Ni-based alloy powder for lamination molding, lamination molded article, and lamination molded article manufacturing method
Patent Information
- Application Number
- JP2024504719
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-01
- Filing Date
- 2023-03-01
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2043-03-01
AI Technical Summary
Ni-based alloys used in additive manufacturing for semiconductor and electronic components face high weld cracking susceptibility and poor high-temperature oxidation resistance due to their high Al content, leading to defects and oxidation issues in complex shapes.
A Ni-based alloy powder with a composition of Al: 3.5-5.5%, Cr: 0.8-4.0%, C: 0.02-0.06%, Si: 1.0-1.8%, Mn: 1.5% or less, and O: 0.001-0.050%, with limited Zr content, optimized for additive manufacturing, which reduces cracking susceptibility and enhances high-temperature oxidation resistance.
The alloy powder results in additively manufactured products with fewer cracks, improved high-temperature oxidation resistance, and reduced defects, suitable for complex shapes in semiconductor and electronic component manufacturing.
Smart Images

Figure 2023167231000001
Abstract
Description
Ni-based alloy powder for additive manufacturing, additively manufactured product, and method for manufacturing additively manufactured product
[0001] The present invention relates to a Ni-based alloy powder for additive manufacturing (hereinafter sometimes referred to as Ni-based alloy powder) suitable for additive manufacturing, an additive manufactured product, and a method for manufacturing an additive manufactured product, and relates to members and parts used in, for example, oxidation furnaces used in semiconductor manufacturing and firing furnaces for electronic components.
[0002] In general, Ni-based alloys with excellent high-temperature oxidation resistance are used for components and parts installed in oxidation furnaces used in semiconductor manufacturing and furnaces used in baking furnaces for electronic components to prevent oxide scale generated from the components and parts from being mixed into the products. As an example of such Ni-based alloys with excellent high-temperature oxidation resistance, as disclosed in Patent Document 1, a Ni-based alloy with excellent high-temperature oxidation resistance has been proposed, which contains, by mass % (hereinafter, % refers to mass %), 3.6 to 4.4% Al, and optionally one or more of 0.1 to 2.5% Si, 0.8 to 4.0% Cr, and 0.1 to 1.5% Mn, with the balance consisting of Ni and inevitable impurities, and which is used as fins and tubes for high-temperature heat exchangers.
[0003] Furthermore, Patent Document 2 proposes a Ni-based alloy that is excellent in hot forgeability and high-temperature oxidation resistance, and that contains 2.0 to 5.0% Al, 0.1 to 2.5% Si, 0.8 to 4.0% Cr, 0.1 to 1.5% Mn, 0.001 to 0.01% B, 0.001 to 0.1% Zr, and the remainder being Ni and unavoidable impurities.
[0004] JP 2003-262491 A JP 2014-080675 A
[0005] However, in recent years, in applications such as furnace components and parts for manufacturing semiconductor products and electronic components, there has been a demand for not only excellent high-temperature oxidation resistance but also the realization of complex shapes such as gas flow paths within the components and parts. It is known that additive manufacturing (hereinafter referred to as additive manufacturing in this invention) using alloy powders is suitable as a means for realizing such complex shapes. Here, although the Ni-based alloys described in Patent Documents 1 and 2 above have excellent high-temperature oxidation resistance, they suffer from high weld crack susceptibility (hereinafter sometimes referred to as crack susceptibility) due to their high Al content. Additive manufacturing involves repeated melting and solidification of individual powders, which corresponds to welding at the microscopic level. Therefore, it is easy to predict that cracks will occur even if the Ni-based alloys described in Patent Documents 1 and 2 above, which have high weld crack susceptibility, are applied to additive manufacturing. Furthermore, poor high-temperature oxidation resistance will result in the appearance of defects caused by oxides. Based on the above, the present invention aims to provide a Ni-based alloy powder that is suitable for producing additively manufactured products that have few cracks and defects and excellent resistance to high-temperature oxidation, an additively manufactured product using this Ni-based alloy powder, and a method for manufacturing the additively manufactured product.
[0006] The present invention provides a Ni-based alloy powder for additive manufacturing, characterized in that it contains, in mass%, 3.5 to 5.5% Al, 0.8 to 4.0% Cr, 0.02 to 0.06% C, 1.0 to 1.8% Si, 1.5% or less Mn, and 0.001 to 0.050% O, with the balance consisting of Ni and unavoidable impurities, and the Zr contained in the unavoidable impurities being limited to 0.01% or less.
[0007] Furthermore, the Ni-based alloy powder for additive manufacturing preferably contains 3.6 to 5.0% Al, 1.5 to 3.0% Cr, 0.03 to 0.05% C, 1.2 to 1.5% Si, 0.2 to 1.0% Mn, and 0.008 to 0.030% O.
[0008] Furthermore, it is preferable that the Vickers hardness of the Ni-based alloy powder for additive manufacturing is in the range of 160 to 220 HV.
[0009] Furthermore, in an integrated distribution curve showing the relationship between particle diameter and volume accumulation from the small particle diameter side, obtained by laser diffraction, the Ni-based alloy powder for additive manufacturing preferably has a particle diameter d10 corresponding to an integrated frequency of 10% by volume of the powder of 10 μm or more and 25 μm or less, a particle diameter d50 corresponding to an integrated frequency of 50% by volume of the powder of 25 μm or more and 40 μm or less, and a particle diameter d90 corresponding to an integrated frequency of 90% by volume of 45 μm or more and 60 μm or less.
[0010] It is also preferable that the uniformity expressed by (d90-d10) / d50 is in the range of 0.8 to 1.2.
[0011] Furthermore, it is preferable that the Ni-based alloy powder for additive manufacturing has an angle of repose measured in accordance with JIS R9301-2-2 of 40 degrees or less.
[0012] The present invention also provides a method for producing an additively manufactured product, characterized by comprising an additive manufacturing process for forming an additively manufactured body using a Ni-based alloy powder containing, in mass %, 3.5 to 5.5% Al, 0.8 to 4.0% Cr, 0.02 to 0.06% C, 1.0 to 1.8% Si, 1.5% or less Mn, 0.001 to 0.050% O, and the remainder being Ni and unavoidable impurities, wherein Zr among the unavoidable impurities is limited to 0.01% or less.
[0013] The present invention also provides a steel sheet containing, by mass%, 3.5 to 5.5% Al, 0.8 to 4.0% Cr, 0.02 to 0.06% C, 1.0 to 1.8% Si, 1.5% or less Mn, and 0.001 to 0.050% O, with the balance being Ni and unavoidable impurities, in which Zr contained in the unavoidable impurities is limited to 0.01% or less, the defect rate is 0.1% or less, and the amount of oxidation per unit area, which is obtained by an oxidation test performed in an atmospheric furnace at 800°C for 950 hours and is expressed as [mass loss before and after oxidation test] / [surface area before oxidation test], is 0.005 mg / mm 2 The additive manufacturing product is characterized by the following:
[0014] The hardness of the layered product is preferably in the range of 210 to 300 HV.
[0015] The Ni-based alloy powder of the present invention is an alloy powder for additive manufacturing that has excellent high-temperature oxidation resistance, low weld crack susceptibility, and is also suitable for suppressing defects. When this Ni-based alloy powder is used to manufacture members and parts for semiconductor and electronic component manufacturing equipment by additive manufacturing, additive manufactured products with few cracks and defects and excellent high-temperature oxidation resistance, and members and parts made of this additive manufactured product, can be obtained.
[0016] FIG. 10 is a diagram showing oxidation test results of additive manufacturing products according to an example of the present invention and a comparative example.
[0017] [Ni-based alloy powder] The present inventors conducted extensive research into alloy compositions and additive manufacturing methods in order to develop a Ni-based alloy powder for additive manufacturing that has excellent high-temperature oxidation resistance and additive manufacturing properties. As a result, they discovered that a Ni-based alloy powder containing, by mass%, 3.5 to 5.5% Al, 0.8 to 4.0% Cr, 0.02 to 0.06% C, 1.0 to 3.0% Si, 1.5% or less Mn, and 0.001 to 0.050% O, with the balance being Ni and unavoidable impurities, and in which the Zr content of the unavoidable impurities is limited to 0.01% or less, has excellent properties in terms of high-temperature oxidation resistance and additive manufacturing properties, allowing for manufacturing with fewer cracks and defects.
[0018] The reasons for the numerical limitations of each component element in the alloy composition of the Ni-based alloy powder of the present invention will be described in detail below. Then, a method for manufacturing the alloy powder and an additive manufacturing product will be described. In this specification, a numerical range expressed using "to" includes the numerical values before and after "to" as the lower and upper limits. The upper and lower limits described in stages can be arbitrarily combined. Furthermore, "%" should be read as "mass %."
[0019] (Al: 3.5 to 5.5%) Al forms an alumina coating on the surface of the additively manufactured product, improving high-temperature oxidation resistance and reducing the occurrence of oxide scale. It is also added to Ni-based alloy powders because it forms a passivation oxide coating on the surface layer, preventing further oxidation of the Ni-based alloy powder. To ensure sufficient high-temperature oxidation resistance, the lower limit of the Al content is 3.5%. On the other hand, if the Al content is too high, microcracks are more likely to occur during additive manufacturing, which involves repeated local melting and solidification. Therefore, the upper limit of the Al content is 5.5%. The preferred Al content is 3.6 to 5.0%, and more preferably 3.7 to 4.1%.
[0020] (Cr: 0.8 to 4.0%) Cr is an element that is effective in improving high-temperature oxidation resistance by stabilizing the alumina coating. In order to ensure sufficient high-temperature oxidation resistance, the lower limit of the Cr content is 0.8%. On the other hand, if the Cr content is too high, the formation of the alumina coating is inhibited, so the upper limit of the Cr content is 4.0%. Furthermore, the Cr content is preferably 1.5 to 3.0%, and more preferably 1.9 to 2.1%.
[0021] (C: 0.02 to 0.06%) C is effective in reducing cracking sensitivity, preventing shrinkage cavities during solidification, and improving tensile strength. In order to sufficiently reduce cracking sensitivity, the lower limit of the C content is 0.02%. On the other hand, if the C content is too high, Cr carbides are formed, reducing corrosion resistance, so the upper limit of the C content is 0.06%. Furthermore, the preferred C content is 0.03 to 0.05%, and more preferably 0.035 to 0.04%.
[0022] (O: 0.001 to 0.050%) O has the effect of instantly bonding mainly with Al during the gas atomization process in the production of Ni-based alloy powder, forming an extremely thin and strong oxide film on the powder surface and suppressing further oxidation. In order to ensure sufficient high-temperature oxidation resistance, the lower limit of the O content is 0.001%. On the other hand, if the O content is too high, the oxide film formed on the powder surface will become apparent as defects during additive manufacturing, so the upper limit of the O content is 0.050%. Furthermore, the preferred O content is 0.008 to 0.030%, and more preferably 0.010 to 0.015%.
[0023] The contents of C and O can be controlled, for example, by melting in a vacuum and controlling the atmosphere by argon gas atomization.
[0024] (Zr: 0.01% or less) Zr is an impurity that is inevitably mixed in when producing Ni-based alloy powder. If the Zr content is high, it forms oxides, which inhibits the formation of an alumina coating. Furthermore, segregation at grain boundaries makes it more likely that microcracks will occur from the grain boundaries. To avoid these problems, Zr is particularly limited. The Zr content should aim for 0%, with the upper limit set at 0.01%. It is preferably 0.001% or less, and more preferably 0.0001% or less.
[0025] (Si: 1.0 to 1.8%) Like Cr, Si stabilizes the alumina coating formed on the additive manufacturing product, thereby improving high-temperature oxidation resistance. In order to ensure sufficient high-temperature oxidation resistance, the lower limit of the Si content is 1.0%. On the other hand, if the Si content is too high, shrinkage cavities are likely to occur during solidification as the individual Ni-based alloy powders repeatedly melt and solidify, so the upper limit of the Si content is 1.8%. Furthermore, the preferred Si content is 1.2 to 1.6%, and more preferably 1.3 to 1.5%.
[0026] (Mn: 1.5% or less) Mn has the effect of suppressing solidification cracking, which is increased by the inclusion of Al. Furthermore, for example, when the additive manufacturing speed is increased, the heat input increases and solidification cracking becomes more likely to occur, so it is preferable to adjust the amount added depending on the additive manufacturing speed. By setting the Mn content to more than 0%, the above effect can be exerted. Furthermore, to effectively exert this effect, it is preferable that the Mn content be 0.1% or more. On the other hand, if the Mn content exceeds 1.5%, high-temperature oxidation resistance decreases. For this reason, the Mn content is set to 1.5% or less. Furthermore, the preferred Mn content is 0.2 to 1.0%, and more preferably 0.4 to 0.6%.
[0027] (Remainder: Ni and Inevitable Impurities) The total amount of unavoidable impurities is preferably 1.0% or less, for example. Each of the unavoidable impurities is preferably 0.5% or less, more preferably 0.1% or less. More specifically, P, S, and N are preferably 0.01% or less, and Fe, B, Ti, Cu, Nb, Mo, and Co are preferably 0.5% or less.
[0028] The component composition of the Ni-based alloy powder of this embodiment can be determined by the following measurement method. As described in the Examples below, the powder for additive manufacturing after classification was dissolved in an appropriate aqueous solution, and the aqueous solution was subjected to high-frequency inductively coupled plasma (ICP) analysis to measure the content of specific components. Note that the content of C, N, and O can be determined by gas analysis using a combustion method.
[0029] (Hardness of Ni-based alloy powder: 160 to 220 HV) The hardness of the Ni-based alloy powder can be 160 HV or more to prevent the particles from being crushed when the powder is spread. On the other hand, if the powder hardness is too high, the manufactured additive manufacturing product is likely to crack, so the upper limit of the hardness can be set to 220 HV. The hardness is preferably 170 to 200 HV, more preferably 180 to 190 HV.
[0030] (Particle size of Ni-based alloy powder: 1 to 200 μm) Additive manufacturing is a manufacturing method in which individual powders are repeatedly melted and solidified to create a shape. Since the particle size requirements for the alloy powder vary depending on the additive manufacturing device, the particle size range of the Ni-based alloy powder can be set to 1 to 200 μm to accommodate various manufacturing devices. For example, in the case of powder bed fusion (PBF), if the particle size of the Ni-based alloy powder is less than 1 μm, fluidity decreases, making it difficult to obtain a sound additively manufactured product. On the other hand, if the particle size of the Ni-based alloy powder exceeds 80 μm, a large layer pitch is required, resulting in reduced dimensional accuracy. Therefore, the particle size range of the Ni-based alloy powder for powder bed fusion can be set to 1 to 80 μm. Preferably, it is 10 to 60 μm. Furthermore, in the case of directed energy deposition (DED), if the particle size of the Ni-based alloy powder is less than 1 μm, the supply amount cannot be increased, resulting in a slow molding speed. On the other hand, if the particle size of the Ni-based alloy powder exceeds 200 μm, the volume required for one melting and solidification is too large, making it more likely that unmelted material will remain. Therefore, the particle size range of the Ni-based alloy powder for the directed energy deposition method can be 20 to 200 μm. Preferably, it is 40 to 120 μm. Powder obtained by gas atomization, which produces a spherical shape, is preferred. The particle size of the powder can be measured using a laser diffraction method (laser diffraction particle size distribution analyzer).
[0031] (Particle size distribution of Ni-based alloy powder) In additive manufacturing, if the powder particle size is too small, the powder layer will be worn or unevenly distributed, resulting in reduced coating properties. On the other hand, if the powder particle size is too large, the laser output may be insufficient, resulting in residual molten material, which tends to increase defects during stacking and reduce surface roughness. For this reason, in the cumulative distribution curve showing the relationship between the particle size determined by the laser diffraction method and the volume cumulative from the small particle diameter side, it is preferable that the particle diameter d10 corresponding to a cumulative frequency of 10% by volume is 10 μm or more and 25 μm or less, the particle diameter d50 corresponding to a cumulative frequency of 50% by volume is 25 μm or more and 40 μm or less, and the particle diameter d90 corresponding to a cumulative frequency of 90% by volume is 45 μm or more and 60 μm or less. Preferably, d10 is 15 μm or more and 20 μm or less, d50 is 30 μm or more and 35 μm or less, and d90 is 50 μm or more and 55 μm or less, and more preferably, d10 is 18 μm or more and 20 μm or less, d50 is 32 μm or more and 34 μm or less, and d90 is 53 μm or more and 55 μm or less.
[0032] (Uniformity of Ni-based alloy powder: 0.8 to 1.2) The particle size of the Ni-based alloy powder of the present invention is defined as the numerical value expressed by (d90 - d10) / d50. The greater the uniformity is than 1, the lower the spreading property tends to be, and the smaller the uniformity is than 1, the lower the yield tends to be, resulting in lower productivity. For this reason, it is preferable that the lower limit of the uniformity is 0.8 and the upper limit is 1.2. The range is also preferably 0.90 to 1.15, and more preferably 0.95 to 1.10.
[0033] (Angle of repose of Ni-based alloy powder: 40 degrees or less) In additive manufacturing, the raw material powder preferably has good fluidity, as this improves spreadability. The fluidity of the Ni-based alloy powder of the present invention is evaluated by the angle of repose in accordance with JIS R9301-2-2. If the angle of repose exceeds 40 degrees, the fluidity is poor and spreadability decreases, so the angle of repose is preferably 40 degrees or less. There is no particular restriction on the lower limit. A more preferred angle of repose is 35 degrees or less, and even more preferably 31 degrees or less. The fluidity of the Ni-based alloy powder having the angle of repose described above is preferably 15 sec / 50 g or more. More preferably, it is 18 sec / 50 g or more, and even more preferably, it is 19 sec / 50 g or more.
[0034] [Method for Producing Alloy Powder] As a method for producing Ni-based alloy powder (alloy powder), for example, a gas atomization method can be used. After raw material powders blended to obtain a specified composition are melted in a crucible, the molten metal is discharged from the bottom of the crucible, and high-pressure gas is sprayed onto the discharged molten metal. The kinetic energy of the high-pressure sprayed medium causes the molten metal to fly as droplets, which are then solidified, thereby producing spherical Ni-based alloy powder. The crucible used in this process is made of Al to prevent the inclusion of Zr impurities. 2 O 3 It is preferably made of
[0035] [Method for manufacturing an additively manufactured product] The method for manufacturing an additively manufactured product of the present invention includes an additive manufacturing step of forming an additively manufactured product using a Ni-based alloy powder containing, in mass %, 3.5 to 5.5% Al, 0.8 to 4.0% Cr, 0.02 to 0.06% C, 1.0 to 1.8% Si, 1.5% or less Mn, 0.001 to 0.050% O, and the balance being Ni and unavoidable impurities, wherein Zr among the unavoidable impurities is limited to 0.01% or less.
[0036] (Additive Manufacturing Process) The additive manufacturing method in the additive manufacturing process is not particularly limited. For example, the Ni-based alloy powder of the present invention can be supplied to a powder bed fusion (PBF) additive manufacturing device, and high energy such as a laser beam or an electron beam is irradiated onto the area where the powder is spread to selectively melt and bond the alloy powder, thereby additively manufacturing a shaped product of a desired shape. Additive manufacturing devices can be classified into powder bed fusion (PBF) and directed energy deposition (DED) devices depending on the shape of the additive manufacturing product, but the additive manufacturing product of this embodiment can be manufactured using either method, and the type of additive manufacturing device is not particularly limited.
[0037] (Heat Treatment of Additive Manufacturing Product) In the manufacturing method of an additive manufacturing product of the present invention, the product manufactured by the additive manufacturing method may be subjected to solution heat treatment for the purpose of removing residual stress and reducing microsegregation. The temperature when performing solution heat treatment is preferably 1000°C or higher to dissolve the microsegregation, and 1200°C or lower because it needs to be lower than the solidus temperature. More preferably, it is 1050°C or higher and 1180°C or lower, and even more preferably, it is 1100°C or higher and 1160°C or lower.
[0038] [Layered manufactured product] The layered manufactured product of the present invention contains, by mass%, 3.5 to 5.5% Al, 0.8 to 4.0% Cr, 0.02 to 0.06%, 1.0 to 1.8% Si, 1.5% or less Mn, and 0.001 to 0.050% O, with the balance being Ni and unavoidable impurities, in which Zr contained in the unavoidable impurities is limited to 0.01% or less, the defect rate is 0.1% or less, and the amount of oxidation per unit area, which is obtained by an oxidation test performed in an atmospheric furnace at 800°C for 950 hours and is expressed as [mass loss before and after oxidation test] / [surface area before oxidation test], is 0.005 mg / mm 2The additively manufactured product is characterized by having excellent high-temperature oxidation resistance due to an alumina coating formed on the surface layer. The uses of the additively manufactured product are not particularly limited, and it is possible to provide, for example, components for semiconductor manufacturing equipment made from the additively manufactured product. The additively manufactured product has excellent high-temperature oxidation resistance, particularly at temperatures above 700°C, and is less likely to develop an oxide coating on the surface even when used in high-temperature environments. Therefore, when the additively manufactured product is used as a component or part to be installed inside an oxidation furnace for semiconductor manufacturing or a baking furnace for electronic component manufacturing, it is effective because it makes oxides less likely to peel from the surface of the component or part, thereby preventing foreign matter from being mixed into manufactured products such as semiconductors and electronic components. Furthermore, additively manufactured products with excellent high-temperature oxidation resistance and complex shapes can be provided not only for semiconductor manufacturing equipment components but also for a wide range of fields, such as parts in the aviation, space, and automotive industries, chemical plants and pharmaceutical manufacturing facilities, and energy fields such as oil and gas.
[0039] (Amount of oxidation per unit area of the additive manufacturing product: 0.5 mg / cm 2 The additive manufacturing product of the present invention has excellent high-temperature oxidation resistance. Here, high-temperature oxidation resistance can be evaluated by the unit area oxidation amount expressed by (Equation 1). In a high-temperature oxidation test conducted in an atmospheric furnace at 800°C for 950 hours, if the unit area oxidation amount is 0.5 mg / cm 2 When the amount of oxidation per unit area is less than 0.4 mg / cm, the growth of the oxide film can be significantly suppressed. 2 The more preferable unit area oxidation amount is 0.3 mg / cm or less. 2 The following is the result.
[0040] [Unit area oxidation amount (mg / cm 2 ) )] = [mass loss before and after oxidation test (mg)] / [surface area before oxidation test (cm 2 )]...(Formula 1)
[0041] (Defect rate of additively manufactured products: 0.1% or less) Since internal defects in additively manufactured products can be the starting point of cracks, it is desirable for the defect rate to be low. The defect rate can be measured as the area ratio of defective parts such as voids and unmelted powder. Details of the measurement conditions will be described later. If the defect rate is 0.1% or less, there will be very few internal defects that can be the starting point of cracks, so the defect rate is set to 0.1% or less. Furthermore, a preferred defect rate is 0.05% or less, and a more preferred defect rate is 0.025% or less.
[0042] (Hardness of additive manufacturing product: 210 to 300 HV) It is desirable that the additive manufacturing product of the present invention has high tensile strength. Therefore, the hardness, which is proportional to the tensile strength, is set to 210 HV or more. On the other hand, from the viewpoint of maintaining machinability and preventing cracking, the upper limit of the hardness is set to 300 HV. Furthermore, the preferred hardness range is 240 to 290 HV, more preferably 260 to 280 HV. Details of the measurement conditions, etc. will be described later.
[0043] Examples of the present invention will be described below. First, as an example, alloy powder a (hereinafter simply referred to as powder) having the composition shown in Table 1 was produced. Furthermore, as comparative examples, alloy powders b to e having the compositions shown in Table 1 were produced. The alloy powder was produced using a vacuum gas atomization method. Raw material powders blended to achieve the specified composition were melted in a high-frequency vacuum melting furnace. Alloy powders a, c, and e were melted in a vacuum furnace using Al. 2 O 3 Alloy powders b and d were ZrO 2 The alloy was melted in a crucible made of aluminum. Argon gas was then sprayed onto the molten metal poured from the bottom of the crucible to refine the particles, which were then solidified in a cooling tower to obtain spherical powder. The resulting powder was then classified to obtain alloy powders a to e with particle sizes ranging from 10 to 60 μm.
[0044]
[0045] The chemical compositions of these alloy powders shown in Table 1 were analyzed using, for example, inductively coupled plasma (ICP) atomic emission spectrometry. Comparing the component compositions of the example powders and comparative example powders shown in Table 1, it can be seen that, compared to example powder a, powder b has a reduced C content and an increased Zr content, powder c has reduced C and Si contents, powder d has an increased Zr content, and powder e has an increased Al content.
[0046] [Evaluation of Ni-based alloy powder properties] The alloy powders a to e were measured for fluidity, angle of repose, and hardness, and the results are shown in Table 2. The measurement methods and conditions are described below.
[0047] (Evaluation of particle size and fluidity) The particle diameters d10, d50, and d90 were measured using a laser diffraction particle size distribution analyzer (Malvern Panalytical: Master Sizer 3000). The measured d10, d50, and d90 were used to calculate the uniformity expressed as (d90-d10) / d50. In addition, the flowability of each powder was measured using a fluidity measuring instrument (Tsutsui Rikagaku Co., Ltd.) in accordance with JIS-Z2502.
[0048] (Evaluation of Angle of Repose) The angle of repose was measured using a multi-function powder property measuring instrument (Multitester MT-02, manufactured by Seishin Co., Ltd.). The measurement was carried out in accordance with JIS R9301-2-2, specifically, alloy powder was supplied to a tray in the measuring instrument, and the angle of the formed peaks was measured. At this time, a 355 μm sieve was used to supply the alloy powder.
[0049] (Hardness Evaluation) After filling 1 g of alloy powder into a 2 mm diameter hole, the alloy powder was embedded in resin using a cold resin embedding vacuum device (Struers: CitoVac). The embedded alloy powder was polished to #1500 with waterproof emery paper, and then polished with diamond paste in the order of particle size 1 μm and 0.3 μm to obtain a mirror finish, thereby obtaining a test piece for hardness evaluation. The Vickers hardness of the mirror-finished surface was measured using a micro Vickers hardness tester (Fature Tech: FM-110). Specifically, a square pyramidal diamond indenter was pressed into powder particles with a particle size of 30 to 40 μm at a total of 10 points, and held at a test load of 25 gf for 15 seconds. The diagonal length of the indentations remaining on the surface was then measured to calculate the hardness, and the average value and standard deviation of the hardness at 10 points for each test piece powder were determined.
[0050]
[0051] The evaluation results of the fluidity, angle of repose, and hardness of powders a to e are shown in Table 2. Comparing the measurement results of the Examples and Comparative Examples, it was found that powder a satisfied the above-mentioned preferred ranges for both particle size distribution and uniformity, which are also related to spreading ability, and even more preferred ranges.
[0052] On the other hand, when comparing the hardness of each powder shown in Table 2, it can be seen that powder c has a lower hardness and powder e has a higher hardness than powders a, b, and d. It is presumed that the decrease in Si content of powder c has contributed to the decrease in powder hardness. It is also presumed that the increase in Al content of powder e has contributed to the improvement in powder hardness. Furthermore, although no clear significant difference is observed in the hardness of powders a, b, and d, the hardness of powders b and d has a high standard deviation and a large variance in the measured values, so it can be said that powder a, which is an example, provides a more stable hardness.
[0053] [Evaluation of properties of additively manufactured products] Additively manufactured products (hereinafter also simply referred to as manufactured products) A to E were produced for each of the alloy powders a to e using an additively manufactured product (M290 manufactured by EOS) that employs a selective laser melting (SLM) method using a laser as a heat source. The additively manufactured products were produced under the conditions of an energy density of 20 to 200 J / mm3 In this example, the parameters are set to 300 W laser power, 1000 mm / s scanning speed, 0.1 mm scanning pitch, and 0.04 mm layer thickness, and the energy density is 75 J / mm 3 It was.
[0054] [Energy density (J / mm 3 ) ]=[Laser power (W)] / ([Scanning speed (mm / s)] × [Scanning pitch (mm)] × [Layer thickness (mm)]) ... (Equation 2)
[0055] Additive manufacturing products A to E were produced as plates (25 mm x 25 mm x 5 mm) and blocks (10 mm x 10 mm x 10 mm). Additive manufacturing products A to E were evaluated for defect rate and hardness, and additive manufacturing products A to C were evaluated for high-temperature oxidation resistance. The results are shown in Table 3 and Figure 1. The measurement methods and conditions are described below.
[0056] (Defect Rate Evaluation) The cross sections of the block material (10 mm x 10 mm x 10 mm) of the additively manufactured products A to E were cut and embedded in resin using a hot resin embedding vacuum device (Struers: CitoPress-30). The additively manufactured products embedded in resin were polished to #1500 with waterproof emery paper, and then polished with diamond paste with particle sizes of 1 μm and 0.3 μm in that order to obtain a mirror finish, thereby obtaining test pieces for defect rate measurement. The mirror-finished surface was checked for crack occurrence and the defect rate was measured using a digital microscope (Keyence: VHX-6000). If fine cracks were observed, the defect rate was not evaluated. The defect rate measurement areas were one location at the center of the mirror-finished surface and four locations approximately 1 mm away from the center toward the four corners. In each measurement area, a surface image of 1.58 mm x 1.25 mm was acquired, and each acquired image was binarized to determine the area of blackened voids and unmelted powder, which was 0.18 μm 2 The above-mentioned portions were identified as defective portions. The area ratio of the defective portions (defect rate) was then calculated, and the average value and standard deviation of the defect rate at five points in each test piece were determined.
[0057] (Hardness Evaluation) The Vickers hardness of the mirror-finished surface was measured using a micro Vickers hardness tester (FM-110 manufactured by Featuretec Co., Ltd.). The measurement area was one location at the center of the mirror-finished surface and four locations approximately 1 mm apart from the center toward the four corners. Specifically, a square pyramidal diamond indenter was pressed into the surface, and a test load of 25 gf was applied and held for 15 seconds. Thereafter, the diagonal length of the indentation remaining on the surface was measured to calculate the hardness, and the average value and standard deviation of the hardness at five points in each test piece were determined.
[0058]
[0059] Table 3 shows the hardness (HV) and defect rate (area %) of the additively manufactured products. The measurement results show that products A, D, and E have higher hardness than products B and C. This is thought to be because products A, D, and E have a higher carbon content than products B and C.
[0060] The measurement results also revealed that molded products A and C were free of fine cracks. Furthermore, the defect rate for molded product A was 0.016%, and that for molded product C was 0.026%. Both defect rates were below 0.1%, which is an excellent result for a composition system with high weld crack susceptibility. This is because most defects in the composition system of Ni-based corrosion-resistant alloys containing Zr are cracks, and it is believed that the occurrence of cracks was prevented by limiting the Zr content of both alloy powders a and c to a low value of 0.01% or less. On the other hand, molded products B, D, and E exhibited numerous cracks. This is believed to be due to the high Zr content of molded products B and D, and the excessive Al content of molded product E. Furthermore, molded products A and C were confirmed to have high internal density and excellent additive manufacturing properties. However, molded product C had low hardness, raising concerns that the tensile strength of the molded product may also be low. It should be noted that the defect rates for molded products B, D, and E could not be calculated due to the large number of cracks that occurred.
[0061] (Evaluation of High-Temperature Oxidation Resistance) To evaluate the high-temperature oxidation resistance of the molded products A and C, which did not develop cracks in the defect evaluation described above, as-molded specimens of the molded plate materials A and C were prepared. For comparison, as-molded specimens of the molded product B were also prepared as an example of a sample in which cracks developed. The surfaces of these plates were polished to #400 with waterproof emery paper, then electropolished. After electropolishing, each plate was degreased by subjecting it to ultrasonic vibration in acetone for 5 minutes to obtain high-temperature oxidation resistance test specimens. After measuring the mass of each test specimen, it was held at 800°C in a small atmospheric furnace, and the oxidation time was set to four stages: 250 hours, 500 hours, 750 hours, and 950 hours. After cooling to room temperature, the mass change of the test specimen was measured at each stage. The amount of oxidation per unit area (mg / cm) of each test specimen was calculated using the above (Equation 1). 2 The measurement results are shown in Figure 1.
[0062] From the results of the high-temperature oxidation resistance test shown in FIG. 1, the amount of oxidation per unit area of the molded product A was 0.23 mg / cm even after 950 hours. 2 On the other hand, the density of the molded article B was maintained at 3.14 mg / cm 2 , and shaped product C is 1.34 mg / cm 2 The amount of oxidation is significantly greater. It was confirmed that shaped product A has extremely excellent high-temperature oxidation resistance, as the amount of oxidation per unit area is suppressed over a long period of time. This is thought to be because alloy powder a contains more Si than alloy powder c, which stabilizes the alumina coating formed on the surface of shaped product A and suppresses further oxidation. On the other hand, shaped product B has a poor high-temperature oxidation resistance because alloy powder b contains more Zr than alloy powders a and c, which causes Zr oxide to form and inhibits the formation of an alumina coating on the surface.
[0063] From the above test results, it was confirmed that alloy powder a, which is an example of the Ni-based alloy powder for additive manufacturing of the present invention, has a composition that is superior in high-temperature oxidation resistance and low in cracking sensitivity compared to alloy powders b to e, which are comparative examples, and also has fluidity and hardness that are suitable for suppressing defects and for laying down during additive manufacturing. Furthermore, with regard to additive manufacturing products produced using alloy powder a, it was confirmed that molded product A, which is an example, is superior in hardness, defect rate, and high-temperature oxidation resistance compared to molded products B to E, which are comparative examples.
Claims
1. A Ni-based alloy powder for additive manufacturing, characterized in that it contains, by mass%, Al: 3.5 to 5.5%, Cr: 0.8 to 4.0%, C: 0.02 to 0.06%, Si: 1.0 to 1.8%, Mn: 1.5% or less, O: 0.001 to 0.050%, with the balance consisting of Ni and unavoidable impurities, and Zr among the unavoidable impurities being limited to 0.01% or less.
2. The Ni-based alloy powder for additive manufacturing according to claim 1, characterized in that the contents are, in mass%, Al: 3.6 to 5.0%, Cr: 1.5 to 3.0%, C: 0.03 to 0.05%, Si: 1.2 to 1.5%, Mn: 0.2 to 1.0%, and O: 0.008 to 0.030%.
3. The Ni-based alloy powder for additive manufacturing according to claim 1 or 2, characterized in that the Vickers hardness is in the range of 160 to 220 HV.
4. A Ni-based alloy powder for additive manufacturing according to claim 1 or 2, characterized in that in an cumulative distribution curve showing the relationship between particle diameter and volume accumulation from the small particle diameter side, obtained by laser diffraction, the particle diameter d10 corresponding to a cumulative frequency of 10 volume % is 10 μm or more and 25 μm or less, the particle diameter d50 corresponding to a cumulative frequency of 50 volume % is 25 μm or more and 40 μm or less, and the particle diameter d90 corresponding to a cumulative frequency of 90 volume % is 45 μm or more and 60 μm or less.
5. The Ni-based alloy powder for additive manufacturing according to claim 4, characterized in that the uniformity expressed by (d90-d10) / d50 is in the range of 0.8 to 1.
2.
6. The Ni-based alloy powder for additive manufacturing according to claim 1 or 2, characterized in that the angle of repose measured in accordance with JIS R9301-2-2 is 40 degrees or less.
7. A method for manufacturing an additively manufactured product, comprising an additive manufacturing process of forming an additively manufactured product using a Ni-based alloy powder containing, by mass%, Al: 3.5 to 5.5%, Cr: 0.8 to 4.0%, C: 0.02 to 0.06%, Si: 1.0 to 1.8%, Mn: 1.5% or less, O: 0.001 to 0.050%, with the balance being Ni and unavoidable impurities, wherein Zr among the unavoidable impurities is limited to 0.01% or less.
8. A steel sheet containing, by mass%, Al: 3.5 to 5.5%, Cr: 0.8 to 4.0%, C: 0.02 to 0.06%, Si: 1.0 to 1.8%, Mn: 1.5% or less, and O: 0.001 to 0.050%, with the balance consisting of Ni and unavoidable impurities, in which the Zr contained in the unavoidable impurities is limited to 0.01% or less, the defect rate is 0.1% or less, and the unit area oxidation amount, obtained by an oxidation test performed in an atmospheric furnace at 800°C for 950 hours, expressed as [mass loss before and after oxidation test] / [surface area before oxidation test], is 0.005 mg / mm 2 An additively manufactured product characterized by:
9. The additively manufactured product according to claim 8, characterized in that the Vickers hardness is in the range of 210 to 300 HV.