Sintered electrode, battery component, and method for manufacturing the sintered electrode and battery component, solid electrolyte precursor solution, solid electrolyte precursor, and solid electrolyte

A sintered electrode with a carbon electrode and alkali ion-conducting solid electrolyte addresses safety and temperature operation challenges in sodium batteries, ensuring low reactivity and efficient performance.

KR103046141B1Active Publication Date: 2026-11-10NIPPON ELECTRIC GLASS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
KR1020227021635
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-02
Filing Date
2021-07-02
Publication Date
2026-11-10
Estimated Expiration
2041-07-02

AI Technical Summary

Technical Problem

Conventional all-solid-state sodium batteries face safety concerns due to the reactivity of sodium metal in the negative electrode with moisture and operational challenges at both high and low temperatures.

Method used

A sintered electrode composed of a carbon electrode material, such as graphite or hard carbon, combined with an alkali ion-conducting solid electrolyte, preferably NASICON-type crystals, is used, which is coated with an alkaline ion-conducting solid electrolyte, enhancing safety and enabling operation at low temperatures.

Benefits of technology

The sintered electrode provides enhanced safety by reducing moisture reactivity and allows the battery to operate effectively at low temperatures with high charge/discharge efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022066154785-PCT00001_ABST
    Figure 112022066154785-PCT00001_ABST
Patent Text Reader

Abstract

The present invention provides a sintered electrode, a battery component, and a method for manufacturing the sintered electrode and the battery component, which can increase safety and also operate the battery at low temperatures. The sintered electrode (3) of the present invention is characterized by comprising a carbon electrode material made of graphite or hard carbon and an alkali ion-conducting solid electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a sintered electrode and a battery component using the same, a method for manufacturing the sintered electrode and the battery component, an alkaline ion conductive solid electrolyte precursor solution, an alkaline ion conductive solid electrolyte precursor, and an alkaline ion conductive solid electrolyte. Background Technology

[0002] Lithium-ion rechargeable batteries have established themselves as indispensable high-capacity and lightweight power sources for mobile devices and electric vehicles. However, current lithium-ion rechargeable batteries primarily use flammable organic electrolytes as their electrolytes, raising concerns about risks such as fire. As a solution to this problem, the development of all-solid-state lithium-ion batteries using solid electrolytes instead of organic electrolytes is underway. However, because there are concerns regarding the global surge in the price of lithium raw materials, research on all-solid-state sodium-ion batteries has recently been conducted as an alternative.

[0003] Patent Document 1 below discloses an example of a sodium battery. This sodium battery has a positive electrode, a negative electrode, and a sulfide-based solid electrolyte. A metal sulfide or sodium metalate is used for the positive electrode. A sodium metal or a sodium alloy is used for the negative electrode. Prior art literature

[0004] Japanese Patent Publication No. 2017-208324 The problem to be solved

[0005] However, in a sodium battery as described in Patent Document 1, the sodium metal used in the negative electrode is prone to reacting with moisture, so it is difficult to sufficiently increase safety.

[0006] In addition, conventional all-solid-state sodium batteries often operate at relatively high temperatures, such as 60°C or higher, and there was also a problem that they were difficult to operate sufficiently at low temperatures.

[0007] The objective of the present invention is to provide a sintered electrode, a battery component, a method for manufacturing the sintered electrode and the battery component, a solid electrolyte precursor solution, a solid electrolyte precursor, and a solid electrolyte, which can increase safety and also enable the battery to operate at low temperatures. means of solving the problem

[0008] The sintered electrode according to the present invention is characterized by comprising a carbon electrode material made of graphite or hard carbon and an alkali ion-conducting solid electrolyte.

[0009] It is desirable for an alkaline ion-conducting solid electrolyte to have sodium ion conductivity.

[0010] It is desirable that the alkaline ion-conducting solid electrolyte be composed of oxides.

[0011] The sintered electrode according to the present invention comprises a mixed phase of a carbon electrode material and an alkaline ion-conducting solid electrolyte, and preferably the mixed phase consists of particles, with an average particle size of 10 μm or less.

[0012] It is preferable that the carbon electrode material is a particulate carbon electrode material and that the particulate carbon electrode material is covered by a coating layer consisting of an alkaline ion-conducting solid electrolyte.

[0013] It is preferable that the carbon electrode material is a particulate carbon electrode material, and that the particulate carbon electrode material is covered by a coating layer consisting of a carbon electrode material different from the particulate carbon electrode material and an alkaline ion-conducting solid electrolyte.

[0014] The alkaline ion-conducting solid electrolyte is a NASICON-type crystal, and also has the general formula Na 1+x Zr2P 3-x Si x O 12It is preferable to include at least one of a first compound represented by (0≤x≤3) and a second compound in which a portion of Zr of the first compound is substituted with at least one element selected from the group consisting of Ca, Mg, Ba, Sr, Al, Nb, Ta, In, Ga and a group 3 element.

[0015] It is desirable for the alkali ion-conducting solid electrolyte to have at least one of a β-alumina type crystal and a β"-alumina type crystal.

[0016] Alkali ion-conducting solid electrolyte has the general formula Li7La3Zr2O 12 , Li7La3Zr 2-x M x O 12 (M is at least one selected from Nb, Ga, and Ta, 0 <x<2) 또는 Li 7-3x Al x La3Zr2O 12 (0 <x<2.3)로 나타내어지는 결정상을 갖는 것이 바람직하다.

[0017] The sintered electrode according to the present invention preferably comprises 0% to 20% by weight of at least one carbon-based conductive additive selected from carbon black, acetylene black, Ketjenblack, carbon nanotubes, and vapor phase carbon fiber carbon conductive additive (VGCF).

[0018] It is preferable that the sintered electrode according to the present invention is a negative electrode.

[0019] It is preferable that the sintered electrode according to the present invention is capable of absorbing and releasing alkali ions at 30°C after heat treatment in an inert atmosphere at 500°C.

[0020] It is preferable that the sintered electrode according to the present invention has a charge / discharge efficiency of 90% or more and can be reversibly charged / discharged when charged / discharged at a cutoff voltage of 9V to 0.001V.

[0021] A battery member according to the present invention is characterized by having a solid electrolyte layer and a sintered electrode laminated on the solid electrolyte layer.

[0022] It is preferable that the thickness of the solid electrolyte layer be 5 nm to 1 mm.

[0023] The battery according to the present invention is characterized by having the battery member.

[0024] A method for manufacturing a sintered electrode according to the present invention is characterized by comprising a process for obtaining a mixture of an alkaline ion-conducting solid electrolyte precursor and a carbon electrode material precursor by mixing an alkaline ion-conducting solid electrolyte precursor and a carbon electrode material precursor, wherein the carbon electrode material precursor is a precursor of a carbon electrode material made of graphite or hard carbon, a process for forming a material layer for forming an electrode containing the mixture after the mixing process, and a process for sintering the material layer for forming an electrode.

[0025] In a process of firing the electrode-forming material layer, the electrode-forming material layer is composed of a paste or compact containing an alkaline ion-conducting solid electrolyte precursor and a carbon electrode material precursor, and it is preferable to obtain the alkaline ion-conducting solid electrolyte and the carbon electrode material simultaneously.

[0026] In a process for forming a material layer for forming an electrode, after performing a first firing process to obtain a carbon electrode material by firing a mixture, a material layer for forming an electrode comprising a paste or a compact including an alkali ion-conducting solid electrolyte precursor and a carbon electrode material is formed, and in a process for firing the material layer for forming an electrode, it is preferable to obtain an alkali ion-conducting solid electrolyte from the alkali ion-conducting solid electrolyte precursor.

[0027] After the mixing process, a third firing process is further provided to simultaneously obtain an alkali ion-conducting solid electrolyte and a carbon electrode material by firing the mixture, and in the process of forming a material layer for forming an electrode, it is preferable to form a material layer for forming an electrode consisting of a paste or a compact, comprising an alkali ion-conducting solid electrolyte and a carbon electrode material.

[0028] A method for manufacturing a sintered electrode in another aspect of the present invention is characterized by comprising: a mixing process for obtaining a mixture of an alkaline ion-conducting solid electrolyte precursor and a particulate carbon electrode material by mixing an alkaline ion-conducting solid electrolyte precursor and a particulate carbon electrode material made of graphite or hard carbon; a process for forming an electrode-forming material layer made of a paste or compacted body comprising the alkaline ion-conducting solid electrolyte precursor and the particulate carbon electrode material after the mixing process; and a process for obtaining a particulate carbon electrode material covered by a coating layer made of an alkaline ion-conducting solid electrolyte by calcining the electrode-forming material layer and obtaining an alkaline ion-conducting solid electrolyte from the alkaline ion-conducting solid electrolyte precursor.

[0029] A method for manufacturing a sintered electrode in another aspect of the present invention is characterized by a process of obtaining a mixture of an alkaline ion-conducting solid electrolyte precursor, a carbon electrode material precursor, and a particulate carbon electrode material made of graphite or hard carbon by mixing an alkaline ion-conducting solid electrolyte precursor, a carbon electrode material precursor, and a particulate carbon electrode material made of graphite or hard carbon, wherein the carbon electrode material precursor is a carbon electrode material precursor made of graphite or hard carbon, a mixing process in which, after the mixing process, a material layer for forming an electrode made of a paste or a compacted body containing the mixture is formed, and a material layer for forming an electrode is sintered and an alkaline ion-conducting solid electrolyte and a carbon electrode material are obtained from the alkaline ion-conducting solid electrolyte precursor and the carbon electrode material precursor, thereby obtaining a particulate carbon electrode material covered by a coating layer made of an alkaline ion-conducting solid electrolyte and a carbon electrode material.

[0030] The method for manufacturing a battery member according to the present invention is a method for manufacturing a battery member comprising a laminate of a sintered electrode and a solid electrolyte layer, wherein the method comprises a process for obtaining a mixture of an alkaline ion-conducting solid electrolyte precursor and a carbon electrode material precursor by mixing an alkaline ion-conducting solid electrolyte precursor and a carbon electrode material precursor, wherein the carbon electrode material precursor is a precursor of a carbon electrode material made of graphite or hard carbon; a process for forming an electrode-forming material layer containing the mixture after the mixing process; a process for obtaining a sintered electrode and a laminate of a sintered electrode and a solid electrolyte layer by firing the electrode-forming material layer.

[0031] It is preferable to obtain an alkali ion-conducting solid electrolyte and a carbon electrode material simultaneously by forming a material layer for forming an electrode as a paste or compact containing an alkali ion-conducting solid electrolyte precursor and a carbon electrode material precursor, and by firing the material layer for forming the electrode.

[0032] In a process for forming a material layer for forming an electrode, after performing a first firing process to obtain a carbon electrode material by firing a mixture, a material layer for forming an electrode comprising a paste or a compacted body including an alkali ion-conducting solid electrolyte precursor and a carbon electrode material is formed, and a sintered electrode is obtained; preferably, the process is a second firing process to obtain an alkali ion-conducting solid electrolyte by firing the material layer for forming an electrode.

[0033] After the mixing process, there is a third sintering process to simultaneously obtain an alkali ion-conducting solid electrolyte and a carbon electrode material by sintering the mixture, and in the process of forming a material layer for forming an electrode, it is preferable that the process of forming a material layer for forming an electrode made of a paste or a compacted body including an alkali ion-conducting solid electrolyte and a carbon electrode material, and obtaining a sintered electrode, is a fourth sintering process for sintering the material layer for forming an electrode.

[0034] A method for manufacturing a battery member in another aspect of the present invention is a method for manufacturing a battery member comprising a laminate of a sintered electrode and a solid electrolyte layer, characterized by comprising: a mixing process for obtaining a mixture of an alkaline ion-conducting solid electrolyte precursor and a particulate carbon electrode material made of graphite or hard carbon by mixing an alkaline ion-conducting solid electrolyte precursor and a particulate carbon electrode material; a process for forming an electrode-forming material layer made of a paste or a compacted body containing the alkaline ion-conducting solid electrolyte precursor and the particulate carbon electrode material after the mixing process; a process for obtaining a sintered electrode and a laminate of a sintered electrode and a solid electrolyte layer by firing the electrode-forming material layer and obtaining an alkaline ion-conducting solid electrolyte from the alkaline ion-conducting solid electrolyte precursor, and obtaining the particulate carbon electrode material covered by a coating layer made of the alkaline ion-conducting solid electrolyte.

[0035] It is preferable to further provide a lamination process for laminating a solid electrolyte layer and a material layer for forming an electrode, and to perform a process for obtaining a sintered electrode after the lamination process.

[0036] It is preferable to further provide a lamination process for laminating a solid electrolyte forming material layer comprising a paste or compact body containing a solid electrolyte precursor and an electrode forming material layer, and to obtain a sintered electrode and a solid electrolyte layer simultaneously by sintering the electrode forming material layer and the solid electrolyte forming material layer after the lamination process.

[0037] The alkali ion conductive solid electrolyte precursor solution according to the present invention is characterized by comprising an alkali metal element, a transition metal element, and a carbonate ion.

[0038] It is desirable for carbonate ions to be coordinated to transition metal elements.

[0039] It is preferable that the transition metal element be at least one selected from the group consisting of group 3 elements and group 4 elements.

[0040] The alkaline ion-conducting solid electrolyte precursor solution according to the present invention preferably has a pH of 7 or higher.

[0041] As the counterion of the carbonate ion, NR4 + It is preferable to include (in the formula, each R is independently selected from the group consisting of H, CH3, C2H5 and CH2CH2OH, at least one substituent).

[0042] The alkaline ion-conducting solid electrolyte precursor solution according to the present invention is preferably a precursor solution of a solid electrolyte composed of NASICON-type crystals.

[0043] The alkaline ion-conducting solid electrolyte precursor solution according to the present invention is preferably a precursor solution of a sodium ion-conducting solid electrolyte.

[0044] The alkaline ion-conducting solid electrolyte precursor according to the present invention is characterized by being composed of a gel or a dried product of the alkaline ion-conducting solid electrolyte precursor solution.

[0045] The alkaline ion-conducting solid electrolyte according to the present invention is characterized by being composed of a calcined product of the alkaline ion-conducting solid electrolyte precursor. Effects of the invention

[0046] According to the present invention, a sintered electrode, a battery component, a method for manufacturing the sintered electrode and the battery component, a solid electrolyte precursor solution, a solid electrolyte precursor, and a solid electrolyte can be provided, which can increase safety and also enable the battery to be operated at low temperatures. Brief explanation of the drawing

[0047] FIG. 1 is a schematic cross-sectional view showing a battery member according to a first embodiment of the present invention. FIG. 2 is an SEM image showing a sintered electrode according to one embodiment of the present invention. FIGS. 3(a) and FIGS. 3(b) are schematic cross-sectional views illustrating a method for manufacturing a battery member according to a first embodiment of the present invention. Figure 4 is a diagram showing the results of the charge / discharge test of the comparative example. Figure 5 is a diagram showing the results of a charge / discharge test of Example 1 of the present invention. FIG. 6 is a diagram showing the charge / discharge test results when the test battery manufactured in Example 1 of the present invention is charged and discharged at a cutoff voltage of 9V to 0.001V. Figure 7 is a diagram showing the XRD (X-ray diffraction) charts after drying and after calcination of the alkali ion-conducting solid electrolyte precursor prepared in Example 2 and Reference Example of the present invention. FIGS. 8(a) and FIGS. 8(b) are schematic cross-sectional views illustrating a method for manufacturing a battery member according to a second embodiment of the present invention. FIGS. 9(a) and FIGS. 9(b) are schematic cross-sectional views illustrating a method for manufacturing a battery member according to a third embodiment of the present invention. FIGS. 10(a) and FIGS. 10(b) are schematic cross-sectional views illustrating a method for manufacturing a battery member according to a fourth embodiment of the present invention. FIGS. 11(a) to 11(c) are schematic cross-sectional views for explaining a method for manufacturing a battery member according to Variant Example 1 of the fourth embodiment of the present invention. FIGS. 12(a) to 12(c) are schematic cross-sectional views for explaining a method for manufacturing a battery member according to Variant Example 2 of the fourth embodiment of the present invention. FIGS. 13(a) and FIGS. 13(b) are schematic cross-sectional views illustrating a method for manufacturing a battery member according to a fifth embodiment of the present invention. FIGS. 14(a) and FIGS. 14(b) are schematic cross-sectional views illustrating a method for manufacturing a battery member according to a sixth embodiment of the present invention. FIGS. 15(a) and FIGS. 15(b) are schematic cross-sectional views illustrating a method for manufacturing a sintered electrode according to the seventh embodiment of the present invention. FIGS. 16(a) and FIGS. 16(b) are schematic cross-sectional views illustrating a method for manufacturing a sintered electrode according to the eighth embodiment of the present invention. FIGS. 17(a) and FIGS. 17(b) are schematic cross-sectional views illustrating a method for manufacturing a sintered electrode according to a ninth embodiment of the present invention. FIG. 18 is a schematic cross-sectional view showing a battery member according to a second embodiment of the present invention. FIGS. 19(a) and FIGS. 19(b) are schematic cross-sectional views illustrating a method for manufacturing a battery member according to the 10th embodiment of the present invention. FIGS. 20(a) and FIGS. 20(b) are schematic cross-sectional views illustrating a method for manufacturing a battery member according to the eleventh embodiment of the present invention. FIGS. 21(a) and FIGS. 21(b) are schematic cross-sectional views illustrating a method for manufacturing a sintered electrode according to the 12th embodiment of the present invention. FIG. 22 is a schematic cross-sectional view showing a battery member according to a third embodiment of the present invention. FIGS. 23(a) and FIGS. 23(b) are schematic cross-sectional views illustrating a method for manufacturing a battery member according to the 13th embodiment of the present invention. FIG. 24 is a diagram showing the results of a charge / discharge test of Example 3 of the present invention. Specific details for implementing the invention

[0048] Preferred embodiments are described below. However, the following embodiments are merely examples, and the present invention is not limited to the following embodiments. Additionally, in the drawings, components having substantially the same function may be referred to by the same reference numerals.

[0049] [Battery component]

[0050] (First embodiment)

[0051] FIG. 1 is a schematic cross-sectional view showing a battery member according to a first embodiment of the present invention. FIG. 1 is also a schematic cross-sectional view of the member when viewed from the side direction. The following schematic cross-sectional views other than FIG. 1 are the same.

[0052] A battery member (1) comprises a solid electrolyte layer (2), a sintered electrode (3) according to one embodiment of the present invention, and a current collector (4). The solid electrolyte layer (2) has alkaline ion conductivity. More specifically, in this embodiment, the solid electrolyte layer (2) has sodium ion conductivity. In particular, the solid electrolyte layer (2) may have lithium ion conductivity. Furthermore, the solid electrolyte layer (2) is preferably as thin as possible to increase energy density, and specifically, the thickness is preferably 1 mm or less, more preferably 500 μm or less, and even more preferably 100 μm or less. The lower limit is not specifically limited, but in reality, it is preferable to be 5 nm or more to ensure mechanical strength or separator function.

[0053] The solid electrolyte layer (2) has a first main surface (2a) and a second main surface (2b). The first main surface (2a) and the second main surface (2b) face each other. A sintered electrode (3) is laminated on the first main surface (2a) of the solid electrolyte layer (2). A current collector (4) is laminated on the sintered electrode (3). The current collector (4) is made of a suitable metal thin film. Additionally, the battery member (1) does not necessarily have to have a current collector (4). Furthermore, in the embodiments described below, the current collector (4) may be omitted from the drawings.

[0054] In this embodiment, the sintered electrode (3) is a negative electrode. By stacking a positive electrode on the second main surface (2b) of the solid electrolyte layer (2), an all-solid-state battery can be obtained.

[0055] The sintered electrode (3) comprises a carbon electrode material and an alkaline ion-conducting solid electrolyte. The carbon electrode material is made of graphite or hard carbon. In this embodiment, the alkaline ion-conducting solid electrolyte has sodium ion conductivity. In particular, the alkaline ion-conducting solid electrolyte may have lithium ion conductivity.

[0056] The sintered electrode (3) comprises a mixed phase (5) of a carbon electrode material and an alkaline ion-conducting solid electrolyte. The mixed phase (5) is in a particulate form. The particulate mixed phases (5) are bonded together by sintering.

[0057] FIG. 2 is an SEM image showing a sintered electrode according to an embodiment of the present invention. In FIG. 2, it is confirmed that the particles are bonded together. Each of these particles forms a mixed phase (5). In the mixed phase (5), it is confirmed that the boundary between the carbon electrode material and the alkali ion-conducting solid electrolyte cannot be distinguished. Thus, in the mixed phase (5), the carbon electrode material and the alkali ion-conducting solid electrolyte are uniformly mixed. The average particle size of each particle constituting the mixed phase (5) is preferably 10 μm or less, more preferably 3 μm or less, even more preferably 500 nm or less, and particularly preferably 300 nm or less. By doing so, the density of the sintered electrode (3) can be increased.

[0058] Returning to FIG. 1, it is preferable that the sintered electrode (3) includes a conductive agent (6). By including the conductive agent (6), a conductive path is formed, which can reduce the internal resistance of the sintered electrode (3). If the amount of the conductive agent (6) added is excessive, the amount of shrinkage increases during drying or sintering of the paste, making it difficult to form the electrode; therefore, it is preferable that the amount added is 0% to 20% by weight, and more preferable that it is 0.1% to 10% by weight. In particular, the sintered electrode (3) does not necessarily have to include the conductive agent (6). Furthermore, the sintered electrode (3) does not include a binder (organic binder).

[0059] The battery member (1) comprises a carbon electrode material made of graphite or hard carbon and a sintered electrode (3) of the present invention, which includes an alkaline ion-conducting solid electrolyte. Unlike an electrode made of sodium metal, the sintered electrode (3) has low reactivity to moisture. Furthermore, since it can be used in all-solid-state batteries and does not require an organic electrolyte, the risk of ignition is even lower. Therefore, safety can be enhanced. In addition, by using the battery member (1), the battery can be operated at low temperatures. Details of this effect will be explained below with reference to the manufacturing method of the first embodiment of the present invention and an example using the same. In addition, in this specification, embodiments of the present invention are described by assigning different serial numbers to the battery member and the manufacturing method. Specifically, the battery member according to the first to third embodiments of the present invention and the manufacturing method of the battery member or the sintered electrode according to the first to thirteenth embodiments of the present invention will be described below.

[0060] [Manufacturing Method]

[0061] (First embodiment)

[0062] FIGS. 3(a) and FIGS. 3(b) are schematic cross-sectional views for explaining a method for manufacturing a battery component according to a first embodiment. First, the electrode paste (13A) and the solid electrolyte layer (2) shown in FIG. 3(a) are prepared. In addition, the paste (13A) is a material layer for forming an electrode in the present invention. In this specification, the term "material layer for forming an electrode" refers to a material layer for obtaining (forming) a sintered electrode by firing. The material layer for forming an electrode may, for example, be composed of a paste such as in the present embodiment, or may be composed of a compacted body.

[0063] In obtaining the paste (13A), an alkaline ion-conducting solid electrolyte precursor is prepared. Additionally, at this step, it is preferable to prepare a solution of the alkaline ion-conducting solid electrolyte precursor. Specific examples of the alkaline ion-conducting solid electrolyte precursor and the solution thereof will be described later. Furthermore, a carbon electrode material precursor (a precursor of a carbon electrode material consisting of graphite or hard carbon) is prepared. Suitable sugars, biomass, or polymers may be used as the carbon electrode material precursor.

[0064] Next, the alkali ion-conducting solid electrolyte precursor solution and the carbon electrode material precursor are mixed and then dried. By doing so, a mixture of the alkali ion-conducting solid electrolyte precursor and the carbon electrode material precursor is obtained. Next, the powder obtained by grinding the mixture is mixed with a conductive agent (6) and a binder in an organic solvent. For example, N-methylpyrrolidone can be used as the organic solvent. By doing so, a paste (13A) is obtained.

[0065] Meanwhile, the solid electrolyte layer (2) can be obtained by mixing raw material powders, molding the mixed raw material powders, and then firing them. For example, the solid electrolyte layer (2) can be obtained by slurrying the raw material powders to produce a green sheet, and then firing the green sheet. In addition, the solid electrolyte layer (2) may be obtained by the sol-gel method.

[0066] Next, as shown in FIG. 3(a), a paste (13A) is applied to the first main surface (2a) of the solid electrolyte layer (2). In this way, a lamination process is performed to laminate the solid electrolyte layer (2) and the paste (13A) as a material layer for forming electrodes. Next, the laminate of the solid electrolyte layer (2) and the paste (13A) is fired under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1300°C (preferably greater than 800°C and less than or equal to 1150°C). Additionally, the firing may be performed under an inert atmosphere. For example, the firing may be performed under an Ar, Ne, or He atmosphere, or in a vacuum. The firing process in other embodiments is the same.

[0067] By this, an alkali ion-conducting solid electrolyte and a carbon electrode material are obtained simultaneously, thereby obtaining a mixed phase (5) of the alkali ion-conducting solid electrolyte and the carbon electrode material. In this way, as shown in FIG. 3(b), a sintered electrode (3) is obtained, and a laminate of the sintered electrode (3) and the solid electrolyte layer (2) is obtained. If the firing temperature is excessively low, the reaction becomes insufficient, making it difficult to obtain the desired sintered electrode (3). As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. On the other hand, if the firing temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a risk that it will be difficult to obtain an alkali ion-conducting solid electrolyte having the desired composition. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease.

[0068] Next, a current collector (4) is formed on the sintered electrode (3). The method of forming the current collector (4) is not particularly limited, and, for example, physical vapor phase methods such as deposition or sputtering, or chemical vapor phase methods such as thermal CVD, MOCVD, and plasma CVD are listed. In particular, it is not necessary to form a current collector (4).

[0069] By the above, a battery member (1) can be obtained. In addition, the binder is decomposed by the above sintering. Therefore, the sintered electrode (3) in the battery member (1) does not contain a binder. Here, specific examples of the materials of each component in the battery member (1) are described.

[0070] Carbon electrode material precursor;

[0071] Examples of carbon electrode material precursors include sugars, cellulose, D-glucose, sucrose, etc. Examples of carbon electrode material precursors include cone stems, sorbum stems, pine cones, mangosteen, argan shells, rice husks, dandelions, grain straw cores, ramie fibers, cotton, kelp, coconut endocarp, etc. Examples of carbon electrode material precursors include PAN (polyacrylonitrile), pitch, PVC (polyvinyl chloride) nanofibers, polyaniline, sodium polyacrylate, tire (tire polymer), and PAN dope.

[0072] Alkali ion conductive solid electrolyte in the sintered electrode (3);

[0073] It is preferable that the alkaline ion-conducting solid electrolyte be composed of an oxide. Since an alkaline ion-conducting solid electrolyte composed of an oxide is stable against the atmosphere, it can enhance the safety of the battery. Furthermore, generally, alkaline ion-conducting solid electrolytes composed of oxides are hard materials with high Young's modulus, and since it is difficult to soften and flow them through heat treatment, densification by cold pressing or sintering is difficult; however, according to the manufacturing method of the present embodiment, it is possible to obtain a dense sintered body.

[0074] Examples of alkali ion-conducting solid electrolytes include beta-alumina type crystals or NASICON type crystals with excellent sodium ion conductivity. Beta-alumina exists in two crystalline forms: β-alumina (theoretical formula: Na2O·11Al2O3) and β"-alumina (theoretical formula: Na2O·5.3Al2O3). Since β"-alumina is a metastable material, it is typically used with Li2O or MgO added as a stabilizer. Because β"-alumina has higher sodium ion conductivity than β-alumina, it is preferable to use β"-alumina alone or a mixture of β"-alumina and β-alumina, and Li2O-stabilized β"-alumina (Na2O·5.3Al2O3) 1.7 Li 0.3 Al 10.7 O 17 ) or MgO-stabilized β"-alumina((Al 10.32 Mg 0.68 O 16 )(Na 1.68 It is more desirable to use O)).

[0075] As a NASICON-type crystal, the general formula Na 1+x X2P 3-x Si x O 12 Compounds represented by (X is at least one transition metal element selected from Group 4 elements, and 0 ≤ x ≤ 3) are listed. In particular, it is preferable to include at least one of the following first and second compounds. The first compound is of the general formula Na 1+x Zr2P 3-x Si x O 12 It is a compound represented by (0≤x≤3). The second compound is a compound in which a portion of the Zr of the first compound is substituted with at least one element selected from the group consisting of Ca, Mg, Ba, Sr, Al, Nb, Ta, In, Ga, and Group 3 elements. Additionally, as a Group 3 element, at least one element selected from the group consisting of Sc, Y, and La is listed.

[0076] Examples of the first and second compounds include Na3Zr2Si2PO 12 , Na3Zr 1.6 Ti 0.4 Si2PO 12 , Na3Zr 1.88 Y 0.12 Si2PO 12 These can be listed. Another example of a NASICON-type crystal is Na 3.2 Zr 1.3 Si 2.2 P 0.7 O 10.5 , Na3Hf2Si2PO 12 , Na 3.4 Zr 0.9 Hf 1.4 Al 0.6 Si 1.2 P 1.8 O 12 , Na3Zr 1.7 Nb 0.24 Si2PO 12 , Na 3.6 Ti 0.2 Y 0.7 Si 2.8 O9, Na 3.12 Zr 1.88 Y 0.12 Si2PO 12 , Na 3.6 Zr 0.13 Yb 1.67 Si 0.11 P 2.9 O 12 , Na 3.12 Zr 1.88 Y 0.12 Si2PO 12 You can lift the back.

[0077] As an alkaline ion-conducting solid electrolyte, in addition to the above, general formula Na5XSi4O 12A crystal phase represented by is listed. X is at least one selected from Group 3 transition metal elements, specifically rare earth elements. As rare earth elements, in addition to Dy, Gd, Y, and Sm, Sc, La, Ce, Pr, Nd, Pm, Eu, Tb, Ho, Er, Tm, Yb, and Lu are listed. Preferably, Pr, Nd, Sm, Gd, Dy, or Y are used, and more preferably, Y, Sm, Dy, or Gd are used. In addition, some of Si may be substituted with P.

[0078] As an alkaline ion-conducting solid electrolyte, the general formula is Li7La3Zr2O 12 , Li7La3Zr 2-x M x O 12 (M is at least one selected from Nb, Ga, and Ta, 0 <x<2) 또는 Li 7-3x Al x La3Zr2O 12 (0 <x<2.3)로 나타내어지는 결정상이어도 된다.

[0079] Alkali ion-conducting solid electrolyte precursor and its solution;

[0080] When the alkali ion-conducting solid electrolyte is beta-alumina, the alkali ion-conducting solid electrolyte precursor can be obtained by mixing, for example, aluminum nitrate, sodium nitrate, and lithium nitrate. At this time, the ratio of each of the above materials is adjusted to the composition ratio of the desired alkali ion-conducting solid electrolyte.

[0081] Alkali ion-conducting solid electrolytes are NASICON-type crystals or Na5XSi4O 12In the case of a type determination, the alkali ion-conducting solid electrolyte precursor solution is listed as a solution containing carbonate ions, alkali metal elements and transition metal elements constituting the alkali ion-conducting solid electrolyte. Furthermore, in the said solution, the alkali metal elements are included in the state of alkali ions, and the transition metal elements are included in the state of transition metal ions. The alkali ion-conducting solid electrolyte precursor consists, for example, of a gel or dried product of the alkali ion-conducting solid electrolyte precursor solution. And, the alkali ion-conducting solid electrolyte consists of a calcined product of the alkali ion-conducting solid electrolyte precursor.

[0082] The alkali metal element in the alkali ion-conducting solid electrolyte precursor or the solution thereof is, for example, at least one selected from the group consisting of Li, Na, and K. The transition metal element is, for example, at least one selected from the group consisting of Group 3 and Group 4 elements. The transition metal element is preferably Ti, Zr, Hf, Sc, Y, La, Sm, Dy, or Gd, more preferably Zr, Hf, Sc, Y, La, Sm, Dy, or Gd, even more preferably Zr, Hf, Sc, Y, La, or Sm, and particularly preferably Zr, Hf, Y, La, or Sm. In addition to these transition metal elements, at least one selected from the group consisting of Ca, Mg, Ba, Sr, Al, Nb, Ta, In, and Ga may be included. In the alkali ion-conducting solid electrolyte precursor solution, the carbonate ion may be included as a carbonate (transition metal carbonate) or as a mixture of carbonate ions and carbonates. In the above case, the alkali ion-conducting solid electrolyte precursor solution is suitable, for example, as a precursor solution of a sodium ion-conducting solid electrolyte.

[0083] In addition, it is possible to use a solution containing nitrate ions instead of carbonate ions in the alkaline ion-conducting solid electrolyte precursor solution. In particular, for the following reasons, it is preferable that the alkaline ion-conducting solid electrolyte precursor solution be a solution containing carbonate ions.

[0084] When a solution containing nitrate ions is used as a precursor solution for an alkaline ion-conducting solid electrolyte, components in the solution precipitate unevenly during mixing or drying, and heterogeneous phases tend to form after calcination, which cause a decrease in ion conductivity. Furthermore, significant weight loss occurs due to the decomposition of nitrate ions during the calcination process, making it difficult to form a uniform thin film layer. In addition, NO generated during the calcination process x There is a possibility that manufacturing costs for equipment used to treat corrosive gases, such as those mentioned above, may increase. Additionally, since solutions containing nitrate ions are strongly acidic, a high level of chemical durability is required for manufacturing equipment; consequently, manufacturing costs may also increase in this regard.

[0085] Meanwhile, when a solution containing carbonate ions is used as an alkali ion-conducting solid electrolyte precursor solution, transition metal elements in transition metal oxides, such as ZrO2 or Y2O3, which normally dissolve only in acidic regions, dissolve by receiving coordination from carbonate ions and forming complexes, thereby allowing for the preparation of a neutral to weakly basic (pH 7 or higher, 7.5 or higher, 8 or higher, 8.5 or higher, particularly 9 or higher) metal salt solution. In this case, in addition to the alkali metal component constituting the alkali ion-conducting solid electrolyte becoming soluble in the solution as a carbonate or hydroxide, the Si component constituting the same alkali ion-conducting solid electrolyte can also be added as water glass (sodium silicate: Na2O·nSiO2). Therefore, an alkali ion-conducting solid electrolyte precursor solution can be easily prepared.

[0086] In addition, in the alkaline ion-conducting solid electrolyte precursor solution, it is desirable that carbonate ions are bidentately coordinated to transition metal elements. In this case, the transition metal elements are more likely to exist stably in the solution.

[0087] In addition, as the counterion of the carbonate ion, NR4 + It is preferable to include (in the formula, each R is independently selected from at least one substituent from the group consisting of H, CH3, C2H5 and CH2CH2OH). By doing so, the transition metal element is more likely to exist stably in the solution.

[0088] An alkaline ion-conducting solid electrolyte precursor solution can be obtained, for example, by mixing water glass (sodium silicate), tripolyphosphate, and an aqueous solution of zirconium ammonia carbonate.

[0089] Challenge preparation (6);

[0090] For example, conductive carbon can be used as the conductive agent (6). Examples of conductive carbon include acetylene black, carbon black, Ketjen black, carbon nanotubes, and vapor phase carbon fiber conductive agent (VGCF). It is preferable that the conductive agent (6) be a carbon-based conductive agent made of the materials described above.

[0091] bookbinder;

[0092] A binder is a material used to integrate raw materials (raw material powders) together. Examples of binders include cellulose derivatives such as carboxymethylcellulose, hydroxypropylmethylcellulose, hydroxypropylcellulose, ethylcellulose, hydroxyethylcellulose, and hydroxymethylcellulose, or water-soluble polymers such as polyvinyl alcohol; thermosetting resins such as thermosetting polyimide, phenolic resin, epoxy resin, urea resin, melamine resin, unsaturated polyester resin, and polyurethane; polycarbonate-based resins such as polypropylene carbonate; polyvinylidene fluoride, polyacrylic acid, sodium polyacrylate, polyacrylonitrile, polyethylene oxide, and butyral resin.

[0093] Solid electrolyte layer (2);

[0094] A solid electrolyte such as an alkaline ion-conducting solid electrolyte can be used in the sintered electrode (3).

[0095] The whole house (4);

[0096] The material of the current collector (4) is not particularly limited, but metal materials such as aluminum, nickel, titanium, silver, copper, stainless steel, tungsten, or alloys thereof may be used. The metal materials may be used alone or in combination. Also, the alloys thereof are alloys containing at least one of the metals.

[0097] In the following, the details of the effects of the present invention are shown by comparing examples and comparative examples.

[0098] [Example 1]

[0099] Preparation of Alkaline Ion Conductive Solid Electrolyte Precursors

[0100] The composition ratio is Na3Zr2Si2PO 12 To obtain NASICON-type crystals, water glass (sodium silicate: Na2O·nSiO2), aqueous solution of ammonium zirconium carbonate ((NH4)2Zr(OH)2(CO3)2), sodium tripolyphosphate (Na5P3O2) 10A total of 25g of ) was weighed. These were added to 150g of pure water and stirred with a hot stirrer at 50°C for 24 hours. By doing so, an alkaline ion-conducting solid electrolyte precursor solution (pH=9.7) was obtained. Next, this solution was gelled by leaving it overnight in a constant temperature bath at approximately 5°C. By the above, an alkaline ion-conducting solid electrolyte precursor was prepared.

[0101] <Preparation of a Mixture of Alkali Ion Conductive Solid Electrolyte Precursor and Carbon Electrode Material Precursor>

[0102] A mixture was obtained by mixing sucrose (sucrose), a hard carbon source that is a carbon electrode material precursor, and an alkaline ion-conducting solid electrolyte precursor in a stirrer for 1 hour at a weight ratio of 4:1. Next, the mixture was dried in a constant temperature bath at 60°C for 12 hours, and then vacuum dried at 100°C for 6 hours, and then ground into a powder using a mortar and pestle.

[0103] Preparation of Electrode Paste

[0104] Powder of a mixture of an alkali ion-conducting solid electrolyte precursor and a carbon electrode material precursor and a conductive aid (acetylene black) were weighed in a weight ratio of 19:1. To these, a PPC (polypropylene carbonate) binder was added in an external ratio of 15 wt%, and an electrode paste was obtained by mixing with a self-rotating mixer in an N-methylpyrrolidone solvent.

[0105] <Fabrication of Battery Components>

[0106] 500㎛ thick Na3Zr2Si2PO 12A solid electrolyte layer composed of was prepared separately. An electrode paste was applied to the first main surface of the solid electrolyte layer to a thickness of 70 μm and dried in a dryer at 50°C to form an electrode-forming material layer. After drying, the material was calcined at 1000°C for 2 hours under a nitrogen atmosphere (N2: 99.9999%) and Na3Zr2Si2PO 12 A sintered electrode was obtained by precipitating a mixed phase of an alkaline ion conductive solid electrolyte having the composition of and a carbon electrode material made of hard carbon. Next, a current collector was formed on the sintered electrode by a sputtering method. The current collector is made of an aluminum thin film. By the above, a battery component was obtained. In addition, the sintered electrode of this embodiment is a negative electrode.

[0107] <Fabrication of Test Cells>

[0108] A test cell was fabricated by attaching metallic sodium as a counter electrode to the second main surface of the solid electrolyte layer inside a glove box.

[0109] [Comparative Example]

[0110] A test cell was fabricated in the same manner as in Example 1, except that the negative electrode was a mixture of hard carbon and a PEO (polyethylene oxide)-based polymer solid electrolyte (a mixture of PEO and NaPF6 in a weight ratio of 9:1).

[0111] Charge / Discharge Test

[0112] Charge and discharge tests of the test battery were performed in a constant temperature bath at 30°C. Specifically, charging (insertion of sodium ions) was performed at a cutoff voltage of 0.001V, and discharging (detachment of sodium ions) was performed at a cutoff voltage of 2.5V, and the charge capacity and discharge capacity were measured. At this time, in Example 1, the actual capacity was set to the weight of the fabricated negative electrode, i.e., the sintered electrode × 300mAh / g, and the current value was set to a rate of 0.1C, and charging and discharging were performed. At 60°C, the charge capacity and discharge capacity were measured in the same manner as above.

[0113] Figure 4 is a diagram showing the results of the charge-discharge test of the comparative example. Figure 5 is a diagram showing the results of the charge-discharge test of Example 1.

[0114] As shown in Figure 4, in the comparative example, at 60°C, both the charge capacity and discharge capacity were approximately 250 mAh / g to 280 mAh / g. However, at 30°C, both the charge capacity and discharge capacity were less than 10 mAh / g and did not operate sufficiently. This difference is due to the large change in ionic conductivity with respect to temperature change in polymer-based electrodes.

[0115] In this regard, as shown in FIG. 5, it is confirmed that in Example 1, the charging capacity and discharging capacity both exceed 350 mAh / g not only at 60°C but also at 30°C. Thus, it is confirmed that a battery using the battery component of the present invention operates sufficiently even at a low temperature of 30°C. Furthermore, since it does not require an organic electrolyte, the risk of ignition is low and safety can be increased.

[0116] Next, regarding the alkali ion-conducting solid electrolyte precursor solution, the details of the effects of the present invention are shown by comparing examples and reference examples.

[0117] [Example 2]

[0118] An alkaline ion-conducting solid electrolyte precursor solution was obtained in the same manner as in Example 1. This solution was gelled by leaving it overnight in a constant temperature bath at approximately 5°C to obtain an alkaline ion-conducting solid electrolyte precursor.

[0119] The obtained alkali ion-conducting solid electrolyte precursor was dried in a constant temperature bath at 60°C for 12 hours, and then vacuum dried at 100°C for 6 hours. When the alkali ion-conducting solid electrolyte precursor after drying was analyzed by XRD, it was confirmed that it was amorphous and that each component was homogeneously dispersed, as shown in the XRD chart of Fig. 7.

[0120] An alkaline ion-conducting solid electrolyte was obtained by calcining the dried alkaline ion-conducting solid electrolyte precursor at 1000°C for 3 hours. The obtained alkaline ion-conducting solid electrolyte was analyzed by XRD, and as shown in Fig. 7, the desired NASICON-type crystal (Na3Zr2Si2PO4) was formed. 12 It was confirmed that ) is precipitating (the plot “●” in the chart “After Calcination of Example 2” in Fig. 7 represents Na3Zr2Si2PO 12 It indicates the peak position of the crystal). In addition, the ionic conductivity of the alkaline ion-conducting solid electrolyte was measured to be 1.5×10 -4 It was S.

[0121] In addition, ionic conductivity is 1 to 10 by the AC impedance method after forming a gold electrode as an ion blocking electrode on the surface of an alkaline ion-conducting solid electrolyte. 7 Measurements were performed in the frequency range of Hz, and resistance values ​​were obtained from the Cole-Cole plot. Ionic conductivity was calculated from the obtained resistance values. In addition, measurements by the AC impedance method were performed at 20°C.

[0122] [Reference Example]

[0123] An alkaline ion-conducting solid electrolyte precursor was obtained in the same manner as in Example 2, except that an aqueous solution of zirconium nitrate (ZrO(NO3)2) was used instead of an aqueous solution of zirconium ammonium carbonate.

[0124] The obtained alkali ion-conducting solid electrolyte precursor was dried in the same manner as in Example 2, and the alkali ion-conducting solid electrolyte precursor after drying was analyzed by XRD (X-ray diffraction). As shown in Fig. 7, it was confirmed that sodium nitrate had precipitated and the mixture was heterogeneous (the plot "○" in the chart "After Drying Reference Example" in Fig. 7 indicates the peak position of the sodium nitrate crystal).

[0125] An alkaline ion-conducting solid electrolyte was obtained by calcining the dried alkaline ion-conducting solid electrolyte precursor at 1000°C for 3 hours. The obtained alkaline ion-conducting solid electrolyte was analyzed by XRD, and as shown in Fig. 7, NASICON-type crystals (Na3Zr2Si2PO4) were obtained. 12 Along with the precipitation of ), it was confirmed that some heterogeneous phases were precipitating. The ionic conductivity of the alkaline ion-conducting solid electrolyte was measured in the same manner as in Example 2, and was 6.0 × 10⁻⁶. -7 It was low as S. This is thought to be due to the low ionic conductivity of the precipitated heterogeneous phase.

[0126] The method for manufacturing a battery member (1) according to the first embodiment described above includes a process of heating at approximately 1000°C. Therefore, the sintered electrode (3) is difficult to decompose even if it is subjected to heat treatment again. For example, the sintered electrode (3) can absorb and release alkali ions at 30°C after heat treatment in an inert atmosphere at 500°C. In this way, heat resistance can be effectively increased. On the other hand, a general electrode containing a binder as a solid electrolyte cannot absorb and release alkali ions at 30°C because, when heat treatment is performed in an inert atmosphere at 500°C, the binder decomposes and loses its function as a solid electrolyte. Furthermore, it has been confirmed that the sintered electrode (3) of the present invention is difficult to decompose even when a voltage of about 8V to 9V is applied. For example, FIG. 6 is a diagram showing the results of a charge-discharge test when the test cell prepared in Example 1 above was charged and discharged at a cutoff voltage of 9V to 0.001V. As shown in FIG. 6, even when a high voltage of 9V is applied, no plateau caused by decomposition appears, and reversible charging and discharging was possible with a charge-discharge efficiency of 90% or more. In this way, the withstand voltage can be increased. Furthermore, the carbon electrode material precursor used in the production of the sintered electrode (3) can be a sugar such as sucrose or biomass, and can be easily obtained. Therefore, productivity can be effectively increased.

[0127] Here, in the example shown above, water is used as the solvent when mixing the alkali ion-conducting solid electrolyte precursor and the carbon electrode material precursor. In particular, since sugars such as sucrose have high solubility in water, the uniformity of the mixture can be effectively increased when mixing the alkali ion-conducting solid electrolyte precursor and the carbon electrode material precursor. In the battery member of this embodiment, since the precursors of both are homogeneously mixed before obtaining the alkali ion-conducting solid electrolyte and the carbon electrode material, the contact area can be effectively increased, and high power and high-speed charging and discharging become possible.

[0128] In the following, another example of a method for manufacturing a battery component is presented.

[0129] [Manufacturing Method]

[0130] Hereinafter, a method for manufacturing a battery member or a method for manufacturing a sintered electrode according to the 2nd to 9th embodiments of the present invention will be described.

[0131] (Second embodiment)

[0132] FIGS. 8(a) and FIGS. 8(b) are schematic cross-sectional views illustrating a method for manufacturing a battery component according to a second embodiment. First, the electrode paste (13B) and the solid electrolyte layer (2) shown in FIG. 8(a) are prepared. The paste (13B) is a material layer for forming the electrode in the present invention.

[0133] In obtaining the paste (13B), a powder of a mixture of an alkali ion-conducting solid electrolyte precursor and a carbon electrode material precursor is obtained by the same manufacturing method as according to the first embodiment. Next, the powder of the mixture is calcined under an N2 atmosphere at a temperature of 200°C or higher and 800°C or lower. Additionally, considering the calcination temperature of the second calcination process described later, the upper limit may be 500°C or lower. By this, a carbon electrode material is obtained from the carbon electrode material precursor. This process is the first calcination process. Through the first calcination process, a powder of a mixture of an alkali ion-conducting solid electrolyte precursor and a carbon electrode material is obtained. If the calcination temperature is excessively low, it becomes difficult for the carbon electrode material precursor to change into a carbon electrode material. On the other hand, if the calcination temperature is excessively high, the alkali ion-conducting solid electrolyte precursor tends to change into an alkali ion-conducting solid electrolyte.

[0134] Next, the powder of the above mixture is ground and mixed with a conductive agent (6) and a binder in an organic solvent to obtain a paste (13B). Next, as shown in FIG. 8(a), the paste (13B) is applied to the first main surface (2a) of the solid electrolyte layer (2). Thus, a lamination process is performed to laminate the solid electrolyte layer (2) and the paste (13B) as a material layer for forming electrodes. Next, the laminate of the solid electrolyte layer (2) and the paste (13B) is calcined under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1300°C (preferably greater than 800°C and less than or equal to 1150°C). By doing so, an alkaline ion conductive solid electrolyte is obtained from an alkaline ion conductive solid electrolyte precursor, thereby obtaining a mixed phase (5) of an alkaline ion conductive solid electrolyte and a carbon electrode material. This process is a second calcination process. In the second firing process, firing is performed at a higher temperature than in the first firing process. Through the second firing process, a sintered electrode (3) is obtained as shown in FIG. 8(b). In this way, a laminate of the sintered electrode (3) and the solid electrolyte layer (2) is obtained. If the firing temperature is excessively low, the reaction becomes insufficient, making it difficult to obtain the desired sintered electrode (3). As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. On the other hand, if the firing temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a risk that it will be difficult to obtain an alkali ion-conducting solid electrolyte having the desired composition. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. Next, a current collector (4) is formed on the sintered electrode (3). By the above, a battery member (1) can be obtained.

[0135] In the first embodiment shown in FIGS. 3(a) and 3(b), during the sintering process, both the reaction of becoming an alkaline ion-conducting solid electrolyte precursor and the reaction of becoming a carbon electrode material precursor occur. Consequently, there are many decomposition components during the sintering process, and the difference between the thickness of the paste (13A) and the thickness of the sintered electrode (3) is large. Specifically, the thickness of the sintered electrode (3) tends to become thinner than the thickness of the paste (13A).

[0136] In this embodiment, a first firing process is performed before the process of forming a material layer for forming an electrode, that is, before the process of forming the paste (13B). By doing so, a reaction to obtain a carbon electrode material from a carbon electrode material precursor is performed before the formation of the paste (13B). Therefore, the decomposition component in the second firing process after forming the paste (13B) is small. Consequently, the difference between the thickness of the paste (13B) and the thickness of the sintered electrode (3) is small. Thus, it is easy to adjust the thickness of the sintered electrode (3). Furthermore, even if the thickness of the paste (13B) is increased, it is difficult for problems such as cracks to occur in the sintered electrode (3) obtained after firing. As a result, since the thickness of the sintered electrode (3) can be easily increased, the capacity can be easily increased. In particular, in the first embodiment, the firing process for obtaining the sintered electrode (3) is performed only once, so the process can be simplified.

[0137] (Third embodiment)

[0138] FIGS. 9(a) and FIGS. 9(b) are schematic cross-sectional views illustrating a method for manufacturing a battery component according to a third embodiment. First, the electrode paste (13C) and the solid electrolyte layer (2) shown in FIG. 9(a) are prepared. The paste (13C) is a material layer for forming the electrode in the present invention.

[0139] In obtaining the paste (13C), a powder of a mixture of an alkali ion-conducting solid electrolyte precursor and a carbon electrode material precursor is obtained by the same manufacturing method as according to the first embodiment. Next, the powder of the mixture is calcined under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1150°C (preferably greater than 800°C and less than or equal to 1100°C). By doing so, the alkali ion-conducting solid electrolyte and the carbon electrode material are obtained simultaneously. This process is the third calcination process. By the third calcination process, a powder of a mixture of an alkali ion-conducting solid electrolyte and a carbon electrode material is obtained. If the calcination temperature is excessively low, it becomes difficult to obtain the powder of a mixture of an alkali ion-conducting solid electrolyte and a carbon electrode material. On the other hand, if the calcination temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a risk that it will become difficult to obtain an alkali ion-conducting solid electrolyte having a desired composition.

[0140] Next, the powder of the above mixture is ground and mixed with a conductive agent (6) and a binder in an organic solvent to obtain a paste (13C). Next, as shown in FIG. 9(a), the paste (13C) is applied to the first main surface (2a) of the solid electrolyte layer (2). In this way, a lamination process is performed to laminate the solid electrolyte layer (2) and the paste (13C) as a material layer for forming an electrode. Next, the laminate of the solid electrolyte layer (2) and the paste (13C) is sintered under an N2 atmosphere at a temperature of 600°C or higher and 1300°C or lower (preferably 900°C or higher and 1250°C or lower). This process is the fourth sintering process. In the fourth sintering process, sintering is performed at a higher temperature than in the third sintering process. By the fourth sintering process, a sintered electrode (3) is obtained as shown in FIG. 9(b). If the firing temperature is excessively low, there is a risk that the sinterability of the sintered electrode (3) or the bonding between the sintered electrode (3) and the solid electrolyte layer (2) will be insufficient. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. On the other hand, if the firing temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a risk that it will be difficult to obtain an alkali ion-conducting solid electrolyte having a desired composition. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. Next, a current collector (4) is formed on the sintered electrode (3). By the above, a battery member (1) can be obtained.

[0141] In this embodiment, a third sintering process is performed before the process of forming the paste (13C). By doing so, before the formation of the paste (13C), both the reaction of becoming an alkaline ion-conducting solid electrolyte precursor and the reaction of becoming a carbon electrode material precursor are carried out. Therefore, the decomposition component in the fourth sintering process after forming the paste (13C) is even smaller. Consequently, the difference between the thickness of the paste (13C) and the thickness of the sintered electrode (3) is even smaller. Therefore, it is easier to adjust the thickness of the sintered electrode (3). Furthermore, since the thickness of the sintered electrode (3) can be made even thicker, the capacity can be made even more easily. In particular, in the second embodiment, the battery member (1) can be manufactured at a lower temperature than in the third embodiment.

[0142] (Fourth embodiment)

[0143] FIGS. 10(a) and FIGS. 10(b) are schematic cross-sectional views for explaining a method for manufacturing a battery component according to a fourth embodiment. First, a paste (22) containing a solid electrolyte precursor and a compacted body (23A) shown in FIG. 10(a) is prepared. The compacted body (23A) is a material layer for forming an electrode in the present invention. The paste (22) is a material layer for forming a solid electrolyte in the present invention. In this specification, a material layer for forming a solid electrolyte refers to a material layer for obtaining (forming) a solid electrolyte layer by firing. The material layer for forming a solid electrolyte may be composed of, for example, a paste such as in the present embodiment, or may be composed of a compacted body.

[0144] In obtaining the compacted body (23A), a powder of a mixture of an alkaline ion-conducting solid electrolyte precursor and a carbon electrode material precursor is obtained by the same manufacturing method as according to the first embodiment. Next, the powder of the mixture and the conductive agent (6) are mixed, and then press-molded to obtain the compacted body (23A) of the alkaline ion-conducting solid electrolyte precursor, the carbon electrode material precursor, and the conductive agent (6). For press-molding, for example, a uniaxial press may be used. Also, it is not necessary to add the conductive agent (6).

[0145] Meanwhile, the paste (22) can be obtained by adding the mixed raw material powder to an organic solvent. Next, as shown in FIG. 10(a), the paste (22) is applied onto a suitable substrate (27). A plate made of a suitable metal or ceramic, etc., can be used as the substrate (27). Next, a compacted body (23A) is laminated onto the paste (22). Next, the laminate of the paste (22) and the compacted body (23A) is fired under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1300°C (preferably greater than 800°C and less than or equal to 1150°C). By doing this, as shown in FIG. 10(b), a solid electrolyte layer (2) and a sintered electrode (3) are obtained simultaneously. In this way, a laminate of the solid electrolyte layer (2) and the sintered electrode (3) is obtained. If the firing temperature is too low, the reaction becomes insufficient, making it difficult to obtain the desired sintered electrode (3). In addition, it becomes difficult to obtain the desired solid electrolyte layer (2). Furthermore, there is a concern that the bonding between the sintered electrode (3) and the solid electrolyte layer (2) may become insufficient. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. On the other hand, if the firing temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a concern that it may become difficult to obtain an alkali ion-conducting solid electrolyte having the desired composition. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. Next, as shown in FIG. 10(b), the laminate of the solid electrolyte layer (2) and the sintered electrode (3) is peeled off from the substrate (27), and a current collector (4) is formed on the sintered electrode (3). Additionally, after forming the current collector (4) on the sintered electrode (3), the laminate of the solid electrolyte layer (2) and the sintered electrode (3) may be peeled off from the substrate (27). By the above, a battery component (1) can be obtained.

[0146] In this embodiment, since the solid electrolyte layer (2) and the sintered electrode (3) are obtained simultaneously, productivity can be increased. Furthermore, since a paste (22) is used in the production of the solid electrolyte layer (2), the solid electrolyte layer (2) can be easily made thin. Additionally, a modified example of this embodiment is shown below.

[0147] (Variation Example 1 of the 4th embodiment)

[0148] FIGS. 11(a) to 11(c) are schematic cross-sectional views for explaining a method for manufacturing a battery component according to Variant Example 1 of the fourth embodiment. In this variant example, as shown in FIG. 11(a), a paste (22) is applied onto a compact (23A). Next, as in the fourth embodiment, a laminate of the paste (22) and the compact (23A) is sintered under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1300°C (preferably greater than 800°C and less than or equal to 1150°C). By doing so, as shown in FIG. 11(b), a solid electrolyte layer (2) and a sintered electrode (3) are obtained simultaneously. If the sintering temperature is excessively low, the reaction becomes insufficient, making it difficult to obtain the desired sintered electrode (3). Additionally, it becomes difficult to obtain the desired solid electrolyte layer (2). In addition, there is a concern that the bonding between the sintered electrode (3) and the solid electrolyte layer (2) may become insufficient. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. Meanwhile, if the firing temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a concern that it may be difficult to obtain an alkali ion-conducting solid electrolyte having a desired composition. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. Next, as shown in FIG. 11(c), a current collector (4) is formed on the sintered electrode (3). By the above, a battery member (21) can be obtained.

[0149] In the battery member (1) manufactured in the fourth embodiment, as shown in FIG. 1, when viewed in a planar view, the outer periphery of the solid electrolyte layer (2) is located outside the outer periphery of the sintered electrode (3). Also, in this specification, "when viewed in a planar view" refers to the direction viewed from above in FIG. 1. Meanwhile, as shown in FIG. 11(a), in this modified example, a paste (22) is applied on a compact (23A). Therefore, in the battery member (21) shown in FIG. 11(c), when viewed in a planar view, the positions of the outer periphery of the solid electrolyte layer (2) and the outer periphery of the sintered electrode (3) are the same.

[0150] (Variation of the 4th embodiment 2)

[0151] FIGS. 12(a) to 12(c) are schematic cross-sectional views for explaining a method for manufacturing a battery component according to Variant Example 2 of the fourth embodiment. In this variant example, instead of the paste (22) shown in FIG. 10(a), a compacted body (22A) shown in FIG. 12(a) is prepared. The compacted body (22A) is a material layer for forming a solid electrolyte in the present invention. The compacted body (22A) can be obtained by press-molding mixed raw material powders. Next, a compacted body (23A) as a material layer for forming an electrode is laminated on the compacted body (22A) as a material layer for forming a solid electrolyte. Next, in the same manner as in the fourth embodiment, the laminate of the compacted body (22A) and the compacted body (23A) is sintered under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1300°C (preferably greater than 800°C and less than or equal to 1150°C). By this, as shown in FIG. 12(b), a solid electrolyte layer (2) and a sintered electrode (3) are obtained simultaneously. If the firing temperature is excessively low, the reaction becomes insufficient, making it difficult to obtain the desired sintered electrode (3). Also, it becomes difficult to obtain the desired solid electrolyte layer (2). Furthermore, there is a risk that the bonding between the sintered electrode (3) and the solid electrolyte layer (2) will be insufficient. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. On the other hand, if the firing temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, making it difficult to obtain an alkali ion-conducting solid electrolyte with a desired composition. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. Next, as shown in FIG. 12(c), a current collector (4) is formed on the sintered electrode (3). By the above, a battery member (21) can be obtained.

[0152] (Fifth embodiment)

[0153] FIGS. 13(a) and FIGS. 13(b) are schematic cross-sectional views illustrating a method for manufacturing a battery component according to a fifth embodiment. First, a compacted body (23B) and a paste (22) shown in FIG. 13(a) are prepared. The compacted body (23B) is a material layer for forming an electrode in the present invention.

[0154] In obtaining the compacted body (23B), a powder of a mixture of an alkaline ion-conducting solid electrolyte precursor and a carbon electrode material precursor is obtained by following the same manufacturing method as the first embodiment. Next, the powder of the mixture is calcined under an N2 atmosphere at a temperature of 200°C or higher and 800°C or lower. Additionally, considering the calcination temperature of the second calcination process described later, the upper limit may be 500°C or lower. This process is the same as the first calcination process as the second embodiment. Specifically, in this process, a powder of a mixture of an alkaline ion-conducting solid electrolyte precursor and a carbon electrode material is obtained. If the calcination temperature is excessively low, it becomes difficult for the carbon electrode material precursor to change into a carbon electrode material. On the other hand, if the calcination temperature is excessively high, the alkaline ion-conducting solid electrolyte precursor tends to change into an alkaline ion-conducting solid electrolyte. Next, the powder of the mixture and the conductive agent (6) are mixed, and then the compacted body (23B) is obtained by press molding.

[0155] Meanwhile, as shown in FIG. 13(a), a paste (22) is applied as a material layer for forming a solid electrolyte on a suitable substrate (27). Next, a compacted body (23B) is laminated onto the paste (22). Next, the laminate of the paste (22) and the compacted body (23B) is sintered under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1300°C (preferably greater than 800°C and less than or equal to 1150°C). This process is the same as the second sintering process as in the second embodiment. By doing so, as shown in FIG. 13(b), a solid electrolyte layer (2) and a sintered electrode (3) are obtained simultaneously. In this way, a laminate of the solid electrolyte layer (2) and the sintered electrode (3) is obtained. If the sintering temperature is too low, the reaction becomes insufficient, making it difficult to obtain the desired sintered electrode (3). Also, it becomes difficult to obtain the desired solid electrolyte layer (2). In addition, there is a concern that the bonding between the sintered electrode (3) and the solid electrolyte layer (2) may become insufficient. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. Meanwhile, if the firing temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a concern that it may be difficult to obtain an alkali ion-conducting solid electrolyte having a desired composition. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. Next, after peeling off the laminate of the solid electrolyte layer (2) and the sintered electrode (3) from the substrate (27), a current collector (4) is formed on the sintered electrode (3). By the above, a battery member (1) can be obtained. In this embodiment, since the solid electrolyte layer (2) is obtained simultaneously with the sintered electrode (3), productivity can be increased. Furthermore, it is easy to adjust the thickness of the sintered electrode (3) in the same way as in the second embodiment. In addition, since the thickness of the sintered electrode (3) can be easily increased, the capacity can be easily increased.

[0156] (6th embodiment)

[0157] FIGS. 14(a) and FIGS. 14(b) are schematic cross-sectional views illustrating a method for manufacturing a battery component according to a sixth embodiment. First, a compacted body (23C) and a paste (22) of a solid electrolyte shown in FIG. 14(a) are prepared. The compacted body (23C) is a material layer for forming an electrode in the present invention.

[0158] In obtaining a compact (23C), a powder of a mixture of an alkali ion-conducting solid electrolyte precursor and a carbon electrode material precursor is obtained by the same manufacturing method as according to the first embodiment. Next, the powder of the mixture is calcined under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1150°C (preferably greater than 800°C and less than or equal to 1100°C). By doing so, an alkali ion-conducting solid electrolyte and a carbon electrode material are obtained simultaneously. This process is a third calcination process, similar to the third embodiment. By the third calcination process, a powder of a mixture of an alkali ion-conducting solid electrolyte and a carbon electrode material is obtained. If the calcination temperature is excessively low, it becomes difficult to obtain a powder of a mixture of an alkali ion-conducting solid electrolyte and a carbon electrode material. On the other hand, if the calcination temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a risk that it will become difficult to obtain an alkali ion-conducting solid electrolyte having a desired composition. Next, after mixing the powder of the above mixture and the conductive agent (6), a compacted body (23C) is obtained by press molding.

[0159] Meanwhile, as shown in FIG. 14(a), a paste (22) is applied as a material layer for forming a solid electrolyte on a suitable substrate (27). Next, a compacted body (23C) is laminated on the paste (22). Next, the laminate of the paste (22) and the compacted body (23C) is sintered under an N2 atmosphere at a temperature of 600°C or higher and 1300°C or lower (preferably above 800°C and below 1250°C). This process is a fourth sintering process, similar to the third embodiment. Through the fourth sintering process, a solid electrolyte layer (2) and a sintered electrode (3) are obtained simultaneously, as shown in FIG. 14(b). In this way, a laminate of the solid electrolyte layer (2) and the sintered electrode (3) is obtained. If the firing temperature is excessively low, there is a risk that the sinterability of the sintered electrode (3) or the bonding between the sintered electrode (3) and the solid electrolyte layer (2) will be insufficient. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. On the other hand, if the firing temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a risk that it will be difficult to obtain an alkali ion-conducting solid electrolyte having a desired composition. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. Next, the laminate of the solid electrolyte layer (2) and the sintered electrode (3) is peeled off from the substrate (27), and then a current collector (4) is formed on the sintered electrode (3). By the above, a battery member (1) can be obtained.

[0160] In this embodiment, since the solid electrolyte layer (2) and the sintered electrode (3) are obtained simultaneously, productivity can be increased. Furthermore, as in the third embodiment, the thickness of the sintered electrode (3) is more easily adjusted. Also, since the thickness of the sintered electrode (3) can be made thicker more easily, the capacity can be made much more easily.

[0161] However, the sintered electrode (3) according to one embodiment of the present invention may be used alone. An example of a method for manufacturing the sintered electrode (3) is shown below.

[0162] (Seventh embodiment)

[0163] FIGS. 15(a) and FIGS. 15(b) are schematic cross-sectional views for explaining a method for manufacturing a sintered electrode according to the seventh embodiment. First, as shown in FIG. 15(a), a compacted body (23A) is prepared in the same manner as in the fourth embodiment. The compacted body (23A) is a material layer for forming an electrode, comprising an alkaline ion-conducting solid electrolyte precursor, a carbon electrode material precursor, and a conductive agent (6). In particular, the material layer for forming an electrode does not necessarily have to include a conductive agent (6). Next, the compacted body (23A) is sintered under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1300°C (preferably greater than 800°C and less than or equal to 1150°C). By doing so, the alkaline ion-conducting solid electrolyte and the carbon electrode material are obtained simultaneously, thereby obtaining a mixed phase (5) of the alkaline ion-conducting solid electrolyte and the carbon electrode material. In this way, as shown in FIG. 15(b), a sintered electrode (3) can be obtained. If the firing temperature is too low, the reaction becomes insufficient, making it difficult to obtain the desired sintered electrode (3). As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. On the other hand, if the firing temperature is too high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a risk that it will be difficult to obtain an alkali ion-conducting solid electrolyte having the desired composition. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease.

[0164] (Eighth embodiment)

[0165] FIGS. 16(a) and FIG. 16(b) are schematic cross-sectional views illustrating a method for manufacturing a sintered electrode according to the eighth embodiment. First, as shown in FIG. 16(a), a compacted body (23B) is prepared in the same manner as in the fifth embodiment. Specifically, a powder of a mixture of an alkali ion-conducting solid electrolyte precursor and a carbon electrode material precursor is calcined under an N2 atmosphere at a temperature of 200°C or higher and 800°C or lower. Additionally, considering the calcination temperature of the second calcination process described later, the upper limit may be set to 500°C or lower. By doing so, a carbon electrode material is obtained from the carbon electrode material precursor. This process is the same as the first calcination process in the fifth embodiment. Through the first calcination process, a powder of a mixture of an alkali ion-conducting solid electrolyte precursor and a carbon electrode material is obtained. If the calcination temperature is excessively low, it becomes difficult for the carbon electrode material precursor to transform into a carbon electrode material. Meanwhile, if the firing temperature is excessively high, the alkaline ion conductive solid electrolyte precursor tends to change into an alkaline ion conductive solid electrolyte. Next, after mixing the powder of the above mixture and the conductive aid (6), a compacted body (23B) is obtained by press molding.

[0166] Next, the compacted body (23B) is sintered under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1300°C (preferably greater than 800°C and less than or equal to 1150°C). By doing so, an alkaline ion-conducting solid electrolyte is obtained from an alkaline ion-conducting solid electrolyte precursor, thereby obtaining a mixed phase (5) of an alkaline ion-conducting solid electrolyte and a carbon electrode material. This process is a second sintering process, similar to the fifth embodiment. In the second sintering process, sintering is performed at a higher temperature than in the first sintering process. By doing so, a sintered electrode (3) is obtained as shown in FIG. 16(b). If the sintering temperature is excessively low, the reaction becomes insufficient, making it difficult to obtain the desired sintered electrode (3). As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. Meanwhile, if the sintering temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a concern that it will be difficult to obtain an alkali ion-conducting solid electrolyte having the desired composition. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease.

[0167] (Ninth embodiment)

[0168] FIGS. 17(a) and FIGS. 17(b) are schematic cross-sectional views illustrating a method for manufacturing a sintered electrode according to the ninth embodiment. First, as shown in FIG. 17(a), a compacted body (23C) is prepared in the same manner as in the sixth embodiment. Specifically, a powder of a mixture of an alkali ion-conducting solid electrolyte precursor and a carbon electrode material precursor is calcined under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1150°C (preferably greater than 800°C and less than or equal to 1100°C). By doing so, the alkali ion-conducting solid electrolyte and the carbon electrode material are obtained simultaneously. This process is the same third calcination process as in the sixth embodiment. Through the third calcination process, a powder of a mixture of the alkali ion-conducting solid electrolyte and the carbon electrode material is obtained. If the calcination temperature is excessively low, it becomes difficult to obtain a powder of a mixture of the alkali ion-conducting solid electrolyte and the carbon electrode material. Meanwhile, if the firing temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a concern that it will be difficult to obtain an alkali ion-conducting solid electrolyte having the desired composition. Next, after mixing the powder of the above mixture and the conductive agent (6), a compacted body (23C) is obtained by press molding.

[0169] Next, the compacted body (23C) is sintered under an N2 atmosphere at a temperature of 600°C or higher and 1300°C or lower (preferably 900°C or higher and 1250°C or lower). This process is the same as the fourth sintering process as in the sixth embodiment. In the fourth sintering process, sintering is performed at a higher temperature than in the third sintering process. By doing so, a sintered electrode (3) is obtained as shown in FIG. 17(b). If the sintering temperature is excessively low, there is a risk that the sinterability of the sintered electrode (3) will be insufficient. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease. On the other hand, if the sintering temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a risk that it will be difficult to obtain an alkali ion-conducting solid electrolyte having a desired composition. As a result, the internal resistance of the sintered electrode (3) increases, and the charge / discharge efficiency tends to decrease.

[0170] [Battery component]

[0171] (Second embodiment)

[0172] FIG. 18 is a schematic cross-sectional view showing a battery member according to a second embodiment. This embodiment differs from the first embodiment in that it does not have a current collector and has a configuration of a sintered electrode (33). Except for the above, the battery member (31) of this embodiment has the same configuration as the battery member (1) of the first embodiment. In addition, the battery member (31) may have a current collector.

[0173] The sintered electrode (33) comprises a particulate carbon electrode material (38) and a coating layer (39). The D50 of the particulate carbon electrode material (38) is 1 μm. The particulate carbon electrode material (38) is made of graphite or hard carbon. Furthermore, regarding the particulate carbon electrode material (38), it is preferable that the D50 is 50 μm or less, and more preferable that it is 10 μm or less. This can increase the density of the sintered electrode (33). The lower limit of the D50 of the particulate carbon electrode material (38) is not specifically limited, but is, for example, 10 nm, 0.1 μm, 0.3 μm, 0.5 μm, or 0.6 μm.

[0174] As shown in FIG. 18, the particulate carbon electrode material (38) is covered by a coating layer (39). The coating layer (39) is made of an alkaline ion-conducting solid electrolyte. In this embodiment, the alkaline ion-conducting solid electrolyte has sodium ion conductivity. In particular, the alkaline ion-conducting solid electrolyte may have lithium ion conductivity. The particulate carbon electrode materials (38) are joined together through the coating layer (39). Additionally, the sintered electrode (33) is joined to the solid electrolyte layer (2) by the coating layer (39).

[0175] It is preferable that the sintered electrode (33) includes a conductive agent (6). By including the conductive agent (6), a conductive path is formed, which can reduce the internal resistance of the sintered electrode (33). In particular, the sintered electrode (33) does not necessarily have to include the conductive agent (6). Additionally, the sintered electrode (33) does not include a binder.

[0176] In the battery member (31) of the present embodiment, safety can be improved and heat resistance and voltage resistance can be increased, just like in the battery member (1) of the first embodiment. In addition, in the battery member (31) of the present embodiment, it is easy to increase the thickness of the sintered electrode (33) (high loading capacity) by appropriately adjusting the amount of particulate carbon electrode material (38). In addition, performance can be easily adjusted by selecting the particulate carbon electrode material (38) used. In addition, the sintered electrode (33) according to one embodiment of the present invention may be used alone.

[0177] In the following, examples of a method for manufacturing a battery member (31) of the present embodiment and a method for manufacturing a sintered electrode (33) are shown.

[0178] [Manufacturing Method]

[0179] Hereinafter, a method for manufacturing a battery member or a method for manufacturing a sintered electrode according to the 10th to 12th embodiments of the present invention will be described.

[0180] (10th embodiment)

[0181] FIGS. 19(a) and FIGS. 19(b) are schematic cross-sectional views for explaining a method for manufacturing a battery component according to the tenth embodiment. First, a paste (43) and a solid electrolyte layer (2) shown in FIG. 19(a) are prepared. The paste (43) is a material layer for forming an electrode in the present invention.

[0182] In obtaining the paste (43), an alkaline ion-conducting solid electrolyte precursor is prepared in the same manner as the manufacturing method according to the first embodiment. Additionally, a particulate carbon electrode material (38) is prepared. Next, the alkaline ion-conducting solid electrolyte precursor and the particulate carbon electrode material (38) are mixed and then dried. By doing so, a powder of the mixture of the alkaline ion-conducting solid electrolyte precursor and the particulate carbon electrode material (38) is obtained. Next, the powder of the mixture is added to an organic solvent and mixed with a conductive agent (6) and a binder. For example, N-methylpyrrolidone can be used as the organic solvent. By doing so, the paste (43) is obtained. In particular, it is not necessary to add the conductive agent (6).

[0183] Next, as shown in FIG. 19(a), a paste (43) is applied to the first main surface (2a) of the solid electrolyte layer (2). In this way, a lamination process is performed to laminate the solid electrolyte layer (2) and the paste (43) as a material layer for forming electrodes. Next, the laminate of the solid electrolyte layer (2) and the paste (43) is sintered under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1300°C (preferably greater than 800°C and less than or equal to 1150°C). By doing so, as shown in FIG. 19(b), an alkaline ion conductive solid electrolyte is obtained from an alkaline ion conductive solid electrolyte precursor, thereby obtaining a coating layer (39) made of the alkaline ion conductive solid electrolyte. At this time, particulate carbon electrode materials (38) are bonded together with the coating layer (39) interposed, and a sintered electrode (33) is obtained. Additionally, a laminate of a sintered electrode (33) and a solid electrolyte layer (2) is obtained. At the same time, the sintered electrode (33) is bonded to the solid electrolyte layer (2) by the coating layer (39). By the above, a battery member (31) is obtained. If the firing temperature is excessively low, the reaction becomes insufficient, making it difficult to obtain the desired sintered electrode (33). As a result, the internal resistance of the sintered electrode (33) increases, and the charge / discharge efficiency tends to decrease. Additionally, there is a risk that the bonding between the sintered electrode (33) and the solid electrolyte layer (2) will be insufficient. On the other hand, if the firing temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a risk that it will be difficult to obtain the coating layer (39) made of an alkali ion-conducting solid electrolyte having the desired composition. As a result, the internal resistance of the sintered electrode (33) increases, and the charge / discharge efficiency tends to decrease.

[0184] (11th embodiment)

[0185] FIGS. 20(a) and FIGS. 20(b) are schematic cross-sectional views illustrating a method for manufacturing a battery component according to the eleventh embodiment. First, a compacted body (53) and a paste (22) shown in FIG. 20(a) are prepared. The compacted body (53) is a material layer for forming an electrode in the present invention. The paste (22) is a material layer for forming a solid electrolyte in the present invention.

[0186] In obtaining the compacted body (53), the powder of the mixture of the alkali ion-conducting solid electrolyte precursor and the particulate carbon electrode material (38) is obtained in the same manner as the manufacturing method according to the 10th embodiment. Next, the powder of the mixture and the conductive aid (6) are mixed, and then the compacted body (53) is obtained by press molding.

[0187] Meanwhile, the paste (22) can be obtained by adding the mixed raw material powder to an organic solvent. Next, as shown in FIG. 20(a), the paste (22) is applied onto a suitable substrate (27). Next, a lamination process is performed in which a compacted body (53) as a material layer for forming an electrode is laminated onto the paste (22) as a material layer for forming a solid electrolyte. Next, the laminate of the paste (22) and the compacted body (53) is sintered under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1300°C (preferably greater than 800°C and less than or equal to 1150°C). By doing so, as shown in FIG. 20(b), a solid electrolyte layer (2) and a sintered electrode (33) are obtained simultaneously. In this way, a laminate of the sintered electrode (33) and the solid electrolyte layer (2) is obtained. If the sintering temperature is excessively low, the reaction becomes insufficient, making it difficult to obtain the desired sintered electrode (33). As a result, the internal resistance of the sintered electrode (33) tends to increase, and the charge / discharge efficiency tends to decrease. Additionally, it becomes difficult to obtain the desired solid electrolyte layer (2). Furthermore, there is a concern that the bonding between the sintered electrode (33) and the solid electrolyte layer (2) may become insufficient. Meanwhile, if the firing temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a concern that it becomes difficult to obtain a coating layer (39) or a solid electrolyte layer (2) made of an alkali ion-conducting solid electrolyte having the desired composition. As a result, the internal resistance of the sintered electrode (33) tends to increase, and the charge / discharge efficiency tends to decrease.

[0188] In addition, the paste (22) may be applied to the compact (53) in the same manner as shown in FIG. 11(a). Alternatively, instead of the paste (22), the compact (22A) in the same manner as shown in FIG. 12(a) may be prepared. In this case, the compact (53) as a material layer for forming electrodes and the compact (22A) as a material layer for forming solid electrolytes may be laminated, and then sintered.

[0189] (12th embodiment)

[0190] FIGS. 21(a) and FIGS. 21(b) are schematic cross-sectional views for explaining a method for manufacturing a sintered electrode according to the 12th embodiment. First, as shown in FIG. 21(a), a compacted body (53) is prepared in the same manner as in the 11th embodiment. The compacted body (53) is a material layer for forming an electrode in the present invention. Next, the compacted body (53) is sintered under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1300°C (preferably greater than 800°C and less than or equal to 1150°C). By doing so, a sintered electrode (33) is obtained as shown in FIG. 21(b). If the sintering temperature is excessively low, the reaction becomes insufficient, making it difficult to obtain the desired sintered electrode (33). As a result, the internal resistance of the sintered electrode (33) increases, and the charge / discharge efficiency tends to decrease. Meanwhile, if the firing temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a concern that it will be difficult to obtain a coating layer (39) made of an alkali ion-conducting solid electrolyte having a desired composition. As a result, the internal resistance of the sintered electrode (33) increases, and the charge / discharge efficiency tends to decrease.

[0191] In addition, a paste (43) as a material layer for forming an electrode, identical to the 10th embodiment shown in FIG. 19(a), may be applied to a suitable substrate and then fired to obtain a sintered electrode (33).

[0192] [Battery component]

[0193] (Third embodiment)

[0194] FIG. 22 is a schematic cross-sectional view showing a battery member according to a third embodiment. This embodiment differs from the second embodiment in the composition of the coating layer (49) in the sintered electrode (73). Except for the above, the battery member (41) of this embodiment has the same composition as the battery member (31) of the second embodiment.

[0195] The coating layer (49) comprises a carbon electrode material and an alkaline ion-conducting solid electrolyte. The carbon electrode material is a material included separately from the particulate carbon electrode material (38) and is made of graphite or hard carbon. In this embodiment, the alkaline ion-conducting solid electrolyte has sodium ion conductivity. In particular, the alkaline ion-conducting solid electrolyte may have lithium ion conductivity. The coating layer (49) comprises a mixture of the carbon electrode material and the alkaline ion-conducting solid electrolyte. The mixture is in the form of particles. The particulate mixtures are bonded together by sintering. The particles of the particulate carbon electrode material (38) are bonded together through the coating layer (49). Additionally, the sintered electrode (73) is bonded to the solid electrolyte layer (2) by the coating layer (49).

[0196] In the battery member (41) of the present embodiment, safety can be improved and heat resistance and voltage resistance can be increased, just like in the battery member (1) of the first embodiment. In addition, in the battery member (41) of the present embodiment, by appropriately adjusting the amount of particulate carbon electrode material (38), it is easy to increase the thickness of the sintered electrode (73) (high loading capacity). Furthermore, as shown in Example 3 described later, the battery member (41) of the present embodiment has the characteristic of having excellent first charge / discharge efficiency (irreversible capacity).

[0197] [Manufacturing Method]

[0198] Hereinafter, a method for manufacturing a battery member according to the 13th embodiment of the present invention will be described.

[0199] (13th embodiment)

[0200] FIGS. 23(a) and FIGS. 23(b) are schematic cross-sectional views illustrating a method for manufacturing a battery component according to the 13th embodiment. First, a paste (83) and a solid electrolyte layer (2) are prepared. The paste (83) is a material for forming electrodes in the present invention.

[0201] In obtaining the paste (83), the alkali ion-conducting solid electrolyte precursor and the carbon electrode material precursor are prepared in the same manner as the manufacturing method according to the first embodiment. Additionally, the particulate carbon electrode material (38) is prepared. Next, the alkali ion-conducting solid electrolyte precursor, the carbon electrode material precursor, and the particulate carbon electrode material (38) are mixed and then dried. By doing so, a powder of the mixture of the alkali ion-conducting solid electrolyte precursor, the carbon electrode material precursor, and the particulate carbon electrode material (38) is obtained. Next, the powder of the mixture is added to an organic solvent and mixed with a conductive agent (6) and a binder. For example, N-methylpyrrolidone can be used as the organic solvent. By doing so, the paste (83) is obtained. In particular, it is not necessary to add the conductive agent (6).

[0202] Next, as shown in FIG. 23(a), a paste (83) is applied to the first main surface (2a) of the solid electrolyte layer (2). In this way, a lamination process is performed to laminate the solid electrolyte layer (2) and the paste (83) as a material layer for forming electrodes. Next, the laminate of the solid electrolyte layer (2) and the paste (83) is sintered under an N2 atmosphere at a temperature greater than 500°C and less than or equal to 1300°C (preferably greater than 800°C and less than or equal to 1150°C). By doing so, the alkali ion-conducting solid electrolyte precursor and the carbon electrode material precursor become a mixed phase of the carbon electrode material and the alkali ion-conducting solid electrolyte, and simultaneously, as shown in FIG. 23(b), a coating layer (49) is formed on the surface of the particulate carbon electrode material (38) because it is composed of the said mixed phase. At this time, the particulate carbon electrode materials (38) are bonded together through the coating layer (49), and a sintered electrode (73) is obtained. Additionally, a laminate of a sintered electrode (73) and a solid electrolyte layer (2) is obtained. At the same time, the sintered electrode (73) is bonded to the solid electrolyte layer (2) by the coating layer (49). By the above, a battery member (41) is obtained. If the firing temperature is excessively low, the reaction becomes insufficient, making it difficult to obtain the desired sintered electrode (73). As a result, the internal resistance of the sintered electrode (73) increases, and the charge / discharge efficiency tends to decrease. Additionally, there is a risk that the bonding between the sintered electrode (73) and the solid electrolyte layer (2) will be insufficient. On the other hand, if the firing temperature is excessively high, the alkali component evaporates from the alkali ion-conducting solid electrolyte precursor, and there is a risk that it will be difficult to obtain the coating layer (49) containing the alkali ion-conducting solid electrolyte having the desired composition. As a result, the internal resistance of the sintered electrode (73) increases, and the charge / discharge efficiency tends to decrease.

[0203] In addition, as shown in the 11th embodiment of FIG. 20, a battery member may be obtained by applying a paste as a material layer for forming a solid electrolyte onto a suitable substrate, stacking a compacted body as a material layer for forming an electrode onto the paste, and firing. Here, the compacted body can be obtained by press molding after mixing a conductive aid into a powder of a mixture of an alkali ion-conducting solid electrolyte precursor, a carbon electrode material precursor, and a particulate carbon electrode material. In addition, as shown in the 12th embodiment of FIG. 21, a sintered electrode may be obtained by firing the compacted body.

[0204] Hereinafter, an example of a battery member according to the third embodiment is shown.

[0205] [Example 3]

[0206] The composition ratio is Na3Zr2Si2PO 12 To obtain NASICON-type crystals, a total of 25 g of water glass (sodium silicate), an aqueous solution of zirconium ammonium carbonate, and sodium tripolyphosphate were weighed. These were added to 150 g of pure water and stirred with a hot stirrer at 50°C for 24 hours. By this, an alkali ion-conducting solid electrolyte precursor solution was obtained. Next, this solution was gelled by leaving it overnight in a constant temperature bath at approximately 5°C. By the above, an alkali ion-conducting solid electrolyte precursor was prepared.

[0207] <Preparation of a Mixture of Alkali Ion Conductive Solid Electrolyte Precursor and Carbon Electrode Material Precursor>

[0208] A mixture was obtained by mixing sucrose (sucrose), a hard carbon source that is a carbon electrode material precursor, and an alkaline ion-conducting solid electrolyte precursor in a stirrer for 1 hour at a weight ratio of 4:1. Next, the mixture was dried in a constant temperature bath at 60°C for 12 hours, and then vacuum dried at 100°C for 6 hours, after which it was ground into a powder using a mortar and pestle.

[0209] Preparation of Electrode Paste

[0210] Powder of a mixture of alkali ion-conducting solid electrolyte precursors and carbon electrode material precursors, and hard carbon powder (average particle size D 50 =1㎛) and a conductive additive (acetylene black) were weighed in a weight ratio of 57:40:3. To these, a PPC (polypropylene carbonate) binder was added in an external ratio of 15 wt%, and an electrode paste was obtained by mixing with a self-rotating mixer in an N-methylpyrrolidone solvent.

[0211] <Fabrication of Battery Components>

[0212] 500㎛ thick Na3Zr2Si2PO 12 A solid electrolyte layer composed of was prepared separately. An electrode paste was applied to the first main surface of the solid electrolyte layer to a thickness of 70 μm and dried in a drying oven at 50°C. After drying, the electrode was sintered at 1000°C for 2 hours under a nitrogen atmosphere (N2: 99.9999%) to obtain a sintered electrode in which hard carbon powder is covered by a coating layer. The coating layer was Na3Zr2Si2PO 12 It was formed by precipitating a mixed phase of an alkaline ion conductive solid electrolyte having the composition and a carbon electrode material consisting of hard carbon. Next, a current collector was formed on the sintered electrode by a sputtering method. The current collector is made of an aluminum thin film. By the above, a battery component was obtained. In addition, the sintered electrode of this embodiment is a negative electrode.

[0213] <Fabrication of Test Cells>

[0214] A test cell was fabricated by attaching metallic sodium as a counter electrode to the second main surface of the solid electrolyte layer inside a glove box.

[0215] Charge / Discharge Test

[0216] Charge and discharge tests were performed on the test battery in a constant temperature bath at 60°C. Specifically, charging (insertion of sodium ions) was performed at a cutoff voltage of 0.001V, and discharging (detachment of sodium ions) was performed at a cutoff voltage of 2.5V to measure the charge capacity and discharge capacity. At this time, in Example 3, the practical capacity was set to the weight of the fabricated negative electrode, i.e., the sintered electrode × 300mAh / g, and the current value was set to a rate of 0.1C, and charging and discharging were performed. The results of the charge and discharge test are shown in FIG. 24.

[0217] As shown in FIG. 24, the charging capacity was 379 mAh / g, the discharging capacity was 293 mAh / g, and the first charge-discharge efficiency was 77.3%. Since the first charge-discharge efficiency at 60°C in Example 1, which relates to a battery member according to the first embodiment of the present invention described above, was 68%, it is confirmed that Example 3, which relates to a battery member according to the third embodiment, has superior first charge-discharge efficiency.

[0218] The above describes embodiments using a carbon electrode material composed of graphite or hard carbon as an active material. Although the carbon electrode material composed of graphite or hard carbon is primarily used as a negative electrode active material, the present invention can also be applied when a positive electrode active material is used instead of the carbon electrode material. For example, in the method for manufacturing a battery member according to the second embodiment of the present invention shown in FIG. 18 and a battery member according to the 10th to 12th embodiments of the present invention shown in FIG. 19 to 21, it is possible to use a positive electrode active material instead of a particulate carbon electrode material (38). By doing so, a sintered electrode comprising a positive electrode active material and an alkali ion-conducting solid electrolyte can be obtained. Alternatively, a battery member having a solid electrolyte layer and the sintered electrode laminated on the solid electrolyte layer can be obtained. The positive electrode active material is not particularly limited, but for example, general formula Nax M y P2O z Crystals or crystallized glasses represented by (M is at least one transition metal element selected from Fe, Cr, Mn, Co and Ni, 1.20≤x≤2.10, 0.95≤y≤1.60) are listed.

[0219] [Example 4]

[0220] Preparation of Alkaline Ion Conductive Solid Electrolyte Precursors

[0221] Composition ratio Li7La3Zr2O 12 In order to obtain the crystal, a total of 25 g of lithium acetate dihydrate CH3COOLi·2H2O, lanthanum acetate hex.5 hydrate La(CH3COO)3·1.5H2O, and zirconium(IV) propoxide solution Zr(OCH2CH2CH3)4 were weighed. These were added to 150 g of pure water and stirred with a hot stirrer at 50°C for 24 hours. By this, an alkali ion-conducting solid electrolyte precursor solution was obtained. Next, this solution was gelled by leaving it overnight in a constant temperature bath at about 5°C. By the above, an alkali ion-conducting solid electrolyte precursor was prepared.

[0222] <Preparation of a Mixture of Alkali Ion Conductive Solid Electrolyte Precursor and Carbon Electrode Material Precursor>

[0223] Using sucrose (sucrose), a hard carbon source that is a carbon electrode material precursor, and the alkaline ion-conducting solid electrolyte precursor obtained above, a powder of a mixture of an alkaline ion-conducting solid electrolyte precursor and a carbon electrode material precursor was obtained by the same method as in Example 1.

[0224] Preparation of Electrode Paste

[0225] Using the powder of the mixture of the alkali ion-conducting solid electrolyte precursor and the carbon electrode material precursor obtained above, an electrode paste was obtained by the same method as in Example 1.

[0226] <Fabrication of Battery Components>

[0227] Li7La3Zr2O with a thickness of 500㎛ 12 A solid electrolyte layer composed of was prepared separately. An electrode paste was applied to the first main surface of the solid electrolyte layer to a thickness of 70 μm and dried in a dryer at 50°C to form a material layer for electrode formation. After drying, the material was calcined at 1000°C for 2 hours under a nitrogen atmosphere (N2: 99.9999%), and Li7La3Zr2O 12 A sintered electrode was obtained by precipitating a mixed phase of an alkaline ion conductive solid electrolyte having the composition of and a carbon electrode material made of hard carbon. Next, a current collector was formed on the sintered electrode by a sputtering method. The current collector is made of a copper foil. By the above, a battery component was obtained. In addition, the sintered electrode of this embodiment is a negative electrode.

[0228] <Fabrication of Test Cells>

[0229] A test battery was fabricated by attaching metallic lithium as a counter electrode to the second main surface of the solid electrolyte layer inside a glove box.

[0230] Charge / Discharge Test

[0231] A charge-discharge test of the test battery was performed in a constant temperature bath at 60°C. Specifically, charging (lithium ion insertion) was performed at a cutoff voltage of 0.001V, and discharging (lithium ion extraction) was performed at a cutoff voltage of 1.5V, and the charge capacity and discharge capacity were measured. At this time, the actual capacity was set to the weight of the fabricated negative electrode, i.e., the sintered electrode × 400mAh / g, and the current value was set to a rate of 0.1C, and charging and discharging were performed. As a result, the charge capacity was 419mAh / g, the discharge capacity was 314mAh / g, and the first charge-discharge efficiency was 74.9%. Explanation of the symbols

[0232] 1… Battery component 2… solid electrolyte layer 2a, 2b… the first, second sides 3… Sintered body electrode 4… the whole house 5… mixed phase 6… Challenge Formula 13A∼13C… Paste 21… Battery component 22… Paste 22A… Compactor 23A∼23C… Compactor 27… entry 31… Battery component 33… Sintered body electrode 38… Particulate carbon electrode material 39… coating layer 41… Battery component 43… Paste 49… coating layer 53… Compactor 73… Sintered body electrode 83… Paste

Claims

Claim 1 A sintered electrode comprising a carbon electrode material made of graphite or hard carbon and an alkali ion-conducting solid electrolyte, a plurality of mixed phases of the carbon electrode material and the alkali ion-conducting solid electrolyte, each of the plurality of mixed phases being composed of particles, the average particle size of the particles being 10 μm or less, wherein in the mixed phases, the carbon electrode material and the alkali ion-conducting solid electrolyte are mixed such that the boundary between the carbon electrode material and the alkali ion-conducting solid electrolyte cannot be distinguished, and the particle-based mixed phases are bonded to each other. Claim 2 In claim 1, the sintered electrode wherein the alkaline ion-conducting solid electrolyte has sodium ion conductivity. Claim 3 A sintered electrode according to claim 1 or 2, wherein the alkali ion-conducting solid electrolyte is composed of an oxide. Claim 4 delete Claim 5 A sintered electrode according to claim 1 or 2, wherein the carbon electrode material is a particulate carbon electrode material and the particulate carbon electrode material is covered by a coating layer made of the alkaline ion-conducting solid electrolyte. Claim 6 A sintered electrode according to claim 1 or 2, wherein the carbon electrode material is a particulate carbon electrode material, and the particulate carbon electrode material is covered by a coating layer consisting of a carbon electrode material different from the particulate carbon electrode material and the alkali ion-conducting solid electrolyte. Claim 7 In claim 1 or 2, the alkali ion-conducting solid electrolyte is a NASICON-type crystal, and also has the general formula Na 1+x Zr2P 3-x Si x O 12 A sintered electrode comprising at least one of a first compound represented by (0≤x≤3) and a second compound in which a portion of Zr of the first compound is substituted with at least one element selected from the group consisting of Ca, Mg, Ba, Sr, Al, Nb, Ta, In, Ga and a group 3 element. Claim 8 A sintered electrode according to claim 1 or 2, wherein the alkali ion-conducting solid electrolyte has at least one of a β-alumina type crystal and a β"-alumina type crystal. Claim 9 In claim 1 or 2, the alkali ion-conducting solid electrolyte is of the general formula Li7La3Zr2O 12 , Li7La3Zr 2-x M x O 12 (M is at least one selected from Nb, Ga, and Ta, 0 <x<2) 또는 Li 7-3x Al x La3Zr2O 12 (0 <x<2.3)로 나타내어지는 결정상을 갖는, 소결체 전극. Claim 10 A sintered electrode according to claim 1 or 2, comprising 0% to 20% by weight of at least one carbon-based conductive agent selected from carbon black, acetylene black, Ketjenblack, carbon nanotubes, and vapor phase carbon fiber carbon conductive agent (VGCF). Claim 11 A sintered electrode, which is a negative electrode, according to claim 1 or 2. Claim 12 A sintered electrode according to claim 1 or 2, capable of absorbing and releasing alkali ions at 30°C after heat treatment in an inert atmosphere at 500°C. Claim 13 A sintered electrode according to claim 1 or 2, having a charge / discharge efficiency of 90% or more when charged / discharged at a cutoff voltage of 9V to 0.001V and capable of reversibly charging / discharging. Claim 14 A battery member comprising a solid electrolyte layer and a sintered electrode described in claim 1 or 2 laminated on the solid electrolyte layer. Claim 15 A battery member according to claim 14, wherein the thickness of the solid electrolyte layer is 5 nm to 1 mm. Claim 16 A battery having a battery member as described in claim 14. Claim 17 A method for manufacturing a sintered electrode according to claim 1, comprising a process of obtaining a mixture of an alkaline ion-conducting solid electrolyte precursor and a carbon electrode material precursor by mixing an alkaline ion-conducting solid electrolyte precursor and a carbon electrode material precursor, wherein the carbon electrode material precursor is a precursor of a carbon electrode material made of graphite or hard carbon, a process of forming an electrode-forming material layer containing the mixture after the mixing process, and a process of sintering the electrode-forming material layer. Claim 18 A method for manufacturing a sintered electrode according to claim 17, wherein the electrode-forming material layer is formed from a paste or compact comprising the alkali ion-conducting solid electrolyte precursor and the carbon electrode material precursor, and in a process of sintering the electrode-forming material layer, the alkali ion-conducting solid electrolyte and the carbon electrode material are obtained simultaneously. Claim 19 A method for manufacturing a sintered electrode according to claim 17, wherein, in a process for forming a material layer for forming an electrode, a first firing process is performed to obtain a carbon electrode material by firing the mixture, and then, a material layer for forming an electrode is formed by a paste or compact comprising the alkali ion conductive solid electrolyte precursor and the carbon electrode material, and in a process for firing the material layer for forming an electrode, an alkali ion conductive solid electrolyte is obtained from the alkali ion conductive solid electrolyte precursor. Claim 20 A method for manufacturing a sintered electrode according to claim 17, further comprising a third sintering process to simultaneously obtain an alkali ion-conducting solid electrolyte and a carbon electrode material by sintering the mixture after the mixing process, and in the process of forming the electrode-forming material layer, forming the electrode-forming material layer composed of a paste or a compact body comprising the alkali ion-conducting solid electrolyte and the carbon electrode material. Claim 21 A method for manufacturing a sintered electrode according to claim 1, comprising: a mixing process for obtaining a mixture of an alkali ion-conducting solid electrolyte precursor and a particulate carbon electrode material made of graphite or hard carbon by mixing the alkali ion-conducting solid electrolyte precursor and the particulate carbon electrode material; a process for forming an electrode-forming material layer made of a paste or compacted body comprising the alkali ion-conducting solid electrolyte precursor and the particulate carbon electrode material after the mixing process; and a process for obtaining the particulate carbon electrode material covered by a coating layer made of the alkali ion-conducting solid electrolyte by calcining the electrode-forming material layer and obtaining an alkali ion-conducting solid electrolyte from the alkali ion-conducting solid electrolyte precursor. Claim 22 A method for manufacturing a sintered electrode according to claim 1, comprising a process of obtaining a mixture of the alkali ion-conducting solid electrolyte precursor, the carbon electrode material precursor, and the particulate carbon electrode material by mixing the alkali ion-conducting solid electrolyte precursor, the carbon electrode material precursor, and the particulate carbon electrode material, wherein the carbon electrode material precursor is a precursor of the carbon electrode material made of graphite or hard carbon; a mixing process in which the carbon electrode material precursor is a precursor of the carbon electrode material made of graphite or hard carbon; a process of forming an electrode-forming material layer made of a paste or a compacted body containing the mixture after the mixing process; and a process of obtaining the particulate carbon electrode material covered by a coating layer made of the alkali ion-conducting solid electrolyte and the carbon electrode material by calcining the electrode-forming material layer and obtaining the alkali ion-conducting solid electrolyte and the carbon electrode material from the alkali ion-conducting solid electrolyte precursor and the carbon electrode material precursor. Claim 23 A method for manufacturing a battery member comprising a laminate of a sintered electrode and a solid electrolyte layer as described in claim 1, comprising: a process of obtaining a mixture of the alkali ion-conducting solid electrolyte precursor and the carbon electrode material precursor by mixing the alkali ion-conducting solid electrolyte precursor and the carbon electrode material precursor, wherein the carbon electrode material precursor is a precursor of a carbon electrode material made of graphite or hard carbon; a process of forming an electrode-forming material layer comprising the mixture after the mixing process; a process of obtaining a sintered electrode by firing the electrode-forming material layer; and a process of obtaining a laminate of the sintered electrode and the solid electrolyte layer. Claim 24 A method for manufacturing a battery member according to claim 23, wherein the electrode-forming material layer is formed from a paste or compact comprising the alkali ion-conducting solid electrolyte precursor and the carbon electrode material precursor, and the alkali ion-conducting solid electrolyte and the carbon electrode material are obtained simultaneously by firing the electrode-forming material layer. Claim 25 A method for manufacturing a battery member according to claim 23, wherein, in the process of forming the electrode-forming material layer, a first firing process is performed to obtain a carbon electrode material by firing the mixture, and then the electrode-forming material layer is formed from a paste or compact comprising the alkali ion-conducting solid electrolyte precursor and the carbon electrode material, and the process of obtaining the sintered electrode is a second firing process to obtain an alkali ion-conducting solid electrolyte by firing the electrode-forming material layer. Claim 26 A method for manufacturing a battery member according to claim 23, further comprising a third firing process for simultaneously obtaining an alkali ion-conducting solid electrolyte and a carbon electrode material by firing the mixture after the mixing process, wherein in the process of forming the electrode-forming material layer, the electrode-forming material layer is formed by a paste or compact body comprising the alkali ion-conducting solid electrolyte and the carbon electrode material, and the process of obtaining the sintered electrode is a fourth firing process for firing the electrode-forming material layer. Claim 27 A method for manufacturing a battery member comprising a laminate of a sintered electrode and a solid electrolyte layer as described in claim 1, comprising: a mixing process for obtaining a mixture of an alkali ion-conducting solid electrolyte precursor and a particulate carbon electrode material made of graphite or hard carbon by mixing the alkali ion-conducting solid electrolyte precursor and the particulate carbon electrode material; a process for forming an electrode-forming material layer made of a paste or a compacted body containing the alkali ion-conducting solid electrolyte precursor and the particulate carbon electrode material after the mixing process; a process for obtaining a sintered electrode by calcining the electrode-forming material layer and obtaining an alkali ion-conducting solid electrolyte from the alkali ion-conducting solid electrolyte precursor, and obtaining the particulate carbon electrode material covered by a coating layer made of the alkali ion-conducting solid electrolyte; and a process for obtaining a laminate of the sintered electrode and the solid electrolyte layer. Claim 28 A method for manufacturing a battery member according to any one of claims 23 to 27, further comprising a lamination process for laminating the solid electrolyte layer and the electrode forming material layer, and performing a process for obtaining the sintered electrode after the lamination process. Claim 29 A method for manufacturing a battery member according to any one of claims 23 to 27, further comprising a lamination process for laminating a solid electrolyte forming material layer made of a paste or compacted body containing a solid electrolyte precursor and an electrode forming material layer, and by sintering the electrode forming material layer and the solid electrolyte forming material layer after the lamination process, thereby simultaneously obtaining the sintered electrode and the solid electrolyte layer. Claim 30 delete Claim 31 delete Claim 32 delete Claim 33 delete Claim 34 delete Claim 35 delete Claim 36 delete Claim 37 delete Claim 38 delete

Citation Information

Patent Citations

  • Graphite negative electrode material of low-temperature lithium ion battery and preparation method thereof

    CN108987687A

  • All solid battery

    JP2011150817A

  • All-solid battery

    JP2014053181A

  • Method for preparing a solid-state battery by sintering under pulsating current

    KR1020130034010A

  • Solid-state battery electrolyte having increased stability towards cathode materials

    WO2019094359A1