Filler composition, silicone resin composition and heat dissipating part
A filler composition with three types of fillers of specific sizes addresses the challenge of heat dissipation in electronic components, achieving improved thermal conductivity and heat dissipation in electronic components.
Patent Information
- Application Number
- JP2020567734
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-01-25
- Filing Date
- 2020-01-24
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2040-01-24
AI Technical Summary
Existing heat dissipation materials struggle to effectively manage the increasing heat generated by miniaturized and high-performance electronic components, particularly in applications like electric vehicles, where high voltages and large currents generate significant heat.
A filler composition comprising three types of fillers with specific average particle diameters (0.3 to 1.0 μm, 3 to 15 μm, and 35 to 140 μm) selected from alumina, magnesia, AlN-coated alumina, AlN, and SN, optimized to enhance thermal conductivity by filling gaps and forming efficient heat paths.
The filler composition significantly improves thermal conductivity, enabling the production of heat dissipating components with enhanced heat dissipation properties.
Smart Images

Figure 0007596151000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a filler composition, a silicone resin composition, and a heat dissipating part. [Background technology]
[0002] In recent years, electrical devices have become smaller and more powerful. As a result of this miniaturization and higher performance, the packaging density of electronic components that make up the electronic devices has increased, increasing the need to effectively dissipate heat generated by the electronic components.
[0003] Furthermore, in power device applications such as electric vehicles, which are environmentally friendly, high voltages and / or large currents may be applied to electronic components, generating large amounts of heat, and there is an increased need to dissipate the heat more effectively than ever before. As a technique for responding to such demands, for example, Patent Document 1 discloses a thermally conductive resin composition containing three types of fillers. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2009-164093 A Summary of the Invention [Problem to be solved by the invention]
[0005] The demand for heat dissipation from electronic components and the like is increasing, and materials with even better heat dissipation properties are being sought. [Means for solving the problem]
[0006] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that the heat dissipation properties can be further improved by using three types of fillers with different particle sizes that have excellent heat dissipation properties. More specifically, the present invention provides the following.
[0007] [1] A filler composition comprising a filler (A1) having an average particle size of 0.3 to 1.0 μm, a filler (A2) having an average particle size of 3 to 15 μm, and a filler (A3) having an average particle size of 35 to 140 μm, wherein the filler (A1), the filler (A2), and the filler (A3) are at least one selected from alumina, magnesia, AlN-coated alumina, AlN, and SN. [2] The filler composition according to [2], wherein at least one of the filler (A1), the filler (A2) and the filler (A3) is an AlN-coated alumina. [3] The filler composition according to [2], wherein the amount of AlN coating in the AlN-coated alumina is 10 to 40 mass %.
[0008] [4] The filler composition according to any one of [1] to [3], wherein at least one of the filler (A1), the filler (A2) and the filler (A3) is magnesia. [5] A silicone resin composition comprising the filler composition (A) according to any one of [1] to [4] and a silicone resin (B). [6] A heat dissipation part made using the silicone resin composition according to [5]. Effect of the Invention
[0009] By using the filler composition of the present invention or a resin composition containing the filler composition, a heat dissipating part having excellent heat dissipation properties can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiments of the present invention will be described in detail, however, the present invention is not limited to the following embodiments.
[0011] The filler composition of the present invention contains a filler (A1) having an average particle size of 0.3 to 1.0 μm, a filler (A2) having an average particle size of 3 to 15 μm, and a filler (A3) having an average particle size of 35 to 140 μm, and the fillers (A1), (A2) and (A3) are at least one selected from alumina, magnesia, AlN-coated alumina, AlN and SN.
[0012] The filler composition of the present invention is characterized by containing ultrafine powder filler (A1), fine powder filler (A2) and coarse powder filler (A3) having specific average particle diameters. If any one of the upper limit or lower limit of the average particle diameter of any of the fillers (A1), (A2) and (A3) is outside the range, the desired effect cannot be obtained. The effect of the present invention is that by using the fillers (A1), (A2) and (A3) having three different average particle diameters, the gaps between the fillers (A3) are filled with the filler (A2), and the gaps between the fillers (A2) are filled with the filler (A1), and the gaps between the fillers (A2) are filled with the filler (A1), and thus a heat path between the fillers is formed, which is thought to improve thermal conductivity.
[0013] The average particle diameter of the filler (A1) is 0.3 μm or more. By making the average particle diameter of the filler (A1) 0.3 μm or more, the filler (A1) can efficiently enter the gaps between the fillers (A2) to increase the filling rate and improve the thermal conductivity. The average particle diameter of the filler (A1) is preferably 0.4 μm or more, more preferably 0.5 μm or more. In addition, the average particle diameter of the filler (A1) is 1.0 μm or less. By making the average particle diameter of the filler (A1) 1.0 μm or less, the number of particles of the filler (A1) dispersed in the filler increases, and the distance between the fillers is narrowed. Therefore, the heat path efficiency is improved, and the thermal conductivity can be increased. The average particle diameter of the filler (A1) is preferably 0.9 μm or less, more preferably 0.8 μm or less.
[0014] In this specification, the average particle size is a value based on mass-based particle size measurement by laser diffraction light scattering method, and is measured using Malvern's "Mastersizer 3000, wet dispersion unit: Hydro MV installed". For the measurement, water is used as the solvent, and dispersion is performed for 2 minutes as pretreatment by applying 200W output using Tommy Seiko's "Ultrasonic Generator UD-200 (with ultra-micro tip TP-040 installed)". The filler after dispersion is dropped into the dispersion unit so that the laser scattering intensity is 10 to 15%. The stirring speed of the dispersion unit stirrer is 1750 rpm, and there is no ultrasonic mode. The particle size distribution is analyzed by dividing the particle size range of 0.01 to 3500 μm into 100 parts. The refractive index of water is 1.33, and the refractive index of the filler is various literature values. In the measured particle size distribution, the particles with a cumulative mass of 50% are the average particle size.
[0015] The filler (A1) having the above average particle size may be a commercially available product, or may be prepared by a known method (the same applies to the filler (A2) and filler (A3)).
[0016] From the viewpoint of enhancing the effects of the present invention, it is preferable that the content of the filler (A1) in the filler composition is 5% by volume or more. The content of the filler (A1) is more preferably 7% by volume or more, and even more preferably 10% by volume or more. In addition, it is preferable that the upper limit is 20% by volume or less, from the viewpoint of enhancing the effects of the present invention. The content of the filler (A1) is more preferably 18% by volume or less, and even more preferably 15% by volume or less. By setting the content of the filler (A1) in this range, it becomes easy to highly fill the filler composition.
[0017] The shape of the filler (A1) is preferably spherical from the viewpoint of improving the filling property. By making it spherical, frictional resistance with the resin can be reduced, and high filling is possible. As for the degree of sphericity, the average sphericity is preferably 0.80 or more. The average sphericity of the filler (A1) is more preferably 0.82 or more, and even more preferably 0.85 or more.
[0018] In this specification, the average sphericity of the filler (A1) is measured by the following method. The filler and ethanol are mixed to prepare a slurry containing 1% by mass of the filler, and the slurry is dispersed for 2 minutes at output level 8 using a BRANSON SONIFIER 450 (crushing horn 3 / 4'' solid type). The dispersed slurry is dropped onto a sample stage coated with carbon paste using a dropper. The filler dropped onto the sample stage is left in the air until it dries, and then osmium coating is performed. An image taken with a JEOL scanning electron microscope JSM-6301F type at a magnification of 50,000 times and a resolution of 1280 x 960 pixels is imported into a personal computer. The image is used to analyze the image using Mountech's image analyzer MacView Ver. 4, and the particles are recognized using a simple import tool, and the sphericity is measured from the projected area (A) and perimeter (PM) of the particles. If the area of a perfect circle corresponding to the perimeter (PM) is (B), then the sphericity of the particle is A / B. If we assume a perfect circle (radius r) with the same perimeter as the perimeter (PM) of the sample, then PM=2πr, B=πr. 2 Therefore, B = π × (PM / 2π) 2 The sphericity of each particle is given by: Sphericity = A / B = A × 4π / (PM) 2 The sphericity of 200 particles thus obtained having an equivalent circle diameter of any projected area of 10 μm or more is calculated, and the average value is taken as the average sphericity.
[0019] The average particle diameter of the filler (A2) is 3 μm or more. By making the average particle diameter of the filler (A2) 3 μm or more, the filler (A2) can efficiently enter the gaps of the filler (A3) to increase the filling rate and improve the thermal conductivity. The average particle diameter of the filler (A2) is preferably 4 μm or more, more preferably 5 μm or more. In addition, the average particle diameter of the filler (A2) is 15 μm or less. By making the average particle diameter of the filler (A2) 15 μm or less, the filler (A2) can efficiently enter the gaps of the filler (A3) to increase the filling rate and improve the thermal conductivity. The average particle diameter of the filler (A2) is preferably 12 μm or less, more preferably 10 μm or less.
[0020] The content of the filler (A2) in the filler composition is preferably 25% by volume or more from the viewpoint of enhancing the effects of the present invention. The content of the filler (A2) is more preferably 28% by volume or more, and even more preferably 30% by volume or more. The upper limit is preferably 50% by volume or less from the viewpoint of enhancing the effects of the present invention. The content of the filler (A2) is more preferably 45% by volume or less, and even more preferably 40% by volume or less. By setting the content of the filler (A2) within this range, high filling of the filler composition becomes easy.
[0021] The shape of the filler (A2) is preferably spherical from the viewpoint of improving the filling property. By making it spherical, frictional resistance with the resin can be reduced, and high filling is possible. As for the degree of sphericity, the average sphericity is preferably 0.80 or more. The average sphericity of the filler (A2) is more preferably 0.82 or more, and even more preferably 0.85 or more.
[0022] In this specification, the average sphericity of the filler (A2) was measured in the same manner as that of the filler (A1) described above, except that the photographing magnification of the scanning electron microscope was changed to 2000 times.
[0023] The average particle diameter of the filler (A3) is 35 μm or more. The filler (A3) is a particle component that is the main particle of the filler, and by making the average particle diameter of the filler (A3) 35 μm or more, the heat path effect due to the contact between the particles can be improved. In addition, the specific surface area of the particles is reduced, so that the filling rate can be increased, and the thermal conductivity can be further increased. The average particle diameter of the filler (A3) is preferably 45 μm or more, more preferably 60 μm or more. In addition, the average particle diameter of the filler (A3) is 140 μm or less. By making the average particle diameter of the filler (A3) 140 μm or less, the surface smoothness of the resin composite filled with the filler can be maintained, and the interface resistance can be reduced, so that the thermal conductivity can be increased. The average particle diameter of the filler (A3) is preferably 130 μm or less, more preferably 120 μm or less.
[0024] The content of the filler (A3) in the filler composition is preferably 50% by volume or more from the viewpoint of enhancing the effects of the present invention. The content of the filler (A3) is more preferably 53% by volume or more, and even more preferably 55% by volume or more. The upper limit is preferably 70% by volume or less from the viewpoint of enhancing the effects of the present invention. The content of the filler (A3) is more preferably 65% by volume or less, and even more preferably 60% by volume or less. By setting the content of the filler (A3) within this range, high filling of the filler composition becomes easy.
[0025] The shape of the filler (A3) is preferably spherical from the viewpoint of improving the filling property. By making it spherical, frictional resistance with the resin can be reduced, and high filling is possible. As for the degree of sphericity, it is preferable that the average sphericity is 0.80 or more. The average sphericity of the filler (A3) is more preferably 0.82 or more, and even more preferably 0.85 or more.
[0026] In this specification, the average sphericity of the filler (A3) was measured in the same manner as for the filler (A1) described above, except that the photographing magnification of the scanning electron microscope was changed to 200x.
[0027] The filler composition of the present invention may contain components other than the filler (A1), filler (A2) and filler (A3) (including fillers (A1), (A2) and (A3) whose average particle size is outside the above range). Examples of components other than the fillers include yttrium oxide, boron nitride, calcium oxide, iron oxide and boron oxide. These other components may be intentionally contained in small amounts or may be contained as impurities. However, from the viewpoint of enhancing the effects of the present invention, the total amount of the filler (A1), filler (A2) and filler (A3) is preferably 90% by volume or more, more preferably 95% by volume or more, and even more preferably 97% by volume or more.
[0028] By using at least one selected from alumina, magnesia, AlN-coated alumina, AlN, and SN as the filler (A1), filler (A2), and filler (A3), a filler composition with excellent heat dissipation properties can be obtained. In the present invention, it is preferable to use alumina, magnesia, and AlN-coated alumina as the filler (A1), filler (A2), and filler (A3).
[0029] In order to obtain a filler composition with excellent thermal conductivity, it is preferable to use AlN-coated alumina. In particular, when the amount of AlN coating of the AlN-coated alumina is 10 mass% or more relative to 100 mass% of the raw material alumina, the AlN coating layer on the alumina surface can be thickened, so that the heat pass property of the particle surface is greatly improved and the thermal conductivity can be increased. For this reason, the lower limit of the above-mentioned AlN coating amount is preferably 10 mass% or more, more preferably 12 mass% or more, and even more preferably 14 mass% or more. In addition, if the amount of AlN coating is 40 mass% or less, the surface of the AlN-coated alumina can be smoothed, the filling rate can be increased, and the thermal conductivity can be increased. For this reason, the upper limit is preferably 40 mass% or less, more preferably 37 mass% or less, and even more preferably 33 mass% or less. In particular, by using AlN-coated alumina as the filler (A3), the thermal conductivity can be effectively increased. This is considered to be due to the fact that the filler (A3), which has the largest average particle diameter among the three types of filler (A1), filler (A2), and filler (A3), has a large effect on the thermal conductivity.
[0030] The AlN-coated alumina preferably used in the present invention can be produced by the following method. First, spherical alumina particles and carbon are mixed. 20 to 35 mass% of carbon is mixed with 65 to 80 mass% of spherical alumina particles, out of a total of 100 mass% of spherical alumina particles and carbon. Commercially available products can be used as spherical alumina particles, and the average particle size of the spherical alumina used may be appropriately determined according to the average particle sizes of the fillers (A1), (A2) and (A3) contained in the filler composition. Examples of carbon include EC black, acetylene black, carbon black and powdered graphite. In order to obtain AlN-coated alumina with high sphericity, it is preferable to use carbon having an average particle size of 30 nm or more and 60 nm or less and a specific surface area of 20 m. 2 / g or more 50m 2 / g or less, bulk density is 0.10g / cm 3 More than 0.20g / cm 3 It is preferable to use the following carbon: By using carbon having these characteristics, a reducing reaction atmosphere is formed during the firing process described below, and the carbon also acts as a spacer to suppress adhesion of alumina particles to each other, thereby making it possible to obtain AlN-coated alumina with high sphericity. The mixing is performed under conditions that allow the spherical alumina particles and carbon to be uniformly dispersed. There are no particular limitations on the mixing method, and either wet mixing or dry mixing can be used.
[0031] Next, 60 to 68 g of the mixture of spherical alumina particles and carbon is sintered for surface nitriding. The sintering atmosphere is a nitrogen atmosphere, and the flow rate of N2 gas is controlled in the range of 3 to 6 L / min. The sintering time is 4 to 12 hours, and the sintering temperature is 1500 to 1700°C. This sintering produces AlN-coated alumina. The sintering conditions for the above surface nitriding are appropriately adjusted according to the desired amount of AlN coating. The higher the sintering temperature, the longer the sintering time, and the higher the N2 gas flow rate, the greater the amount of AlN coating.
[0032] Next, the AlN-coated alumina is sintered to remove carbon remaining on the surface thereof in an air atmosphere at a sintering temperature of 600 to 900° C. for a sintering time of 2 to 6 hours.
[0033] In order to obtain a filler composition having excellent thermal conductivity, it is preferable to use magnesia as the filler (A1), filler (A2) and filler (A3). Magnesia has high thermal conductivity, and can provide a filler composition having particularly excellent thermal conductivity. Examples of methods for producing magnesia include a method of calcining magnesium carbonate (also called magnesite) and a method of adding calcium hydroxide to seawater or an aqueous magnesium chloride solution (bittern or brine) to generate magnesium hydroxide, which is then filtered, dried and calcined. In order to obtain magnesia with high sphericity, a method of melting and spheroidizing the magnesium powder obtained by the above-mentioned method by plasma spraying or the like can be mentioned. Furthermore, if the filler (A3) is magnesia, the thermal conductivity of the filler composition can be increased more efficiently than if AlN-coated alumina is used.
[0034] The filler composition of the present invention can be preferably used as a raw material for a member that requires thermal conductivity by adding it to a resin. The resin is preferably a silicone resin. The silicone resin composition of the present invention will be described below.
[0035] The silicone resin composition of the present invention includes the filler composition (A) of the present invention and a silicone resin (B). By combining the filler composition (A) of the present invention with the silicone resin (B), the filling rate of the filler composition (A) can be increased. As a result, a silicone resin composition with excellent thermal conductivity can be obtained.
[0036] The silicone resin (B) is not particularly limited. For example, peroxide curing type, condensation reaction curing type, addition reaction curing type, ultraviolet curing type, and other silicone resins can be used as the silicone resin (B).
[0037] By making the content of the silicone resin (B) in the silicone resin composition of the present invention 30% by volume or less, the effect of improving the thermal conductivity by the filler composition (A) of the present invention can be enhanced. Therefore, the content of the silicone resin (B) in the silicone resin composition of the present invention is preferably 30% by volume or less. More preferably, it is 25% by volume or less, and even more preferably, it is 20% by volume or less. On the other hand, if the content of the silicone resin (B) is too small, it becomes difficult to mold the silicone resin composition to produce a desired part. Therefore, the content of the silicone resin (B) is preferably 12% by volume or more. More preferably, it is 15% by volume or more, and even more preferably, it is 17% by volume or more.
[0038] The content of the filler composition (A) in the silicone resin composition of the present invention is preferably 70% by volume or more from the viewpoint of increasing the thermal conductivity of the silicone resin composition. More preferably, it is 75% by volume or more, and even more preferably, it is 78% by volume or more. On the other hand, if the content of the filler composition (A) is high, molding of the silicone resin composition may become difficult. For this reason, the content of the filler composition (A) is preferably 88% by volume or less. More preferably, it is 85% by volume or less, and even more preferably, it is 83% by volume or less. The silicone resin composition of the present invention is characterized in that it can increase the filling rate of the filler composition.
[0039] The silicone resin composition may contain components other than the filler composition (A) and the silicone resin (B), but the other components may reduce the filling rate of the filler composition or the other components themselves may have low thermal conductivity. Therefore, it is preferable that the other components are less. Specifically, it is preferable that the filler composition (A) and the silicone resin (B) are contained in a total of 90 volume % or more. More preferably, it is 95 volume % or more, and even more preferably, it is 97 volume % or more.
[0040] By using the silicone resin composition of the present invention, a resin composition with high thermal conductivity can be obtained. In particular, according to a preferred embodiment of the present invention, it is possible to achieve a thermal conductivity of 5.3 W / m·K or more as measured by the method described in the Examples. It is quite possible to achieve an upper limit of about 11.0 W / m·K, for example.
[0041] As described above, the silicone resin composition of the present invention has excellent thermal conductivity. Therefore, the silicone resin composition of the present invention can be preferably used for electronic parts. Specifically, it can be preferably used as a material for heat dissipation parts such as semiconductor encapsulation materials and heat dissipation sheets. The method of applying the silicone resin composition of the present invention to electronic parts such as semiconductor encapsulation materials and heat dissipation sheets can be a conventionally known method. EXAMPLES
[0042] 1. Preparation of Silicone Resin Composition Silicone resin compositions of Examples 1 to 5 and Comparative Examples 1 to 6 were produced.
[0043] [Filler] The following fillers were used: The average particle size was measured by the method described above. Alumina having the average particle size shown in Table 1 was used. The average particle size was measured using the method described above. The sphericity measured using the method described above is also shown in Table 1. The refractive index of alumina was 1.77 when measuring the average particle size.
[0044] AlN-coated alumina (average particle size: 50 μm) was produced by the following method. 50 g of "DAW-45" manufactured by Denka Co., Ltd. was used as alumina, and 10 g of "HS-100" manufactured by Denka Co., Ltd. was used as carbon. These were mixed and fired in a nitrogen atmosphere with an N2 amount of 3 L / min at a firing temperature of 1600°C for a firing time of 12 hours so that the amount of AlN coating was 15 mass%. Then, firing was performed in an air atmosphere at 700°C for 4 hours to remove carbon. The average particle size and sphericity of the obtained AlN-coated alumina were measured by the above-mentioned method. The average particle size was 50 μm. The refractive index of the AlN-coated alumina when measuring the average particle size was 1.77.
[0045] AlN-coated alumina (average particle size: 55 μm) was produced by the following method. 50 g of "DAW-45" manufactured by Denka was used as alumina, and 18 g of "HS-100" manufactured by Denka was used as carbon. These were mixed and fired in a nitrogen atmosphere with an N2 flow rate of 6 L / min at a firing temperature of 1600°C for 24 hours so that the amount of AlN coating was 31 mass%. After that, firing was performed in an air atmosphere at 700°C for 4 hours to remove carbon. The average particle size and sphericity of the obtained AlN-coated alumina were measured using the methods described above. The average particle size was 55 μm.
[0046] The magnesia has the average particle size and sphericity shown in Table 1. The refractive index of the magnesia when measuring the average particle size was 1.74.
[0047] [Silicone resin] The following silicone resins were used: (Silicone resin B) Silicone resin "SE-1885" manufactured by Toray Dow Corning The filler composition and silicone resin were mixed in the ratio shown in Table 1 to produce a silicone resin composition having a thickness of 3 mm.
[0048] [Thermal conductivity measurement] Thermal conductivity was measured by a steady-state method in accordance with ASTM D5470. Measurements were performed using a resin material thermal resistance measuring device TRM-046RHHT manufactured by Hitachi Technology and Services, Ltd. The silicone resin composition was processed to a width of 10 mm x 10 mm and a thickness of 3 mm, and the thermal resistance in the thickness direction was measured while applying a load of 2 N. The measurement results are shown in Table 1.
[0049] [Table 1]
Claims
1. A filler (A1) having an average particle size of 0.3 to 1.0 μm, a filler (A2) having an average particle size of 3 to 15 μm, and a filler (A3) having an average particle size of 45 to 140 μm, The content of the filler (A1) is 5 vol% to 20 vol%, the content of the filler (A2) is 25 vol% to 50 vol%, and the content of the filler (A3) is 53 vol% to 70 vol%, The filler (A1), the filler (A2), and the filler (A3) are at least one selected from alumina, magnesia, AlN-coated alumina, AlN, and SN, At least one of the filler (A1), the filler (A2), and the filler (A3) is AlN-coated alumina or magnesia; A filler composition, wherein the average sphericity of the filler (A1), the filler (A2) and the filler (A3) is 0.82 or more.
2. 2. The filler composition according to claim 1, wherein the amount of AlN coated in the AlN-coated alumina is 10 to 40 mass %.
3. A silicone resin composition comprising the filler composition (A) according to claim 1 or 2 and a silicone resin (B).
4. A heat dissipating part comprising the silicone resin composition according to claim 3.
Citation Information
Patent Citations
Highly thermally conductive inorganic powder and resin composition compounded therewith
JP2004244491A
Highly heat-conductive resin compound, highly heat-conductive resin molded article, compounding particle for heat-releasing sheet, highly heat-conductive resin compound, highly heat-conductive resin molded article, heat-releasing sheet, and method for producing the same
JP2007277406A
Insulating sheet and multilayer structure
JP2009164093A
Alumina blend particle and resin molding
JP2009274929A
Method for producing alumina particle with aln modified layer, and modified alumina powder
JP2011219309A