of the vapor-deposited film 150 nm or less, the occurrence of cracks in the vapor-deposited film can be prevented. In addition, if the thickness of the vapor-deposited film is within the above range, the recyclability of the laminate when used as a packaging container is not impaired.
[0082] The deposition film can be formed by a conventional method. Examples of the deposition film include physical vapor deposition (PVD) methods such as vacuum deposition, sputtering, and ion plating, and chemical vapor deposition (CVD) methods such as plasma chemical vapor deposition, thermal chemical vapor deposition, and photochemical vapor deposition.
[0083] The vapor-deposited film may be a single layer formed by one vapor deposition process, or a multilayer formed by multiple vapor deposition processes. In the case of a multilayer film, each layer may be made of the same material or different materials. In addition, each layer may be formed by the same method or different methods.
[0084] As an apparatus used in the method for forming a vapor-deposited film by the PVD method, a plasma-assisted vacuum film-forming apparatus can be used. An embodiment of a method for forming a vapor-deposited film using a plasma-assisted vacuum film-forming apparatus will be described below.
[0085] In one embodiment of the present invention, as shown in Figures 15 and 16, the vacuum deposition apparatus includes a vacuum container A, an unwinding section B, a deposition drum C, a winding section D, a transport roll E, an evaporation source F, a reactive gas supply section G, an adhesion protection box H, a deposition material I, and a plasma gun J. 15 is a schematic cross-sectional view of the vacuum film-forming apparatus in the XZ plane, and FIG. 16 is a schematic cross-sectional view of the vacuum film-forming apparatus in the XY plane.
[0086] 15, the first substrate 11A to be wound around the film-forming drum C is placed with its surface resin layer surface facing downward in the upper part of the vacuum container A, and an electrically grounded deposition-protection box H is placed below the film-forming drum C in the vacuum container A. An evaporation source F is placed on the bottom surface of the deposition-protection box H. The film-forming drum C is placed in the vacuum container A so that the surface resin layer surface of the first substrate 11A wound around the film-forming drum C is located at a position facing the upper surface of the evaporation source F with a certain gap therebetween.
[0087] In addition, transport rolls E are disposed between the unwinding section B and the film-forming drum C, and between the film-forming drum C and the winding section D. The vacuum vessel is connected to a vacuum pump (not shown). The evaporation source F is for holding the evaporation material I, and is equipped with a heating device (not shown). The reactive gas supply unit G is a portion that supplies a reactive gas (such as oxygen, nitrogen, helium, argon, and a mixture of these gases) that reacts with the evaporated deposition material.
[0088] The deposition material I, which is heated and evaporated from the evaporation source F, is irradiated onto the surface resin layer of the first base material 11A, and at the same time, plasma is also irradiated onto the surface resin layer from the plasma gun J, thereby forming a deposition film. Details of this formation method are disclosed in JP 2011-214089 A.
[0089] As the plasma generating device used in the plasma chemical vapor deposition method, a device generating high frequency plasma, pulse wave plasma, microwave plasma, etc. may be used. Also, a device having two or more film formation chambers may be used. The device is preferably equipped with a vacuum pump so that each film formation chamber can be kept under vacuum. The degree of vacuum in each deposition chamber is 1×10 Pa or more. -6 It is preferable that the pressure is 0.1 Pa or less. An embodiment of a method for forming a vapor-deposited film using a plasma generating device will be described below.
[0090] First, the first substrate is sent into the film-forming chamber and transported at a predetermined speed onto the cooling electrode drum via an auxiliary roll. Next, a mixed gas composition containing a film-forming monomer gas containing an inorganic oxide, oxygen gas, an inert gas, etc. is supplied from the gas supply device into the film-forming chamber, plasma is generated on the surface resin layer by glow discharge, and the plasma is irradiated to form a vapor-deposited film containing an inorganic oxide on the surface resin layer. Details of this formation method are disclosed in JP 2012-076292 A.
[0091] FIG. 17 is a schematic diagram showing the configuration of a plasma enhanced chemical vapor deposition apparatus used in a CVD method.
[0092] In one embodiment, as shown in FIG. 17, the plasma chemical vapor deposition apparatus unwinds the first substrate 11A from the unwinding section B1 arranged in the vacuum vessel A1, and further transports the first substrate 11A on the circumferential surface of the cooling / electrode drum C1 at a predetermined speed via the transport roll E1. Oxygen, nitrogen, helium, argon and their mixed gases are supplied from the reactive gas supply G1, and a film-forming monomer gas or the like is supplied from the raw material gas supply section I1. The mixed gas composition for deposition consisting of these is adjusted and introduced into the vacuum vessel A1 through the raw material supply nozzle H1. Then, plasma is generated by glow discharge plasma F1 on the surface resin layer of the first substrate 11A transported on the circumferential surface of the cooling / electrode drum C1, and the plasma is irradiated to form a deposition film. At this time, a predetermined power is applied to the cooling / electrode drum C1 from a power source K1 arranged outside the vacuum vessel A1, and a magnet J1 is arranged near the cooling / electrode drum C1 to promote the generation of plasma. Next, after the deposition film is formed, the first base material 11A is wound up at a predetermined winding speed by a winding section D1 via a transport roll E1. In the drawing, L1 represents a vacuum pump.
[0093] As an apparatus used in the method for forming a vapor-deposited film, a continuous vapor-deposited film-forming apparatus equipped with a plasma pretreatment chamber and a film-forming chamber can be used.
[0094] An embodiment of a method for forming a vapor-deposited film using the apparatus will be described below. First, in the plasma pretreatment chamber, plasma is irradiated from a plasma supply nozzle onto the surface resin layer of the first substrate. Then, in the film formation chamber, a deposition film is formed on the plasma-treated surface resin layer. Details of this formation method are disclosed in International Publication WO2019 / 087960.
[0095] The surface of the deposited film is preferably subjected to the above-mentioned surface treatment, which can improve adhesion to adjacent layers.
[0096] In the laminate of the present invention, the vapor-deposited film is preferably a vapor-deposited film formed by a CVD method, and more preferably a carbon-containing silicon oxide vapor-deposited film formed by a CVD method, which can suppress the deterioration of the gas barrier property even after the laminate is bent.
[0097] The carbon-containing silicon oxide vapor deposition film contains silicon, oxygen, and carbon. In the carbon-containing silicon oxide vapor deposition film, the carbon ratio C is preferably 3% or more, more preferably 5% or more, and even more preferably 10% or more, relative to 100% of the total of the three elements silicon, oxygen, and carbon. In the carbon-containing silicon oxide vapor deposition film, the carbon ratio C is preferably 50% or less, more preferably 40% or less, and even more preferably 35% or less, relative to 100% of the total of the three elements silicon, oxygen, and carbon. By setting the carbon ratio C in the carbon-containing silicon oxide vapor-deposited film within the above range, it is possible to suppress a decrease in the gas barrier properties even after the laminate is bent. In this specification, the ratio of each element is based on moles.
[0098] In one embodiment of the carbon-containing silicon oxide vapor-deposited film, the silicon ratio Si is preferably 1% or more, more preferably 3% or more, and even more preferably 8% or more, based on 100% of the total of the three elements silicon, oxygen, and carbon. The silicon ratio Si is preferably 45% or less, more preferably 38% or less, and even more preferably 33% or less, based on 100% of the total of the three elements silicon, oxygen, and carbon. In one embodiment of the carbon-containing silicon oxide vapor-deposited film, the ratio O of oxygen is preferably 10% or more, more preferably 20% or more, and even more preferably 25% or more, based on the total of the three elements silicon, oxygen, and carbon (100%), and is preferably 70% or less, more preferably 65% or less, and even more preferably 60% or less. By setting the silicon ratio Si and oxygen ratio O in the carbon-containing silicon oxide vapor-deposited film within the above ranges, deterioration of the gas barrier properties can be further suppressed even after the laminate is bent.
[0099] In one embodiment of the carbon-containing silicon oxide vapor-deposited film, the oxygen ratio O is preferably higher than the carbon ratio C, and the silicon ratio Si is preferably lower than the carbon ratio C. The oxygen ratio O is preferably higher than the silicon ratio Si, that is, the ratios are preferably in the order of O, C, and Si. This makes it possible to further suppress the deterioration of the gas barrier properties even after the laminate is bent.
[0100] The proportions C, Si, and O in the carbon-containing silicon oxide vapor-deposited film can be measured by narrow scan analysis using X-ray photoelectron spectroscopy (XPS) under the following measurement conditions. (Measurement conditions) Equipment used: "ESCA-3400" (manufactured by Kratos) [1] Spectral collection conditions Incident X-ray: MgKα (monochromatic X-ray, hν=1253.6eV) X-ray output: 150W (10kV 15mA) X-ray scanning area (measurement area): Approx. 6 mm φ Photoelectron capture angle: 90 degrees [2] Ion sputtering conditions Ion species: Ar + Acceleration voltage: 0.2 (kV) Emission current: 20 (mA) Etching range: 10mmφ Ion sputtering time: 30 seconds, spectrum collected
[0101] (Barrier coat layer) In one embodiment of the present invention, a barrier coat layer may be provided on the vapor-deposited film. By forming a barrier coat layer on the surface of the vapor-deposited film, the oxygen barrier property and water vapor barrier property of the laminate are further improved.
[0102] In one embodiment, the barrier coat layer contains a gas barrier resin such as an ethylene-vinyl alcohol copolymer (EVOH), polyvinyl alcohol (PVA), polyacrylonitrile, polyamides such as nylon 6, nylon 6,6, and polymetaxylylene adipamide (MXD6), polyester, polyurethane, and (meth)acrylic resin. Among these, polyvinyl alcohol is preferred from the viewpoints of oxygen barrier property and water vapor barrier property. Furthermore, by including polyvinyl alcohol in the barrier coat layer, the occurrence of cracks in the vapor-deposited film can be effectively prevented.
[0103] The content of the gas barrier resin in the barrier coat layer is preferably 50% by mass or more, more preferably 75% by mass or more. By making the content of the gas barrier resin in the barrier coat layer 50% by mass or more, the oxygen barrier property and the water vapor barrier property can be further improved. The content of the gas barrier resin in the barrier coat layer is preferably 95% by mass or less, more preferably 90% by mass or less.
[0104] The barrier coat layer may contain additives such as those exemplified in the description of the first substrate, as long as the additives do not impair the characteristics of the present invention.
[0105] The thickness of the barrier coat layer is preferably 0.01 μm or more, more preferably 0.1 μm or more. The thickness of the barrier coat layer is preferably 10 μm or less, more preferably 5 μm or less. By making the thickness of the barrier coat layer 0.01 μm or more, the oxygen barrier property and water vapor barrier property of the laminate can be further improved. On the other hand, by making the thickness of the barrier coat layer 10 μm or less, the processability of the laminate can be improved. In addition, as long as the thickness of the barrier coat layer is within the above range, recycling suitability is not impaired even when a different material other than polypropylene is used.
[0106] The barrier coat layer can be formed by dissolving or dispersing the gas barrier resin in water or a suitable solvent, applying the solution, and drying the solution. Alternatively, the barrier coat layer can be formed by applying a commercially available barrier coat agent and drying the solution.
[0107] In another embodiment, the barrier coat layer is a gas barrier coating film containing at least one resin composition such as a hydrolysate of a metal alkoxide or a hydrolysis condensate of a metal alkoxide obtained by polycondensing a mixture of a metal alkoxide and a water-soluble polymer by a sol-gel method in the presence of a sol-gel catalyst, water, an organic solvent, etc. In one embodiment, the gas barrier coating film is a gas barrier coating film of a mixture of a metal alkoxide and a water-soluble polymer, or a gas barrier coating film of a mixture of a metal alkoxide, a water-soluble polymer, and a silane coupling agent. By providing such a barrier coat layer on the vapor-deposited film, the occurrence of cracks in the vapor-deposited film can be effectively prevented.
[0108] In one embodiment, the metal alkoxide is represented by the following general formula: R 1 n M(OR 2 ) m (In the formula, R 1 , R 2 each represents an organic group having 1 to 8 carbon atoms, M represents a metal atom, n represents an integer of 0 or more, m represents an integer of 1 or more, and n+m represents the atomic valence of M.
[0109] As the metal atom M, for example, silicon, zirconium, titanium, aluminum, etc. can be used. R 1 and R 2 Examples of the organic group represented by the formula (I) include alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, and an i-butyl group.
[0110] Examples of metal alkoxides satisfying the above general formula include tetramethoxysilane (Si(OCH3)4), tetraethoxysilane (Si(OC2H5)4), tetrapropoxysilane (Si(OC3H7)4), and tetrabutoxysilane (Si(OC4H9)4).
[0111] It is preferable to use a silane coupling agent together with the metal alkoxide. As the silane coupling agent, known organic reactive group-containing organoalkoxysilanes can be used, and in particular, organoalkoxysilanes having epoxy groups are preferred. As organoalkoxysilanes having epoxy groups, for example, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane can be mentioned.
[0112] Two or more of the above silane coupling agents may be used, and the silane coupling agent is preferably used in an amount within the range of about 1 to 20 parts by mass per 100 parts by mass of the total amount of the above metal alkoxides.
[0113] As the water-soluble polymer, polyvinyl alcohol and an ethylene-vinyl alcohol copolymer are preferred, and from the viewpoints of oxygen barrier properties, water vapor barrier properties, water resistance and weather resistance, it is preferred to use these in combination.
[0114] The content of the water-soluble polymer in the gas barrier coating film is preferably 5 parts by mass or more and 500 parts by mass or less per 100 parts by mass of the metal alkoxide. By making the content of the water-soluble polymer in the gas barrier coating film 5 parts by mass or more per 100 parts by mass of the metal alkoxide, the oxygen barrier property and water vapor barrier property of the laminate can be further improved. Also, by making the content of the water-soluble polymer in the gas barrier coating film 500 parts by mass or less per 100 parts by mass of the metal alkoxide, the film formability of the gas barrier coating film can be improved.
[0115] In the gas barrier coating film, the ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) is preferably 4.5 or less, more preferably 3.5 or less, by mass. The ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) is preferably 1.0 or more, more preferably 1.7 or more, by mass. By setting the ratio of metal alkoxide to water-soluble polymer to be 4.5 or less, it is possible to suppress the deterioration of the gas barrier property even after the laminate is bent. By setting the ratio of metal alkoxide to water-soluble polymer to be 1.0 or more, the heat resistance of the laminate can be improved, and the deterioration of the gas barrier property can be suppressed even after the laminate is subjected to retort treatment and boiling treatment. The above ratio is a solid content ratio.
[0116] In the surface of the gas barrier coating film, the ratio of silicon atoms to carbon atoms (Si / C) measured by X-ray photoelectron spectroscopy (XPS) is preferably 1.60 or less, more preferably 1.35 or less, and preferably 0.50 or more, more preferably 0.90 or more. By setting the ratio of silicon atoms to carbon atoms to be 1.60 or less, it is possible to suppress the deterioration of the gas barrier properties even after the laminate is bent. By setting the ratio of silicon atoms to carbon atoms to be 0.50 or more, the heat resistance of the laminate can be improved, and the deterioration of the gas barrier properties of the laminate can be suppressed even after the laminate is subjected to retort treatment and boiling treatment. The above range of the ratio of silicon atoms to carbon atoms can be achieved by appropriately adjusting the ratio of the metal alkoxide to the water-soluble polymer. In this specification, the ratio of silicon atoms to carbon atoms is based on moles.
[0117] The ratio of silicon atoms to carbon atoms by X-ray photoelectron spectroscopy (XPS) can be measured by narrow scan analysis under the following measurement conditions. (Measurement conditions) Equipment used: "ESCA-3400" (manufactured by Kratos) [1] Spectral collection conditions Incident X-ray: MgKα (monochromatic X-ray, hν=1253.6eV) X-ray output: 150W (10kV 15mA) X-ray scanning area (measurement area): Approx. 6 mm φ Photoelectron capture angle: 90 degrees [2] Ion sputtering conditions Ion species: Ar + Acceleration voltage: 0.2 (kV) Emission current: 20 (mA) Etching range: 10mmφ Ion sputtering time: 30 seconds + 30 seconds + 60 seconds (total 120 seconds) and a spectrum was collected.
[0118] The thickness of the gas barrier coating film is preferably 0.01 μm or more, more preferably 0.1 μm or more. The thickness of the gas barrier coating film is preferably 100 μm or less, more preferably 50 μm or less. This makes it possible to further improve the oxygen barrier property and water vapor barrier property while maintaining recyclability. By making the thickness of the gas barrier coating film 0.01 μm or more, the oxygen barrier property and water vapor barrier property of the laminate can be improved, and the occurrence of cracks in the vapor-deposited film can be prevented. By setting the thickness of the gas barrier coating film to 100 μm or less, the recyclability of a packaging container produced using the laminate of the present invention and a sealant layer made of polypropylene can be improved.
[0119] The gas barrier coating film can be formed by applying a composition containing the above-mentioned materials by a conventionally known means such as roll coating using a gravure roll coater or the like, spray coating, spin coating, dipping, brushing, bar coding, or an applicator, and then polycondensing the composition by a sol-gel method. As the sol-gel catalyst, an acid or an amine compound is preferable. As the amine compound, a tertiary amine that is substantially insoluble in water and soluble in an organic solvent is preferable, and examples thereof include N,N-dimethylbenzylamine, tripropylamine, tributylamine, and tripentylamine. Among these, N,N-dimethylbenzylamine is preferable. The sol-gel catalyst is preferably used in the range of 0.01 to 1.0 part by mass, and more preferably 0.03 to 0.3 part by mass, per 100 parts by mass of the metal alkoxide. By using a sol-gel catalyst in an amount of 0.01 part by mass or more per 100 parts by mass of the metal alkoxide, the catalytic effect can be improved, and by using a sol-gel catalyst in an amount of 1.0 part by mass or less per 100 parts by mass of the metal alkoxide, the thickness of the gas barrier coating film formed can be made uniform.
[0120] The composition may further contain an acid, which is used as a catalyst in the sol-gel process, mainly for hydrolysis of metal alkoxides, silane coupling agents, and the like. Examples of acids that can be used include mineral acids such as sulfuric acid, hydrochloric acid, and nitric acid, and organic acids such as acetic acid, tartaric acid, etc. The amount of acid used is preferably 0.001 mol or more and 0.05 mol or less based on the total molar amount of the metal alkoxide and the alkoxide portion (e.g., silicate portion) of the silane coupling agent. The catalytic effect can be improved by using an acid in an amount of 0.001 mole or more relative to the total molar amount of the metal alkoxide and the alkoxide portion (e.g., silicate portion) of the silane coupling agent. The thickness of the gas barrier coating film formed can be made uniform by using an acid in an amount of 0.05 mole or less relative to the total molar amount of the metal alkoxide and the alkoxide portion (e.g., silicate portion) of the silane coupling agent.
[0121] The composition preferably contains water in an amount of 0.1 to 100 moles, more preferably 0.8 to 2 moles, per mole of the total molar amount of the metal alkoxides. By controlling the water content to 0.1 moles or more per mole of the total molar amount of the metal alkoxides, the oxygen barrier property and water vapor barrier property of the laminate of the present invention can be improved. Also, by controlling the water content to 100 moles or more per mole of the total molar amount of the alkoxides, the hydrolysis reaction can be carried out quickly.
[0122] The composition may contain an organic solvent, such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, or n-butanol.
[0123] Hereinafter, one embodiment of the method for forming a gas barrier coating film will be described.
[0124] First, a composition is prepared by mixing a metal alkoxide, a water-soluble polymer, a sol-gel catalyst, water, an organic solvent, and optionally a silane coupling agent, etc. In the composition, a polycondensation reaction gradually proceeds. Next, the composition is applied onto the vapor-deposited film by the above-mentioned conventionally known method and dried. This drying process further advances the polycondensation reaction between the metal alkoxide and the water-soluble polymer (and the silane coupling agent, if the composition contains a silane coupling agent) to form a composite polymer layer. Finally, the composition is heated at a temperature of 20° C. to 250° C., preferably 50° C. to 220° C., for 1 second to 10 minutes to form a gas barrier coating film.
[0125] A printed layer may be formed on the surface of the barrier coat layer. The method for forming the printed layer is as described above.
[0126] (Sealant layer) The sealant layer contains a polyolefin having a melting point of 110°C or more. This improves the heat resistance of the laminate. In addition, a packaging container produced using the laminate has heat resistance. The polyolefin is not particularly limited as long as it has a melting point of 110°C or more, and examples thereof include polyethylene and polypropylene. In this specification, "polyolefin having a melting point of 110°C or higher" means a polyolefin having a maximum peak temperature of 110°C or higher in DSC.
[0127] The sealant layer preferably comprises a sealant material having a melting point of 150° C. or greater. Packaging containers such as pouches for retort or boiling are filled with contents and then subjected to retort or boiling treatment, which may result in a decrease in gas barrier properties and heat sealability. By including a sealant material having a melting point of 150°C or higher in the sealant layer, a packaging container made using a laminate having the sealant layer can effectively suppress the decrease in gas barrier properties and heat sealability even during heat treatment such as retort or boiling (suitability for retort treatment, suitability for boiling treatment). Retort processing is a process in which the contents are filled into a retort pouch, sealed, and then the retort pouch is heated under pressure using steam or heated water. Retort processing is performed, for example, at 121°C for 3 minutes. Boiling processing is performed, for example, at 90°C for 3 minutes.
[0128] Conventionally, a laminate in which a substrate and a sealant layer are made of different resin materials has been used to manufacture a packaging container. However, since it is difficult to separate the substrate and the sealant layer after collecting used packaging containers, the current situation is that the laminate has not been actively recycled. By forming the first substrate and the sealant layer from the same material, it is not necessary to separate the first substrate and the sealant layer, and the recyclability can be improved. That is, from the viewpoint of the recyclability of the packaging container produced using the laminate, it is preferable that the sealant layer contains polypropylene having a melting point of 150° C. or more. Furthermore, when the sealant layer contains the polypropylene, the oil resistance of a packaging container produced using the laminate can be improved. The polypropylene may be any of a homopolymer, a random copolymer and a block copolymer. Among these, from the viewpoint of suitability for retort treatment and boiling treatment, a block copolymer is preferred. In addition, the use of the block copolymer can improve the impact resistance of packaging containers such as retort or boiling pouches produced using the laminate of the present invention, i.e., packaging containers such as retort or boiling pouches produced using the laminate of the present invention can be prevented from breaking due to impact when dropped, etc. As the block copolymer, for example, a propylene-ethylene block copolymer can be used.
[0129] "Propylene-ethylene block copolymer" refers to a polymer having the structural formula shown in formula (1) below: In formula (1), m1, m2, and m3 each represent an integer of 1 or greater.
[0130] [ka]
[0131] "Propylene-ethylene random copolymer" refers to a polymer having the structural formula shown in formula (2) below: In formula (2), m and n each represent an integer of 1 or more.
[0132] [ka]
[0133] As long as the characteristics of the present invention are not impaired, the sealant layer may contain a sealant material other than polypropylene, for example, polyethylene. This allows the sealant layer to have an island-in-a-sea structure. The "island-in-a-sea structure" here means a structure in which polyethylene is discontinuously dispersed within a region in which polypropylene is continuous. When the sealant layer contains a sealant material other than polypropylene, the sealant layer is not limited to one having an island-in-sea structure, and may be one in which two materials are in a compatible state.
[0134] The sealant layer may contain the above-mentioned heat seal modifiers and additives, provided that the properties of the present invention are not impaired.
[0135] The sealant layer may have a single-layer structure or a multi-layer structure.
[0136] The thickness of the sealant layer is preferably 15 μm or more, more preferably 20 μm or more, and is preferably 100 μm or less, more preferably 70 μm or less. By making the thickness of the sealant layer 15 μm or more, the laminate strength, retort treatment suitability, and boiling treatment suitability of a packaging container including the laminate of the present invention can be further improved. Moreover, by setting the thickness of the sealant layer to 100 μm or less, the processability of the laminate of the present invention can be further improved.
[0137] The sealant layer may be formed by laminating a heat-sealable stretched or unstretched film via a conventionally known adhesive, or by applying and drying a heat-sealing agent. The term "unstretched film" is a concept that includes not only a film that is not stretched at all, but also a film that is slightly stretched due to the tension applied during film formation.
[0138] (adhesive layer) The adhesive layer contains at least one adhesive, and may be a one-component curing type, a two-component curing type, or a non-curing type adhesive. The adhesive may be a solvent-free adhesive or a solvent-based adhesive, but from the viewpoint of environmental load, a solvent-free adhesive is preferably used. Examples of solventless adhesives include polyether adhesives, polyester adhesives, silicone adhesives, epoxy adhesives, and urethane adhesives, and among these, two-liquid curing urethane adhesives are preferably used. Examples of the solvent-based adhesive include rubber-based adhesives, vinyl-based adhesives, silicone-based adhesives, epoxy-based adhesives, phenol-based adhesives, and olefin-based adhesives.
[0139] The thickness of the adhesive layer is not particularly limited, and can be, for example, 0.1 μm or more and 10 μm or less.
[0140] (Second base material) The second substrate serves to hold each layer. The second substrate contains a resin material, such as polyolefin, vinyl resin, polyester, (meth)acrylic resin, cellulose resin, etc. Among these, polypropylene is particularly preferred from the viewpoint of the recyclability of the laminate.
[0141] The second substrate may contain additives similar to those described above, provided that the additives do not impair the characteristics of the present invention.
[0142] The second base material may have the above-mentioned vapor deposition film or barrier coat layer on its surface.
[0143] The second base material is preferably a resin film made of the above-mentioned resin material, and the resin film is preferably one that has been subjected to a stretching treatment. The stretching treatment may be uniaxial stretching or biaxial stretching.
[0144] In the embodiment in which the second substrate is provided, it is particularly preferable from the viewpoint of recyclability that the second substrate be formed from a stretched polypropylene resin film.
[0145] The thickness of the second substrate is preferably 10 μm or more, and more preferably 50 μm or less, and more preferably 40 μm or less. By setting the thickness of the second base material to 10 μm or more, the strength of the laminate can be further improved. Moreover, by setting the thickness of the second base material to 50 μm or less, the processability of the laminate can be further improved.
[0146] The second substrate can be provided via the above-mentioned adhesive layer.
[0147] The second base material may have a printed layer formed on its surface. The method for forming the printed layer is as described above.
[0148] (Middle class) In one embodiment, the laminate may have an intermediate layer between the vapor deposition film and the sealant layer (between the barrier coat layer and the sealant layer when a barrier coat layer is provided). The intermediate layer contains a resin material, such as polyolefin, vinyl resin, polyester, (meth)acrylic resin, cellulose resin, etc. Among these, polypropylene is particularly preferred from the viewpoint of the recyclability of the laminate.
[0149] The intermediate layer may contain additives similar to those described above, provided that the additives do not impair the characteristics of the present invention.
[0150] The intermediate layer may have the above-mentioned vapor deposition film or barrier coat layer on its surface.
[0151] The intermediate layer is preferably made of a resin film made of the above-mentioned resin material, and the resin film is preferably subjected to a stretching treatment.
[0152] In the embodiment having an intermediate layer, it is particularly preferred to use a stretched polypropylene resin film as the intermediate layer. When a stretched polypropylene resin film is used for the intermediate layer, the ease of tearing can be improved compared to when no stretched film is used. This is because when no stretched film is used for the intermediate layer, the film constituting the heat seal layer is unstretched and therefore flexible and easily stretched, which is thought to result in poor ease of tearing related to film residue and difficulty in opening when opening. In addition, wrinkles that may occur due to thermal shrinkage during retort treatment, boiling treatment, or heating during heat sealing can be reduced, and the appearance can be improved. Furthermore, when the laminate is used as a lid material, the occurrence of wrinkles after heat sealing can be prevented, and the appearance can be improved.
[0153] The thickness of the intermediate layer is preferably 10 μm or more, and more preferably 50 μm or less, and more preferably 40 μm or less. By making the thickness of the intermediate layer 10 μm or more, the strength of the laminate can be further improved. Moreover, by setting the thickness of the intermediate layer to 50 μm or less, the processability of the laminate can be further improved.
[0154] The intermediate layer can be provided via the above-mentioned adhesive layer.
[0155] The intermediate layer may have a printed layer formed on its surface. The method for forming the printed layer is as described above.
[0156] In one embodiment, the intermediate layer may be the second substrate.
[0157] [Laminate in the second embodiment] As shown in FIG. 18, the laminate 10B of the present invention includes a first substrate 11, a vapor-deposited film 12, and a sealant layer 13. The first substrate 11 includes at least a polypropylene resin layer 14 and a surface coat layer 15. In one embodiment of the present invention, the laminate 10 may further include a barrier coat layer 16 between the vapor-deposited film 12 and the sealant layer 13, as shown in FIG. In one embodiment of the present invention, the laminate may further include a second substrate. When the laminate includes a second substrate, the laminate 10 may include a second substrate 17, a deposition film 12, a first substrate 11, and a sealant layer 13 in this order as shown in FIG. 20, may include a second substrate 17, a first substrate 11, a deposition film 12, and a sealant layer 13 in this order as shown in FIG. 21, or may include a first substrate 11, a deposition film 12, a second substrate 17, and a sealant layer 13 in this order as shown in FIG. 22. The second substrate 17 in the laminate 10 of FIG. 20 and FIG. 21 and the first substrate 11 in the laminate 10 of FIG. 22 may be located in the outermost layer of the laminate 10. In one embodiment of the present invention, the laminate 10 may include an adhesive layer (not shown) between any of the vapor-deposited film, the sealant layer, the first substrate, and the second substrate. In another embodiment, the laminate of the present invention may include an intermediate layer between the vapor-deposited film and the sealant layer, and the intermediate layer may be the second substrate.
[0158] The haze value of the laminate is preferably 20% or less, and more preferably 5% or less, which can improve the transparency of the laminate.
[0159] In the laminate in the second embodiment, the laminate strength between the first substrate and the vapor-deposited film is preferably 3 N or more, more preferably 4 N or more, and even more preferably 5.5 N or more, per 15 mm width. The upper limit of the laminate strength in the laminate in the second embodiment may be 20 N or less. The method for measuring the laminate strength of the laminate will be described later in the Examples.
[0160] The tensile strength of the laminate in one direction may be 30 MPa or more, or 35 MPa or more. The tensile strength of the laminate in one direction may be 70 MPa or less, or 50 MPa or less. The one direction of the laminate may be the machine direction (MD direction). The tensile strength of the laminate in a direction perpendicular to the one direction may be 40 MPa or more, or 60 MPa or more. The tensile strength of the laminate in a direction perpendicular to the one direction may be 150 MPa or less, or 100 MPa or less. The direction perpendicular to the one direction may be the transverse direction (TD) of the laminate. In this specification, the tensile strength of the laminate is measured in accordance with JIS K7127: 1999. As a measuring device, a tensile tester STA-1150 manufactured by Orientec Co., Ltd. can be used. The test piece may be a rectangular laminate cut out from the laminate with a width of 10 mm and a length of 150 mm. The distance between the pair of chucks holding the test piece at the start of the measurement is 50 mm, and the tensile speed is 300 mm / min. In this specification, unless otherwise specified, the environment during the measurement of the tensile strength is a temperature of 23°C and a relative humidity of 50%.
[0161] The loop stiffness in one direction of the laminate may be 30 mN or more, 50 mN or more, or 70 mN or more. The loop stiffness in one direction of the laminate may be 200 mN or less, 150 mN or less, or 120 mN or less. The one direction of the laminate may be the machine direction (MD direction). The loop stiffness of the laminate in a direction perpendicular to the one direction may be 30 mN or more, 50 mN or more, or 70 mN or more. The loop stiffness of the laminate in a direction perpendicular to the one direction may be 200 mN or less, 150 mN or less, or 130 mN or less. The direction perpendicular to the one direction may be the transverse direction (TD) of the laminate. The method for measuring the loop stiffness is as explained in the first embodiment.
[0162] The piercing strength of the laminate may be 10N or more, or 15N or more. The puncture strength of the laminate is measured in accordance with JIS Z1707 7.4. A specific measurement method will be described in the examples below.
[0163] As in the first embodiment, the sealant layer is preferably made of the same material as the polypropylene resin layer of the first base material, i.e., polypropylene, which can improve the recyclability of the packaging container produced using the laminate of the present invention.
[0164] When the sealant layer is made of polypropylene, the content of polypropylene in the total amount of resin materials contained in the laminate of the present invention is preferably 80% by mass or more, and more preferably 95% by mass or more, which can further improve the recyclability of packaging containers produced using the laminate of the present invention.
[0165] Hereinafter, the laminate in the second aspect of the present invention will be described. However, since the layers other than the surface coating layer constituting the first substrate are the same as those in the laminate in the first aspect described above, a description thereof will be omitted here.
[0166] (Surface coating layer) The first base material has a surface coating layer containing a resin material having a polar group on a polypropylene resin layer, which allows a highly adhesive vapor-deposited film to be formed on the surface coating layer, thereby improving the gas barrier properties. In addition, as described below, a packaging container produced using a laminate having the surface coating layer has high laminate strength. In one embodiment, the surface coating layer may be provided on the polypropylene resin layer, i.e., the surface coating layer may be adjacent to the polypropylene resin layer.
[0167] The surface coating layer includes a resin material having a polar group. In the present invention, the polar group refers to a group containing one or more heteroatoms. Examples of the polar group include an ester group, an epoxy group, a hydroxyl group, an amino group, an amide group, a carboxyl group, a carbonyl group, a carboxylic anhydride group, a sulfone group, a thiol group, and a halogen group. Among these, from the viewpoint of lamination of the packaging container, a carboxyl group, a carbonyl group, an ester group, a hydroxyl group, and an amino group are preferred, and a carboxyl group and a hydroxyl group are more preferred.
[0168] As the resin material having a polar group, polyester, polyethyleneimine, hydroxyl group-containing (meth)acrylic resin, polyamide such as nylon 6, nylon 6,6, MXD nylon, amorphous nylon, polyurethane, etc. are preferable. By using such a resin material, the adhesion of the evaporated film formed on the surface coating layer can be significantly improved, and the gas barrier properties of the film can be effectively improved.
[0169] In one embodiment, the resin material having a polar group is preferably a hydroxyl group-containing (meth)acrylic resin. This can improve the heat resistance of the laminate. In addition, even after the laminate is subjected to a retort treatment and a boiling treatment, the deterioration of the gas barrier property can be suppressed.
[0170] In one embodiment of the present invention, the hydroxyl group-containing (meth)acrylic resin used to form the surface coating layer is a polymer of a neutral monomer and a hydroxyl group-containing (meth)acrylic monomer. Examples of neutral monomers include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, styrene, vinyl toluene, and vinyl acetate. Examples of hydroxyl group-containing (meth)acrylic monomers include 2-hydroxyethyl (meth)acrylate and hydroxypropyl (meth)acrylate.
[0171] The glass transition temperature (Tg) of the hydroxyl group-containing (meth)acrylic resin is preferably 50° C. or higher, and more preferably 70° C. or higher. The glass transition temperature (Tg) of the hydroxyl group-containing (meth)acrylic resin is preferably 200° C. or lower, and more preferably 150° C. or lower. By adjusting the glass transition temperature (Tg) of the hydroxyl group-containing (meth)acrylic resin to 50° C. or higher, blocking resistance can be improved. By setting the glass transition temperature (Tg) of the hydroxyl group-containing (meth)acrylic resin to 200°C or lower, the reactivity of an isocyanate compound can be improved when the hydroxyl group-containing (meth)acrylic resin is used together with an isocyanate compound to form a surface coating layer. In this specification, Tg can be measured in accordance with JIS K7121:2012 (Method for measuring transition temperature of plastics). Specifically, Tg can be determined by measuring a DSC curve at a heating rate of 10° C. / min using a differential scanning calorimetry (DSC) device.
[0172] The number average molecular weight of the hydroxyl group-containing (meth)acrylic resin is preferably 10,000 or more. The number average molecular weight of the hydroxyl group-containing (meth)acrylic resin is preferably 100,000 or less. By adjusting the number average molecular weight of the hydroxyl group-containing (meth)acrylic resin to 10,000 or more, blocking resistance can be improved. By adjusting the number average molecular weight of the hydroxyl group-containing (meth)acrylic resin to 100,000 or more, the ease of forming the surface coating layer can be improved. In this specification, the number average molecular weight can be measured by gel permeation chromatography (GPC). In GPC measurement, the number average molecular weight of a polymer is generally measured in terms of standard polystyrene.
[0173] The hydroxyl value of the hydroxyl-containing (meth)acrylic resin is preferably 20 mg KOHL / g or more, more preferably 30 mg KOHL / g or more, and is preferably 200 mg KOHL / g or less, more preferably 150 mg KOHL / g or less. By making the hydroxyl value of the hydroxyl-containing (meth)acrylic resin 20 mg KOHL / g or more, the reactivity of an isocyanate compound when used together with the hydroxyl-containing (meth)acrylic resin to form a surface coating layer can be improved. By setting the hydroxyl value of the hydroxyl-containing (meth)acrylic resin to 200 mg KOHL / g or less, the amount of isocyanate compound used can be reduced, leading to reduced production costs. In this specification, the hydroxylation can be measured in accordance with JIS K0070:1992 (Test methods for oxidation, saponification value, ester value, iodine value, hydroxyl value and unsaponifiable matter of chemical products).
[0174] In the present invention, the surface coating layer can be formed using a water-based emulsion or a solvent-based emulsion. Specific examples of the water-based emulsion include a polyamide-based emulsion, a polyethylene-based emulsion, and a polyurethane-based emulsion. Specific examples of the solvent-based emulsion include a polyester-based emulsion.
[0175] The content of the resin material having a polar group in the surface coating layer is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.
[0176] As long as the characteristics of the present invention are not impaired, the surface coating layer may contain a resin material other than the resin material having a polar group. In one embodiment of the present invention, the surface coating layer may contain an isocyanate compound. The surface coating layer may contain additives, such as crosslinking agents, antioxidants, antiblocking agents, slip agents, UV absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, and modifying resins, as long as the additives do not impair the properties of the present invention.
[0177] The ratio of the thickness of the surface coating layer to the total thickness of the first substrate is preferably 0.08% or more, more preferably 0.2% or more, even more preferably 1% or more, and even more preferably 3% or more. The ratio of the thickness of the surface coating layer to the total thickness of the first substrate is preferably 20% or less, and more preferably 10% or less. By setting the ratio of the thickness of the surface coating layer to the total thickness of the first base material to be 0.08% or more, the adhesion of the vapor-deposited film can be further improved, the gas barrier property can be further improved, and the laminate strength of the packaging container can be further improved. By setting the ratio of the thickness of the surface coating layer to the total thickness of the first substrate to 20% or less, the film-forming property and processability of the first substrate can be further improved. In addition, as described later, the recyclability of a packaging container produced using the laminate of the present invention and a sealant layer made of polypropylene can be improved.
[0178] The thickness of the surface coating layer is preferably 0.02 μm or more, more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and even more preferably 0.2 μm or more. The thickness of the surface coating layer is preferably 10 μm or less, and more preferably 5 μm or less. By making the thickness of the surface coating layer 0.02 μm or more, the adhesion of the evaporated film can be improved, the gas barrier property can be improved, and the laminate strength of the packaging container can be improved. By setting the thickness of the surface coating layer to 10 μm or less, the film-forming property and processing suitability of the first substrate can be further improved. In addition, as described later, the recyclability of a packaging container produced using the laminate of the present invention and a sealant layer made of polypropylene can be improved.
[0179] The first substrate can be produced offline. Specifically, a resin composition containing polypropylene is formed into a film using a T-die method, an inflation method, or the like, and then the film is stretched, and a coating liquid for forming a coat is applied onto the resin film, followed by drying. The first substrate can be manufactured in-line. Specifically, a resin composition containing polypropylene is formed into a film using a T-die method or an inflation method, and then stretched in the machine direction (MD direction), a coating liquid for forming a coat is applied to the resin film, dried, and then stretched in the transverse direction (TD direction). Stretching in the transverse direction may be performed first. Stretching in both the machine direction and the transverse direction may be performed before or after applying the coating liquid for forming a coat.
[0180] [Packaging container] The packaging container of the present invention is characterized by comprising the laminate. Examples of the packaging container include packaging products (packaging bags), lids, and laminate tubes. In the present invention, since the laminate is particularly excellent in suitability for retort treatment and boiling treatment, the packaging container is preferably a retort pouch or a boiling pouch among packaging bags.
[0181] Examples of packaging bags include packaging bags of various shapes, such as standing pouch type, side seal type, two-sided seal type, three-sided seal type, four-sided seal type, envelope seal type, grommet seal type (pillow seal type), pleated seal type, flat bottom seal type, square bottom seal type, and gusset type.
[0182] The retort or boiling pouch, which is a preferred embodiment of the present invention, will now be described.
[0183] The retort or boiling pouch 30 of the present invention is formed by bonding two laminates together (the shaded areas are heat-sealed areas) as shown in Fig. 23. After the contents are filled into the non-heat-sealed side of this retort or boiling pouch 30, this side is also heat-sealed. When the tensile strength of the first substrate in the longitudinal direction (MD direction) is greater than the tensile strength in the transverse direction (TD direction), it is preferable to fabricate the packaging bag so that the longitudinal direction (MD direction) of the first substrate corresponds to the transverse direction of the retort or boiling pouch 30, and the transverse direction (TD direction) of the first substrate corresponds to the longitudinal direction of the retort or boiling pouch 30. This configuration makes it extremely easy to tear the packaging container in the transverse direction. The same applies to the packaging containers exemplified below.
[0184] The retort or boiling pouch shown in FIG. 24 is a standing type retort or boiling pouch 40. As shown in FIG. 24, a standing type retort or boiling pouch 40 is composed of a body portion (side sheets) 41 and a bottom portion (bottom sheet) 42. At least one of the side sheet 41 and the bottom sheet 42 of the standing type retort or boiling pouch 40 is made of the laminate of the present invention.
[0185] In one embodiment, the body 41 of the standing retort or boiling pouch 40 can be formed by bag making so that the sealant layer of the laminate of the present invention becomes the innermost layer. In another embodiment, the side sheet 41 can be formed by preparing two sheets of the laminate of the present invention, overlapping them with the sealant layers facing each other, inserting two sheets of laminate folded in a V shape into both ends of the overlapped laminate so that the sealant layers are on the outside, and heat sealing them. According to such a production method, a stand-type retort or boiling pouch having a body with side gussets can be made.
[0186] In one embodiment, the bottom sheet 42 of the standing retort or boiling pouch 40 can be formed by inserting the laminate of the present invention between pre-formed side sheets and heat sealing it. More specifically, the laminate can be folded in a V-shape with the sealant layer facing outward, inserted between pre-formed side sheets and heat sealing it.
[0187] The packaging container may also be provided with easy-opening means 51 as shown in FIGS. As shown in FIG. 23, examples of the easy-to-open means 51 include a notch 52 which serves as a starting point for tearing, and a half-cut line 53 formed by laser processing or a cutter as a path for tearing.
[0188] The heat sealing can be performed by a known method such as bar sealing, rotary roll sealing, belt sealing, impulse sealing, high frequency sealing, ultrasonic sealing, etc.
[0189] The contents filled in the packaging container are not particularly limited and may be liquid, powder, or gel. The contents may be food or non-food.
[0190] <Other aspects> In another aspect, the present invention provides a laminate comprising: At least a first substrate, a vapor-deposited film, and a sealant layer are provided, The first base material includes a polypropylene resin layer and a surface resin layer provided on one surface of the polypropylene resin layer, the vapor-deposited film is provided on a surface resin layer of the first substrate, The first base material is subjected to a stretching treatment, The surface resin layer contains a resin material having a melting point of 180° C. or more, The vapor-deposited film is composed of an inorganic oxide, The sealant layer is a laminate comprising a polyolefin having a melting point of 110° C. or higher. In one embodiment, the surface resin layer is provided on the polypropylene resin layer. In one embodiment, the first base material includes an adhesive resin layer between the polypropylene resin layer and the surface resin layer, the adhesive resin layer is provided on the polypropylene resin layer, The surface resin layer is provided on the adhesive resin layer. In one embodiment, the surface resin layer includes a resin material having a melting point of 180° C. or more and 265° C. or less. In one embodiment, the resin material of the surface resin layer has a melting point TA, The polypropylene of the polypropylene resin layer has a melting point TB, The difference between the melting point TA and the melting point TB is 20°C or more and 80°C or less. In one embodiment, the resin material of the surface resin layer is made of a polymer having a polar group. In one embodiment, the resin material of the surface resin layer is one or more resin materials selected from nylon 6, nylon 6,6, MXD nylon, and amorphous nylon. In one embodiment, the ratio of a thickness of the surface resin layer to a total thickness of the first base material is 1% or more and 10% or less. In one embodiment, the first substrate is a co-extruded film. In another aspect, the present invention provides a laminate comprising: At least a first substrate, a vapor-deposited film, and a sealant layer are provided, The first base material includes a polypropylene resin layer and a surface coating layer provided on one surface of the polypropylene resin layer, the vapor-deposited film is provided on a surface coating layer of the first substrate, The first base material is subjected to a stretching treatment, the surface coating layer contains a resin material having a polar group, The vapor-deposited film is composed of an inorganic oxide, The sealant layer is a laminate comprising a polyolefin having a melting point of 110° C. or higher. In one embodiment, the resin material of the surface coating layer is one or more resin materials selected from polyester, polyethyleneimine, hydroxyl group-containing (meth)acrylic resin, nylon 6, nylon 6,6, MXD nylon, amorphous nylon, and polyurethane. In one embodiment, the surface coating layer is a layer formed using a water-based emulsion or a solvent-based emulsion. In one embodiment, the ratio of a thickness of the surface coating layer to a total thickness of the first base material is 0.08% or more and 20% or less. In one embodiment, the surface coating layer has a thickness of 0.02 μm or more and 10 μm or less. In one embodiment, the sealant layer comprises a sealant material having a melting point of 150° C. or greater. In one embodiment, the sealant layer comprises polypropylene having a melting point of 150° C. or greater. In one embodiment, the laminate further comprises a second substrate. In one embodiment, the second substrate comprises polypropylene. In one embodiment, the first substrate and the deposited film are located between the second substrate and the sealant layer. In one embodiment, the laminate further comprises an intermediate layer between the deposition film and the sealant layer, The intermediate layer is the second substrate. In one embodiment, the intermediate layer is made of a polypropylene resin film that has been subjected to a stretching treatment. In one embodiment, a barrier coat layer is further provided between the vapor deposition film and the sealant layer. In one embodiment, the barrier coat layer is a gas barrier coating film of a mixture of a metal alkoxide and a water-soluble polymer, or a gas barrier coating film of a mixture of a metal alkoxide, a water-soluble polymer, and a silane coupling agent. In one embodiment, the laminate is used in a packaging container. In another embodiment, the present invention is a pouch for retort or boiling, comprising the laminate. In one embodiment, the retort or boiling pouch includes a notch. In one embodiment, the retort or boiling pouch includes a half-cut line. EXAMPLES
[0191] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0192] Example 1 Polyamide (Ube Industries, Ltd., polyamide 6, melting point: 220 ° C.), adhesive resin (Mitsui Chemicals, Inc., Admer QF500, maleic anhydride modified polypropylene), and polypropylene (Japan Polypropylene, Novatec FL203D, melting point: 160 ° C.) were co-extruded, and then stretched 5 times in the machine direction (MD direction) and 10 times in the transverse direction (TD direction) by a sequential biaxial stretching device to produce a 21 μm thick substrate comprising a surface resin layer (0.4 μm) made of polyamide, an adhesive resin layer (1 μm) made of adhesive resin, and a polypropylene resin layer (19.6 μm) made of polypropylene. The ratio of the thickness of the surface resin layer made of polyamide to the layer thickness of the substrate was 2%.
[0193] On the surface resin layer of the substrate prepared as described above, a carbon-containing silicon oxide vapor deposition film having a thickness of 12 nm was formed by a roll-to-roll method using a low-temperature plasma chemical vapor deposition apparatus while applying tension to the substrate (CVD method). The vapor deposition film formation conditions were as follows: (Formation conditions) Hexamethyldisiloxane:oxygen gas:helium=1:10:10 (unit: slm) Cooling / electrode drum power supply: 22kw Line speed: 100m / min
[0194] In the carbon-containing silicon oxide vapor deposition film, the carbon percentage C, silicon percentage Si, and oxygen percentage O were 32.7%, 29.8%, and 37.5%, respectively, based on the total of the three elements silicon, oxygen, and carbon, which is 100%. The percentages of each element were measured by narrow scan analysis using X-ray photoelectron spectroscopy (XPS) under the following measurement conditions. (Measurement conditions) Equipment used: "ESCA-3400" (manufactured by Kratos) [1] Spectral collection conditions Incident X-ray: MgKα (monochromatic X-ray, hν=1253.6eV) X-ray output: 150W (10kV 15mA) X-ray scanning area (measurement area): Approx. 6 mm φ Photoelectron capture angle: 90 degrees [2] Ion sputtering conditions Ion species: Ar + Acceleration voltage: 0.2 (kV) Emission current: 20 (mA) Etching range: 10mmφ Ion sputtering time: 30 seconds, spectrum collected
[0195] 385g of water, 67g of isopropyl alcohol, and 9.1g of 0.5N hydrochloric acid were mixed to obtain a solution with a pH of 2.2. 175g of tetraethoxysilane as a metal alkoxide and 9.2g of glycidoxypropyltrimethoxysilane as a silane coupling agent were mixed into this solution while cooling to 10°C to obtain solution A. Solution B was obtained by mixing 14.7 g of polyvinyl alcohol having a saponification degree of 99% or more and a polymerization degree of 2400 as a water-soluble polymer, 324 g of water, and 17 g of isopropyl alcohol. Solution A and solution B were mixed in a ratio of 6.5:3.5 by mass to obtain a barrier coating agent.
[0196] The barrier coating agent was coated on the vapor-deposited film formed on the substrate by spin coating, and the coating was heated in an oven at 80° C. for 60 seconds to form a barrier coating layer with a thickness of 300 nm.
[0197] On the barrier coat layer formed as described above, a 70 μm-thick unstretched polypropylene film (ZK207, melting point 163° C., containing propylene-ethylene block copolymer, manufactured by Toray Film Processing Co., Ltd.) was dry laminated as a sealant layer via a polyurethane adhesive (Takelac A-969V / Takenate A-5 (mixing ratio 3 / 1), manufactured by Mitsui Chemicals, Inc.), and allowed to stand at 40° C. for 24 hours to obtain a laminate of the present invention. The thickness of the adhesive layer formed by the polyurethane adhesive was 1 μm. The polypropylene content in the laminate was 92% by mass.
[0198] Example 2 A solution for forming a surface coating layer having the following composition was applied to the corona-treated surface of a 20 μm-thick biaxially oriented polypropylene film (ME-1, manufactured by Mitsui Chemicals Tocello Co., Ltd.) with one side corona-treated, and then dried to form a surface coating layer with a thickness of 0.5 μm, thereby producing a substrate. (Preparation of solution for forming surface coating layer) A hydroxyl-containing (meth)acrylic resin (number average molecular weight 25,000, glass transition temperature 99°C, hydroxyl value 80 mg KOHL / g) was diluted with a mixed solvent of methyl ketone and ethyl acetate (mixing ratio 1:1) to a solid concentration of 10 mass% to prepare the base resin. A solution containing tolylene diisocyanate in ethyl acetate (solid content 75% by mass) was added to the base material as a curing agent to obtain a solution for forming a surface coating layer. The amount of the curing agent used was 10 parts by mass relative to 100 parts by mass of the base material.
[0199] On the surface coating layer of the substrate prepared as described above, a carbon-containing silicon oxide vapor deposition film having a thickness of 12 nm was formed by a roll-to-roll method using a low-temperature plasma chemical vapor deposition apparatus while applying tension to the substrate (CVD method). The vapor deposition film formation conditions were as follows. (Formation conditions) Hexamethyldisiloxane:oxygen gas:helium=1:10:10 (unit: slm) Cooling / electrode drum power supply: 22kw Line speed: 100m / min
[0200] The carbon ratio C, silicon ratio Si, and oxygen ratio O in the carbon-containing silicon oxide vapor-deposited film were measured in the same manner as in Example 1. The carbon ratio C, silicon ratio Si, and oxygen ratio O were 32.7%, 29.8%, and 37.5%, respectively, relative to the total of the three elements silicon, oxygen, and carbon, which was 100%.
[0201] 385g of water, 67g of isopropyl alcohol, and 9.1g of 0.5N hydrochloric acid were mixed to obtain a solution with a pH of 2.2. 175g of tetraethoxysilane as a metal alkoxide and 9.2g of glycidoxypropyltrimethoxysilane as a silane coupling agent were mixed into this solution while cooling to 10°C to obtain solution A. Solution B was obtained by mixing 14.7 g of polyvinyl alcohol having a saponification degree of 99% or more and a polymerization degree of 2400 as a water-soluble polymer, 324 g of water, and 17 g of isopropyl alcohol. Solution A and solution B were mixed in a ratio of 6.5:3.5 by mass to obtain a barrier coating agent.
[0202] The barrier coating agent was coated on the vapor-deposited film formed on the substrate by spin coating, and the coating was heated in an oven at 80° C. for 60 seconds to form a barrier coating layer with a thickness of 300 nm.
[0203] On the barrier coat layer formed as described above, a 70 μm-thick unstretched polypropylene film (ZK207, manufactured by Toray Film Processing Co., Ltd.) was dry laminated as a sealant layer via a polyurethane adhesive (Takelac A-969V / Takenate A-5 (mixture ratio 3 / 1), manufactured by Mitsui Chemicals, Inc.), and allowed to stand at 40° C. for 24 hours to obtain a laminate of the present invention. The thickness of the adhesive layer formed by the polyurethane adhesive was 1 μm. The polypropylene content in the laminate was 92% by mass.
[0204] Comparative Example 1 The above polypropylene (Novatec FL203D, manufactured by Japan Polypropylene Corporation, melting point: 160°C) was extruded and then stretched 5 times in the machine direction (MD) and 10 times in the transverse direction (TD) using a sequential biaxial stretching device to produce a propylene film with a thickness of 20 μm. A laminate was produced in the same manner as in Example 1, except that the substrate in Example 1 was changed to the polypropylene film produced as described above.
[0205] <<Gas barrier property evaluation>> The laminates obtained in the above examples and comparative examples were cut out to obtain test pieces. The test pieces were used to measure the oxygen permeability (cc / m 2 ·day·atm) and water vapor transmission rate (g / m 2 ·day) was measured by the following method, and the results are summarized in Table 1.
[0206] [Oxygen permeability] Using an oxygen permeability measuring device (OX-TRAN2 / 20 manufactured by MOCON), the test piece was set so that the substrate side was the oxygen supply side, and the oxygen permeability was measured in an environment of 23°C and a relative humidity of 90% RH in accordance with JIS K 7126. [Water vapor permeability] Using a water vapor transmission rate measuring device (MOCON, PERMATRAN-w 3 / 33), the substrate side of the test piece was set to be the water vapor supply side, and the water vapor transmission rate was measured in an environment of 40°C and a relative humidity of 90% RH in accordance with JIS K 7129.
[0207] <<Laminate strength test>> The laminates obtained in the above Examples and Comparative Examples were cut into strips of 15 mm width, and the laminate strength (N / 15 mm) of the samples was measured using a tensile tester (Tensilon universal material testing machine, manufactured by Orientec Co., Ltd.) in accordance with JIS K6854-2, at a peel speed of 50 mm / min and 90° peeling (T-peel method). Specifically, first, a laminate was cut out, and a strip-shaped test piece 70 was prepared by peeling the substrate side 71 and the sealant layer side 72 by 15 mm in the long side direction as shown in FIG. 25. Then, as shown in FIG. 26, the already peeled parts of the substrate side 71 and the sealant layer side 72 were gripped by the grips 73 of the measuring device. The grips 73 were pulled at a speed of 50 mm / min in opposite directions perpendicular to the surface direction of the part where the substrate side 71 and the sealant layer side 72 are still laminated, and the average value of the tensile stress in the stable region (see FIG. 27) was measured. The interval S between the grips 73 when the pulling started was 30 mm, and the interval S between the grips 73 when the pulling ended was 60 mm. FIG. 27 is a diagram showing the change in tensile stress with respect to the interval S between the grips 73. As shown in FIG. 27, the change in tensile stress with respect to the interval S passes through the first region and enters the second region (stable region) where the change rate is smaller than that in the first region. The average value of the tensile stress in the stable region was measured for the five test pieces 70, and the average value was determined as the laminate strength. The measurement was performed in an environment of a temperature of 23° C. and a relative humidity of 50%. The measurement results are summarized in Table 1.
[0208] <<Gas barrier property evaluation after retort treatment>> [Oxygen permeability] Two sheets of each of the laminates obtained in the above-mentioned Examples and Comparative Examples were prepared, placed face to face, and heat sealed at three sides to produce a retort pouch as shown in FIG. This retort pouch was filled with 100 mL of tap water, and the remaining side was heat sealed to form a retort pouch for filling with contents.
[0209] The retort pouch filled with the contents was subjected to a retort treatment at 121°C for 30 minutes at 2 atmospheres. Subsequently, after the retort treatment, the retort pouch filled with the contents was cut out to obtain a test piece.
[0210] Using an oxygen permeability measuring device (OX-TRAN10 / 50A manufactured by MOCON), the test piece was set so that the substrate side was the oxygen supply side, and the oxygen permeability was measured in an environment of 30°C and relative humidity of 70% RH in accordance with JIS K 7126. The measurement results are summarized in Table 1.
[0211] [Water vapor permeability] The water vapor transmission rate of the test piece after the retort treatment was measured using a water vapor transmission rate measuring device (PERMATRAN-w 3 / 33, manufactured by MOCON) in an environment of 40°C and relative humidity of 90% RH in accordance with JIS K 7129, with the test piece being set so that the substrate side was the water vapor supply side. The measurement results are summarized in Table 1.
[0212] <<Laminate strength after retort treatment>> After the retort treatment, the retort pouch filled with the contents was cut out and cut into strips of 15 mm width to obtain samples. In the same manner as above, the laminate strength (N / 15 mm) of this sample was measured using a tensile tester (Orientec Co., Ltd., Tensilon universal material testing machine) in accordance with JIS K6854-2 at a peel speed of 50 mm / min and 90° peel (T-shaped peel method). The measurement results are summarized in Table 1.
[0213] [Table 1]
[0214] Example 3-1 In the same manner as in Example 1, a substrate was prepared, and a vapor-deposited film was formed on the substrate.
[0215] A barrier coat layer was formed on the vapor deposition film such that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 5.1 on a mass basis.
[0216] The ratio of Si element to C element present on the barrier coat layer surface was measured. The measurement was performed by narrow scan analysis under the following measurement conditions using X-ray photoelectron spectroscopy (XPS). In the following examples, the ratio of Si element to C element present on the barrier coat layer surface was measured in the same manner. (Measurement conditions) Equipment used: "ESCA-3400" (manufactured by Kratos) [1] Spectral collection conditions Incident X-ray: MgKα (monochromatic X-ray, hν=1253.6eV) X-ray output: 150W (10kV 15mA) X-ray scanning area (measurement area): Approx. 6 mm φ Photoelectron capture angle: 90 degrees [2] Ion sputtering conditions Ion species: Ar + Acceleration voltage: 0.2 (kV) Emission current: 20 (mA) Etching range: 10mmφ Ion sputtering time: 30 seconds + 30 seconds + 60 seconds (total 120 seconds) and a spectrum was collected.
[0217] Next, a 70 μm-thick unstretched polypropylene film (ZK207, manufactured by Toray Film Processing Co., Ltd.) was dry laminated onto the barrier coat layer with a two-component curing polyurethane adhesive to form a sealant layer, thereby obtaining a laminate in the first embodiment.
[0218] Example 3-2 A laminate in the first embodiment was produced in the same manner as in Example 3-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 4.1 by mass.
[0219] Example 3-3 A laminate in the first embodiment was produced in the same manner as in Example 3-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 3.3 by mass.
[0220] Examples 3-4 A laminate in the first embodiment was produced in the same manner as in Example 3-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 2.7 by mass.
[0221] Examples 3-5 A laminate in the first embodiment was produced in the same manner as in Example 3-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 1.9 by mass.
[0222] Examples 3-6 A laminate according to the first aspect was produced in the same manner as in Example 3-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 1.5 by mass.
[0223] Example 4-1 A laminate in the first embodiment was produced in the same manner as in Example 3-1, except that the formation of the vapor-deposited film was changed as follows. A continuous vapor deposition film formation device having a pretreatment section in which an oxygen plasma pretreatment device was placed, which was an actual device, and a film formation section separated from each other was used on the surface resin layer. In the pretreatment section, plasma was introduced from a plasma supply nozzle under the conditions described below while applying tension to the multilayer substrate by roll-to-roll movement, and oxygen plasma pretreatment was performed. In the film formation section, which was continuously transported, a 12 nm thick aluminum oxide (alumina) vapor deposition film was formed on the oxygen plasma treated surface under the conditions described below using a reactive resistance heating method as a heating means for vacuum vapor deposition (PVD method). (Formation conditions) (Oxygen plasma pretreatment conditions) Plasma intensity: 200W·sec / m 2 Plasma formation gas ratio: oxygen:argon = 2:1 Voltage applied between pretreatment drum and plasma supply nozzle: 340V (Film formation conditions) -Conveying speed: 400m / min Oxygen gas supply: 20,000sccm
[0224] Example 4-2 A laminate in the first embodiment was produced in the same manner as in Example 4-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 4.1 by mass.
[0225] Example 4-3 A laminate in the first embodiment was produced in the same manner as in Example 4-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 3.3 by mass.
[0226] Example 4-4 A laminate in the first embodiment was produced in the same manner as in Example 4-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 2.7 by mass.
[0227] Examples 4-5 A laminate in the first embodiment was produced in the same manner as in Example 4-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 1.9 by mass.
[0228] Examples 4-6 A laminate in the first embodiment was produced in the same manner as in Example 4-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 1.5 by mass.
[0229] Example 5-1 In the same manner as in Example 2, a substrate was prepared, and a vapor-deposited film was formed on the substrate.
[0230] Next, a barrier coat layer was formed on the vapor deposition film such that the solid content ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 5.1 on a mass basis.
[0231] Next, a 70 μm-thick unstretched polypropylene film (ZK207, manufactured by Toray Film Processing Co., Ltd.) was dry laminated onto the barrier coat layer with a two-component curing polyurethane adhesive to form a sealant layer, thereby obtaining a laminate in the second embodiment.
[0232] Example 5-2 A laminate in the second embodiment was produced in the same manner as in Example 5-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 4.1 by mass.
[0233] Example 5-3 A laminate in the second embodiment was produced in the same manner as in Example 5-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 3.3 by mass.
[0234] Example 5-4 A laminate in the second embodiment was produced in the same manner as in Example 5-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 2.7 by mass.
[0235] Example 5-5 A laminate in the second embodiment was produced in the same manner as in Example 5-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 1.9 by mass.
[0236] Examples 5-6 A laminate in the second embodiment was produced in the same manner as in Example 5-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 1.5 by mass.
[0237] Example 6-1 A laminate according to the second embodiment was produced in the same manner as in Example 5-1, except that the formation of the vapor-deposited film was changed as follows. On the surface coating layer, a silicon oxide (silica) vapor deposition film with a thickness of 20 nm was formed (PVD method) by applying tension to the substrate by roll to roll using an induction heating vacuum deposition device equipped with a plasma gun. The vapor deposition film formation conditions were as follows: (Formation conditions) (Plasma irradiation conditions) Line speed: 30m / min ·Vacuum degree: 1.7×10 -2 Pa Power: 5.7kw Acceleration voltage: 151V Ar gas flow rate: 7.5sccm (Film formation conditions) Deposition material: SiO Reactive gas: O2 Reaction gas flow rate: 100sccm
[0238] Example 6-2 A laminate in the second embodiment was produced in the same manner as in Example 6-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 4.1 by mass.
[0239] Example 6-3 A laminate in the second embodiment was produced in the same manner as in Example 6-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 3.3 by mass.
[0240] Example 6-4 A laminate in the second embodiment was produced in the same manner as in Example 6-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 2.7 by mass.
[0241] Example 6-5 A laminate in the second embodiment was produced in the same manner as in Example 6-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 1.9 by mass.
[0242] Example 6-6 A laminate in the second embodiment was produced in the same manner as in Example 6-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 1.5 by mass.
[0243] Example 7-1 A laminate according to the second embodiment was produced in the same manner as in Example 5-1, except that the formation of the vapor-deposited film was changed as follows.
[0244] A continuous vapor deposition film formation device having a pretreatment section in which an oxygen plasma pretreatment device was placed, which was an actual device, and a film formation section separated from each other was used on the surface coating layer. In the pretreatment section, while tension was applied to the multilayer substrate by roll-to-roll, plasma was introduced from a plasma supply nozzle under the conditions described below to perform oxygen plasma pretreatment. In the film formation section, which was continuously transported, a 12 nm thick aluminum oxide (alumina) vapor deposition film was formed on the oxygen plasma treated surface under the conditions described below using a reactive resistance heating method as a heating means for the vacuum deposition method (PVD method). (Formation conditions) (Oxygen plasma pretreatment conditions) Plasma intensity: 200W·sec / m 2 Plasma formation gas ratio: oxygen:argon = 2:1 Voltage applied between pretreatment drum and plasma supply nozzle: 340V (Film formation conditions) -Conveying speed: 400m / min Oxygen gas supply: 20,000sccm
[0245] Example 7-2 A laminate in the second embodiment was produced in the same manner as in Example 7-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 4.1 by mass.
[0246] Example 7-3 A laminate in the second embodiment was prepared in the same manner as in Example 7-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 3.3 by mass.
[0247] Example 7-4 A laminate in the second embodiment was prepared in the same manner as in Example 7-1, except that the barrier coat layer was formed so that the solids ratio of the metal alkoxide to the water-soluble polymer (metal alkoxide / water-soluble polymer) was 2.7 by mass.
[0248] Example 7-5 A laminate in the second embodiment was produced in the same manner as in Example 7-1, except that the barrier coat layer was formed so that the solids ratio of metal alkoxide to water-soluble polymer (metal alkoxide / water-soluble polymer) was 1.9 by mass.
[0249] Examples 7-6 A laminate in the second embodiment was produced in the same manner as in Example 7-1, except that the barrier coat layer was formed so that the solids ratio of metal alkoxide to water-soluble polymer (metal alkoxide / water-soluble polymer) was 1.5 by mass.
[0250] <<Gas barrier property evaluation after lamination>> The laminates obtained in Examples 3 to 7 were cut out to obtain test pieces. Using these test pieces, the oxygen permeability (cc / m 2 ·day·atm) and water vapor transmission rate (g / m 2 ·day) was measured. The results are summarized in Tables 2 to 6. Note that in Tables 2 to 6, the units of oxygen permeability and water vapor permeability are omitted.
[0251] <<Gas barrier property evaluation after boiling treatment>> Two sheets of each of the laminates obtained in Examples 3 to 7 were prepared, placed face to face, and heat sealed at three sides to produce a boiling pouch as shown in FIG. This boiling pouch was filled with 100 mL of tap water, and the remaining side was heat sealed to form a content-filled boiling pouch. The contents-filled boiling pouch was subjected to a boiling treatment at 95°C for 30 minutes. Then, a laminate was cut out from the contents-filled boiling pouch after the boiling treatment to obtain a test piece. The oxygen transmission rate (cc / m 2 ·day·atm) and water vapor transmission rate (g / m 2·day) was measured. The results are summarized in Tables 2 to 6. Note that in Tables 2 to 6, the units of oxygen permeability and water vapor permeability are omitted.
[0252] <<Gas barrier property evaluation after retort treatment>> Two sheets of each of the laminates obtained in Examples 3 to 7 were prepared, placed face to face, and heat sealed at three sides to produce a retort pouch as shown in FIG. This retort pouch was filled with 100 mL of tap water, and the remaining side was heat sealed to form a retort pouch for filling with contents. The contents-filled boiling pouch was subjected to a retort treatment at 121°C for 30 minutes at 2 atm. Then, a laminate was cut out from the contents-filled retort pouch after the retort treatment to obtain a test piece. The oxygen transmission rate (cc / m 2 ·day·atm) and water vapor transmission rate (g / m 2 ·day) was measured. The results are summarized in Tables 2 to 6. Note that in Tables 2 to 6, the units of oxygen permeability and water vapor permeability are omitted.
[0253] <<Gas barrier property evaluation after Gelbo flex test>> A cylindrical bag was produced using the laminate obtained in Examples 3 to 7. Using this bag, the Gelbo flex test in accordance with ASTM F392 was repeated 10 times. Thereafter, the laminate was cut out from the bag to obtain a test piece. The oxygen permeability (cc / m 2 ·day·atm) and water vapor transmission rate (g / m 2 ·day) was measured. The results are summarized in Tables 2 to 6. Note that in Tables 2 to 6, the units of oxygen permeability and water vapor permeability are omitted.
[0254] [Table 2]
[0255] [Table 3]
[0256] [Table 4]
[0257] [Table 5]
[0258] [Table 6]
[0259] Example 8-1 In the same manner as in Example 1, a substrate was prepared, a vapor-deposited film was formed on the surface resin layer, and a barrier coat layer was formed on the vapor-deposited film.
[0260] Next, a printing layer was formed on the barrier coat layer. The printing layer had a thickness of 1 μm.
[0261] Next, a 60 μm-thick unstretched polypropylene film (Toray Film Processing Co., Ltd., ZK500, melting point 164°C, containing propylene-ethylene block copolymer, polyethylene, and thermoplastic elastomer) was dry laminated onto the printed layer as a sealant layer via a polyurethane adhesive (Mitsui Chemicals, Inc., Takelac A-969V / Takenate A-5 (mixing ratio 3 / 1)), and left to stand at 40°C for 24 hours to obtain a laminate in the first embodiment. The thickness of the adhesive layer was 4 μm. The obtained laminate had a substrate, a vapor deposition film, a barrier coat layer, a printed layer, an adhesive layer, and a sealant layer, in this order. The total thickness of the laminate was 85 μm. The polypropylene content in the laminate was 91 mass %.
[0262] Example 8-2 In the same manner as in Example 1, a substrate was prepared, a vapor-deposited film was formed on the surface resin layer, and a barrier coat layer was formed on the vapor-deposited film.
[0263] Separately, a biaxially oriented polypropylene resin film having a thickness of 20 μm was prepared. A printed layer was formed on the biaxially oriented polypropylene resin film. The printed layer had a thickness of 1 μm. Next, the barrier coat layer of the above substrate was dry laminated onto the printed layer via a polyurethane adhesive (Takelac A-969V / Takenate A-5 (mixture ratio 3 / 1) manufactured by Mitsui Chemicals, Inc.) and left to stand at 40°C for 24 hours to obtain a prelaminate.
[0264] Next, a 60 μm-thick unstretched polypropylene film (ZK500, manufactured by Toray Film Processing Co., Ltd.) was dry laminated onto the biaxially oriented polypropylene resin film of the pre-laminate via a polyurethane adhesive (Takelac A-969V / Takenate A-5 (mixing ratio 3 / 1), manufactured by Mitsui Chemicals, Inc.), and left to stand at 40° C. for 24 hours to obtain a laminate in the first embodiment. The thickness of the adhesive layer was 4 μm. The obtained laminate had a first substrate, a vapor deposition film, a barrier coat layer, an adhesive layer, a printing layer, a second substrate, an adhesive layer, and a sealant layer, in this order. The total thickness of the laminate was 109 μm. The polypropylene content in the laminate was 89 mass %.
[0265] Example 9-1 In the same manner as in Example 2, a substrate was prepared, a vapor-deposited film was formed on the surface coating layer, and a barrier coating layer was formed on the vapor-deposited film.
[0266] Next, a printing layer was formed on the barrier coat layer. The printing layer had a thickness of 1 μm.
[0267] Next, a 60 μm-thick unstretched polypropylene film (ZK500, manufactured by Toray Film Processing Co., Ltd.) was dry laminated onto the printed layer as a sealant layer via a polyurethane adhesive (Takelac A-969V / Takenate A-5 (mixing ratio 3 / 1), manufactured by Mitsui Chemicals, Inc.), and left to stand at 40° C. for 24 hours to obtain a laminate in the second embodiment. The thickness of the adhesive layer was 4 μm. The obtained laminate had a substrate, a vapor deposition film, a barrier coat layer, a printed layer, an adhesive layer, and a sealant layer, in this order. The total thickness of the laminate was 85 μm. The polypropylene content in the laminate was 91 mass %.
[0268] Example 9-2 In the same manner as in Example 2, a substrate was prepared, a vapor-deposited film was formed on the surface coating layer, and a barrier coating layer was formed on the vapor-deposited film.
[0269] Separately, a biaxially oriented polypropylene resin film having a thickness of 20 μm was prepared. A printed layer was formed on the biaxially oriented polypropylene resin film. The printed layer had a thickness of 1 μm. Next, the barrier coat layer of the above substrate was dry laminated onto the printed layer via a polyurethane adhesive (Takelac A-969V / Takenate A-5 (mixture ratio 3 / 1) manufactured by Mitsui Chemicals, Inc.) and left to stand at 40°C for 24 hours to obtain a prelaminate.
[0270] Next, a 60 μm-thick unstretched polypropylene film (ZK500, manufactured by Toray Film Processing Co., Ltd.) was dry laminated onto the biaxially oriented polypropylene resin film of the pre-laminate via a polyurethane adhesive (Takelac A-969V / Takenate A-5 (mixture ratio 3 / 1), manufactured by Mitsui Chemicals, Inc.), and left to stand at 40° C. for 24 hours to obtain a laminate in the second embodiment. The thickness of the adhesive layer was 4 μm. The obtained laminate had a first substrate, a vapor deposition film, a barrier coat layer, an adhesive layer, a printing layer, a second substrate, an adhesive layer, and a sealant layer, in this order. The total thickness of the laminate was 109 μm. The polypropylene content in the laminate was 89 mass %.
[0271] <<Tensile strength measurement>> The tensile strength in the machine direction (MD) and the transverse direction (TD) of the laminates produced in Examples 8 and 9 was measured. The tensile strength of the laminates was measured in accordance with JIS K7127:1999. The tensile tester used was a tensile tester STA-1150 manufactured by Orientec Co., Ltd. The test piece may be a rectangular film cut from the laminate with a width of 10 mm and a length of 150 mm. The distance between the pair of chucks holding the test piece at the start of the measurement is 50 mm, and the tensile speed is 300 mm / min. The environment during the measurement was set to a temperature of 23°C and a relative humidity of 50%. The measurement results are summarized in Table 7.
[0272] <<Loop stiffness measurement>> The loop stiffness was measured for the laminates of Examples 8 and 9. The specific measurement method was as described with reference to Figures 8 to 14. The measurement results are summarized in Table 7.
[0273] <<Measurement of puncture strength>> The piercing strength of the laminates of Examples 8 and 9 was measured in accordance with JIS Z1707 7.4. A Tensilon universal material testing machine RTC-1310 manufactured by A&D was used as the measuring device. Specifically, as shown in FIG. 28, a semicircular needle 111 having a diameter of 1.0 mm and a tip shape radius of 0.5 mm was pierced into a test piece 110 in a fixed state at a speed of 50 mm / min (50 mm per minute), and the maximum value of the stress until the needle 111 penetrated the test piece 110 was measured. The maximum value of the stress was measured for five or more test pieces 111, and the average value was taken as the piercing strength of the laminate. The environment during the measurement was a temperature of 23° C. and a relative humidity of 50%. The measurement results are summarized in Table 7.
[0274] [Table 7] [Explanation of symbols]
[0275] 10A: laminate, 11A: first substrate, 12A: vapor deposition film, 13A: sealant layer, 14A: polypropylene resin layer, 15A: surface resin layer, 16A: barrier coat layer, 17A: adhesive resin layer, 10B: laminate, 11B: first substrate, 12B: vapor deposition film, 13B: sealant layer, 14B: polypropylene resin layer, 15B: surface coat layer, 16B: barrier coat layer, 17B: second substrate, 20: test piece, 20x: inner surface, 20y: outer surface, 21: loop portion, 22: middle portion, 23: fixing portion, 25: loop stiffness measuring device, 26: chuck portion, 26A: first chuck, 26B: second chuck, 27: support member, 28: load cell, 30: retort or boiling pouch, 40: standing type Retort or boiling pouch, 41: body (side sheet), 42: bottom (bottom sheet), 51: easy-opening means, 52: notch, 53: half-cut line, 70: test piece, 71: substrate side, 72: sealant layer side, 73: grip, 110: test piece, 111: needle, A: vacuum vessel, B: unwinding section, C: film-forming drum, D: winding section, E: transport roll, F: evaporation source, G: reactive gas supply section, H: deposition protection box, I: deposition material, J: plasma gun, A1: vacuum vessel, B1: unwinding section, C1: cooling / electrode drum, D1: winding section, E1: transport roll, F1: glow discharge plasma, G1: reactive gas supply section, H1: raw material supply nozzle, I1: raw material gas supply section, J1: magnet, K1: power source, L1: vacuum pump
Claims
1. A laminate comprising: At least a first substrate, a second substrate, a vapor deposition film, a barrier coat layer, and a sealant layer are included, the first base material is a biaxially stretched resin film including a polypropylene resin layer, a surface resin layer provided on one surface of the polypropylene resin layer, and an adhesive resin layer between the polypropylene resin layer and the surface resin layer; the adhesive resin layer is provided on the polypropylene resin layer, the surface resin layer is provided on the adhesive resin layer, the vapor-deposited film is provided on a surface resin layer of the first substrate, The surface resin layer contains a resin material having a melting point of 180° C. or more, the resin material is vinyl resin, nylon 6, nylon 6,6, MXD nylon or polyester; the second substrate comprises polypropylene; The vapor-deposited film is composed of an inorganic oxide, the barrier coat layer is a gas barrier coating film of a mixture of a metal alkoxide and a water-soluble polymer, or a gas barrier coating film of a mixture of a metal alkoxide, a water-soluble polymer, and a silane coupling agent; The laminate, wherein the sealant layer comprises a polyolefin having a melting point of 110° C. or higher.
2. The laminate according to claim 1 , wherein the surface resin layer contains a resin material having a melting point of 180° C. or more and 265° C. or less.
3. The resin material of the surface resin layer has a melting point TA, The polypropylene of the polypropylene resin layer has a melting point TB, The laminate according to claim 1 or 2, wherein a difference between the melting point TA and the melting point TB is 20° C. or more and 80° C. or less.
4. 4. The laminate according to claim 1, wherein the resin material of the surface resin layer is made of a polymer having a polar group.
5. The laminate according to any one of claims 1 to 4, wherein a ratio of a thickness of the surface resin layer to a total thickness of the first base material is 1% or more and 10% or less.
6. The laminate of any one of claims 1 to 5, wherein the sealant layer comprises a sealant material having a melting point of 150°C or higher.
7. The laminate of any one of claims 1 to 6, wherein the sealant layer comprises polypropylene.
8. The laminate according to any one of claims 1 to 7, wherein the content of polypropylene relative to the total amount of resin materials contained in the laminate is 80 mass% or more.
9. The laminate according to any one of claims 1 to 8, wherein the first substrate and the deposited film are located between the second substrate and the sealant layer.
10. An intermediate layer is provided between the vapor-deposited film and the sealant layer, The laminate according to any one of claims 1 to 8, wherein the intermediate layer is the second substrate.
11. The laminate according to claim 10, wherein the intermediate layer is made of a polypropylene resin film that has been subjected to a stretching treatment.
12. The laminate according to any one of claims 1 to 11, wherein the barrier coat layer is located between the vapor-deposited film and the sealant layer.
13. The laminate according to any one of claims 1 to 12, which is used for a packaging container.
14. A retort or boiling pouch comprising the laminate according to any one of claims 1 to 13.
15. 15. The retort or boil pouch of claim 14 comprising a notch.
16. 16. The retort or boil pouch of claim 14 or 15, comprising a half-cut line.
Citation Information
Patent Citations
Gas barrier laminated film
JP1997226070A
Laminate
JP2001191462A
Gas barrier packaging material
JP2005074643A
Liquid soup packaging material
JP2008207868A
Pouch container
JP2009057093A