Perovskite-based oxidation catalyst for anion exchange membrane water electrolysis and method for producing the oxidation catalyst using coprecipitation method

The perovskite-based oxide catalyst, produced via coprecipitation at low temperatures, addresses the issues of high-temperature particle growth by ensuring a uniform particle size and oxygen vacancy sites, enhancing conductivity and durability for anion exchange membrane water electrolysis.

JP7595768B2Active Publication Date: 2024-12-06HANWHA SOLUTIONS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023530706
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-24
Filing Date
2021-11-23
Publication Date
2024-12-06
Estimated Expiration
2041-11-23

AI Technical Summary

Technical Problem

Existing perovskite-based oxidation catalysts for anion exchange membrane water electrolysis suffer from high-temperature particle growth, leading to reduced surface area and insufficient electrical conductivity and durability, making them unsuitable for commercial applications.

Method used

A perovskite-based oxide catalyst represented by La1-xSrxCoy is produced through a coprecipitation method at low temperatures, allowing for controlled particle size and distribution, and incorporating oxygen vacancy sites for enhanced catalytic activity and conductivity.

Benefits of technology

The catalyst exhibits superior electrical conductivity, catalytic activity, and durability, suitable for anion exchange membrane water electrolysis systems, with a large surface area and stable performance even after numerous cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595768000003
    Figure 0007595768000003
  • Figure 0007595768000004
    Figure 0007595768000004
  • Figure 0007595768000005
    Figure 0007595768000005
Patent Text Reader

Abstract

The present invention relates to an oxidation catalyst for anion exchange membrane water electrolysis that exhibits excellent catalytic activity and electrical conductivity, a uniform particle size distribution, a large surface area, and excellent durability, a method for producing the same, and an oxidation electrode for anion exchange membrane water electrolysis and an anion exchange membrane water electrolysis system including the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Cross-reference to related application(s) This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0158897 filed on November 24, 2020, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a perovskite-based oxidation catalyst for anion exchange membrane water electrolysis that exhibits excellent catalytic activity and electrical conductivity, uniform particle size distribution, wide surface area, and excellent durability, a method for producing the oxidation catalyst using a coprecipitation method, and an oxidation electrode for anion exchange membrane water electrolysis and an anion exchange membrane water electrolysis system including the same. [Background technology]

[0003] Water electrolysis is a technology that produces hydrogen by electrically splitting water, which was developed in the 1800s and has been used for commercial hydrogen production since the 1920s. Recently, as the need for and share of renewable energy has increased significantly, it has been attracting attention as a solution for low-carbon, green hydrogen production.

[0004] The main water electrolysis technologies currently being commercially applied are the alkaline water electrolysis (AWE) system and the proton exchange membrane water electrolysis (PEMWE) system.

[0005] Among these, alkaline water electrolysis is cost-competitive because it uses inexpensive nickel-based electrodes and porous membranes, but it has the disadvantage that it can only operate at low current density because the gap between the porous diaphragm and the electrode is wide, resulting in high internal resistance.Also, alkaline water electrolysis systems have the disadvantages of being large in stack volume, high operating costs, and being difficult to connect to renewable energy sources such as wind or solar power because it is difficult to change the current density suddenly due to the use of porous diaphragms.

[0006] Meanwhile, cation exchange membrane water electrolysis systems are currently being developed on a megawatt scale. Such cation exchange membrane water electrolysis systems can be operated at high current density, allowing for a compact system design, and produce high purity hydrogen while maintaining low initial output pressure and minimum load. In addition, their fast response speed makes them suitable for producing hydrogen in conjunction with renewable energy.

[0007] However, the cation exchange membrane water electrolysis system has a drawback in that the overall manufacturing cost is significantly increased because an expensive precious metal catalyst and a bipolar plate made of precious metal must be used to prevent corrosion.

[0008] Therefore, an anion exchange membrane water electrolysis system has been proposed as a technology to replace the alkaline water electrolysis system and the cation exchange membrane water electrolysis system currently being applied commercially, and interest and research thereon have been significantly increased.

[0009] Such an anion exchange membrane water electrolysis system can be designed compactly and can use non-precious metal materials because it is operated in the same atmosphere as the alkaline water electrolysis system. Therefore, such an anion exchange membrane water electrolysis system can be considered as a system that can utilize the advantages of both the alkaline water electrolysis system and the cation exchange membrane water electrolysis system.

[0010] However, in order to improve the performance of such an anion exchange membrane water electrolysis system, an oxidation catalyst that exhibits excellent electrical conductivity and catalytic activity and also has high durability is required at an oxidation electrode (anode) where an oxygen generation reaction accompanied by a larger overvoltage, for example, the reaction represented by the following reaction formula, occurs.

[0011] [Reaction Scheme 1] 4OH - →O2+2H2O+4e -

[0012] Considering that the anion exchange membrane water electrolysis system operates at a low temperature of about 100° C. or less, precious metal catalysts such as IrO2 or RuO2 have been considered as oxidation catalysts that meet the above requirements. However, these precious metal catalysts are expensive and difficult to commercialize, making it difficult to utilize the advantages of the anion exchange membrane water electrolysis system.

[0013] Therefore, research has been ongoing recently to apply layered double hydroxides (LDH), perovskite-based compounds, or spinel-based compounds as the oxidation catalyst. However, although the layered double hydroxides and spinel-based compounds have relatively high catalytic activity, they have low electrical conductivity and are therefore not suitable for use as oxidation catalysts.

[0014] In contrast, perovskite-based compounds are oxides represented by the general formula ABO3 (A is an alkaline earth metal or rare earth metal, and B is a transition metal), and their lattice oxygen reversibly participates in the oxygen evolution reaction, exhibiting excellent catalytic activity, as well as excellent electrical conductivity through doping with various metal atoms.

[0015] However, since the existing perovskite-based compounds are mainly produced by a solid-phase reaction at a relatively high temperature exceeding 1000°C, the particle size of the compound particles increases and the surface area decreases during the high-temperature reaction process, which often reduces the catalytic activity.In addition, the existing perovskite-based compounds do not have sufficient electrical conductivity and durability, so that a good oxidation catalyst that is applied to an anion exchange membrane water electrolysis system and shows excellent properties has not yet been developed.

[0016] Therefore, there is a continuing need for the development of perovskite-based oxidation catalysts that have excellent catalytic activity, electrical conductivity, and durability, and that can be manufactured to have large surface areas. Summary of the Invention [Problem to be solved by the invention]

[0017] Therefore, an object of the present invention is to provide a perovskite-based oxidation catalyst for anion exchange membrane water electrolysis, which can be provided to have a uniform particle size distribution and a wide surface area at a relatively low temperature and can have a large number of oxygen vacancies, and thus exhibits excellent catalytic activity, electrical conductivity, and durability, and a manufacturing method thereof.

[0018] Another object of the present invention is to provide an oxidation electrode for anion exchange membrane water electrolysis, and an anion exchange membrane water electrolysis system, which contain the oxidation catalyst. [Means for solving the problem]

[0019] Therefore, the present invention provides a perovskite-based oxidation catalyst for anion exchange membrane water electrolysis, comprising a perovskite-based oxide represented by the following Chemical Formula 1:

[0020] [Chemical formula 1] La 1-x Sr x Chief of Staff 3-y

[0021] In the above Chemical Formula 1, 0≦x≦1 and 0≦y≦0.3.

[0022] The present invention also relates to a method for producing a catalyst precursor comprising the steps of co-precipitating a lanthanum salt, a strontium salt and a cobalt salt in an aqueous solvent having a pH of 12 or greater in the presence of a chelating agent to form a catalyst precursor; and The method for preparing the perovskite-based oxidation catalyst including the oxide of Formula 1 includes calcining the catalyst precursor at a temperature of 500° C. or more to form the perovskite-based oxide of Formula 1.

[0023] The present invention also relates to a porous metal structure; and The present invention provides an oxidation electrode for anion exchange membrane water electrolysis, comprising a catalyst layer including the perovskite-based oxidation catalyst formed on the porous metal structure.

[0024] The present invention also relates to an anion exchange membrane; a reduction electrode located on one side of the anion exchange membrane; and An anion exchange membrane water electrolysis system is provided, the anion exchange membrane water electrolysis system including the oxidation electrode located on the other side of the anion exchange membrane such that the catalyst layer is in contact with the anion exchange membrane. Effect of the Invention

[0025] The perovskite-based oxidation catalyst of the present invention can be prepared and provided by precisely controlling the composition of constituent atoms at a relatively low temperature using a coprecipitation method, and as a result, the oxidation catalyst of the present invention can be provided with smaller particle size, uniform particle size distribution, and a larger surface area.

[0026] In addition, the oxidation catalyst of the present invention can be prepared and provided to have a large number of oxygen vacancies in the lattice structure by adjusting the molar ratio of lanthanum and strontium contained therein. Such oxygen vacancies can act as catalytic active sites and promote charge transfer.

[0027] Therefore, it was confirmed that the perovskite-based oxidation catalyst of the present invention not only has excellent electrical conductivity and catalytic activity, but also has very excellent durability due to its structural stability.

[0028] Due to the excellent overall physical properties of the oxidation catalyst, the perovskite-based oxidation catalyst can be very suitably applied to an anion exchange membrane water electrolysis system. [Brief description of the drawings]

[0029] [Figure 1] 1a to 1f are scanning electron microscope (SEM) photographs of the anion-exchange membrane water electrolysis oxidation catalysts prepared in Examples 1 to 6. [Diagram 2] 2a to 2e are scanning electron microscope (SEM) photographs of the anion exchange membrane water electrolysis oxidation catalysts prepared in Examples 6 to 10 (however, FIG. 2a for Example 6 is shown on a different scale from FIG. 1f). [Diagram 3] FIG. 3 is a photograph showing a comparison of the results when the oxidation catalysts of Examples 6 to 10 were dispersed in a solvent. [Figure 4] FIG. 4a is a diagram showing a comparison of the results of XRD analysis of the oxidation catalysts of Examples 1 to 6, and FIG. 4b is a diagram showing an enlarged XRD spectrum of the oxidation catalyst of Example 6 for crystal structure analysis. [Diagram 5] FIG. 5a is a linear sweep voltage (LSV) graph showing the current density (mA / cm2) measured in the voltage range of 1.2 to 1.8 V for the oxidation catalysts of Examples 1 to 6, and FIG. 5b is an LSV graph showing the current density (mA / cm2) measured in the voltage range of 1.2 to 1.8 V for the oxidation catalysts of Examples 6 to 10. [Figure 6] FIG. 6 is a graph showing the results of measuring the Tafel slope for the oxidation catalysts of Examples 6 to 10. [Figure 7] FIG. 7 is a graph showing the results of measuring the impedance at 1.62 V for the oxidation catalysts of Examples 6 to 8. [Figure 8]8a to 8c are diagrams showing the results of evaluating the durability of the oxidation catalyst of Example 7 by operating it for 1000 cycles using a CV (Cyclic voltammetry) method and a LSV (Linear sweep voltage) method. [Figure 9a] FIG. 9a is a graph showing the results of measuring the change in current density while increasing the voltage in the anion exchange membrane water electrolysis system manufactured using the oxidation catalyst of Example 7. [Figure 9b] FIG. 9b is a graph showing the results of measuring the voltage change over operation time at a constant current density for the anion exchange membrane water electrolysis system manufactured using the oxidation catalyst of Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] In the present invention, the terms "first", "second", etc. are used to describe various components, and the terms are used only for the purpose of distinguishing one component from another component.

[0031] In addition, the terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In this specification, the terms "include", "includes", "has" and the like are intended to specify the presence of an embodied feature, number, step, component, or combination thereof, and should be understood not to preclude the presence or additional possibility of one or more other features, numbers, steps, components, or combinations thereof.

[0032] In addition, in this specification, when a layer or element is referred to as being formed "on" another layer or element, this means that the layer or element is formed directly on the layer or element, or that other layers or elements may be additionally formed between the layers, on the object, or on the substrate.

[0033] The present invention can be modified in various ways and can have various forms, and will be described in detail below by taking specific embodiments as examples. However, it should be understood that the present invention is not limited to the specific disclosed embodiments, but includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention.

[0034] Hereinafter, an oxidation catalyst for anion exchange membrane water electrolysis and a manufacturing method thereof according to embodiments of the present invention, as well as an oxidation electrode and an anion exchange membrane water electrolysis system including the same will be described in detail.

[0035] According to one embodiment of the present invention, there is provided a perovskite-based oxidation catalyst for anion exchange membrane water electrolysis, comprising a perovskite-based oxide represented by the following Chemical Formula 1:

[0036] [Chemical formula 1] La 1-x Sr x Chief of Staff 3-y

[0037] In the above Chemical Formula 1, 0≦x≦1 and 0≦y≦0.3.

[0038] The present inventors have conducted extensive research to develop an oxidation catalyst having excellent general properties suitable for application to an anion exchange membrane water electrolysis system. As a result of such research, it has been found that the perovskite-based oxide of Formula 1 can be prepared and provided at a low temperature, for example, 1000° C. or less, by using a coprecipitation method.

[0039] Therefore, it has been confirmed that the oxide particles can be prevented from agglomerating and growing during a high-temperature solid-phase reaction process, and the perovskite-based oxide can be provided with a smaller particle size and a uniform particle size distribution. In addition, by enabling a low-temperature production process using the co-precipitation method, it is possible to prevent surface defects or oxygen vacancies, which can act as catalytic active sites in the lattice structure of the perovskite-based oxide, from being filled by a high-temperature reaction. Therefore, the oxidation catalyst of one embodiment can exhibit a larger surface area and excellent oxidation catalytic activity.

[0040] In addition, it was confirmed that the perovskite oxide contains two rare earth metal elements, lanthanum and strontium, and can be prepared and provided to have a large number of oxygen vacancies in the lattice structure by adjusting the molar ratio of lanthanum and strontium. It is predicted that the generation of such oxygen vacancies occurs when lanthanum ions having an oxidation number of +3 are replaced by strontium ions having an oxidation number of +2, resulting in oxygen deficiency. The oxygen vacancies in the lattice structure can act as catalytic active sites and promote the transfer of charges, so that the oxidation catalyst containing the perovskite oxide of Formula 1 can simultaneously exhibit excellent catalytic activity and electrical conductivity.

[0041] Furthermore, it has been confirmed that the perovskite-based oxide has excellent structural stability and therefore has excellent durability, maintaining excellent electrical conductivity and activity even when operated for up to about 1000 cycles.

[0042] As a result, the oxidation catalyst of an embodiment includes the perovskite-based compound of Formula 1, and can exhibit excellent electrical conductivity, catalytic activity, and durability, and can be provided with a large surface area, so that the oxidation catalyst can be very suitably applied to an anion exchange membrane water electrolysis system and its oxidation electrode (anode).

[0043] Meanwhile, in the above formula 1, x represents the molar ratio of strontium, and y represents the ratio of oxygen vacancy sites. In the oxide of formula 1, the oxygen vacancy sites can act as catalytic active sites and promoters that facilitate the generation of intermediate products in the oxygen generation reaction of the following reaction formula 1 that occurs at the oxidation electrode of a water electrolysis system, and can promote the transfer of charges.

[0044] [Reaction Scheme 1] 4OH - →O2+2H2O+4e -

[0045] Therefore, in terms of the excellent electrical conductivity and catalytic activity of the oxidation catalyst of the above-described embodiment, y can have a value exceeding 0, and can have a range of 0 < y ≦ 0.3, or 0.0001 ≦ y ≦ 0.1. However, if the ratio of oxygen defect sites increases excessively, the structural stability of the oxidation catalyst may decrease.

[0046] The ratio of the oxygen defect sites can be adjusted by the temperature in the coprecipitation reaction stage during the production process of Chemical Formula 1, the molar ratio of strontium, etc. More specifically, in order to increase the ratio of the oxygen defect sites, it is preferable to increase the ratio x at which lanthanum ions having an oxidation number of +3 are substituted with strontium ions having an oxidation number of +2. In such an aspect, x preferably has a range of 0.7 ≦ x ≦ 1.

[0047] However, within the range of 0.8 ≦ x ≦ 1, the oxide of Chemical Formula 1 can have a plate-like particle form, and as the molar ratio of x increases, the particle size can become larger and the surface area of the oxidation catalyst can decrease. In such an aspect, x more preferably has a range of 0.7 ≦ x ≦ 0.9.

[0048] The molar ratio of x described above, specifically the molar ratios of lanthanum, strontium, and cobalt, can be confirmed by elemental analysis of the oxidation catalyst by a method such as ICP or by XRD analysis, and the ratio y of the oxygen defect sites can be confirmed by XRD analysis of the oxidation catalyst.

[0049] On the other hand, the perovskite oxide of Chemical Formula 1 contained in the oxidation catalyst of the above-described embodiment can have a spherical, amorphous, or plate-like primary particle; or a secondary particle form in which such primary particles are aggregated.

[0050] More specifically, the particle shape of the catalyst can be adjusted by controlling the molar ratio of the lanthanum and strontium and the manufacturing conditions described below. For example, when the molar ratio x of strontium is 0.6 or less, it has been confirmed that the catalyst is mainly manufactured in the form of secondary particles in which spherical or amorphous primary particles are aggregated, and the particle size decreases as x increases. In contrast, when x is increased to 0.8 or more, it has been confirmed that the catalyst is mainly manufactured in the form of plate-shaped primary particles, and the particle size increases as x increases due to the particles agglomerating. This is because Sr has a large ionic radius. 2+ ion (1.44Å) is La 3+ This is predicted to be due to a change in the crystal lattice structure caused by substitution at the ion (1.36 Å) site.

[0051] At this time, the primary particles of the perovskite oxide may have a particle size of 10 nm to 3 μm. More specifically, when the x is 0.6 or less, the spherical or amorphous primary particles mainly formed may have a particle size within a range of, for example, 10 nm to 400 nm or 20 nm to 100 nm, and the plate-shaped primary particles may have a particle size of, for example, 400 nm to 3 μm or 1 to 2 μm. At this time, the "particle size" may be defined as the longest straight line distance among the straight lines connecting any two points on the surface of each primary particle.

[0052] The perovskite oxide preferably has a particle size of 10 nm to 1.5 μm or 10 nm to 1 μm in terms of a large surface area and catalytic activity, and preferably has a spherical shape or an irregular particle shape close thereto. The perovskite oxide is produced by the production method described below and can have a monodisperse particle size distribution, resulting in a more uniform particle size distribution and a large surface area.

[0053] The particle size and particle size distribution can be determined by analyzing the oxidation catalyst with an electron microscope or by using a general laser particle size analyzer.

[0054] Meanwhile, the perovskite-based oxide may be used as an oxidation catalyst for anion exchange membrane water electrolysis by itself, or may be used in a state where a small amount of a different element is doped. By adding such an additional dopant, the catalytic active sites are increased, and the activity and electrical conductivity of the oxide as an oxidation catalyst can be further improved. The type of the dopant that can be added is not particularly limited, and for example, one or more different elements selected from the group consisting of Ba, Fe, Ni, and Mn may be doped.

[0055] The perovskite oxide having the above-mentioned excellent catalytic activity, electrical conductivity, and large surface area can be prepared by a preparation method using a coprecipitation method. Therefore, according to another embodiment of the present invention, the preparation method of the perovskite-based oxidation catalyst of the above-mentioned embodiment is applied.

[0056] In another such embodiment, the method includes the steps of co-precipitating a lanthanum salt, a strontium salt, and a cobalt salt in an aqueous solvent having a pH of 12 or greater in the presence of a chelating agent to form a catalyst precursor; and The catalyst precursor is calcined at a temperature of 500° C. or more to form the perovskite-based oxide of Formula 1.

[0057] In the manufacturing method according to this embodiment, the constituent atoms of the catalyst precursor and the perovskite oxide can be precisely controlled to the atomic level by using a coprecipitation method, and the particle size of the oxide particles can be controlled to a desired small range, and the oxide particles can be manufactured to have a more uniform particle size distribution.

[0058] It was also confirmed that by using the coprecipitation method, the perovskite-based oxide and oxidation catalyst can be produced by carrying out a low-temperature heat treatment at about 500 to 1000° C., or about 600 to 900° C. in the subsequent calcination step.

[0059] This prevents the surface area of ​​the oxidation catalyst particles from increasing and the surface defects or oxygen vacancies from being filled, which may cause a decrease in catalytic activity, as occurs in conventional high-temperature solid-phase reactions and heat treatments. However, if the heat treatment temperature is too high, the particle size of the oxidation catalyst increases, the surface area decreases, and the catalytic active sites decrease, which may adversely affect catalytic activity.

[0060] Furthermore, in the manufacturing method of the other embodiment, a form of a metal acid addition salt having a relatively low unit price can be used as a reactant, so that the oxidation catalyst of one embodiment having excellent overall physical properties can be manufactured more economically.

[0061] Meanwhile, in the manufacturing method according to the other embodiment, the aqueous medium having a pH of 12 or more may be prepared by treating a neutral aqueous medium, for example, distilled water, with a plurality of pH regulators in multiple steps.

[0062] According to a specific example, the neutral aqueous solvent is treated with a first pH adjuster containing ammonium hydroxide or ammonium sulfate to maintain a pH of 6 to 7, and then further treated with a second pH adjuster containing ammonium oxalate, potassium hydroxide or sodium hydroxide to obtain an aqueous solvent having a pH of 13 or more, or 13.5 or more, or 13.5 to 14. Such a multi-step process allows for more precise control of the pH required for the coprecipitation method.

[0063] In the coprecipitation step, the lanthanum salt and the strontium salt may exist in various forms depending on the pH of the aqueous medium. 3+ , La(OH) 2+ , La(OH)2 + , La(OH)4 - or La(OH)3, but at pH 6 and above, La(OH) 2+ , La(OH)2 + , and La(OH)3 forms, and above pH 9, La(OH)4 -In addition, strontium salts can produce Sr ions in aqueous media. 2+ At pH 12 and above, it exists in the form of Sr 2+ +OH - →SrOH - It can be precipitated in the form.

[0064] In other words, when the pH of the aqueous solvent in the coprecipitation step is adjusted to the aforementioned range of 12 or more, the forms of existence of these lanthanum salts and strontium salts are appropriately adjusted, and thus a catalyst precursor having an appropriate atomic composition is obtained by coprecipitation reaction with a cobalt complex compound described below.

[0065] In addition, in the coprecipitation step, the chelating agent is used to control the reaction rate of the coprecipitation reaction and more effectively obtain a catalyst precursor with a desired structure. More specifically, the chelating agent can first form a coordinate bond with the cobalt salt to form a cobalt complex compound. Therefore, this cobalt complex compound gradually reacts with the lanthanum salt and the strontium salt to produce a catalyst precursor having a desired atomic composition, uniform particle size distribution, and lattice structure according to a stoichiometric ratio, and an oxidation catalyst using the same.

[0066] The type of the chelating agent is not particularly limited, but an ammonium salt compound may be used taking into consideration appropriate reactivity with the cobalt salt, and specific examples thereof include one or more selected from the group consisting of ammonium hydroxide (NHOH), ammonium sulfate ((NH)SO), ammonium nitrate (NHNO), and monoammonium phosphate ((NH)HPO).

[0067] For example, when ammonium hydroxide is used as the chelating agent, the reaction between the chelating agent and a cobalt salt can be carried out in two steps as shown in the following reaction scheme 2.

[0068] [Reaction Scheme 2] M 2+ +nNH4OH→[M(NH3) n ] 2++2H2O 1st stage [M(NH3) n ] 2+ +2OH - +nH2O→M(OH)2+nNH4OH 2 steps

[0069] In the above reaction scheme 2, M includes Co.

[0070] In the first step, primary particles having a nanoscale particle size may be formed, and in the second step, the primary particles may be aggregated by the Ostwald ripening phenomenon to form secondary particles having a nearly microscale particle size. As the cobalt complex compound is formed, the complex compound gradually reacts with the lanthanum salt and the strontium salt to produce a catalyst precursor having a desired particle size range, uniform particle size distribution, controlled atomic composition and lattice structure.

[0071] In this coprecipitation step, Co 2+ The ions are in the air. 3+ Or Co 4+ However, if such oxidation and phase transition occurs, it may be difficult to control the atomic composition, particle size, and particle size distribution according to the stoichiometric ratio of the catalyst precursor. Therefore, the coprecipitation step is preferably performed in an atmosphere that is free of oxygen or air or in an inert atmosphere.

[0072] Meanwhile, in the coprecipitation step, the types of the lanthanum salt, strontium salt, and cobalt salt are not particularly limited, and may have a general salt form known to be usable in a coprecipitation reaction. However, as a more specific example, the lanthanum salt, strontium salt, and cobalt salt may have the form of an acid addition salt such as a nitrate salt in which a nitrate ion is bound to these metals, or a hydrate thereof.

[0073] In this manner, in the manufacturing method of another embodiment, a catalyst precursor and an oxidation catalyst can be manufactured using an acid addition salt having a relatively low unit price as a reactant, thereby improving the economic efficiency and mass productivity of the overall oxidation catalyst manufacturing process.

[0074] In addition, in the co-precipitation step, as described above, the catalyst precursor and the oxidation catalyst can be prepared by controlling the atomic composition according to a stoichiometric ratio while controlling the rate of the co-precipitation reaction. Therefore, in the method according to the other embodiment, the lanthanum salt, the strontium salt, and the cobalt salt can be co-precipitated in a molar ratio corresponding to the molar ratio of each metal contained in the oxidation catalyst, that is, the molar ratio of the lanthanum salt:strontium salt:cobalt salt is 1-x:x:1 (0≦x≦1).

[0075] In order to form a cobalt complex compound at an appropriate ratio using the above-mentioned chelating agent and to suitably control the reaction rate, it is preferable that the chelating agent is used so that the ratio of its concentration to the total concentration of the metal salt satisfies the ratio of the concentration of the metal salt:the concentration of the chelating agent is 1:0.6 to 1:6, or 1:0.7 to 1:3, or 1:0.8 to 1:1.2.

[0076] Meanwhile, as described above, such a coprecipitation reaction step may be carried out in an oxygen or air-free atmosphere or in an inert atmosphere such as nitrogen gas, and may be carried out at a temperature of, for example, 20 to 100°C or 50 to 80°C in order to appropriately control the reaction rate.

[0077] Through the above-mentioned coprecipitation reaction step, a catalyst precursor containing each metal element in the desired atomic composition can be prepared. Such a catalyst precursor can be in the form of a hydroxide compound containing each metal element of cobalt, lanthanum, and strontium in the same molar ratio as the oxidation catalyst formed in the subsequent step. More specifically, the catalyst precursor can be prepared by mixing La 1-x Sr x It may be produced in particulate form comprising the compound Co(OH)2 (0≦x≦1).

[0078] Meanwhile, after the coprecipitation step, if necessary, a step of drying the catalyst precursor at a temperature of 50° C. or more, or 50 to 100° C., or 60 to 90° C. may be further performed, and before the drying step, a step of washing the catalyst precursor one or more times, or 1 to 3 times, using water such as distilled water or alcohol such as ethanol may be further performed.

[0079] After the catalyst precursor is prepared through the above-mentioned process, it may be calcined at a temperature of 500° C. or more, or 500 to 1000° C., or 600 to 900° C., in an air atmosphere to prepare an oxidation catalyst according to an embodiment.

[0080] However, as described above, if the calcination temperature is excessively high, the particle size of the oxidation catalyst may become large, resulting in a small surface area, and the catalytic active sites may become clogged, adversely affecting the activity of the oxidation catalyst, which is not preferable.

[0081] Through the above-described process, an oxidation catalyst for anion exchange membrane water electrolysis according to an embodiment having a large surface area, excellent catalytic activity, electrical conductivity, and excellent durability can be economically and efficiently produced. Due to the above-described excellent general physical properties, such an oxidation catalyst can be suitably used in an oxidation electrode of an anion exchange membrane water electrolysis system.

[0082] The oxidation electrode may have the same structure as a general oxidation electrode for an anion exchange membrane water electrolysis system, except that it includes the oxidation catalyst of the embodiment. For example, the oxidation catalyst may include a porous metal structure and a catalyst layer including the perovskite-based oxidation catalyst of the embodiment formed on the porous metal structure.

[0083] In addition, the porous metal structure may include nickel metal, and more specifically, may be in the form of nickel foam, which is a porous structure of nickel metal. In addition, on one side of such a porous metal structure, the oxidation catalyst is applied in an amount of 0.1 to 10 mg / cm per unit area of ​​the porous metal structure.2 and the oxidation catalyst may be contained in the pores of the metal structure.

[0084] Within the above range, as the content of the oxidation catalyst increases, the performance of the anion exchange membrane water electrolysis system may be improved, but if the content of the oxidation catalyst increases too much, the performance of the water electrolysis system may decrease.

[0085] The thickness of the catalyst layer containing the oxidation catalyst can be increased in proportion to the content of the oxidation catalyst, and is not particularly limited.

[0086] Meanwhile, the porous metal structure may be nickel foam, which has been commercially available for some time, and the porosity of the nickel foam may be 50 to 200 PPI (pores per inch), specifically 70 to 170 PPI, for example 110 PPI.

[0087] The thickness of the porous metal structure may be 150 to 350 μm, specifically 200 to 300 μm, for example 250 μm.

[0088] The above-described oxidation electrode may be manufactured by a method for manufacturing an oxidation electrode in a general anion exchange membrane water electrolysis system, except for the use of an oxidation catalyst according to an embodiment, and therefore, further description thereof will be omitted.

[0089] According to another embodiment of the present invention, there is provided an anion exchange membrane water electrolysis system including the oxidation electrode. The water electrolysis system may include an anion exchange membrane, a reduction electrode located on one side of the anion exchange membrane, and the oxidation electrode of the above or another embodiment located on the other side of the anion exchange membrane such that the catalyst layer is in contact with the anion exchange membrane.

[0090] This may be the case where the water electrolysis performance is improved by including the oxidation catalyst and oxidation electrode of the above-mentioned embodiment.

[0091] Hereinafter, the description of the oxidation electrode will be omitted, and the other components will be described in detail.

[0092] The water electrolysis system of the above embodiment may include a potentiostat coupled to the reduction electrode and the oxidation electrode, respectively. The oxidation electrode may be the oxidation electrode of the above-mentioned embodiment, and the reduction electrode may be a composite of platinum (Pt) and carbon (C) coated on carbon paper.

[0093] Such a water electrolysis system may include only one cell including the oxidation and reduction electrodes and the anion exchange membrane, but may also include a plurality of such cells, stacked in series to form a water electrolysis stack.

[0094] The water electrolysis stack may include an electrolyte tank, which may serve to store an alkaline aqueous solution such as potassium hydroxide (KOH) or sodium hydroxide (NaOH) and supply the alkaline aqueous solution to the anion exchange membrane.

[0095] When an alkaline aqueous solution is supplied from the electrolyte tank to the anion exchange membrane and a DC power supply is applied to the oxidation electrode and the reduction electrode, hydroxide ions (OH - ) reacts catalytically on the surface of the oxidizing electrode to generate oxygen, water, and electrons, and the electrons can be transferred to the reducing electrode along an external conductor. On the surface of the reducing electrode, the electrons and water react catalytically to generate hydrogen and hydroxide ions (OH - The oxygen generated at the oxidation electrode and the hydrogen generated at the reduction electrode can be transferred to and stored in a storage tank outside the unit cell.

[0096] Other features can be realized by referring to water electrolysis systems widely known in the art.

[0097] Preferred examples are presented below for better understanding of the invention. However, the following examples are merely for illustrating the invention and are not intended to limit the invention.

[0098] Examples 1 to 10: Chemical Formula 1 (La 1-x Sr x Chief of Staff 3-y ) Oxidation Catalyst Production First, the reactor was filled with 1 to 4 L of distilled water (DIW), and an aqueous ammonia solution (ammonium hydroxide) was added as a first pH regulator, and the mixture was stirred at 600 rpm or more to maintain the pH inside the reactor at 7 and the internal temperature at room temperature up to 60° C. An NaOH solution was added as a second pH regulator to maintain the pH inside the reactor at 13.5 or more.

[0099] Then, an aqueous solution of ammonium hydroxide (NH4OH) was mixed as a chelating agent. Next, the molar ratio of lanthanum salt: strontium salt: cobalt salt was controlled to produce a metal aqueous solution with a molar ratio of 1-x:x:1, and the metal salt was used as the raw material. At this time, La(NO3)3, Sr(NO3)2, and Co(NO3)2 were used as the metal salts and dissolved in distilled water. In addition, in Examples 1 to 10, the molar ratio of x was varied as shown in the composition in Table 1 below.

[0100] The mixture of the metal solution, NaOH, and NH4OH thus prepared was fed into the reactor using a metering pump. The reactor was then stirred at a speed of 600-1,000 rpm to carry out the co-precipitation reaction. The molar ratio of metal ions to ammonium hydroxide solution as a chelating agent was adjusted to 1:0.7-1:6. The co-precipitation reaction was carried out for 4 hours or more. After the co-precipitation reaction was completed, the precipitate was separated using a centrifuge and washed with distilled water (DIW) and ethanol, respectively. It was then dried in an oven at 80°C for 12 hours.

[0101] Thereafter, the mixture was calcined under an air atmosphere under the conditions shown in Table 1 below to prepare oxidation catalysts containing the perovskite oxide of Chemical Formula 1 of Examples 1 to 10, respectively.

[0102] [Table 1]

[0103] <Experimental Example 1> SEM image measurement First, the oxidation catalysts of Examples 1 to 6, which have different molar ratios x of strontium, were analyzed by scanning electron microscope (SEM), and the photographs are shown in FIGS. 1a to 1f, respectively.

[0104] 1a to 1f, it was confirmed that as the Sr molar ratio x increases, the particle size of the oxidation catalyst particles decreases significantly, but within the range of x between 0.8 and 1, as x increases, plate-shaped particles are produced and their particle size increases. More specifically, it was confirmed that the oxidation catalyst of Example 1 is composed of spherical or irregular primary particles having a particle size of 100 nm or less, and as the Sr content increases, the size of the primary particles decreases to several tens of nm, and when x is 0.8 or more, plate-shaped particles having a micro-scale particle size (e.g., a particle size of 1 μm or more) grow. Specifically, the oxidation catalyst of Example 6 is mostly composed of plate-shaped particles, which is due to the large ionic radius of Sr. 2+ ion (1.44Å) is La 3+ This is predicted to be due to a change in the lattice structure while completely replacing the ionic (1.36 Å) site.

[0105] Meanwhile, the oxidation catalysts of Examples 6 to 10, which were calcined at different temperatures, were analyzed by an electron microscope (SEM), and the photographs are shown in Figures 2a to 2e, respectively (Figure 2a: Example 7, Figure 2b: Example 6, Figures 2c to 2e: Examples 8 to 10; arranged according to increasing calcination temperature). At this time, Figures 1 and 2 are electron microscope photographs at different scales, and Figures 1f and 2b for Example 6 are shown at different scales, respectively.

[0106] 2a to 2e, it was confirmed that the particle size of the oxidation catalyst particles increases with an increase in the calcination temperature, and in particular, it was confirmed that a rapid increase in particle size occurs due to particle aggregation of the oxidation catalyst having a plate-like particle shape at a calcination temperature exceeding 900° C. Therefore, it was confirmed that an excessively high calcination temperature is disadvantageous in terms of catalytic activity, as the particle size increases and the surface area decreases.

[0107] In addition, when the oxidation catalysts of Examples 6 to 10 were dispersed in a solvent (distilled water), as shown in FIG. 3, it was confirmed that the higher the calcination temperature, the lower the degree of dispersion of the oxidation catalyst, which was unsuitable.

[0108] <Experimental Example 2> XRD analysis The oxidation catalysts of Examples 1 to 6 were analyzed by XRD, and their XRD spectra are shown in Fig. 4a for comparison. In addition, the XRD spectrum of the oxidation catalyst of Example 6 is enlarged and shown in Fig. 4b for crystal structure analysis.

[0109] 4a, as the molar ratio x of strontium increases, the XRD peak shifts to a lower angle. It was also confirmed that the oxidation catalysts of Examples 1 to 4, in which x is 0.6 or less, have a trigonal structure (twisted cubic), while the oxidation catalysts of Examples 5 and 7, in which x is 0.8 or more, have a lattice structure with oxygen vacancies.

[0110] Also, referring to FIG. 4b, the oxidation catalyst of Example 6 is a hexagonal SrCoO 3-y It was confirmed that the structure is [Zeitschrift fur Naturforschung B | Volume 63: Issue 6]. This was predicted to be due to oxygen deficiency occurring as the +3 oxidation state of lanthanum ions is replaced by +2 oxidation state of strontium ions.

[0111] <Experimental Example 3> Evaluation of electrochemical properties (measurement of current density by voltage, etc.) First, the electrochemical evaluation results of the oxidation catalysts prepared in Examples 1 to 6 are shown in FIG. 5a.

[0112] More specifically, for the oxidation catalysts of Examples 1 to 6, the current density (mA / cm ) in the voltage range of 1.2 to 1.8 V was 2 ) and a graph of the LSV (Linear sweep voltage) measured at 10mA / cm 2 The overpotential (mV) at each current density is shown in FIG.

[0113] Referring to FIG. 5a, it was confirmed that as the molar ratio x of Sr increases, the electrical conductivity increases, and therefore the current density increases at the same voltage.

[0114] In addition, the above 10 and 50 mA / cm 2 The overpotential at each current density was measured.

[0115] Measurements were performed using a counter electrode (Pt) and a reference electrode (Hg / HgO). A glassy carbon electrode (3 mm in diameter) was coated with the catalyst and used as the working electrode. The working electrode was prepared by dissolving 5-10 mg of catalyst particles in 1 mL of 5% Nafion solution (ethanol:isopropanol=4:1 (v:v)) and sonicating for 30 min to prepare a uniform catalyst solution. 10 μL of the solution was loaded onto the glassy carbon electrode (loading mass: 0.05 mg / cm). 2 Polarization curves were measured at 5-10 mV / s (1.0 M KOH solution). The initial data were IR corrected.

[0116] As a result of such measurements, the catalyst of Example 5 had a current of 10 mA / cm 2The overpotential at a current density of 50mA / cm is 420mV. 2 It was confirmed that the current density showed an overpotential of 486 mV. In comparison, the catalyst of Example 6 showed an overpotential of 10 mA / cm 2 The overpotential is 410 mV at a current density of 50 mA / cm 2 It was confirmed that the current density showed an overpotential of 470 mV, and it was confirmed that the electrical conductivity and activity of the catalyst improved as the value of x increased.

[0117] Meanwhile, the electrochemical properties of the oxidation catalysts of Examples 6 to 10, which were calcined at different temperatures, were evaluated in the same manner as in FIG. 5a, and the evaluation results are shown in FIG. 5b. Specifically, FIG. 5b shows the current density (mA / cm) in the voltage range of 1.2 to 1.8 V for the oxidation catalysts of Examples 6 to 10. 2 ) and 10mA / cm 2 1 is a graph showing the results of measuring overpotential (mV) at different current densities.

[0118] Referring to FIG. 5b, it was confirmed that as the calcination temperature increases, the overpotential increases at a constant current density, and the electrical conductivity and catalytic activity decrease. 2 It was confirmed that the overvoltage of the catalyst of Example 7 (calcination temperature: 600°C) at the current density was 410mV, and the overvoltage of the catalyst of Example 10 (calcination temperature: 1000°C) increased to 520mV. This is expected to be because as the calcination temperature increases, the surface area decreases due to the sintering effect, resulting in a decrease in the catalytic activity area.

[0119] <Experimental Example 4> Electrochemical characteristic evaluation (Tafel slope) The Tafel slope was measured for the catalysts of Examples 6 to 10, and the results are shown in FIG.

[0120] The Tafel slope refers to the amount of voltage change required to increase the current by 10 times. The smaller the Tafel slope, the more current flows even at a low voltage, indicating excellent electrical conductivity.

[0121] Referring to FIG. 6, it was confirmed that as the calcination temperature increased, the Tafel slope increased from 49 to 60 mV / dec, and the electrical conductivity of the oxidation catalyst decreased.

[0122] For reference, the oxygen evolution reaction (OER) at an oxidation electrode follows the following mechanism.

[0123]

number

[0124] According to the mechanism, it can be confirmed that the reaction rate determining step changes as the firing temperature increases. Under the firing condition of 600°C (Example 7), the Tafel slope is 49 mVdec. -1 and the reaction rate determining step is MO - →MO+e - At 1000°C (Example 10), the rate determining step for the catalyst is MOH+OH - ⇔MO - +H2O. This is expected to be due to the change in the catalyst surface state caused by the calcination temperature.

[0125] <Experimental Example 5> Electrochemical Characterization (Impedance) The results of measuring the impedance at 1.62 V for the oxidation catalysts of Examples 6 to 8 are shown in Fig. 7. These are evaluation results for measuring the charge transfer resistance of the oxidation catalysts.

[0126] As shown in Figure 7, the charge transfer resistance increases as the calcination temperature increases. This is because the surface area decreases as the particles grow and aggregate with the increase in calcination temperature, and the catalytic activity decreases as the catalytic surface area decreases due to the decrease in active sites.

[0127] In addition, when the firing temperature increases under atmospheric conditions, the internal energy of catalyst particles increases, making it easier for them to move to the catalyst surface and filling surface defects, reducing the number of defects. Catalyst surface defects are classified as oxygen vacancies and defects caused by impurities, and as the firing temperature increases, oxygen deficiency and defects caused by impurities decrease. Electrons can easily move to surface oxygen vacancies, but as the number of defects decreases, the electron movement path becomes more restricted, showing a tendency for charge movement resistance to increase.

[0128] <Experimental Example 6> Evaluation of catalyst durability In order to evaluate the durability of the oxidation catalyst prepared in Example 7, the evaluation results after operating for 1000 cycles at a voltage range (1.1-2.1 V) using a cyclic voltammetry (CV) method, and the results of measuring the current density and overvoltage after operating for 1000 cycles at a voltage range (1.1-1.8 V) using a linear sweep voltage (LSV) method are shown in Figures 8a to 8c, respectively.

[0129] 8a to 8c, the catalyst of Example 7 was heated at 800° C., which is before catalyst detachment due to bubbles occurred. th It was confirmed that the structure was stable up to 1000 sq. m and exhibited excellent structural stability and durability.

[0130] <Experimental Example 7> Evaluation of characteristics of anion exchange membrane water electrolysis system Using the oxidation catalyst of Example 7, an anion exchange membrane water electrolysis system was manufactured, comprising: an anion exchange membrane; a reduction electrode located on one side of the anion exchange membrane; and an oxidation electrode containing the oxidation catalyst located on the other side of the anion exchange membrane such that the catalyst layer is in contact with the anion exchange membrane.

[0131] To prepare the catalyst coating ink composition of Example 7, the catalyst was dissolved in a mixed solvent of 90 wt% IPA and 10 wt% DIW at a content of about 1 wt% by using sonication. In addition, 30 wt% of ionomer (Fumatech product) was added to the composition.

[0132] Then, nickel foam with a porosity of 110 PPI and a thickness of 250 μm was placed on a hot plate at 80° C. The ink composition was uniformly sprayed onto the surface of the nickel foam to form a catalyst layer. At this time, the loading amount of the catalyst layer per unit area of ​​the nickel foam was 2.0 mg / cm. 2 An oxidizing electrode was prepared, and an anion exchange membrane water electrolysis cell was prepared using such an oxidizing electrode, a reducing electrode of Pt / C (Pt 40wt%), and an anion exchange membrane of Fumatech FAA-3-50.

[0133] The results of measuring the current density while increasing the voltage for such a water electrolysis cell are shown in Figures 9a and 9b. 2 Example 7: 1.95V voltage at current density.

[0134] This confirmed that the oxidation catalyst of Example 7 exhibited excellent properties in an anion exchange membrane water electrolysis system.

Claims

1. A perovskite-based oxide having the following chemical formula 1, which has the form of spherical, irregular or plate-like primary particles; or secondary particles formed by agglomeration of such primary particles: A perovskite-based oxidation catalyst for anion exchange membrane water electrolysis, wherein the primary particles of the perovskite-based oxide have a particle size of 10 nm to 3 μm and a monodisperse particle size distribution: [Chemical formula 1] L 1-x Sr x Yes 3-y In Formula 1, 0≦x≦1 and 0≦y≦0.

3.

2. 2. The perovskite-based oxidation catalyst for anion exchange membrane water electrolysis according to claim 1, wherein 0.7≦x≦1 and 0<y≦0.

3.

3. doped on the perovskite oxide, 2. The perovskite-based oxidation catalyst for anion exchange membrane water electrolysis according to claim 1, further comprising at least one different element selected from the group consisting of Ba, Fe, Ni and Mn.

4. co-precipitation of a lanthanum salt, a strontium salt and a cobalt salt in the presence of a chelating agent in an aqueous solvent having a pH of 12 or greater to form a catalyst precursor; and A method for preparing a perovskite-based oxidation catalyst, comprising calcining the catalyst precursor at a temperature of 500° C. or more to form a perovskite-based oxide represented by the following Formula 1: [Chemical formula 1] La 1-x Sr x CoO 3-y In Formula 1, 0≦x≦1 and 0≦y≦0.

3.

5. 5. The method for producing a perovskite-based oxidation catalyst according to claim 4, wherein the aqueous solvent having a pH of 13 or more is formed by sequentially adding a first pH adjuster containing ammonium hydroxide or ammonium sulfate and a second pH adjuster containing ammonium oxalate, potassium hydroxide or sodium hydroxide to the aqueous solvent.

6. The chelating agent is ammonium hydroxide (NH 4 OH), ammonium sulfate (NH 4 ) 2 SO 4 ), Ammonium nitrate (NH 4 NO 3 ) and ammonium phosphate monobasic ((NH 4 ) 2 H.P.O. 4 The method for producing the perovskite-based oxidation catalyst according to claim 4, wherein the catalyst comprises at least one selected from the group consisting of:

7. 5. The method for producing a perovskite-based oxidation catalyst according to claim 4, wherein the lanthanum salt, the strontium salt and the cobalt salt are co-precipitated in a molar equivalent ratio of 1-x:x:1 (0≦x≦1).

8. 5. The method for producing a perovskite-based oxidation catalyst according to claim 4, wherein the lanthanum salt, the strontium salt and the cobalt salt are each in the form of an acid addition salt of a metal or a hydrate thereof.

9. The method for producing a perovskite-based oxidation catalyst according to claim 4, wherein the coprecipitation reaction is carried out at a temperature of 20 to 100° C. in an inert atmosphere.

10. The catalyst precursor is La 1-x Sr x Co(OH) 2 The method for producing the perovskite-based oxidation catalyst according to claim 4, comprising a compound of (0≦x≦1).

11. The method for preparing a perovskite-based oxidation catalyst according to claim 4, further comprising drying the catalyst precursor at a temperature of 50° C. or higher after the coprecipitation step.

12. The method for preparing a perovskite-based oxidation catalyst according to claim 4, wherein the calcination step is performed at a temperature of 600 to 900° C. in an air atmosphere.

13. A porous metal structure; and An oxidation electrode for anion exchange membrane water electrolysis, comprising a catalyst layer including a perovskite-based oxidation catalyst including a perovskite-based oxide represented by the following Chemical Formula 1, formed on the porous metal structure: [Chemical formula 1] La 1-x Sr x CoO 3-y In Formula 1, 0≦x≦1 and 0≦y≦0.

3.

14. The oxidation electrode for anion exchange membrane water electrolysis according to claim 13, wherein the porous metal structure comprises nickel foam.

15. The oxidation catalyst is present in an amount of 0.1 to 10 mg / cm per unit area of ​​the porous metal structure. 2 The oxidation electrode for anion exchange membrane water electrolysis according to claim 13, wherein the anion exchange membrane water electrolysis oxidation electrode has a content of

16. Anion exchange membrane; a reduction electrode located on one side of the anion exchange membrane; and 14. The anion exchange membrane water electrolysis system according to claim 13, wherein the catalyst layer is located on the other side of the anion exchange membrane so as to be in contact with the anion exchange membrane.

Citation Information

Patent Citations

  • Air electrode for metal-air battery, membrane-air electrode assembly for metal-air battery including air electrode, and metal-air battery

    JP2012099266A

  • Positive electrode, positive electrode for water electrolysis, electrolysis cell, and method for producing hydrogen

    WO2018155503A1

  • Perovskites for catalyzing oxygen evolution

    WO2019245929A1