【0013】 本発明に係る光拡散フィルムは、打痕や潰れが発生しにくい。
Smart Images

Figure 0007594849000006 
Figure 0007594849000007 
Figure 0007594849000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a light diffusion film that can diffuse or transmit incident light depending on the angle of incidence. [Background technology]
[0002] 2. Description of the Related Art In the field of optical technology, which includes liquid crystal display devices and organic light-emitting devices, the use of a light diffusion film that can strongly diffuse incident light from a specific direction in a specific direction has been considered.
[0003] An example of such a light diffusion film is one having an internal structure with a plurality of regions with a relatively high refractive index within a region with a relatively low refractive index. More specifically, there is a light diffusion film having a louver structure in which a plurality of plate-like regions with different refractive indexes are alternately arranged in any one direction along the film surface, and a light diffusion film having a column structure in which a plurality of pillars with a relatively high refractive index are arranged in a region with a relatively low refractive index.
[0004] As an example of the light diffusion film as described above, Patent Document 1 discloses a light diffusion film obtained by curing a resin composition for light diffusion films, which contains a specified urethane (meth)acrylate compound, a specified (meth)acrylic acid ester compound having an aromatic skeleton, and a specified photopolymerization initiator. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6414883 Summary of the Invention [Problem to be solved by the invention]
[0006] However, conventional light diffusion films have problems in that they are easily dented during production and easily crushed when laminated to other members. If such dents or crushing occurs, liquid crystal displays and the like manufactured using the light diffusion film cannot exhibit the desired performance.
[0007] The present invention has been made in view of the above circumstances, and has an object to provide a light diffusing film in which the occurrence of dents and crushing is suppressed. [Means for solving the problem]
[0008] In order to achieve the above-mentioned object, firstly, the present invention provides a light diffusion film having an internal structure with a plurality of regions having a relatively high refractive index within a region having a relatively low refractive index, wherein the indentation elastic modulus of the light diffusion film at 23°C is 30 MPa or more (Invention 1).
[0009] The light diffusion film of the above invention (Invention 1) has an indentation elastic modulus at 23°C within the above-mentioned range, which effectively prevents dents from occurring during production and crushing when laminated to other components.
[0010] In the above invention (Invention 1), it is preferable that the indentation modulus of the light diffusing film at 23° C. is 500 MPa or less (Invention 2).
[0011] In the above inventions (Inventions 1 and 2), the light diffusion film preferably has a tensile modulus of elasticity at 23° C. of 1 MPa or more and 500 MPa or less (Invention 3).
[0012] In the above inventions (Inventions 1 to 3), the internal structure of the light diffusion film is preferably an internal structure in which a plurality of regions having a relatively high refractive index extend a predetermined length in the film thickness direction within the region having a relatively low refractive index (Invention 4). Effect of the Invention
[0013] The light diffusing film according to the present invention is less susceptible to dents and crushing. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a perspective view illustrating an example of the internal structure (column structure) of a light diffusion film according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a perspective view illustrating a schematic diagram of another example (louver structure) of the internal structure of the light diffusion film according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described. The light diffusing film according to one embodiment of the present invention has an internal structure that includes a plurality of regions of relatively high refractive index within a region of relatively low refractive index.
[0016] 1. Physical properties of light diffusion film (1) Indentation modulus The indentation elastic modulus of the light diffusion film according to this embodiment at 23°C is 30 MPa or more. This allows the light diffusion film according to this embodiment to have moderate elasticity while achieving good light diffusion. This prevents dents from occurring during production, and prevents crushing even when laminated to other members. From this perspective, the indentation elastic modulus of the light diffusion film at 23°C is preferably 50 MPa or more, and particularly preferably 100 MPa or more.
[0017] The upper limit of the indentation elastic modulus of the light diffusion film at 23° C. is not particularly limited, but from the viewpoint of easily achieving good light diffusibility, it is preferably 5000 MPa or less, more preferably 1000 MPa or less, and further preferably 300 MPa or less. Details of the method for measuring the indentation elastic modulus are as described in the test examples described later.
[0018] (2) Tensile modulus The tensile modulus of elasticity of the light diffusion film according to the present embodiment at 23°C is preferably 1 MPa or more, particularly preferably 5 MPa or more, and more preferably 10 MPa or more. The tensile modulus is preferably 500 MPa or less, particularly preferably 100 MPa or less, and more preferably 50 MPa or less. By setting the tensile modulus within these ranges, the indentation modulus of elasticity of the light diffusion film at 23°C can be easily adjusted to the above-mentioned range. The details of the method for measuring the tensile modulus are as described in the test examples described later.
[0019] (3) Thickness The thickness of the light diffusion film according to the present embodiment is preferably 20 μm or more as a lower limit, particularly preferably 50 μm or more, and more preferably 80 μm or more. When the lower limit of the thickness of the light diffusion film is in the above range, it is easy to exhibit the desired light diffusion properties. In addition, the upper limit of the thickness of the light diffusion film is preferably 700 μm or less, particularly preferably 400 μm or less, and more preferably 200 μm or less. When the upper limit of the thickness of the light diffusion film is in the above range, the ratio of the internal structure formation region in the thickness direction can be increased, and the optical properties can be improved.
[0020] (4) Variable haze angle range When the internal structure of the light diffusion film is a column structure described later, 90% of the maximum haze value measured when a light beam is irradiated on one surface of the diffusion film at an incident angle of -50° to 10° with the normal direction of the surface being 0° is set as a threshold value, and the angle range of the incident angle (variable haze angle range) showing a haze value equal to or greater than the threshold value is preferably 20° or more, particularly preferably 30° or more, and more preferably 38° or more. When the variable haze angle range is 20° or more, the angle range of the incident light that can achieve good light diffusion is wider. The upper limit of the variable haze angle range is not particularly limited, and may be, for example, 60° or less, particularly 55° or less, or even 50° or less.
[0021] In addition, when the internal structure of the light diffusion film is a louver structure described later, 30% of the maximum haze value measured when a light beam is irradiated on one surface of the diffusion film at an incident angle of -50° to 10° with the normal direction of the surface being 0° is set as a threshold value, and the angle range of the incident angle (variable haze angle range) showing a haze value equal to or greater than the threshold value is preferably 10° or more, particularly preferably 15° or more, and more preferably 20° or more. When the variable haze angle range is 10° or more, the angle range of the incident light that can achieve good light diffusion is wider. The upper limit of the variable haze angle range is not particularly limited, and may be, for example, 50° or less, particularly 40° or less, or even 30° or less.
[0022] Details of the method for measuring the variable haze angle range are as described in the test examples described later.
[0023] 2. Structure of light diffusion film The material for forming the light diffusion film according to the present embodiment is not particularly limited as long as the light diffusion film satisfies the physical properties related to the indentation elastic modulus described above. For example, the light diffusion film according to the present embodiment may be a film obtained by curing a composition for a light diffusion film that contains a high refractive index component and a low refractive index component having a refractive index lower than that of the high refractive index component.
[0024] In particular, from the viewpoint of easily adjusting the indentation modulus at 23° C. to the above-mentioned range, the light diffusion film according to this embodiment is preferably obtained by curing a composition for light diffusion films that contains a high refractive index component having one or two polymerizable functional groups, a low refractive index component having a refractive index lower than that of the high refractive index component and having one or two polymerizable functional groups, and a multifunctional monomer having three or more polymerizable functional groups. Such a composition for light diffusion films will be described in more detail below.
[0025] (1) Composition for light diffusion film (1-1) High refractive index component The composition for light diffusion film contains a high refractive index component having one or two polymerizable functional groups, so that the internal structure having a plurality of regions with relatively high refractive index in a region with relatively low refractive index can be easily formed. This makes it easier for the obtained light diffusion film to exhibit the desired light diffusion properties. Furthermore, the obtained light diffusion film can easily satisfy the physical properties related to the indentation elastic modulus described above.
[0026] The high refractive index component is not particularly limited as long as it has one or two polymerizable functional groups and the resulting light diffusion film can exhibit the desired light diffusion properties.Preferred examples of the high refractive index component include (meth)acrylic acid esters containing aromatic rings, and particularly (meth)acrylic acid esters containing multiple aromatic rings.In this specification, (meth)acrylic acid means both acrylic acid and methacrylic acid.The same applies to other similar terms.
[0027] Examples of the above-mentioned (meth)acrylic acid esters containing multiple aromatic rings include biphenyl (meth)acrylate, naphthyl (meth)acrylate, anthracyl (meth)acrylate, benzylphenyl (meth)acrylate, biphenyloxyalkyl (meth)acrylate, naphthyloxyalkyl (meth)acrylate, anthracyloxyalkyl (meth)acrylate, benzylphenyloxyalkyl (meth)acrylate, and the like, some of which are substituted with halogen, alkyl, alkoxy, alkyl halide, or the like.
[0028] In addition, the above-mentioned (meth)acrylic acid ester containing a plurality of aromatic rings is preferably a compound containing a biphenyl ring, and in particular, is preferably a biphenyl compound represented by the following general formula (1). When the composition for light diffusion film contains a biphenyl compound represented by general formula (1) as a high refractive index component, the difference in polymerization rate between the high refractive index component and the low refractive index component is easily generated when the composition for light diffusion film is cured, and the compatibility between the high refractive index component and the low refractive index component is easily reduced. This effectively reduces the copolymerization between the two components, and as a result, the above-mentioned internal structure is formed better. In addition, it is easy to increase the refractive index of the high refractive index region derived from the high refractive index component, and it is easy to adjust the difference with the refractive index of the low refractive index region to a desired value. [ka] (In the above general formula (1), R 1 ~R 10 are independent of each other, and R 1 ~R 10 One or two of the above are substituents represented by the following general formula (2), and the rest are any of the following substituents: a hydrogen atom, a hydroxyl group, a carboxyl group, an alkyl group, an alkoxy group, a halogenated alkyl group, a hydroxyalkyl group, a carboxyalkyl group, and a halogen atom. [ka] (In the above general formula (2), R11 is a hydrogen atom or a methyl group, the number of carbon atoms, n, is an integer of 1 to 4, and the number of repetitions, m, is an integer of 1 to 10.
[0029] Preferred examples of the biphenyl compound represented by the above general formula (1) include the compound represented by the following general formula (3) (o-phenylphenoxyethyl acrylate) and the compound represented by the following general formula (4) (o-phenylphenoxyethoxyethyl acrylate). [ka] [ka]
[0030] In the present embodiment, the upper limit of the weight average molecular weight of the high refractive index component is preferably 2500 or less, particularly preferably 1500 or less, and more preferably 1000 or less. By setting the upper limit of the weight average molecular weight of the high refractive index component within the above range, the difference between the weight average molecular weight of the high refractive index component and the weight average molecular weight of the low refractive index component is easily generated, and therefore the difference between the polymerization rate of the high refractive index component and the polymerization rate of the low refractive index component is also easily generated. As a result, it is easy to form a light diffusion film having a desired internal structure.
[0031] In addition, the weight average molecular weight of the high refractive index component in this embodiment is preferably 150 or more as a lower limit, particularly preferably 200 or more, and more preferably 250 or more. By the lower limit of the weight average molecular weight of the high refractive index component being within the above range, it becomes easy to realize a high refractive index, and the high refractive index component is easy to have a desired polymerization rate. As a result, the difference between the polymerization rate of the high refractive index component and the polymerization rate of the low refractive index component is easy to occur, and it becomes easy to form a light diffusion film having a desired internal structure.
[0032] In this specification, the weight average molecular weight is a value measured by gel permeation chromatography (GPC) and converted into standard polystyrene.
[0033] In the present embodiment, the lower limit of the refractive index of the high refractive index component is preferably 1.45 or more, more preferably 1.50 or more, particularly preferably 1.54 or more, and further preferably 1.56 or more. When the lower limit of the refractive index of the high refractive index component is within the above range, it becomes easier to achieve a desired refractive index difference between the relatively low refractive index region and the relatively high refractive index region formed in the light diffusion film.
[0034] In the present embodiment, the upper limit of the refractive index of the high refractive index component is preferably 1.70 or less, more preferably 1.65 or less, and even more preferably 1.59 or less. When the upper limit of the refractive index of the high refractive index component is within the above range, the compatibility between the high refractive index component and the low refractive index component is prevented from decreasing excessively, and it becomes easy to form a desired light diffusion film.
[0035] The refractive index of the high refractive index component mentioned above means the refractive index of the high refractive index component before the composition for light diffusion films is cured, and this refractive index is measured in accordance with JIS K0062:1992.
[0036] In addition, the content of the high refractive index component in the composition for light diffusion film is preferably 25 parts by mass or more, particularly preferably 40 parts by mass or more, and more preferably 50 parts by mass or more, relative to 100 parts by mass of the low refractive index component. In addition, the content of the high refractive index component in the composition for light diffusion film is preferably 400 parts by mass or less, particularly preferably 300 parts by mass or less, and more preferably 200 parts by mass or less, relative to 100 parts by mass of the low refractive index component. By having the content of the high refractive index component in these ranges, the region derived from the high refractive index component and the region derived from the low refractive index component are present in the internal structure of the formed light diffusion film in a desired ratio, and as a result, the light diffusion film is easily able to achieve the desired light diffusion properties.
[0037] (1-2) Low refractive index component The composition for light diffusion film has a refractive index lower than that of the high refractive index component and contains a low refractive index component having one or two polymerizable functional groups, so that the internal structure having a plurality of regions with relatively high refractive index in a region with relatively low refractive index can be easily formed. This makes it easier for the obtained light diffusion film to exhibit the desired light diffusion properties. Furthermore, the obtained light diffusion film can easily satisfy the physical properties related to the indentation elastic modulus described above.
[0038] The low refractive index component is not particularly limited as long as it has a refractive index lower than that of the high refractive index component, has one or two polymerizable functional groups, and the resulting light diffusion film can exhibit the desired light diffusion property.Preferred examples of the low refractive index component include urethane (meth)acrylate, (meth)acrylic polymer having (meth)acryloyl group in the side chain, (meth)acryloyl group-containing silicone resin, unsaturated polyester resin, etc., and it is particularly preferable to use urethane (meth)acrylate.
[0039] The urethane (meth)acrylate is preferably formed from (a) a compound containing at least two isocyanate groups, (b) a polyalkylene glycol, and (c) a hydroxyalkyl (meth)acrylate.
[0040] Preferred examples of the compound (a) containing at least two isocyanate groups include aromatic polyisocyanates such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1,3-xylylene diisocyanate, and 1,4-xylylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, alicyclic polyisocyanates such as isophorone diisocyanate (IPDI) and hydrogenated diphenylmethane diisocyanate, and their biurets, isocyanurates, and adducts (e.g., xylylene diisocyanate-based trifunctional adducts) which are reactants with low-molecular active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. Among these, alicyclic polyisocyanates are preferred, and alicyclic diisocyanates containing only two isocyanate groups are particularly preferred.
[0041] Preferred examples of the above-mentioned (b) polyalkylene glycol include polyethylene glycol, polypropylene glycol, polybutylene glycol, polyhexylene glycol, etc., and among these, polypropylene glycol is preferred.
[0042] The weight average molecular weight of the (b) polyalkylene glycol is preferably 2300 or more, particularly preferably 4300 or more, and more preferably 6300 or more. The weight average molecular weight of the (b) polyalkylene glycol is preferably 19500 or less, particularly preferably 14300 or less, and more preferably 12300 or less. When the weight average molecular weight of the (b) polyalkylene glycol is in the above range, it becomes easy to adjust the weight average molecular weight of the low refractive index component to the range described later.
[0043] Preferred examples of the above-mentioned (c) hydroxyalkyl (meth)acrylate include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, etc. Among these, it is preferable to use 2-hydroxyethyl methacrylate from the viewpoint of decreasing the polymerization rate of the obtained urethane (meth)acrylate and more efficiently forming a predetermined internal structure.
[0044] The synthesis of urethane (meth)acrylate using the above-mentioned components (a) to (c) as materials can be carried out according to a conventional method. In this case, the blending ratio of the components (a) to (c) is preferably a molar ratio of component (a):component (b):component (c)=1-5:1:1-5, more preferably a molar ratio of 1-3:1:1-3, and even more preferably a molar ratio of 2:1:2, from the viewpoint of efficient synthesis of the urethane (meth)acrylate.
[0045] The weight average molecular weight of the low refractive index component in this embodiment is preferably 3000 or more as a lower limit, particularly preferably 5000 or more, and more preferably 7000 or more. By the lower limit of the weight average molecular weight of the low refractive index component being within the above range, the difference between the weight average molecular weight of the high refractive index component and the weight average molecular weight of the low refractive index component is easily generated, and therefore the difference between the polymerization rate of the high refractive index component and the polymerization rate of the low refractive index component is also easily generated. As a result, it is easy to form a light diffusion film having a desired internal structure.
[0046] In addition, the upper limit of the weight average molecular weight of the low refractive index component in this embodiment is preferably not more than 20000, particularly preferably not more than 15000, and further preferably not more than 13000. When the upper limit of the weight average molecular weight of the low refractive index component is within the above range, an excessive decrease in compatibility between the high refractive index component and the low refractive index component is suppressed, and precipitation of the high refractive index component at the stage of applying the composition for a light diffusion film to a process sheet can be effectively suppressed.
[0047] In the present embodiment, the upper limit of the refractive index of the low refractive index component is preferably 1.59 or less, more preferably 1.50 or less, particularly preferably 1.49 or less, and further preferably 1.48 or less. When the upper limit of the refractive index of the low refractive index component is within the above range, a region with a relatively low refractive index and a region with a relatively high refractive index are easily formed in the light diffusion film with a desired refractive index difference.
[0048] In the present embodiment, the lower limit of the refractive index of the low refractive index component is preferably 1.30 or more, more preferably 1.40 or more, and even more preferably 1.46 or more. When the lower limit of the refractive index of the low refractive index component is within the above range, the compatibility between the high refractive index component and the low refractive index component is prevented from being excessively reduced, and it becomes easy to form a desired light diffusion film.
[0049] The refractive index of the low refractive index component mentioned above means the refractive index of the low refractive index component before the composition for light diffusion films is cured, and this refractive index is measured in accordance with JIS K0062:1992.
[0050] In addition, in this embodiment, the difference in refractive index between the high refractive index component and the low refractive index component is preferably 0.01 or more, particularly preferably 0.05 or more, and more preferably 0.1 or more. By having the difference in refractive index within the above range, the light diffusion film formed can easily achieve the desired light diffusion properties. On the other hand, the difference in refractive index between the high refractive index component and the low refractive index component is preferably 0.5 or less, particularly preferably 0.2 or less, from the viewpoint of adjusting the compatibility of these components to an appropriate range.
[0051] (1-3) Polyfunctional monomer By containing a multifunctional monomer having three or more polymerizable functional groups in the above-mentioned content, the composition for light diffusion films makes it easier for the resulting light diffusion films to satisfy the physical properties related to the indentation elastic modulus described above.
[0052] The polyfunctional monomer is not particularly limited as long as it has three or more polymerizable functional groups, and it is particularly preferable to use a polyfunctional (meth)acrylate. As such a polyfunctional (meth)acrylate having three or more polymerizable functional groups, for example, trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, propionic acid modified dipentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propylene oxide modified trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, tris(acryloxyethyl)isocyanurate, propionic acid modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, caprolactone modified dipentaerythritol hexa(meth)acrylate, etc. may be used. These may be used alone or in combination of two or more. Among the above-mentioned polyfunctional (meth)acrylates, it is preferable to use at least one of trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate.
[0053] The content of the polyfunctional monomer in the composition for light diffusion film is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 4 parts by mass or more, based on 100 parts by mass of the total amount of the high refractive index component and the low refractive index component. The content is preferably 14 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 8 parts by mass or less, based on 100 parts by mass of the total amount of the high refractive index component and the low refractive index component. By having the content of the polyfunctional monomer within these ranges, the obtained light diffusion film is more likely to satisfy the physical properties related to the above-mentioned indentation elastic modulus.
[0054] (1-4)Other In addition to the above-mentioned components, the composition for light diffusion films may contain other additives within the range that does not impair the effects of the present invention. Examples of other additives include photopolymerization initiators, antioxidants, ultraviolet absorbers, antistatic agents, polymerization accelerators, polymerization inhibitors, infrared absorbers, plasticizers, diluting solvents, and leveling agents.
[0055] Among the above, the composition for a light diffusion film preferably contains a photopolymerization initiator. When the composition for a light diffusion film contains a photopolymerization initiator, it becomes easy to efficiently form a light diffusion film having a desired internal structure.
[0056] Examples of photopolymerization initiators include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2- propyl) ketone, benzophenone, p-phenylbenzophenone, 4,4-diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tertiary butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylamine benzoic acid ester, oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propane], etc. These may be used alone or in combination of two or more.
[0057] When a photopolymerization initiator is used, the content of the photopolymerization initiator in the composition for light diffusion film is preferably 0.2 parts by mass or more, particularly preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more, relative to 100 parts by mass of the total amount of the high refractive index component and the low refractive index component. The content of the photopolymerization initiator is preferably 20 parts by mass or less, particularly preferably 15 parts by mass or less, and more preferably 10 parts by mass or less, relative to 100 parts by mass of the total amount of the high refractive index component and the low refractive index component. By setting the content of the photopolymerization initiator in the composition for light diffusion film to the above range, it becomes easy to efficiently form a light diffusion film.
[0058] (1-5) Preparation of composition for light diffusion film The composition for a light diffusion film can be prepared by uniformly mixing the above-mentioned high refractive index component, low refractive index component and polyfunctional monomer, as well as other additives such as a photopolymerization initiator, if desired.
[0059] During the mixing, a uniform composition for a light diffusion film may be obtained by stirring while heating to a temperature of 40 to 80° C. Also, a dilution solvent may be added and mixed so that the obtained composition for a light diffusion film has a desired viscosity.
[0060] (2) Internal structure Next, the internal structure of the light diffusion film according to this embodiment will be described in more detail. The light diffusion film according to this embodiment has an internal structure in which a plurality of regions with a relatively high refractive index are provided in a region with a relatively low refractive index. More specifically, the light diffusion film according to this embodiment has an internal structure in which a plurality of regions with a relatively high refractive index extend in a film thickness direction for a predetermined length in a region with a relatively low refractive index. Note that the internal structure here is distinguished from a phase separation structure in which one phase exists in another phase without clear regularity and a sea-island structure in which approximately spherical island components exist in a sea component, in that the regions with a relatively high refractive index extend in the film thickness direction.
[0061] An example of the internal structure in this embodiment is a columnar structure in which a plurality of pillars with a relatively high refractive index are arranged in a region with a relatively low refractive index in the film thickness direction. Another example of the above-mentioned internal structure is a louver structure in which a plurality of plate-like regions with different refractive indexes are alternately arranged in any one direction along the film surface.
[0062] (2-1) Column structure Fig. 1 is a perspective view showing the above-mentioned column structure. As shown in Fig. 1, in the column structure 113, a plurality of pillars 112 having a relatively high refractive index stand in the thickness direction, and a region 114 having a relatively low refractive index is filled around them. Note that, although Fig. 1 shows the pillars 112 as existing throughout the entire thickness direction of the column structure 113, the pillars 112 may not exist at least at one of the upper end and the lower end of the column structure 113 in the thickness direction.
[0063] When light is incident on a light diffusion film having such a column structure 113, it is emitted from the light diffusion film while being strongly diffused with a predetermined opening angle when it is within a predetermined range of incident angles. On the other hand, when the incident light is incident at an angle outside the above-mentioned range of incident angles, the light is transmitted without being diffused, or is emitted with weaker diffusion than the incident light within the range of incident angles. Note that the diffusion caused by the column structure 113 differs from the diffusion caused by the louver structure in that the direction of travel of the emitted light is not limited to a predetermined direction, and is generally referred to as isotropic diffusion.
[0064] In the column structure 113, the difference between the refractive index of the columnar objects 112 having a relatively high refractive index and the refractive index of the region 114 having a relatively low refractive index is preferably 0.01 or more, more preferably 0.05 or more, and even more preferably 0.1 or more. When the difference is 0.01 or more, effective diffusion can be performed. The upper limit of the difference is not particularly limited, and may be, for example, 0.3 or less.
[0065] The above-mentioned columnar object 112 preferably has a structure in which the diameter increases from one surface of the light diffusion film to the other surface. Compared with a columnar object whose diameter hardly changes from one surface to the other surface, the columnar object 112 having such a structure can easily change the traveling direction of light parallel to the axis direction of the columnar object, thereby enabling the light diffusion film to effectively diffuse light.
[0066] In addition, the maximum value of the diameter in the cross section when the columnar object 112 is cut on a plane horizontal to the axial direction is preferably 0.1 μm or more, particularly preferably 0.5 μm or more, and more preferably 1 μm or more. In addition, the maximum value is preferably 15 μm or less, particularly preferably 10 μm or less, and more preferably 5 μm or less. When the maximum value of the diameter is within the above range, the light diffusion film can effectively diffuse light. In addition, the cross-sectional shape when the columnar object 112 is cut on a plane perpendicular to the axial direction is not particularly limited, but is preferably, for example, a circle, an ellipse, a polygon, an irregular shape, or the like.
[0067] In the column structure 113, the distance between adjacent pillars 112 is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more. The distance is preferably 15 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. When the distance between adjacent pillars 112 is within the above range, the light diffusion film can effectively diffuse light.
[0068] In the column structure 113, the pillars 112 may be arranged horizontally with respect to the film thickness direction of the light diffusion film, or may be arranged at a constant inclination angle. The inclination angle when the pillars 112 are arranged at a constant inclination angle, that is, the acute angle between the axis of the pillars 112 of the column structure 113 and the normal line of the light diffusion film, is preferably 1° or more, particularly preferably 5° or more, and more preferably 10° or more. The angle is preferably 50° or less, particularly preferably 40° or less, and more preferably 30° or less. Since the pillars 112 are inclined within the above range, the light diffusion film having such a column structure 113 can diffuse the transmitted light while biasing it in a desired direction.
[0069] The dimensions and predetermined angles related to the internal structure of the column structure 113 can be measured by observing a cross section of the column structure 113 using an optical digital microscope.
[0070] (2-2) Louver structure Fig. 2 is a perspective view that shows the louver structure described above. As shown in Fig. 2, in the louver structure 123, plate-like regions 122 having a relatively high refractive index are alternately arranged in one direction along the film surface, and regions 124 having a relatively low refractive index are filled between them. Note that, although Fig. 2 shows the plate-like regions 122 as existing throughout the entire thickness direction of the louver structure 123, the plate-like regions 122 may not exist at least at one of the upper end and the lower end of the louver structure 123 in the thickness direction.
[0071] Light incident on a light diffusion film having such a louver structure 123 is either diffused when it leaves the light diffusion film or passes through without being diffused, depending on the angle of incidence. Note that a light diffusion film having a louver structure 123 has the property that it is prone to diffusion in a direction perpendicular to the arrangement direction of the plate-like regions 122. Such diffusion, in which the light emitted travels mainly in only a specific direction, is generally called anisotropic diffusion.
[0072] In louver structure 123, the difference between the refractive index of plate-like region 122, which has a relatively high refractive index, and the refractive index of region 124, which has a relatively low refractive index, is preferably 0.01 or more. When the difference is 0.01 or more, the light diffusion film having louver structure 123 can effectively diffuse light. The upper limit of the difference is not particularly limited, and may be, for example, 0.3 or less.
[0073] In the louver structure 123, the thickness (length in the arrangement direction) of each plate-like region 122 is preferably 0.1 μm or more, particularly preferably 0.5 μm or more, and more preferably 1.0 μm or more. The thickness is preferably 15 μm or less, particularly preferably 10 μm or less, and more preferably 5 μm or less. The interval between adjacent plate-like regions 122 is also preferably in the same range as above. When the thickness of the plate-like region 122 and the interval between adjacent plate-like regions 122 are in the above ranges, the light passing through the louver structure 123 can be changed in its traveling direction well, and as a result, the light diffusion film can effectively diffuse the light.
[0074] In the louver structure 123, the plate-like regions 122 may be inclined along the arrangement direction, or may be arranged so as to coincide with the film normal direction without inclination. When the plate-like regions 122 are inclined along the arrangement direction, the inclination angle, i.e., the acute angle between one side of the plate-like regions 122 and the normal line of the light diffusion film, is preferably 1° or more, more preferably 5° or more, particularly preferably 10° or more, and even more preferably 20° or more. The inclination angle is preferably 80° or less, particularly preferably 60° or less, and even more preferably 45° or less. By inclining the plate-like regions 122 within the above range, the light diffusion film having such a louver structure 123 can diffuse light while biasing it in a predetermined direction.
[0075] The dimensions and predetermined angles related to the internal structure of the louver structure 123 can be measured by observing a cross section of the louver structure 123 using an optical digital microscope.
[0076] (2-3) Other internal structures The internal structure of the light diffusion film according to this embodiment may have a structure other than the above-mentioned column structure 113 and louver structure 123. For example, the light diffusion film may have an internal structure in which the columnar object 112 in the above-mentioned column structure 113 is bent in the middle of the thickness direction of the light diffusion film. The light diffusion film may have an internal structure in which the columnar object 112 in the above-mentioned louver structure 123 is bent in the middle of the thickness direction of the light diffusion film. Alternatively, the light diffusion film according to this embodiment ...3 and the louver structure 123, or the above-mentioned bent structure is laminated in any combination.
[0077] 3. Manufacturing method of light diffusion film The method for producing the light diffusion film according to the present embodiment is not particularly limited as long as the obtained light diffusion film can achieve the above-mentioned effects, and can be produced by, for example, a conventional method. More specifically, the above-mentioned composition for light diffusion film is applied to one side of a process sheet to form a coating film, and then the coating film is irradiated with active energy rays to cure, thereby obtaining a light diffusion film.
[0078] The above-mentioned process sheet can be either a plastic film or a paper. Among them, the plastic film can be a polyester film such as a polyethylene terephthalate film, a polyolefin film such as a polyethylene film or a polypropylene film, a cellulose film such as a triacetyl cellulose film, or a polyimide film. The paper can be, for example, a glassine paper, a coated paper, or a laminated paper. The process sheet is preferably a plastic film having excellent dimensional stability against heat or active energy rays. Among the above-mentioned plastic films, the polyester film, the polyolefin film, and the polyimide film are preferably used.
[0079] In addition, in order to facilitate peeling of the cured coating film from the process sheet, it is preferable to provide a release layer on the side of the process sheet to which the composition for a light diffusion film is applied. Such a release layer can be formed using a conventionally known release agent such as a silicone-based release agent, a fluorine-based release agent, an alkyd-based release agent, or an olefin-based release agent.
[0080] Examples of the coating method include knife coating, roll coating, bar coating, blade coating, die coating, and gravure coating. The composition for a light diffusion film may be diluted with a solvent as necessary.
[0081] The coating film is irradiated with active energy rays in different modes depending on the internal structure to be formed. For example, when forming the above-mentioned column structure 113, the coating film is irradiated with parallel light having a high degree of parallelism. Here, parallel light means that the emitted light direction is substantially parallel light that does not spread regardless of the direction from which it is viewed. Such parallel light can be prepared using known means such as a lens or a light-shielding member. During irradiation, it is preferable to irradiate the above parallel light while moving the laminate of the coating film and the process sheet in its longitudinal direction using a conveyor or the like. It is also possible to adjust the inclination angle of the columnar object 112 formed in the column structure 113 by adjusting the irradiation angle of the above parallel light.
[0082] The active energy rays refer to electromagnetic waves or charged particle beams having an energy quantum, and specific examples thereof include ultraviolet rays, electron beams, etc. Among active energy rays, ultraviolet rays are particularly preferred because they are easy to handle.
[0083] When ultraviolet rays are used as the active energy rays to form the column structure 113, the irradiation conditions are as follows: a peak illuminance on the coating surface is 0.1 to 10 mW / cm 2The peak irradiance here means the measured value at the portion where the active energy ray irradiated to the coating film surface shows the maximum value. Furthermore, the integrated light amount on the coating film surface is preferably 5 to 200 mJ / cm. 2 It is preferable to set the above.
[0084] When ultraviolet rays are used as the active energy rays to form the column structure 113, the relative moving speed of the light source of the active energy rays with respect to the laminate is preferably 0.1 to 10 m / min.
[0085] On the other hand, when forming the louver structure 123 described above, a linear light source is used as a light source of active energy rays, and strip-like (almost linear) light that is random in the width direction (TD direction) and approximately parallel in the flow direction (MD direction) is irradiated onto the laminate surface. Note that the inclination angle of the plate-like region 122 formed in the louver structure 123 can also be adjusted by adjusting the irradiation angle of the light.
[0086] When ultraviolet rays are used as the active energy rays to form the louver structure 123, the irradiation conditions are as follows: a peak illuminance on the coating surface is 0.1 to 50 mW / cm 2 Furthermore, it is preferable that the integrated light quantity on the coating surface is 5 to 300 mJ / cm2. 2 The relative moving speed of the light source of the active energy rays with respect to the laminate is preferably 0.1 to 10 m / min or less.
[0087] In order to complete the curing more reliably, it is also preferable to irradiate the laminate with normal active energy rays (active energy rays that have not been converted into parallel or band-like light, scattered light) after the curing using the parallel or band-like light as described above. At this time, in order to cure uniformly, a release sheet may be laminated on the surface of the coating film.
[0088] 4. Use of light diffusion film The use of the light diffusion film according to the present embodiment is not particularly limited, and it can be used in the same manner as a conventional light diffusion film. For example, the light diffusion film according to the present embodiment can be used to manufacture a liquid crystal display device, an organic light emitting device, electronic paper, etc.
[0089] The light diffusion film according to the present embodiment can effectively suppress the occurrence of dents during its production and the occurrence of crushing during lamination to other members. Therefore, the light diffusion film according to the present embodiment can satisfactorily exhibit the desired light diffusibility, and the above-mentioned liquid crystal display device and the like manufactured using such a light diffusion film can also satisfactorily exhibit the desired performance.
[0090] The above-described embodiments are described for the purpose of facilitating understanding of the present invention, and are not described for the purpose of limiting the present invention. Therefore, each element disclosed in the above embodiment is intended to include all design modifications and equivalents that fall within the technical scope of the present invention. EXAMPLES
[0091] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.
[0092] Example 1 1. Preparation of composition for light diffusion film To 40 parts by mass (solids equivalent; same below) of polyether urethane methacrylate having a weight average molecular weight of 9,900 obtained by reacting polypropylene glycol, isophorone diisocyanate, and 2-hydroxyethyl methacrylate as a low refractive index component, 60 parts by mass of o-phenylphenoxyethoxyethyl acrylate having a molecular weight of 268 as a high refractive index component, 5 parts by mass of dipentaerythritol hexaacrylate as a multifunctional monomer (5 parts by mass per 100 parts by mass of the total amount of the high refractive index component and the low refractive index component), and 8 parts by mass of 2-hydroxy-2-methyl-1-phenylpropan-1-one as a photopolymerization initiator were added, and the mixture was heated and mixed at 80°C to obtain a composition for light diffusion films.
[0093] The refractive indices of the high refractive index component and the low refractive index component were measured in accordance with JIS K0062-1992 using an Abbe refractometer (manufactured by Atago Co., Ltd., product name "Abbe refractometer DR-M2", Na light source, wavelength 589 nm), and were found to be 1.58 and 1.46, respectively.
[0094] 2. Formation of light-diffusing film The obtained composition for a light diffusion film was applied to one side of a long polyethylene terephthalate sheet as a processing sheet to form a coating film, thereby obtaining a laminate consisting of the coating film and the processing sheet.
[0095] The obtained laminate was then placed on a conveyor. At this time, the surface of the laminate on the coating side was on the upper side, and the longitudinal direction of the process sheet was parallel to the conveyor flow direction. Then, an ultraviolet spot parallel light source (manufactured by JATEC Co., Ltd.) with a central light beam parallelism controlled within ±3° was installed on the conveyor on which the laminate was placed. At this time, the light source was installed so as to irradiate parallel light in a direction inclined by 15° to the opposite side to the conveyor flow direction with respect to the normal direction of the surface on the coating side of the laminate. In addition, the distance between the surface of the coating film and the light source was set to 240 mm.
[0096] Thereafter, the conveyor was operated to move the laminate at a speed of 0.2 m / min while applying a peak irradiance of 2.00 mW / cm2 to the coating surface. 2 , cumulative light output 53.13mJ / cm 2 The coating film in the laminate was cured by irradiating it with parallel light (ultraviolet light from a high-pressure mercury lamp having a main peak wavelength of 365 nm, with other peaks at 254 nm, 303 nm, and 313 nm) with a parallelism of 2° or less under the conditions above (this curing is sometimes referred to as "primary curing" for convenience).
[0097] Next, from the viewpoint of sufficiently curing the coating film, a 38 μm-thick release sheet having ultraviolet light transmittance (manufactured by Lintec Corporation, product name "SP-PET382050", center line average roughness on the surface on the ultraviolet light irradiated side: 0.01 μm, haze value: 1.80%, image clarity: 425, transmittance at a wavelength of 360 nm: 84.3%) was laminated on the coating film side of the laminate, and then a peak irradiance of 10 mW / cm was applied to the coating film through the release sheet. 2 , cumulative light intensity 150mJ / cm 2 The coating film in the laminate was cured by irradiating it with ultraviolet light (scattered light) under the above conditions (this curing is sometimes referred to as "secondary curing" for convenience). The peak irradiance and integrated light quantity mentioned above were measured by placing a UV METER (manufactured by Eye Graphics, product name "Eye UV Integrated Illuminance Meter UVPF-A1") equipped with a receiver at the position of the coating film.
[0098] Through the above primary and secondary curing, the above-mentioned coating film was cured to obtain a 75μm thick light diffusion film laminated between the release sheet and the process sheet. The thickness of the light diffusion film was measured using a constant pressure thickness measuring device (manufactured by Takara Seisakusho, product name "TECLOCK PG-02J").
[0099] In addition, when the cross section of the formed light diffusion film was observed under a microscope, it was confirmed that a columnar structure consisting of multiple pillars standing in the thickness direction was formed inside the light diffusion film. In particular, it was confirmed that the pillars were inclined at 20° to the opposite side to the conveyor traveling direction with respect to the thickness direction of the light diffusion film (inclination angle -20°). The inclination angle is expressed as 0° in the normal direction to the film surface, plus the conveyor traveling direction, and minus the opposite direction.
[0100] [Examples 2 and 3] A light diffusing film was produced in the same manner as in Example 1, except that the type and thickness of the polyfunctional monomer were changed as shown in Table 1.
[0101] Comparative Example 1 A light diffusing film was produced in the same manner as in Example 1, except that no polyfunctional monomer was used.
[0102] [Test Example 1] (Measurement of indentation elastic modulus) The indentation modulus (MPa) at 23° C. was measured for one surface exposed by peeling off the process sheet and release film from the light diffusion films produced in the Examples and Comparative Examples using an ultra-microhardness tester (Shimadzu Dynamic Ultra-Microhardness Tester DUH-W201S, manufactured by Shimadzu Corporation). The results are shown in Table 1.
[0103] [Test Example 2] (Measurement of tensile modulus) The process sheet and release film were peeled off and removed from the light diffusion films produced in the examples and comparative examples, and the films were cut to a size of 15 mm x 140 mm to obtain test pieces of light diffusion films. The test pieces were measured for tensile modulus at 23°C in accordance with JIS K7127:1999. Specifically, the test pieces were subjected to a tensile test at a speed of 200 mm / min using a tensile tester (manufactured by Shimadzu Corporation, product name "Autograph AG-IS 500N") with a chuck distance set to 100 mm, and the tensile modulus (MPa) was measured. The results are shown in Table 1.
[0104] [Test Example 3] (Evaluation of Impact Suppression) The process sheet was peeled off from the light diffusion film produced in the examples and comparative examples. The laminate consisting of the light diffusion film and the release film obtained in this way was placed on a hard support with the release film side facing up. Then, a point load was applied to the light diffusion film through the release film to make an indentation. Specifically, a load of 225 g was applied for 10 seconds using a hardness tester (manufactured by Kobunshi Keiki Co., Ltd., product name "Asker Hardness Tester C2") with a pressing core tip that is a hemisphere with a diameter of 2.54 mm.
[0105] Five minutes after the application of the point load, the release film was peeled off from the light diffusion film, and the depth of the dents remaining on the exposed surface of the light diffusion film was measured using an optical interference microscope (Veeco, product name "Surface Profiler WYKO NT110"). The dent suppression was evaluated based on the following criteria. The results are shown in Table 1. ⊚: The remaining dent depth was 0 nm or more and 10 nm or less. ◯: The depth of the remaining dent was greater than 10 nm and less than 20 nm. ×: The remaining dents had a depth of more than 20 nm.
[0106] The load applied when applying the point load was changed to 443 g, and the same measurements were carried out to evaluate the suppression of dents. The results are also shown in Table 1.
[0107] [Test Example 4] (Measurement of variable haze) The haze value (%) of the light diffusion film produced in the examples and comparative examples was measured using a variable angle haze meter (manufactured by Toyo Seiki Seisakusho, product name "Haze Guard Plus, variable angle haze meter"). Specifically, after the process sheet and release film were peeled off from the light diffusion film, one side of the light diffusion film was irradiated with light while changing the incident angle with respect to the normal line in the range of -50° to 10° along the longitudinal direction of the light diffusion film, and the haze value (%) was measured in sequence.
[0108] Next, from the results of the sequential measurements, the range of incident angles within the measurement range of incident angles (-50° to 10°) where the haze value was 90% or more was identified, and the difference between the two angles at the end points of the range was calculated, and this was defined as the angle range (variable haze angle range) that provided a haze value of 90% or more. The results are shown in Table 1.
[0109] [Table 1]
[0110] As shown in Table 1, the light diffusing films according to the examples were able to effectively suppress the occurrence of dents. [Industrial Applicability]
[0111] The light diffusing film of the present invention is suitably used in the manufacture of liquid crystal displays and the like. [Explanation of symbols]
[0112] 112...Columnar object with relatively high refractive index 113…Column structure 114...Area with relatively low refractive index 122... Plate-shaped region with relatively high refractive index 123…Louver structure 124...Area with relatively low refractive index
Claims
1. A light diffusing film having an internal structure with a plurality of regions having a relatively high refractive index within a region having a relatively low refractive index, The indentation elastic modulus of the light diffusion film at 23° C. is 30 MPa or more, the internal structure is a louver structure in which a plurality of plate-like regions having different refractive indices are alternately arranged in any one direction along the film surface, The internal structure does not have a structure in which the light diffusion film is bent in the middle of the thickness direction, The composition for forming the light diffusion film does not contain a monomer, oligomer, prepolymer or macromonomer of a photocurable compound having a silicone skeleton. A light diffusing film characterized by:
2. The light diffusing film according to claim 1 , wherein the light diffusing film has an indentation elastic modulus at 23° C. of 500 MPa or less.
3. 3. The light diffusion film according to claim 1, wherein the light diffusion film has a tensile modulus at 23° C. of 1 MPa or more and 500 MPa or less.
Citation Information
Patent Citations
Connection terminal for electric wire and connection of electric wire to its terminal
JP1989014883A
Composition for anisotropic light-diffusing film and anisotropic light-diffusing film
JP2012141591A
Anisotropic optical film
JP2013195672A
Optical anisotropy film
JP2013205468A
Daylighting sheet
JP2016071066A