Ceramic parts and method for manufacturing ceramic parts

Boron carbide ceramic components with controlled residual stress distribution address non-uniform plasma etching issues, enhancing manufacturing efficiency and quality by ensuring uniform plasma distribution and improved shape processability in semiconductor devices.

JP7595668B2Active Publication Date: 2024-12-06SOLMICS CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2022532664
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-29
Filing Date
2021-02-09
Publication Date
2024-12-06
Estimated Expiration
2041-02-09

AI Technical Summary

Technical Problem

The non-uniform plasma distribution on substrates during plasma etching in semiconductor manufacturing leads to inconsistent processing and reduced quality of microelectronic devices, particularly due to high power usage affecting the focus ring, which requires longer chamber opening times and impacts yield.

Method used

The use of boron carbide ceramic components with controlled residual stress distribution, specifically within -600 to +600 MPa difference and standard deviation of 350 MPa or less, in focus rings and other plasma etching equipment parts, manufactured through a process involving slurry preparation, granulation, high-pressure sintering, and heat treatment to ensure uniform stress and improved shape processability.

Benefits of technology

This approach enhances the quality and efficiency of ceramic component production, ensuring uniform plasma distribution, improved etching resistance, and stable shape processing, thereby improving the manufacturing yield and quality of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595668000006
    Figure 0007595668000006
  • Figure 0007595668000007
    Figure 0007595668000007
  • Figure 0007595668000001
    Figure 0007595668000001
Patent Text Reader

Abstract

The present embodiment relates to a ceramic part and a method for manufacturing the ceramic part, and provides a ceramic part containing boron carbide, in which residual stresses S1 and S2 measured at two points on the surface at different distances from the center are respectively set to be a difference of -600 to +600 MPa. According to the present embodiment, it is possible to efficiently manufacture ceramic parts used in equipment for manufacturing semiconductor devices while improving quality.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Embodiments relate to a ceramic part, a method for manufacturing a ceramic part, and a method for manufacturing a semiconductor device. [Background technology]

[0002] In a plasma processing apparatus, an upper electrode and a lower electrode are placed in a chamber, a substrate such as a semiconductor wafer or a glass substrate is placed on the lower electrode, and power is applied between the two electrodes. Electrons accelerated by the electric field between the two electrodes, electrons emitted from the electrodes, or heated electrons collide with molecules of the processing gas to ionize and generate plasma of the processing gas. Active species such as radicals and ions in the plasma perform desired fine processing, such as etching, on the surface of the substrate. In recent years, design rules in the manufacture of fine electronic elements and the like have become increasingly finer, and higher dimensional accuracy is particularly required in plasma etching, so that significantly higher power is used than in the past. Such plasma processing apparatuses are equipped with a focus ring that is affected by the plasma. The focus ring is also called an edge ring, a cold ring, or the like.

[0003] In the case of the focus ring, when the power is high, the center of the substrate is maximized and the edge is minimized due to the wavelength effect in which a standing wave is formed and the skin effect in which the electric field on the surface of the electrode is concentrated in the center, resulting in a severe non-uniformity of the plasma distribution on the substrate. If the plasma distribution on the substrate is non-uniform, the plasma processing is not performed consistently, and the quality of the microelectronic device is reduced. FIG. 1 is a photograph showing a general plasma chamber and focus ring. A high-performance focus ring requires an extended replacement cycle. This extends the cycle of opening the plasma chamber. The extended cycle of opening the chamber improves the yield of microelectronic devices using wafers.

[0004] Related prior patent documents include Korean Patent Publication No. 10-1998-0063542 and Korean Patent Publication No. 10-2006-0106865. Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the embodiment is to provide a method for efficiently manufacturing ceramic components while improving their quality.

[0006] Another object of the present embodiment is to provide a ceramic part that is excellent in properties such as strength and relative density, and is also excellent in shape processability. [Means for solving the problem]

[0007] In order to achieve the above object, the ceramic part according to the embodiment includes: Contains boron carbide, The residual stresses measured on the surface at two points at different distances from the center are S1 and S2, respectively. The difference between S1 and S2 is -600~+600 MPa may be also possible.

[0008] In an embodiment, the ceramic part has residual stresses S1, S2, and S3 at different points on the surface from the center, respectively; The difference between the maximum and minimum values ​​of S1, S2, and S3 is -600 to +600 MPa may be also possible.

[0009] In one embodiment, the ceramic part is a part applied to a plasma etching device, The component has a first height from a reference surface. Placement section and having a second height from the reference plane. Main unit and The body portion includes a body portion upper surface, The placement portion includes a placement portion upper surface, The difference between the residual stress measured on the upper surface of the main body and the residual stress measured on the upper surface of the mounting portion is -600 to +600. MPa may be also possible.

[0010] In order to achieve the above object, the focus ring according to the embodiment includes: Contains boron carbide, A mounting portion having a first height from a reference surface and a main body portion having a second height from the reference surface, the placement portion includes a placement portion upper surface on which an etching target is placed, the body includes a body upper surface that is directly etched by a plasma; a difference between the residual stresses measured at a point PS1 on the upper surface of the mounting portion and a point PS3 on the upper surface of the main body portion is within 40% of the average value of the residual stresses measured at PS1 and PS3; The residual stresses measured on the surface at two points at different distances from the center are S1 and S2, respectively. The difference between S1 and S2 is -600~+600 MPa may be also possible.

[0011] In an embodiment, the standard deviation of residual stress measured on the surface at three different distances from the center may be 350 MPa or less.

[0012] In one embodiment, the device further includes a connection portion between the placement portion and the body portion, the connecting portion includes a connecting portion upper surface that connects the placement portion upper surface and the main body portion upper surface, The connecting portion may have a point PS2 on the upper surface thereof.

[0013] In one embodiment, the difference between the maximum and minimum values ​​of the residual stress measured in each of PS1, PS2, and PS3 may be within 25% of the average of the residual stress measured in each of PS1, PS2, and PS3.

[0014] In an embodiment, the focus ring may have a bending strength of 300 MPa or more.

[0015] In order to achieve the above object, a ceramic part for manufacturing a semiconductor device according to an embodiment includes: Contains boron carbide, The residual stresses measured on the surface at two points at different distances from the center are S1 and S2, respectively. The difference between S1 and S2 is -600~+600 MPa may be also possible.

[0016] In order to achieve the above object, a focus ring for manufacturing semiconductor devices according to an embodiment includes: Contains boron carbide, A mounting portion having a first height from a reference surface and a main body portion having a second height from the reference surface, the placement portion includes a placement portion upper surface on which an etching target is placed, the body includes a body upper surface that is directly etched by a plasma; a difference between the residual stresses measured at a point PS1 on the upper surface of the mounting portion and a point PS3 on the upper surface of the main body portion is within 40% of the average value of the residual stresses measured at PS1 and PS3; The residual stresses measured on the surface at two points at different distances from the center are S1 and S2, respectively. The difference between S1 and S2 is -600~+600 MPa may be also possible.

[0017] In order to achieve the above object, a method for manufacturing a ceramic part according to an embodiment includes: A first step of preparing raw material granules by slurrying and granulating a raw material composition including boron carbide powder; A second step of filling the raw material granules into a molding die and sintering them at a temperature of 1800° C. or more and a pressure of 15 MPa or more to produce a sintered body in which the boron carbide powder particles are necked together; and a third step of manufacturing a ceramic part by heat-treating the sintered body and then shaping the sintered body, The heat treatment includes a first treatment performed at a first temperature for one hour or more and a second treatment performed at a second temperature for one hour or more, the first temperature being higher than the second temperature; Residual stresses measured on the surface of the ceramic component at two points at different distances from the center of the ceramic component are S1 and S2, respectively; The difference between S1 and S2 is -600~+600 MPa may be also possible.

[0018] In one embodiment, the first temperature is 1650° C. or more; The second temperature may be 1400° C. or higher. Effect of the Invention

[0019] The method for manufacturing a ceramic part according to the embodiment can improve the quality and efficiently manufacture ceramic parts used in equipment for manufacturing semiconductor devices.

[0020] The ceramic parts of the embodied embodiments have a relatively uniform distribution of residual stress and are much more easily machinable into shapes while maintaining or even improving other properties such as strength and relative density at excellent levels.

[0021] The focus ring and the manufacturing method of the focus ring according to the embodiment can efficiently and successfully manufacture a focus ring having excellent physical properties such as etching resistance and impact resistance, and also having excellent shape processability. [Brief description of the drawings]

[0022] [Figure 1] 1 is a schematic diagram illustrating a top view of a focus ring, which is an example of a ceramic part according to an embodiment; FIG. [Diagram 2] 1 is a schematic diagram illustrating a cross section of a focus ring, which is an example of a ceramic part according to an embodiment; FIG. BEST MODE FOR CARRYING OUT THEINVENTION

[0023] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS One or more exemplary embodiments will now be described in detail with reference to the accompanying drawings in order to enable those of ordinary skill in the art to easily make and use the present invention. However, the exemplary embodiments may be embodied in many different forms and are not limited to the embodiments set forth herein. Like reference numerals are used throughout the specification to refer to like parts.

[0024] In this specification, when a certain configuration "includes" another configuration, this does not mean to exclude the other configurations, unless specifically stated to the contrary, but rather means that the other configurations may also be included.

[0025] In this specification, when a certain component is said to be "connected" to another component, this includes not only the case where the component is "directly connected" but also the case where the component is "connected via another component between them."

[0026] In this specification, the term "B is located on A" means that B is located on A in direct contact therewith, or that B is located on A with another layer located therebetween, and is not to be interpreted as being limited to B being located in contact with the surface of A.

[0027] As used herein, the term "combinations thereof" contained in a Markush form expression means a mixture or combination of one or more selected from the group of components set forth in the Markush form expression, and is meant to include one or more selected from the group of components.

[0028] In this specification, the phrase "A and / or B" means "A, B, or A and B."

[0029] In this specification, terms such as "first", "second" or "A", "B" are used to distinguish identical terms from each other, unless otherwise specified.

[0030] In this specification, the term "singular" is intended to include the singular or plural as the context requires, unless otherwise specified.

[0031] As used herein, the term "difference" means one value minus another, and unless otherwise specified, is expressed as a larger value minus a smaller value.

[0032] In this specification, boron carbide refers to any compound based on boron and carbon. The boron carbide may be a boron carbide material with or without additives and / or doping materials, specifically, the total of boron and carbon may be 90 mol % or more. The boron carbide may be a boron carbide material with or without additives and / or doping materials, specifically, the total of boron and carbon may be 90 mol % or more. The boron carbide may be a boron carbide material with a total of 95 mol % or more. The boron carbide may be a boron carbide material with a total of 98 mol % or more. The boron carbide may be a boron carbide material with a total of 99 mol % or more. In this specification, boron carbide may be a single phase or a composite phase, or a mixture thereof. The single phase of boron carbide includes both the stoichiometric phase of boron and carbon and the non-stoichiometric phase that deviates from the stoichiometric composition, and the composite phase refers to at least two compounds based on boron and carbon mixed in a predetermined ratio. In addition, boron carbide in this specification includes both the case where impurities are added to the single phase or composite phase of boron carbide to form a solid solution, and the case where impurities that are inevitably added during the process of manufacturing boron carbide are mixed in. Examples of the impurities include metals such as iron, copper, chromium, nickel, and aluminum.

[0033] In this specification, bulk boron carbide is distinguished from a coating layer and refers to deposited boron carbide, sintered boron carbide, etc., having a certain thickness, and is defined as having an average thickness of 1 mm or more for the purpose of distinguishing it from a coating layer.

[0034] In this specification, without any special explanation, "the difference between the A value and the B value is C or less" means that the absolute value of the difference between the A value and the B value is C or less, and more specifically, means that the difference between the A value and the B value is -C to +C.

[0035] In this specification, the residual stress will be explained based on the results measured by X-ray diffraction.

[0036] The present invention will now be described in more detail.

[0037] Manufacturing method for ceramic parts To achieve the above object, a method for manufacturing a ceramic part according to an embodiment includes: A first step of preparing raw material granules by slurrying and granulating a raw material composition including boron carbide powder; A second step of filling the raw material granules into a molding die and sintering them at a temperature of 1800° C. or more and a pressure of 15 MPa or more to produce a sintered body in which the boron carbide powder particles are necked together; and a third step of manufacturing a ceramic part by heat-treating the sintered body and then shaping the sintered body, The heat treatment includes a first treatment performed at a first temperature for one hour or more and a second treatment performed at a second temperature for one hour or more, the first temperature being higher than the second temperature; Residual stresses measured on the surface of the ceramic component at two points at different distances from the center of the ceramic component are S1 and S2, respectively; The difference between S1 and S2 is -600~+600 MPa may be also possible.

[0038] The raw material composition includes boron carbide powder. The boron carbide powder may be high purity (boron carbide content is 99.9% by weight or more). The boron carbide powder may be low purity (boron carbide content is 95% by weight or more and less than 99.9% by weight).

[0039] The boron carbide powder is 50Based on this standard, particles having a particle size of 150 μm or less may be applied.

[0040] The boron carbide powder is 50 The boron carbide powder may have an average particle size of about 1.5 μm or less based on D 50 The boron carbide powder may have an average particle size of about 0.3 μm to about 1.5 μm based on D 50 The boron carbide powder may have an average particle size of about 0.4 μm to about 1.0 μm based on D. 50 Based on the average particle size, the powder may have an average particle size of about 0.4 μm to about 0.8 μm. When a powder having a small average particle size is used, it is possible to more easily obtain a densified sintered body.

[0041] The boron carbide powder is 50 The boron carbide powder may have a particle size of 2 to 10 μm based on D 50 The boron carbide powder may have a particle size of 3 to 8 μm based on D 50 Based on the above, the boron carbide powder may have a particle size of 4 to 6 μm. When using boron carbide powder having such a particle size range, the sintered body can be densified and the productivity of the process can be improved.

[0042] The raw material composition may further include an additive. The additive may be added in the form of a powder, liquid phase, or gas phase in the process of manufacturing the ceramic part. Examples of materials used as the additive include carbon, boron oxide, silicon, silicon carbide, silicon oxide, boron nitride, boron, silicon nitride, etc. The additive may be included in an amount of about 0.1% by weight to about 30% by weight based on the raw material.

[0043] The additive may be a sintering property improver. The sintering property improver is contained in the raw material to improve the physical properties of the sintered body. The sintering property improver may be any one selected from the group consisting of carbon, boron oxide, silicon, silicon carbide, silicon oxide, boron nitride, boron, silicon nitride, and combinations thereof. The sintering property improver may be contained in an amount of about 30% by weight or less based on the whole raw material. Specifically, the sintering property improver may be contained in an amount of about 0.001% by weight to about 30% by weight based on the whole raw material. The sintering property improver may be contained in an amount of about 0.1% by weight to about 15% by weight based on the whole raw material. The sintering property improver may be contained in an amount of about 1% by weight to about 10% by weight based on the whole raw material. If the sintering property improver is contained in an amount exceeding 30% by weight, the strength of the sintered body may be decreased.

[0044] The raw material may include a boron carbide raw material such as boron carbide powder, etc., other than the sintering property improver. The sintering property improver may include boron oxide, carbon, or a combination thereof.

[0045] When carbon is used as the sintering property improving agent, the carbon may be added in the form of a resin such as a phenolic resin or a novolac resin, or the resin may be carbonized through a carbonization process. The carbonization process of the resin may generally be a process of carbonizing a polymer resin. The phenolic resin may have a residual carbon amount of 40% by weight or more.

[0046] When carbon is used as the sintering property improver, the carbon may be applied at 1 to 10% by weight. The carbon may be applied at 1 to 8% by weight. The carbon may be applied at 2 to 6% by weight. The carbon may be applied at 3 to 5% by weight. When carbon is applied as the sintering property improver in such an amount, it is possible to effectively induce the necking phenomenon between particles, and obtain a sintered body having a relatively large particle size and a relatively high relative density. However, when the carbon is contained at more than 10% by weight, excessive gas such as carbon dioxide is generated during the pressure sintering process, which may reduce workability.

[0047] The sintering property improver may be boron oxide, which is typically represented by B2O3, and when boron oxide is used, it produces boron carbide through a chemical reaction with carbon present in the pores of the sintered body, helping to remove residual carbon, thereby providing a more dense sintered body.

[0048] When the boron oxide and the carbon are used together as the sintering property improver, the relative density of the sintered body can be further increased, which means that the carbon regions present in the pores are reduced, resulting in a sintered body with improved density.

[0049] The boron oxide and the carbon may be applied in a weight ratio of 1:0.8 to 4. In this case, a sintered body having a further improved relative density can be obtained.

[0050] The sintering characteristic improver may have a melting point of about 100° C. to about 1000° C. More specifically, the melting point of the additive may be about 150° C. to about 800° C. The melting point of the additive may be about 200° C. to about 400° C. This allows the additive to easily diffuse between the boron carbide particles during the process of sintering the raw material.

[0051] The raw material composition may further contain a dispersant, a solvent, etc., as necessary.

[0052] The raw material composition does not contain any material that may generate solid-state by-products during semiconductor processing, or contains a very low content of such material. For example, examples of materials that may generate by-products include metals such as iron, copper, chromium, nickel, and aluminum. The content of the material that may generate by-products may be 500 ppm or less based on the raw material.

[0053] The slurrying is a process of mixing the raw material composition sufficiently and substantially uniformly by a method such as ball milling. A solvent may be applied, and alcohol such as methanol, ethanol, butanol, etc., or water may be applied as the solvent. The solvent may be applied in an amount of about 60% to about 80% by volume based on the total amount of the slurry. Specifically, polymer balls may be used for ball milling, and the slurry mixing process may be performed for about 5 hours to about 20 hours.

[0054] The granulation may be performed in such a manner that the raw material is granulated by removing a solvent contained in the slurry by evaporation, etc., while the slurry is being sprayed. The granulated raw material particles thus produced may have a generally round shape and a relatively uniform particle size.

[0055] The raw material granules that have been subjected to the granulation process may have a size of 50 to 160 μm. The raw material granules may have a size of 60 to 100 μm. When raw material granules having such characteristics are used, they can be easily filled into a mold in the subsequent process of sintering, etc., and workability can be further improved.

[0056] The second step is to fill the raw material granules into a molding die and sinter them to produce a sintered body in which the boron carbide powder particles are necked together.

[0057] There have been many attempts to manufacture bulk boron carbide sintered bodies by pressure sintering. However, they are usually manufactured and evaluated as small test pieces called coupons, each measuring approximately 30 mm in length and width. It is not easy to manufacture bulk boron carbide sintered bodies (hereafter referred to as boron carbide) that have a relatively large diameter.

[0058] The inventors have experimentally confirmed that when a relatively large sized boron carbide sintered body is manufactured, particularly when the boron carbide sintered body is manufactured by a pressure sintering method, it is stable until it is manufactured into a bulk shape, but when it is processed into a ring shape as described below, cracks, breakage, etc. are likely to occur at a very high rate. And, one of the reasons for this characteristic is believed to be that the boron carbide sintered body has non-uniform residual stress characteristics throughout the entire body.

[0059] The forming die may have a length or diameter of 450 mm or more. Currently, ceramic parts such as focus rings are generally applied in the form of a ring having a diameter of 320 mm or more. Therefore, in order to manufacture the ceramic parts, a bulk boron carbide sintered body having a very large diameter or length is required. In general, the size of the sintered body becomes smaller during the sintering process, and in consideration of the parts lost during the subsequent shape processing, the forming die may have a diameter of 450 mm or more. The forming die may have a diameter of 450 to 600 mm.

[0060] The sintering can be carried out at a sintering temperature and under a sintering pressure.

[0061] The sintering temperature may be about 1800 to about 2500° C. The sintering temperature may be about 1800 to about 2200° C. The sintering pressure may be about 10 to about 110 MPa. The sintering pressure may be about 15 to about 60 MPa. The sintering pressure may be about 17 to about 30 MPa. When the molding step is performed under such sintering temperature and / or sintering pressure, boron carbide with high etching resistance and high density can be produced more efficiently.

[0062] The sintering time may be 0.5 to 10 hours. The sintering time may be 0.5 to 7 hours. The sintering time may be 0.5 to 4 hours.

[0063] The sintering time is very short in the pressure sintering method compared to the sintering process performed under normal pressure, and even with such a short time, it is possible to produce a boron carbide sintered body having the same or even better strength.

[0064] The sintering can be carried out in a reducing atmosphere, which reduces substances such as boron oxide that can be formed when boron carbide powder reacts with oxygen in the air, thereby producing a boron carbide sintered body with high etching resistance, in which the boron carbide content is further increased and the carbon agglomerated regions are reduced.

[0065] During the sintering process, the boron carbide powder grows and necks together to form a sintered body with high strength. It is believed that the additives applied together suppress or promote the growth of the boron carbide powder as their state and composition change depending on the temperature and pressure. In addition, the boron carbide sintered body obtained by sintering with pressure can have a denser microstructure than the boron carbide sintered body obtained by general pressureless sintering.

[0066] In order to improve the shape workability, the sintered body containing bulk boron carbide may be subjected to additional heat treatment or the like.

[0067] The heat treatment includes a first treatment carried out at a first temperature for one hour or more and a second treatment carried out at a second temperature for one hour or more, the first temperature being higher than the second temperature.

[0068] The first temperature may be equal to or higher than 1650° C., and the second temperature may be equal to or higher than 1400° C. When the primary treatment and the secondary treatment are performed within such temperature ranges, the heat treatment can be performed more effectively.

[0069] The first temperature may be a temperature of 1650 to 1950° C. The primary treatment may be performed for 2 to 8 hours.

[0070] The second temperature may be a temperature of 1400 to 1600° C. The secondary treatment may be performed for 2 to 8 hours.

[0071] When the heat treatment is applied at the first and second temperatures, the shape workability of the sintered body is very high, which is believed to be because the heat treatment induces changes in the residual stress distribution.

[0072] The shaping process is a process of separating or removing a portion of the sintered body to process it into an intended shape. The shaping process includes ring shaping, in which the sintered body is processed into the outer shape of a ceramic part such as a ring, and narrow shaping process, in which boron carbide that has been processed into a ring is processed into the shape of a ring-shaped part such as a focus ring.

[0073] The shape machining may be performed by, but is not limited to, electric discharge machining, a water jet method, a laser method, or the like.

[0074] After the boron carbide sintered body has the shape of a ceramic part by the shape processing, it may further undergo a polishing process, which is a process for reducing the surface roughness of the ceramic part. The polishing process may be performed by a polishing process using a slurry containing industrial diamond, and in order to obtain a ceramic part with excellent particle characteristics, it is preferable to process the ceramic part so that the maximum height roughness Rt is 15 μm or less. Specifically, the maximum height roughness Rt of the surface of the ceramic part may be 0 to 25 μm. The maximum height roughness Rt may be 0 to 12 μm. The maximum height roughness Rt may be 0.1 to 10 μm. The maximum height roughness Rt may be 0.1 to 10 μm. The maximum height roughness Rt may be 0 to 2 μm. When the ceramic part has such surface roughness characteristics, it is possible to suppress the ceramic part from forming particles in a plasma chamber by a physical method.

[0075] When the boron carbide sintered body from the second step is immediately shaped without undergoing heat treatment in the third step, the success rate of shaping is extremely low, less than 10%, almost 0%. It is believed that imbalances that occur within the boron carbide, such as imbalances in residual stress, are one of the important reasons why shaping workability is so low.

[0076] The ceramic parts of the embodiment are obtained by shaping a sintered body containing bulk boron carbide having a relatively large area, and the fact that boron carbide is one of the most difficult-to-cut materials is also thought to be one of the factors that affect the success rate of shaping.

[0077] The ceramic part may have a difference between an outer diameter and an inner diameter of 10 to 80 mm. The difference between the outer diameter and the inner diameter may be 15 to 60 mm. The difference between the outer diameter and the inner diameter may be 20 to 50 mm. The ceramic part may be a ring-shaped part having such a shape.

[0078] The ceramic part may have a thickness of 1 to 45 mm. The ceramic part may have a thickness of 1.5 to 40 mm, or the ceramic part may have a thickness of 2 to 38 mm.

[0079] The ceramic part may have an inner diameter of 160 mm or more. The ceramic part may have an inner diameter of 200 mm or more. The ceramic part may have an inner diameter of 300 mm or more. The ceramic part may have an inner diameter of 450 mm or less.

[0080] In order to make a sintered body containing boron carbide have such a large diameter, it is necessary to shape the sintered body having a relatively large area. In addition, boron carbide itself is a high-strength, difficult-to-cut material, and research and development to make boron carbide denser and stronger is ongoing, so the difficulties that may occur when shaping boron carbide become even greater.

[0081] The inventors have confirmed that when the boron carbide sintered body itself is damaged during shaping, for example when phenomena such as the occurrence of fractures or cracks occur, the measured imbalance of residual stress in the boron carbide sintered body is relatively severe. A boron carbide sintered body with fractures or cracks may cause partial unevenness in etching resistance, making it practically impossible to process into the shape of a ring-shaped part, and even if processing is successful, it is subject to disposal. Therefore, the inventors present as one feature of the embodiment that a boron carbide sintered body with a residual stress imbalance below a certain level can be processed into a ring-shaped part.

[0082] In the sintered body that has undergone the heat treatment, the standard deviation of the residual stress measured at positions 1, 2, and 3, which are spaced apart from each other by a distance of 100 mm or more, may be 10% or less of the average of the residual stresses measured at positions 1, 2, and 3. The standard deviation of the residual stress may be 7% or less of the average. The standard deviation of the residual stress may be 5% or less of the average. Furthermore, the standard deviation of the residual stress may be 0% or more of the average. The standard deviation of the residual stress may be 1% or more of the average.

[0083] When the boron carbide sintered body has such a characteristic of the standard deviation of the residual stress, the residual stress is distributed relatively uniformly throughout the boron carbide sintered body, and phenomena such as breakage, cracks, and defects caused by the imbalance of the residual stress can be significantly reduced.

[0084] On the other hand, the boron carbide of the second step (boron carbide before heat treatment, particularly in the case of a sintered body) may have a standard deviation of the residual stress measured at positions 1, 2, and 3, which are spaced apart by a distance of 100 mm or more from each other, that is more than 10% of the average of the residual stress measured at positions 1, 2, and 3.

[0085] The standard deviation of the residual stress of the boron carbide sintered body of the second step and the standard deviation of the residual stress of the boron carbide sintered body of the third step are expressed as relative values ​​to the average value. Usually, the average value of the residual stress of the boron carbide sintered body of the second step is larger than the average value of the residual stress of the boron carbide sintered body of the third step that has been heat-treated, so that the standard deviation value of the residual stress of the boron carbide sintered body that has been heat-treated in the third step may be smaller than that of the boron carbide sintered body before being heat-treated in the second step.

[0086] The positions 1, 2, and 3 may be measured, for example, at the edge, the center, and a point between the edge and the center of the disk-shaped boron carbide sintered body that is 100 mm or more apart from each other, provided that the positions 1, 2, and 3 are not located at the same distance from the center of the disk-shaped sintered body.

[0087] The boron carbide sintered body after the heat treatment in the third step and before shaping may have a standard deviation of residual stress measured at positions 1, 2, and 3, each of which is spaced apart by a distance of 100 mm or more, of 100 MPa or less. The standard deviation of residual stress may be 80 MPa or less. The standard deviation of residual stress may be 50 MPa or less. The standard deviation of residual stress may be 0 MPa or more. The standard deviation of residual stress may be 10 MPa or more. In such cases, more stable shaping is possible.

[0088] In the boron carbide sintered body after the heat treatment in the third step and before shaping, the difference in residual stress measured at positions 1 and 2, which are spaced apart by a distance of 100 mm or more, may be 300 MPa or less. The difference in residual stress measured at positions 1 and 2 may be 250 MPa or less. The difference in residual stress measured at positions 1 and 2 may be 200 MPa or less. The difference in residual stress measured at positions 1 and 2 may be 150 MPa or less. The difference in residual stress measured at positions 1 and 2 may be 120 MPa or less. When the difference in residual stress is relatively small in this way, more stable shaping is possible.

[0089] In the boron carbide sintered body after the heat treatment in the third step and before shaping, the difference between the maximum and minimum values ​​of residual stress measured at positions 1, 2, and 3, each of which is spaced apart by a distance of 100 mm or more, may be 300 MPa or less. The difference between the maximum and minimum values ​​may be 250 MPa or less. The difference between the maximum and minimum values ​​may be 200 MPa or less. The difference between the maximum and minimum values ​​may be 150 MPa or less. The difference between the maximum and minimum values ​​may be 120 MPa or less. When the difference between the maximum and minimum values ​​of residual stress is relatively small in this way, more stable shaping is possible.

[0090] In the boron carbide sintered body after the heat treatment in the third step and before the shape processing, the standard deviation of the residual stress measured at positions 1, 2, and 3, which are spaced apart from each other by 100 mm or more, may be within 7% of the average value of the residual stress measured at the positions 1, 2, and 3. The standard deviation of the residual stress measured at the positions 1, 2, and 3 may be within 5% of the average value of the residual stress measured at the positions 1, 2, and 3. The standard deviation of the residual stress measured at the positions 1, 2, and 3 may be within 3% of the average value of the residual stress measured at the positions 1, 2, and 3. The standard deviation of the residual stress measured at the positions 1, 2, and 3 may be more than 0% of the average value of the residual stress measured at the positions 1, 2, and 3. When the standard deviation of the residual stress has a small value compared to the average value of the residual stress, more stable shape processing is possible.

[0091] The above description of the residual stress has been given for the boron carbide sintered body before shaping, but it can also be partially applied to the boron carbide sintered body after shaping. In particular, the sintered body after shaping has a large difference between the residual stress measured on the surface corresponding to the outer diameter or the upper surface of the body close thereto, and the residual stress measured on the surface corresponding to the inner diameter or the upper surface of the mounting part close thereto.

[0092] When measuring residual stress in a boron carbide sintered body, which is a ring-shaped part, in a ring-shaped part including a body part and a mounting part having different thicknesses with a step therebetween, at least one point (PS3) can be measured on the top surface of the mounting part, and at least another point (PS1) can be measured on the top surface of the body part. When measuring in this manner, the presence or absence of imbalance in residual stress can be more clearly confirmed. The details will be described later.

[0093] The residual stress will be described based on the results measured by X-ray diffraction, although the method for measuring the residual stress is not limited thereto.

[0094] The ceramic component has a first height from a reference surface. Placement sectionand having a second height from the reference plane. Main unit the main body portion includes a main body portion upper surface, and the placement portion includes a placement portion upper surface.

[0095] The upper surface of the main body and the upper surface of the placement portion may be polished.

[0096] A more specific description of the ceramic parts will be omitted since it overlaps with the description below.

[0097] Ceramic parts 10 Fig. 1 is a schematic diagram illustrating a top view of a ceramic part according to an embodiment, and Fig. 2 is a schematic diagram illustrating a cross section of the ceramic part according to an embodiment. The ceramic part according to another embodiment will be described in more detail with reference to Figs. 1 and 2.

[0098] The ceramic part 10 according to the embodiment is Contains boron carbide, The residual stresses measured on the surface at two points at different distances from the center are S1 and S2, respectively. The difference between S1 and S2 is -600~+600 MPa may be also possible.

[0099] The ceramic component 10 includes a mounting portion 200 having a first height and a main body portion 100 having a second height. Although the main body portion 100 and the mounting portion 200 are described as being separate from each other, they may be provided separately from each other, or may be provided integrally without a boundary therebetween.

[0100] The placement portion 200 has a first height.

[0101] The body portion 100 has a second height.

[0102] The first height and the second height refer to the heights from a reference plane (eg, one selected from the bottom surface of the main body and the bottom surface of the placement portion) to the top surface of the main body and the top surface of the placement portion, respectively.

[0103] The first height and the second height may be different from each other, and specifically, the second height may be higher than the first height.

[0104] The placement portion 200 includes a placement portion upper surface 206. The placement portion and the placement portion upper surface may be an integral type without a separate layer, or the placement portion and the placement portion upper surface may be a divided type in which the layers are divided from each other when observed in cross section. In the divided type, the placement portion upper surface may be in the form of a deposition layer or a coating layer. The deposition layer or the coating layer may be, for example, a boron carbide layer. In the case where the placement portion upper surface is divided, the placement portion upper surface in the form of the deposition layer or the coating layer may have a thickness of 1 to 40% of the thickness of the placement portion based on the thickness before etching. The placement portion upper surface may have a thickness of 5 to 25% of the thickness of the placement portion based on the thickness before etching.

[0105] The body portion 100 includes a body portion upper surface 106. The body portion and the body portion upper surface may be of an integral type without a separate layer, or may be of a divided type in which the body portion and the body portion upper surface are divided into layers when observed in cross section. In the divided type, the body portion upper surface may be in the form of a deposition layer or a coating layer. The deposition layer or the coating layer may be, for example, a boron carbide layer. In the case where the body portion upper surface is of a divided type, the body portion upper surface in the form of the deposition layer or the coating layer may have a thickness of 1 to 40% of the thickness of the body portion based on the thickness before etching. The body portion upper surface may have a thickness of 5 to 25% of the thickness of the body portion based on the thickness before etching.

[0106] The ceramic part 10 may further include a connecting portion 150 that connects the mounting portion 200 and the main body portion 100 .

[0107] The placement part 200 and the body part 100 have different heights, and the connection part 150 can connect these different heights.

[0108] Although the main body 100, the placement portion 200, and the connection portion 150 are described as being separate from one another, they may be provided separately from one another or may be provided integrally without any boundary therebetween.

[0109] The connecting portion 150 includes a connecting portion upper surface 156 that connects the placement portion upper surface 206 and the main body portion upper surface 106 .

[0110] The connecting portion 150 and the connecting portion upper surface 156 may be of an integral type without a separate layer division, or may be of a divided type in which the connecting portion and the connecting portion upper surface are divided into layers when observed in cross section. In the divided type, the connecting portion upper surface may be in the form of a deposition layer or a coating layer. The deposition layer or the coating layer may be, for example, a boron carbide layer. In the case where the connecting portion upper surface is of a divided type, the connecting portion upper surface in the form of the deposition layer or the coating layer may have a thickness of 1 to 40% of the thickness of the connecting portion based on the thickness before etching. The connecting portion upper surface may have a thickness of 5 to 25% of the thickness of the connecting portion based on the thickness before etching.

[0111] Exemplarily, the connector angle (As) may be about 30° to about 70° based on the non-exposed surface of the mounting portion. The connector angle may be about 40° to about 60°. When the connector angle is such, the flow of plasma ions can be more stably controlled.

[0112] The connection part angle may be linear or non-linear when the top surface of the connection part is observed in cross-section as a whole, and the connection part angle is measured based on an imaginary line that connects two points, P1 (not shown) where the top surface of the mounting part meets the top surface of the connection part in the cross-section, and P2 (not shown) where the top surface of the connection part meets the top surface of the main body part.

[0113] The placement portion 200, the connection portion 150, and the main body portion 100 may each be ring-shaped, but are not limited to this and can be modified according to the application.

[0114] The ceramic part 10 is formed by forming a sintered body containing boron carbide, and may be composed of 90% by weight or more of boron carbide as a whole. The ceramic part may be composed of 93% by weight or more of boron carbide. The ceramic part 10 may further include an additional coating layer, etc., as necessary.

[0115] The ceramic part 10 may have a bending strength of 300 MPa or more. The bending strength may be 450 MPa or less.

[0116] The ceramic part 10 may have a difference between the outer diameter and the inner diameter of 10 to 80 mm and a thickness of 1 to 45 mm. Specific descriptions of the difference between the outer diameter and the inner diameter and the thickness are omitted because they overlap with the above descriptions.

[0117] The ceramic part 10 may have an inner diameter of 160 mm or more. A specific description of the inner diameter is omitted here because it overlaps with the above description.

[0118] The ceramic part 10 has residual stresses S1 and S2 measured on the surface at two points at different distances from the center, and the difference between S1 and S2 is -600 to +600. MPa The difference between S1 and S2 may be -300 to +300 MPa. The difference between S1 and S2 may be -200 to +200 MPa. The difference between S1 and S2 may be -150 to +150 MPa. A ceramic part having such characteristics can have more stable processability and stability.

[0119] The ceramic part 10 has residual stresses S1, S2, and S3 on the surface at different distances from the center, and the difference between the maximum and minimum values ​​of S1, S2, and S3 is -600 to +600. MPaThe difference between the maximum value and the minimum value may be -300 to +300 MPa. The difference between the maximum value and the minimum value may be -200 to +200 MPa. The difference between the maximum value and the minimum value may be -150 to +150 MPa. A ceramic part having such characteristics can have more stable processability and stability.

[0120] The difference between the maximum and minimum values ​​of the residual stress measured at a point PS1 on the upper surface of the main body and a point PS3 on the upper surface of the mounting portion may be within 40% of the average value of the PS1 and the PS3. The difference between the maximum and minimum values ​​of the residual stress measured at a point PS1 on the upper surface of the main body and a point PS3 on the upper surface of the mounting portion may be within 15% of the average value of the PS1 and the PS3. The difference between the maximum and minimum values ​​of the residual stress measured at a point PS1 on the upper surface of the main body and a point PS3 on the upper surface of the mounting portion may be within 10% of the average value of the PS1 and the PS3. The difference between the maximum and minimum values ​​of the residual stress measured at a point PS1 on the upper surface of the main body and a point PS3 on the upper surface of the mounting portion may be 1 to 10% of the average value of the PS1 and the PS3. A ceramic part having such characteristics can have more stable processability and stability.

[0121] The ceramic part 10 has a residual stress difference between a point PS1 on the upper surface of the main body and a point PS3 on the upper surface of the mounting portion of -600 to +600. MPaThe difference between the residual stress measured at PS1, which is a point on the upper surface of the main body, and the residual stress measured at PS3, which is a point on the upper surface of the mounting portion, may be -300 to +300 MPa. The difference between the residual stress measured at PS1, which is a point on the upper surface of the main body, and the residual stress measured at PS3, which is a point on the upper surface of the mounting portion, may be -200 to +200 MPa. The difference between the residual stress measured at PS1, which is a point on the upper surface of the main body, and the residual stress measured at PS3, which is a point on the upper surface of the mounting portion, may be -150 to +150 MPa. Also, the difference between the residual stress measured at PS1, which is a point on the upper surface of the main body, and the residual stress measured at PS3, which is a point on the upper surface of the mounting portion, may be -130 to +130 MPa. In such a case, a ceramic part having high density and excellent processability can be obtained.

[0122] The ceramic part 10 may have a standard deviation of residual stresses measured at a point PS1 on the upper surface of the main body, a point PS3 on the upper surface of the mounting part, and a point PS2 on the upper surface of the connecting part of 300 MPa or less. The standard deviation of residual stresses may be 250 MPa or less. The ceramic part may have a standard deviation of residual stresses measured at PS1, PS3, and PS2 of 150 MPa or less. The standard deviation of residual stresses may be 75 MPa or less. The standard deviation of residual stresses may be greater than 0 MPa. The standard deviation of residual stresses may be 0.1 MPa or more. When the ceramic part has such a standard deviation, a ceramic part having high density and excellent processability can be obtained.

[0123] The ceramic part 10 may have a standard deviation of the residual stresses measured in the PS1, PS3, and PS2, respectively, that is 20% or less of the average of the residual stresses measured in the PS1, PS2, and PS3. The standard deviation of the residual stresses measured in the PS1, PS3, and PS2, respectively, that is 15% or less of the average of the residual stresses measured in the PS1, PS2, and PS3. The standard deviation of the residual stresses measured in the PS1, PS3, and PS2, respectively, that is 10% or less of the average of the residual stresses measured in the PS1, PS2, and PS3. The standard deviation of the residual stresses measured in the PS1, PS3, and PS2, respectively, that is 8% or less of the average of the residual stresses measured in the PS1, PS2, and PS3. When the ceramic part has such characteristics, a ceramic part having a higher density and excellent processability can be obtained.

[0124] In the ceramic part 10, the difference between the residual stress measured in each of the PS1, PS3, and PS2 and the average of the residual stress measured in each of the PS1, PS2, and PS3 may be -350 to +350 MPa. The difference between the residual stress measured in each of the PS1, PS3, and PS2 and the average of the residual stress measured in each of the PS1, PS2, and PS3 may be -300 to +300 MPa. The difference between the residual stress measured in each of the PS1, PS3, and PS2 and the average of the residual stress measured in each of the PS1, PS2, and PS3 may be -250 to +250 MPa. The difference between the residual stress measured in each of the PS1, PS3, and PS2 and the average of the residual stress measured in each of the PS1, PS2, and PS3 may be -200 to +200 MPa. When the ceramic part has such characteristics, a ceramic part having higher density and excellent processability can be obtained.

[0125] The ceramic part 10 may have a difference between the maximum and minimum values ​​of the residual stresses measured by the PS1, the PS3, and the PS2 within 25% of the average. The ceramic part may have a difference between the maximum and minimum values ​​of the residual stresses measured by the PS1, the PS3, and the PS2 within 20% of the average. The ceramic part may have a difference between the maximum and minimum values ​​of the residual stresses measured by the PS1, the PS3, and the PS2 within 15% of the average. The ceramic part may have a difference between the maximum and minimum values ​​of the residual stresses measured by the PS1, the PS3, and the PS2 within 10% of the average. The ceramic part may have a difference between the maximum and minimum values ​​of the residual stresses measured by the PS1, the PS3, and the PS2 within 5% of the average. The ceramic part may have a difference between the maximum and minimum values ​​of the residual stresses measured by the PS1, the PS3, and the PS2 within 10% of the average. The ceramic part may have a difference between the maximum and minimum values ​​of the residual stresses measured by the PS1, the PS3, and the PS2 within 5% of the average. The ceramic part may have a difference between the maximum and minimum values ​​of the residual stresses measured by the PS1, the PS3, and the PS2 within 1% of the average. When the ceramic part has such a distribution of residual stresses, a more stable shape processing is possible, and a more stable etching-resistant material can be obtained.

[0126] The ceramic part 10 may have a standard deviation of residual stress measured at different points on the surface at different distances from the center of 350 MPa or less. The ceramic part may have a standard deviation of residual stress measured at different points on the surface at different distances from the center of 300 MPa or less. The standard deviation of residual stress measured at different points on the surface at different distances from the center of 250 MPa or less. The standard deviation of residual stress measured at different points on the surface at different distances from the center of 200 MPa or less. The ceramic part may have a standard deviation of residual stress measured at different points on the surface at different distances from the center of 120 MPa or less. The standard deviation of residual stress measured at different points on the surface at different distances from the center of 100 MPa or less. The standard deviation of residual stress measured at different points on the surface at different distances from the center of 0 MPa or more. The standard deviation of residual stress measured at different points on the surface at different distances from the center of 0 MPa or more. According to the results confirmed by the inventors, in the case of a ring-shaped sintered body, the difference between residual stresses measured at multiple points on the surface at the same distance from the center is not large. Therefore, when the focus ring has the above-mentioned characteristics, the distribution of residual stress is substantially uniform, so that the focus ring can be provided with excellent workability, stability, and the like.

[0127] As described above, the ceramic part 10 has been polished, and the maximum height roughness Rt of the upper surface of the main body is 10 μm or less, and the maximum height roughness Rt of the upper surface of the mounting portion may be 15 μm or less.

[0128] The ceramic component 10 may be polished, and the maximum height roughness Rt of the upper surface of the connecting portion may be 30 μm or less. The maximum height roughness Rt of the upper surface of the connecting portion may be 15 μm or less. The maximum height roughness Rt of the upper surface of the connecting portion may be 10 μm. The maximum height roughness Rt of the upper surface of the connecting portion may be 0.1 μm or more.

[0129] In this case, the problem of particle formation that may occur due to physical factors during plasma etching can be substantially suppressed.

[0130] Manufacturing method of focus ring and focus ring A method for manufacturing a focus ring according to an embodiment includes the steps of providing a material including boron carbide before processing, and manufacturing a focus ring by heat-treating the material and then shaping the material.

[0131] The step of manufacturing the focus ring may include a heat treatment process and a shaping process.

[0132] The step of manufacturing the focus ring may include a heat treatment process, a shaping process, and a polishing process.

[0133] The heat treatment includes a first treatment carried out at a first temperature for one hour or more and a second treatment carried out at a second temperature for one hour or more, the first temperature being higher than the second temperature.

[0134] The boron carbide before processing may be manufactured by a method for manufacturing a sintered body. The boron carbide before processing may be manufactured by a method for manufacturing a sintered body under pressure. The boron carbide before processing may be manufactured by a method for manufacturing a sintered body under normal pressure.

[0135] The boron carbide may be produced by a deposition method.

[0136] The method for producing the sintered body includes a first step of preparing raw material granules by slurrying and granulating a raw material composition containing boron carbide powder, and a second step of filling the raw material granules into a molding die and sintering the raw material granules to produce a sintered body in which the boron carbide powder particles are necked together.

[0137] In the method for manufacturing the focus ring, the heat treatment process, the raw material composition, the boron carbide powder, the first step, the second step, sintering, etc. are the same as those described above, so descriptions thereof will be omitted.

[0138] The focus ring includes a mounting portion having a first height from a reference surface and a main body portion having a second height from the reference surface, the mounting portion including a mounting portion upper surface on which an etching target is placed, and the main body portion including a main body portion upper surface that is directly etched by plasma.

[0139] The difference between the residual stresses measured at a point PS1 on the upper surface of the mounting portion and a point PS3 on the upper surface of the main body portion is within 40% of the average value of the residual stresses measured at PS1 and PS3.

[0140] Fabricating the focus ring includes a shaping process that includes etching or cutting the material into a shape of a focus ring that includes the mounting portion and the body portion.

[0141] The step of manufacturing the focus ring may further include a polishing step after the shaping step.

[0142] The polishing step is a step of polishing the upper surface including the upper surface of the mounting portion and the upper surface of the main body portion to adjust the surface roughness.

[0143] The shaping and polishing processes are the same as those described above, and therefore will not be described here.

[0144] The focus ring according to the embodiment includes: Contains boron carbide, A mounting portion having a first height from a reference surface and a main body portion having a second height from the reference surface, the placement portion includes a placement portion upper surface on which an etching target is placed, the body includes a body upper surface that is directly etched by a plasma; a difference between the residual stresses measured at a point PS1 on the upper surface of the mounting portion and a point PS3 on the upper surface of the main body portion is within 40% of the average value of the residual stresses measured at PS1 and PS3; The residual stresses measured on the surface at two points at different distances from the center are S1 and S2, respectively. The difference between S1 and S2 is -600~+600 MPa may be also possible.

[0145] The residual stress measured in PS1 may be greater than the residual stress measured in PS3.

[0146] The focus ring may have a standard deviation of residual stress measured at three points on the surface that are different distances from the center of the focus ring of 350 MPa or less.

[0147] The focus ring may further include a connection portion between the mounting portion and the main body portion.

[0148] The connection portion of the focus ring may include a connection portion upper surface that connects the placement portion upper surface and the main body portion upper surface.

[0149] The focus ring has a point PS2 on the upper surface of the connecting portion.

[0150] The focus ring may be such that a difference between the maximum and minimum values ​​of the residual stress measured in each of the PS1, PS2, and PS3 is within 25% of an average of the residual stress measured in each of the PS1, PS2, and PS3.

[0151] The standard deviation of the residual stresses measured in each of the PS1, PS2, and PS3 may be 20% or less of the average of the residual stresses measured in the PS1, PS2, and PS3.

[0152] The standard deviation of the residual stresses measured in each of the PS1, PS2 and PS3 may be 300 MPa or less.

[0153] The residual stresses measured in the PS1, PS2 and PS3 may have differences from their averages of -350 to +350 MPa.

[0154] The focus ring may have a bending strength of 300 MPa or more.

[0155] The focus ring may have a thickness of 1 to 45 mm.

[0156] The focus ring may include boron carbide and have a thickness of 1 to 45 mm.

[0157] The focus ring may have an inner diameter of the mounting portion of 160 mm or more.

[0158] The focus ring may have a difference between an outer diameter of the main body and an inner diameter of the mounting portion of 10 to 80 mm.

[0159] Other characteristics of the residual stress of the focus ring, the characteristics of the residual stress at two points and three points at different distances from the center, and the characteristics of the surface roughness have been described above, and therefore will not be described here.

[0160] The center of the focus ring refers to the center of the circle in a ring-shaped focus ring, and the center of a non-ring-shaped focus ring refers to the intersection point of the major axis and minor axis.

[0161] Method for manufacturing semiconductor device A method for manufacturing a semiconductor device according to an embodiment includes a process for etching a substrate using the above-described focus ring to manufacture a semiconductor device.

[0162] The substrate may be a Si substrate, a SiC substrate, or a GaN substrate.

[0163] The present invention will be described in more detail with reference to the following specific examples. The following examples are merely illustrative for the purpose of aiding understanding of the present invention, and are not intended to limit the scope of the present invention.

[0164] Example 1. Manufacturing of ceramic parts 1) Manufacturing of disk-shaped sintered bodies using pressure sintering Boron carbide powder (particle size D) was mixed with the content ratio shown in Table 1 below. 50 Raw materials such as cellulose acetate (0.7μm) and phenol resin (residual carbon rate of about 42% by weight) and a solvent were placed in a slurry blender and mixed using a ball mill to produce a slurried raw material. This slurried raw material was spray-dried to produce a granulated raw material.

[0165] The granulated raw material was filled into a disk-shaped molding die, and the temperature, pressure and time shown in Table 1 below were applied to produce a pressure-sintered disk-shaped sintered body (before heat treatment) having a diameter of about 488 mm.

[0166] In heat treatment 1, the pressure-sintered disk-shaped sintered body was heat-treated at a temperature of 1400 to 1600° C. for 2 to 5 hours.

[0167] In heat treatment 2, the pressure sintered disk-shaped sintered body was subjected to a primary treatment at a temperature of 1650 to 1950° C. for 2 to 3.5 hours, and then a secondary treatment at a temperature of 1400 to 1600° C. for 3 to 6 hours.

[0168] In heat treatment 3, the pressure sintered disk-shaped sintered body was subjected to a primary treatment at a temperature of 1650 to 1950° C. for 4 to 6 hours, and then a secondary treatment at a temperature of 1400 to 1600° C. for 3 to 6 hours.

[0169] 2) Manufacturing of disk-shaped sintered bodies using the normal pressure sintering method Boron carbide powder (particle size D) was mixed with the content ratio shown in Table 1 below. 50 Raw materials such as cellulose acetate (0.7μm) and phenol resin (residual carbon rate of about 42% by weight) and a solvent were placed in a slurry blender and mixed using a ball mill to produce a slurried raw material. This slurried raw material was spray-dried to produce a granulated raw material.

[0170] The granulated raw material was filled into a rubber mold having a disk-shaped hollow, loaded into a CIP (Cold Isostatic Press) device, and pressed to produce a green body having an outer diameter of about 488 mm or more. This green body was green processed to have the shape of a focus ring, and then carbonized. The green body that had been carbonized was atmospherically sintered in a sintering furnace at the temperature and time shown in Table 1 below. A disk-shaped sintered body having a diameter of 488 mm and a hollow was produced. Each disk-shaped sintered body is abbreviated as "sample" in Table 1 below.

[0171] [Table 1] *Additive 1 applies phenolic resin. **Additive 2 applies boron oxide.

[0172] 3) Measurement of residual stress in disk-shaped sintered bodies The residual stress of the disk-shaped sintered body was measured using X-ray diffraction.

[0173] Residual stress was measured at three points: position 1, which was the center of a disk-shaped sintered body with a diameter of about 488 mm; position 3, which was within 10% of the diameter from the edge; and position 2, which was the middle point between positions 1 and 3. Positions 1, 2, and 3 are each located at a distance of 100 mm or more. Pressurized sample 2 Using this method, the degree of residual stress with and without heat treatment was confirmed, and the results are shown in Table 2 below.

[0174] The disk-shaped sintered compacts used in the measurements were manufactured in various thicknesses ranging from 8 to 40 mm. In Table 2 below, the normal pressure sintered disk-shaped sintered compacts are abbreviated as normal pressure samples, and the pressure sintered disk-shaped sintered compacts are abbreviated as pressure samples. The heat treatment in Table 2 below was the heat treatment 3 described above. The standard deviation in Table 2 below was calculated by applying the STDEV.P function in Microsoft Excel (the same applies to the measurement of standard deviation below).

[0175] [Table 2]

[0176] Referring to Table 2, it was confirmed that there was a significant difference in residual stress depending on the position between the heat-treated and non-heat-treated pressurized samples. In particular, the average values ​​of residual stress measured at three different positions did not show a large difference, but the standard deviation showed a difference of about 3.6 times or more, and the difference between the maximum and minimum values ​​also showed a difference of about 3.7 times or more. It is believed that such a difference is one of the causes of the crack phenomenon that occurs with a very high probability during the shape processing process described below.

[0177] 4) Shape processing into ring-shaped ceramic parts The pressure-sintered disk-shaped sintered compacts produced in the above 1) were shaped after both heat treatment and no heat treatment. The atmospheric pressure-sintered disk-shaped sintered compacts produced in the above 2) were also shaped. Focus rings having the configurations shown in Figs. 1 and 2 were produced as ceramic parts.

[0178] The ceramic part had a ring-like shape with an outer diameter of about 388 mm, an inner diameter of about 300 mm, a mounting portion on which the edge of the ceramic part was mounted having a height of about 2.5 mm, and an upper surface having a height of about 4.5 mm.

[0179] In the case of the pressureless sintered disk-shaped sintered body, the shape was processed by applying an electric discharge machine, whereas in the case of the pressure sintered disk-shaped sintered body, the shape was processed by applying a water jet method.

[0180] Each sample was evaluated as having shaping workability only if the sintered body did not break or crack until shaping was completed, and the test quantity and success rate of shaping workability (the ratio of focus rings that did not break or crack until shaping was completed to the total number of applied disk-shaped sintered bodies) were evaluated according to each manufacturing method / heat treatment method, and are shown in Table 3 below.

[0181] [Table 3]

[0182] . Referring to Table 3, unlike the case of normal pressure sintering, it was confirmed that in the case of pressure sintering, the presence or absence of heat treatment and the type of heat treatment performed are important in relation to the presence or absence of shape workability. This is considered to be a result related to the measurement results of residual stress in Table 2, and it is considered that the imbalance of residual stress in the sintered body formed during pressure molding causes cracks to occur in the sintered body itself or the sintered body itself to break during the shape processing process of the focus ring, which requires relatively precise shape processing. In the case of heat treatment 2 and heat treatment 3, it is considered that the shape workability was improved due to factors such as removing such residual stress through sufficient heat treatment. The ceramic parts manufactured in this way were subjected to a polishing process and then the following physical property evaluation was applied.

[0183] Example 2. Evaluation of the physical properties of ceramic parts The produced ceramic parts were used to evaluate the following physical properties. 1) Evaluation of relative density The relative density (%) was measured by the Archimedes method, and the results are presented in Table 4 below.

[0184] 2) Evaluation of bending strength Ten ceramic parts were prepared and the flexural strength was measured using UTM equipment (manufacturer: H&P) in accordance with ASTM C 1161 Flexual Strength. The average of the values ​​excluding the minimum and maximum values ​​is shown in Table 4 below.

[0185] 3) Measurement of surface roughness and the presence or absence of particles The presence or absence of particle formation was evaluated based on the presence or absence of particles remaining in the atmosphere during the etching rate characteristic evaluation or in the chamber of the equipment after the evaluation. The surface roughness was measured based on the maximum height roughness, and after measuring four or more samples on each of the top surface of the main body and the top surface of the mounting part, the average was calculated and measured to be about 10.7 μm for the top surface of the main body and about 4.6 μm for the top surface of the mounting part.

[0186] Each ceramic part is abbreviated as "sample" in the following Table 4. The applied ceramic parts all had a thickness of about 5 mm, an outer diameter of about 388 mm, and an inner diameter of 290 mm or more.

[0187] [Table 4]

[0188] From the above results, it was confirmed that the normal pressure sample showed a significant difference in bending strength compared to the pressurized sample. This difference indicates that even samples with similar relative density can show a significant difference in bending strength due to differences in manufacturing methods, and it is believed that the measurement of bending strength is one of the characteristics that can distinguish between pressed ceramic parts and normal pressure ceramic parts.

[0189] It was confirmed that no particles were generated in the plasma atmosphere containing fluorine or chlorine in the plasma equipment for both the pressurized and normal pressure samples. It was also confirmed that machining into the shape of a ceramic part with a relatively small difference between the outer and inner diameters and a relatively thin thickness is possible for both the normal pressure samples and the pressurized samples when they are subjected to heat treatment.

[0190] 4) Measurement of residual stress in ceramic parts The sample that underwent heat treatment 1 was named Sample 1, the sample that underwent heat treatment 2 was named Sample 2, and the sample that underwent heat treatment 3 was named Sample 3. The residual stress was measured on the surface of the ring-shaped part using X-ray diffraction.

[0191] The residual stress of the ceramic part manufactured as described above was measured on the top surface of the main body (PS1, 206 in FIG. 2), the top surface of the connection part (PS2, 156 in FIG. 2), and the top surface of the mounting part (PS3, 106 in FIG. 2), and the results are shown in Table 5 below. The top surface of the main body is indicated as position 1, the top surface of the connection part as position 2, and the top surface of the mounting part as position 3.

[0192] Additionally, although not shown in the table below, no significant differences in residual stress were observed between the top surfaces of the main body portions of the same sample, between the top surfaces of the connecting portions of the same sample, or between the top surfaces of the mounting portions of the same sample.

[0193] [Table 5] *All difference values ​​are absolute values. Abbreviated as PS1, PS2, and PS3, they represent the residual stress values ​​at each point. **% difference means the % difference value relative to the mean value. #Residual stress and standard deviation are obtained by averaging residual stress values ​​measured several times while rotating a sample using XRD, and the standard deviation of the measured values ​​used to calculate the residual stress is presented as the standard deviation.

[0194] Referring to the results in Table 5, it was shown that the sintered body was processed into a ring-shaped part by performing the heat treatment of the embodiment. All of the above samples 1 to 3 have in common that they can be shaped, but there were differences in the level of residual stress measured for each.

[0195] The difference in residual stress values ​​between PS3 and PS1 was greatest for sample 1, followed by sample 3 and sample 2. On the other hand, the standard deviation of the residual stress values ​​measured at positions PS1 to PS3 was smallest for sample 3, followed by sample 2. The average residual stress itself was greater for sample 3 than for sample 2. It is believed that there may be some difference in the residual stress values ​​remaining in the material itself due to various reasons such as the manufacturing process and processing method. Such differences between residual stress values ​​are believed to indicate an imbalance in residual stress within the same sample, and therefore the lower the value or ratio, the higher the processing efficiency and the more applicable various processing methods are.

[0196] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the appended claims also fall within the scope of the present invention. [Explanation of symbols]

[0197] 1 Etching target 10 Focus ring, ceramic part 100 Main body 200 Placement section 106 Main body top surface 206 Top surface of mounting section 150 Connection section 156 Top surface of connection part

Claims

1. 1. A ceramic component comprising boron carbide, The sum of carbon and boron in the ceramic part is 90 mol % or more, Residual stresses measured on the surface of the ceramic component at two points at different distances from the center of the ceramic component are S1 and S2, respectively; The S1 and S2 are spaced apart from each other by 100 mm or more. A ceramic part, wherein the difference between S1 and S2 is −150 to +150 MPa.

2. Residual stresses on the surface at different distances from the center of the ceramic component are S1, S2, and S3, respectively; The S1, S2 and S3 are spaced apart from each other by 100 mm or more, The ceramic part according to claim 1, wherein the difference between the maximum value and the minimum value in S1, S2, and S3 is −150 to +150 MPa.

3. The ceramic part is a part applied to a plasma etching device, The component includes a mounting portion having a first height from a reference surface and a main body portion having a second height from the reference surface; The body portion includes a body portion upper surface, The placement portion includes a placement portion upper surface, 2. The ceramic part according to claim 1, wherein a difference between the residual stress measured on the upper surface of the main body and the residual stress measured on the upper surface of the mounting portion is −150 to +150 MPa.

4. 1. A focus ring comprising boron carbide, the focus ring contains carbon and boron in a total amount of 90 mol % or more, The device includes a mounting portion having a first height from a reference surface and a main body portion having a second height from the reference surface, the placement portion includes a placement portion upper surface on which an etching target is placed, the body includes a body upper surface that is directly etched by a plasma; a difference between the residual stresses measured at a point PS1 on the upper surface of the mounting portion and a point PS3 on the upper surface of the main body portion is within 40% of an average value of the residual stresses measured at PS1 and PS3; Residual stresses measured at two points on the surface of the focus ring that are spaced apart from the center of the focus ring are S1 and S2, respectively; The S1 and S2 are spaced apart from each other by 100 mm or more. The difference between S1 and S2 is −150 to +150 MPa.

5. 5. The focus ring of claim 4, wherein a standard deviation of residual stresses measured at three points on the surface of the focus ring that are different distances from a center of the focus ring is 350 MPa or less.

6. A connecting portion is further included between the mounting portion and the main body portion, the connecting portion includes a connecting portion upper surface that connects the placement portion upper surface and the main body portion upper surface, The focus ring of claim 4 , further comprising a point PS2 on the upper surface of the connecting portion.

7. 7. The focus ring of claim 6, wherein a difference between a maximum value and a minimum value of the residual stresses measured at each of PS1, PS2, and PS3 is within 25% of an average of the residual stresses measured at each of PS1, PS2, and PS3.

8. 5. The focus ring according to claim 4, wherein the focus ring has a bending strength of 300 MPa or more.

9. A first step of preparing raw material granules by slurrying and granulating a raw material composition including boron carbide powder; A second step of filling the raw material granules into a molding die and sintering them at a temperature of 1800° C. or more and a pressure of 15 MPa or more to produce a sintered body in which the boron carbide powder particles are necked together; and a third step of heat-treating the sintered body and then shaping the same to manufacture a ceramic part. The heat treatment includes a first treatment performed at a first temperature for one hour or more and a second treatment performed at a second temperature for one hour or more, the first temperature being higher than the second temperature; The sum of carbon and boron in the ceramic part is 90 mol % or more, Residual stresses measured on the surface of the ceramic component at two points at different distances from the center of the ceramic component are S1 and S2, respectively; The S1 and S2 are spaced apart from each other by 100 mm or more. The method for manufacturing a ceramic part, wherein the difference between S1 and S2 is −150 to +150 MPa.

10. The first temperature is equal to or greater than 1650° C. The method of claim 9, wherein the second temperature is 1400° C. or higher.

Citation Information

Patent Citations

  • Preparation of boron carbide system polycrystal high density molded article by non-pressure sintering

    JP1995097264A

  • Boron carbide joined body, method for producing the same and plasma-resistant member

    JP2001261457A

  • Cutting tool

    JP2003231005A

  • Low thermal expansion ceramic member, method of manufacturing the same, and member for semiconductor manufacture apparatus

    JP2004161512A

  • Free-standing silicon carbide articles formed by chemical vapor deposition and methods for making them

    JP2007513257A