All Solid State Rechargeable Battery

Incorporating endothermic materials in the positive electrode layer of all-solid-state secondary batteries addresses safety concerns by absorbing heat through decomposition reactions, preventing exothermic reactions and maintaining charging capacity.

KR103047640B1Active Publication Date: 2026-11-11SAMSUNG SDI CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020210084111
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-03
Filing Date
2021-06-28
Publication Date
2026-11-11
Estimated Expiration
2041-06-28

AI Technical Summary

Technical Problem

All-solid-state secondary batteries face safety concerns due to potential exothermic reactions with oxygen generation at high temperatures, which can lead to ignition, especially when placed in environments above 200°C.

Method used

Incorporating an endothermic material, such as carbonate or hydroxide compounds, into the positive electrode layer to induce a decomposition reaction that absorbs heat, thereby suppressing exothermic reactions and maintaining safety even at high temperatures.

Benefits of technology

The endothermic material effectively suppresses rapid heat generation and exothermic reactions, enhancing the safety of all-solid-state secondary batteries by ensuring a sufficient endothermic effect while maintaining charging capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112021074435897-PAT00001_ABST
    Figure 112021074435897-PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to an all-solid-state secondary battery comprising a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein the positive electrode layer comprises a plate-shaped positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, wherein the positive electrode layer contains a heat-absorbing material that absorbs heat through a decomposition reaction, and the content of the heat-absorbing material in the positive electrode layer is in the range of 1 part by weight or more and 30 parts by weight or less when the total weight of the positive electrode active material layer is 100 parts by weight.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] This is about all-solid-state secondary batteries. Background Technology

[0002] Although all-solid-state secondary batteries are safer than secondary batteries using organic electrolytes, there is a concern that oxygen may be generated during charging if the all-solid-state secondary battery is placed in a high-temperature environment such as 200°C or higher, or depending on the composition of the positive electrode active material. If this oxygen causes an exothermic reaction with the sulfide-based solid electrolyte, the temperature of the all-solid-state battery rises further, and there is a concern that it may ignite if conditions such as the presence of flammable materials nearby are met.

[0003] [Prior Art Literature]

[0004] [Patent Document 1] Publication No. JP 1999-191417 The problem to be solved

[0005] In order to further enhance the safety of the all-solid-state secondary battery, an all-solid-state secondary battery is provided that can suppress the aforementioned exothermic reaction even under high temperature environments such as 200°C or higher. means of solving the problem

[0006] As a technology for suppressing heat generation in secondary batteries, a secondary battery of a liquid system containing a compound whose decomposition reaction is an endothermic reaction (hereinafter also referred to as an endothermic substance), as described in Patent Document 1, for example, is being considered. However, when the aforementioned endothermic substance was actually applied to an all-solid-state secondary battery, it was discovered that the decomposition reaction of the endothermic substance, i.e., the endothermic reaction, is difficult to occur in the all-solid-state secondary battery compared to the secondary battery of the liquid system described in Patent Document 1. Therefore, as a result of repeated examinations regarding the conditions and the content of the endothermic substance required to sufficiently induce an endothermic reaction in the all-solid-state secondary battery, the present invention was completed.

[0007] In other words, an all-solid-state secondary battery according to one embodiment comprises a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein the positive electrode layer comprises a plate-shaped positive current collector and a positive active material layer located on the positive current collector, wherein the positive electrode layer contains a heat-absorbing material that absorbs heat through a decomposition reaction, and wherein the content of the heat-absorbing material in the positive electrode layer is in the range of 1 part by weight or more and 30 parts by weight or less when the total weight of the positive active material layer is 100 parts by weight.

[0008] According to the all-solid-state secondary battery configured in this way, since the anode layer in the oxidizing environment during charging contains an endothermic material, the decomposition reaction of the endothermic material is likely to occur during charging, and a sufficient endothermic effect can be exerted even at temperatures below 200°C. As a result, for the all-solid-state secondary battery, rapid heat generation at temperatures above 200°C, where oxygen may be generated during charging, can be prevented.

[0009] In addition, the content of the endothermic material in the anode layer is in the range of 1 part by weight or more and 30 parts by weight or less when the total weight of the anode active material layer is 100 parts by weight, so that sufficient endothermic effect can be achieved while sufficiently securing the charging capacity of the anode layer.

[0010] If the above-mentioned heat-absorbing material is contained within the positive active material layer or disposed between the positive active material layer and the positive current collector, it is desirable because the heat-absorbing material can be reliably placed in an oxidizing environment during charging.

[0011] As a specific embodiment, the endothermic substance may be a carbonate compound and / or a hydroxide compound.

[0012] Examples of the above carbonate compounds include lithium carbonate.

[0013] Examples of the above hydroxide compounds include aluminum hydroxide.

[0014] When the above solid electrolyte layer contains a sulfide-based solid electrolyte, an exothermic reaction is likely to occur when the battery is placed in a high-temperature environment, so the effects of the present invention can be significantly exhibited.

[0015] From the perspective of suppressing deformation of the battery, etc., it is desirable that the difference between the volume inside the outer body at 80°C and the volume at 25°C be within 5% of the volume at 25°C.

[0016] An outer body is additionally provided to accommodate the anode layer, the cathode layer, and the solid electrolyte layer inside, and when the outer body is in the form of a film, the volume change caused by the decomposition reaction of the endothermic material is likely to affect the total volume of the battery, so the effects of the present invention can be significantly exhibited. Effects of the invention

[0017] The safety of the all-solid-state secondary battery can be further enhanced, the aforementioned exothermic reaction can be suppressed even under high-temperature environments, and rapid heat generation during charging can be suppressed. Brief explanation of the drawing

[0018] FIG. 1 is a cross-sectional view showing the schematic configuration of an all-solid-state secondary battery according to one embodiment. FIG. 2 is a cross-sectional view showing the schematic configuration of an all-solid-state secondary battery according to another embodiment. FIG. 3 is a cross-sectional view showing the schematic configuration of an all-solid-state secondary battery according to another embodiment. Specific details for implementing the invention

[0019] Preferred embodiments are described in detail below with reference to the attached drawings. Meanwhile, for components having substantially the same functional configuration in this specification and drawings, redundant descriptions are omitted by assigning the same reference numerals.

[0020] <1. Basic configuration of an all-solid-state secondary battery according to the present embodiment>

[0021] The all-solid-state secondary battery (1) according to the present embodiment comprises, as shown in FIG. 1, a positive electrode layer (10), a negative electrode layer (20), and a solid electrolyte layer (30), and an outer body (40) that accommodates them inside.

[0022] (1-1. Anode)

[0023] The positive electrode layer (10) includes a positive electrode current collector (11) and a positive electrode active material layer (12). Examples of positive electrode current collectors (11) include a plate-shaped or thin-shaped body made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or alloys thereof. The positive electrode current collector (11) may be omitted. The positive electrode active material layer (12) includes a positive electrode active material and a solid electrolyte. Meanwhile, the solid electrolyte included in the positive electrode active material layer (12) may or may not be of the same type as the solid electrolyte included in the solid electrolyte layer (30). Details of the solid electrolyte will be explained in detail in the section on the solid electrolyte layer (30).

[0024] The positive electrode active material may be any positive electrode active material capable of reversibly absorbing and releasing lithium ions. For example, the positive electrode active material may be formed using lithium salts such as lithium cobaltate (hereinafter referred to as LCO), lithium nickel oxide, lithium nickel cobalt oxide, lithium cobalt aluminum oxide (hereinafter referred to as NCA), lithium cobalt manganese oxide (hereinafter referred to as NCM), lithium manganate, and lithium iron phosphate, as well as nickel sulfide, copper sulfide, lithium sulfide, sulfur, iron oxide, or vanadium oxide. Each of these positive electrode active materials may be used individually, or two or more may be used in combination.

[0025] In addition, the positive electrode active material is preferably formed by including a lithium salt of a transition metal oxide having a layered rock salt type structure among the lithium salts described above. Here, "layered rock salt type structure" refers to a cubic rock salt type structure. <111> It is a structure in which oxygen atomic layers and metal atomic layers are alternately arranged in a regular pattern, and as a result, each atomic layer forms a two-dimensional plane. Also, the "cubic rock salt type structure" refers to a sodium chloride type structure, which is a type of crystal structure, and specifically, it refers to a structure in which face-centered cubic lattices formed by each of the cation and anion are arranged such that they are offset from each other by only half of the corners of the unit cell.

[0026] As lithium salts of transition metal oxides possessing such a layered rock salt-type structure, for example, LiNi x Co y Al z O2(NCA), or LiNi x Co y Mn z O2(NCM) (where 0 <x<1, 0<y<1, 0<z<1, 및 x+y+z=1)등의 삼원계 전이금속산화물의 리튬 염을 들 수 있다.

[0027] When the positive active material includes a lithium salt of a ternary transition metal oxide having the above-mentioned layered rock salt structure, the energy density and thermal stability of the all-solid-state secondary battery (1) can be improved.

[0028] The positive electrode active material may be covered by a coating layer. Here, the coating layer of the present embodiment may be any known coating layer for the positive electrode active material of an all-solid-state secondary battery. Examples of the coating layer include Li2O-ZrO2.

[0029] In addition, when the positive active material is formed from a lithium salt of a ternary transition metal oxide such as NCA or NCM and includes nickel (Ni) as the positive active material, the capacity density of the all-solid-state secondary battery (1) can be increased, and metal leaching from the positive active material in the charged state can be reduced. Accordingly, the all-solid-state secondary battery (1) according to the present embodiment can improve long-term reliability and cycle characteristics in the charged state. To further exhibit these characteristics, it is more desirable to have a high nickel (Ni) content. The nickel content in the positive active material is preferably at least 60 mol%, and is also preferably 80 mol%. On the other hand, if it is 95 mol% or less, it is desirable because it can suppress the decrease in battery capacity during charge-discharge evaluation.

[0030] Here, the shape of the positive active material may include, for example, a particle shape such as a regular sphere or an elliptical sphere. In addition, the particle size of the positive active material is not particularly limited and may be within a range applicable to the positive active material of a conventional all-solid-state secondary battery. Meanwhile, the content of the positive active material in the positive layer (10) is also not particularly limited and may be within a range applicable to the positive layer (10) of a conventional all-solid-state secondary battery. Furthermore, in addition to the positive active material and solid electrolyte described above, the positive active material layer (12) may appropriately incorporate additives such as a conductivity aid, a binder, a filler, a dispersant, and an ion conductivity aid.

[0031] Examples of conductive aids that can be incorporated into the positive active material layer (12) include graphite, carbon black, acetylene black, ketjen black, carbon fiber, metal powder, etc. Also, examples of binders that can be incorporated into the positive active material layer (12) include styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc. Additionally, known materials that can generally be used as electrodes of all-solid-state secondary batteries may be used as fillers, dispersants, ion conductive aids, etc. that can be incorporated into the positive active material layer (12).

[0032] (1-2. Cathode layer)

[0033] The negative electrode layer (20) includes a negative electrode current collector (21) and a negative electrode active material layer (22). The negative electrode current collector (21) is preferably composed of a material that does not react with lithium, that is, does not form either an alloy or a compound. Examples of materials constituting the negative electrode current collector (21) include copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), and nickel (Ni). The negative electrode current collector (21) may be composed of any one of these metals, or may be composed of an alloy or clad material of two or more metals. The negative electrode current collector (21) is, for example, plate-shaped or thin-walled.

[0034] The negative electrode active material layer (22) includes a negative electrode active material. The negative electrode active material may include, for example, amorphous carbon and an alloy-forming element that forms an alloy with lithium. As the alloy-forming element, one or more selected from gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, and zinc may be included. Here, as the amorphous carbon, examples include carbon black, graphene, graphite, etc. As the carbon black, examples include acetylene black, furnace black, ketjen black, etc. Also, to improve electronic conductivity, the surface of silicon may be coated with a carbon layer with a thickness of about 1 to 10 nm.

[0035] Here, when one or more of gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, and zinc are used as the alloy-forming elements, the negative electrode active material is preferably in the form of particles, for example, and the particle size is 4 μm or less, more preferably 300 nm or less. In this case, the characteristics of the all-solid-state secondary battery (1) are also improved. Here, the particle size of the negative electrode active material may be, for example, a median diameter (so-called D50) measured using a laser particle size distribution meter. In addition to the above, additives used in conventional all-solid-state secondary batteries, such as binders, fillers, dispersants, ion conductivity aids, etc., may be appropriately mixed into the negative electrode active material layer (22).

[0036] (1-3. Solid Electrolyte Layer)

[0037] The solid electrolyte layer (30) is formed between the anode layer (10) and the cathode layer (20) and contains a solid electrolyte.

[0038] The solid electrolyte is composed of, for example, sulfide-based solid electrolyte materials. Examples of sulfide-based solid electrolyte materials include Li2S-P2S5, Li2S-P2S-LiX (where X is a halogen element, e.g., I, Cl), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, and Li2S-P2S5-Z m S n (m and n are integers, and Z is Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q Examples include (p and q are integers, and M is P, Si, Ge, B, Al, Ga, or In). Here, the sulfide-based solid electrolyte material is produced by processing starting materials (e.g., Li2S, P2S5, etc.) by a melt quenching method or a mechanical milling method. Additionally, heat treatment may be performed after this process. The solid electrolyte may be amorphous, crystalline, or a mixture of both.

[0039] In addition, as a solid electrolyte, it is preferable to use a sulfide solid electrolyte material that includes at least sulfur (S), phosphorus (P), and lithium (Li) as constituent elements among the above-mentioned sulfide solid electrolyte materials, and it is more preferable to use one that includes Li2S-P2S5. Here, when using a sulfide-based solid electrolyte material that includes Li2S-P2S5 to form the solid electrolyte, the molar ratio of Li2S to P2S5 may be selected, for example, in the range of Li2S:P2S5 = 50:50 to 90:10.

[0040] Additionally, the solid electrolyte layer (30) may further include a binder. Examples of binders included in the solid electrolyte layer (30) include styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc. The binder in the solid electrolyte layer (30) may be of the same type as the binder in the positive electrode active material layer (12) and the negative electrode active material layer (22), or it may be different.

[0041] (1-4. Exterior Body)

[0042] As described above, the outer body (40) accommodates the anode layer (10), the cathode layer (20), and the solid electrolyte layer (30) inside, and may be formed by a flexible film, for example. As the film, for example, a laminate film formed by inserting a metal thin film such as aluminum or SUS into a resin such as polypropylene or polyethylene may be used. The thickness of the laminate film used as the outer body (40) may be, for example, 30 μm or more and 150 μm or less. Other materials may be rigid metals. For example, a can made of aluminum or SUS may be used. In this case, the shape of the outer body may be rectangular or cylindrical.

[0043] <2. Characteristic configuration of the all-solid-state secondary battery according to the present embodiment>

[0044] The above positive active material layer (12) contains an endothermic material that absorbs heat through a decomposition reaction. Examples of the endothermic material include carbonate compounds, hydroxide compounds, and compounds containing crystal water. Examples of carbonate compounds include carbonates and bicarbonates. Among these, examples include lithium carbonate, rubidium carbonate, barium carbonate, cobalt carbonate, iron carbonate, nickel carbonate, zinc carbonate, sodium bicarbonate, potassium bicarbonate, rubidium bicarbonate, and cesium bicarbonate.

[0045] Examples of the above hydroxide compounds include zinc hydroxide, aluminum hydroxide, cadmium hydroxide, chromium hydroxide, cobalt hydroxide, nickel hydroxide, manganese hydroxide, calcium hydroxide, magnesium hydroxide, zirconium hydroxide, iron hydroxide, and nickel hydroxide.

[0046] In addition, compounds containing crystal water include, for example, aluminum oxide hydrate, barium nitrate hydrate, calcium sulfate hydrate, cobalt phosphate hydrate, antimony oxide hydrate, tin oxide hydrate, titanium oxide hydrate, bismuth oxide hydrate, and tungsten oxide hydrate.

[0047] As for the endothermic material, only one of the aforementioned materials may be used, or multiple types may be used in combination.

[0048] It is preferable that the content of the endothermic material be in the range of 1 part by weight or more and 30 parts by weight or less when the entire positive active material layer (12) is 100 parts by weight. It is more preferable that the content of the endothermic material be 5 parts by weight or more and 25 parts by weight or less, and even more preferable that it be 5 parts by weight or more and 10 parts by weight or less.

[0049] <3. Method for manufacturing an all-solid-state secondary battery according to the present embodiment>

[0050] Next, a method for manufacturing an all-solid-state secondary battery (1) according to the present embodiment will be described. The all-solid-state secondary battery (1) according to the present embodiment can be manufactured by manufacturing a positive electrode layer (10), a negative electrode layer (20), and a solid electrolyte layer (30) respectively, stacking each of the layers, and finally covering them with an outer body (40).

[0051] (3-1. Anode Layer Fabrication Process)

[0052] First, a slurry (the slurry may be a paste, and other slurries may be the same) is prepared by adding materials constituting the positive active material layer (12) (positive active material, endothermic material, binder, etc.) to a non-polar solvent such as dehydrated xylene. Next, the obtained slurry is applied over the positive current collector (11) and dried. Next, the positive layer (10) is prepared by applying pressure to the obtained laminate (for example, applying pressure using hydrostatic pressure). The pressure process may be omitted. The positive layer (10) may also be prepared by forming a mixture of materials constituting the positive active material layer (12) into a pellet shape or by stretching it into a sheet shape. When the positive layer (10) is prepared by these methods, the positive current collector (11) may be pressed onto the prepared pellet or sheet.

[0053] (3-2. Cathode Layer Fabrication Process)

[0054] First, a slurry is prepared by adding a negative electrode active material layer material (negative electrode active material, alloy non-forming element, binder, etc.) constituting the negative electrode active material layer (22) to a polar solvent or a non-polar solvent. Next, the obtained slurry is applied onto a negative electrode current collector (21) and dried. Next, the negative electrode layer (20) is prepared by applying pressure to the obtained laminate (for example, applying pressure using hydrostatic pressure). The pressure application process may be omitted.

[0055] (3-3. Solid Electrolyte Layer Fabrication Process)

[0056] The solid electrolyte layer (30) can be produced using a solid electrolyte formed from a sulfide-based solid electrolyte material. First, the starting material is processed by a melt quenching method or a mechanical milling method. For example, when using the melt quenching method, a predetermined amount of starting material (e.g., Li2S, P2S5, etc.) is mixed and formed into a pellet shape, and then reacted in a vacuum at a predetermined reaction temperature and quenched to produce a sulfide-based solid electrolyte material. Meanwhile, the reaction temperature of the mixture of Li2S and P2S5 is preferably 400°C to 1000°C, and more preferably 800°C to 900°C. Also, the reaction time is preferably 0.1 hours to 12 hours, and more preferably 1 hour to 12 hours. In addition, the quenching temperature of the reactant is typically 10°C or lower, preferably 0°C or lower, and the quenching rate is typically about 1°C / sec to 10000°C / sec, preferably about 1°C / sec to 1000°C / sec.

[0057] In addition, when using the mechanical milling method, sulfide-based solid electrolyte materials can be produced by stirring and reacting starting materials (e.g., Li2S, P2S5, etc.) using a ball mill or the like. Meanwhile, although the stirring speed and stirring time in the mechanical milling method are not particularly limited, a faster stirring speed can accelerate the formation rate of the sulfide-based solid electrolyte material, and a longer stirring time can increase the conversion rate of the raw materials to the sulfide-based solid electrolyte material.

[0058] Subsequently, a particulate solid electrolyte can be produced by heat-treating the mixed raw materials obtained by the melt quenching method or mechanical milling method at a predetermined temperature and then grinding them. If the solid electrolyte has a glass transition point, it may change from an amorphous to a crystalline state through heat treatment.

[0059] Furthermore, the solid electrolyte obtained by the above method can be formed into a solid electrolyte layer (30) by forming a film using a known film formation method, such as aerosol deposition, cold spray, or sputtering. Meanwhile, the solid electrolyte layer (30) may be formed by applying pressure to a solid electrolyte particle. Alternatively, the solid electrolyte layer (30) may be formed by mixing the solid electrolyte, a solvent, and a binder, applying and drying the mixture, and applying pressure.

[0060] (3-4. Assembly Process of All-Solid State Secondary Batteries)

[0061] A positive electrode layer (10), a negative electrode layer (20), and a solid electrolyte layer (30) produced by the above method can be laminated so that the positive electrode layer (10) and the negative electrode layer (20) and the solid electrolyte layer (30) are interlocked, and the entire set of these is covered from both sides with a laminate film forming an outer body (40), and then pressurized (e.g., pressurized using hydrostatic pressure) to produce an all-solid-state secondary battery (1) according to the present embodiment.

[0062] <4. Effects of the present embodiment>

[0063] According to the all-solid-state secondary battery configured in this way, since the positive active material layer in an oxidizing environment during charging contains an endothermic material, the decomposition reaction of the endothermic material occurs at an appropriate temperature range and can exhibit a sufficient endothermic effect.

[0064] Since the content of the endothermic material is 1 part by weight or more and 30 parts by weight or less, the charging capacity of the positive active material layer (12) can be sufficiently secured while the endothermic effect can be sufficiently exerted.

[0065] <5. Regarding other embodiments of the present invention>

[0066] <5-1. Composition of an all-solid-state secondary battery according to a second embodiment of the present invention>

[0067] As illustrated in FIG. 2, the positive layer (10) may additionally have a conductive layer (13) formed between the positive current collector (11) and the positive active material layer (12). The conductive layer (13) is a layer that protects the positive current collector and, for example, contains a conductive material and a binder.

[0068] As a conductive material contained in the conductive layer (13), graphite, carbon black, acetylene black, Ketjen black, carbon fiber, metal powder, etc. may be used. Also, as a binder contained in the conductive layer (13), examples include styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, etc. The conductive layer (13) thus composed may also contain the aforementioned heat-endorsing material. As a specific composition of the conductive layer (13) when containing the heat-endorsing material, for example, the content of the conductive material in the conductive layer (13) may be 6% by weight or more and 54% by weight or less, the content of the heat-endorsing material may be 24% by weight or more and 81% by weight or less, and the content of the binder may be 10% by weight or more and 40% by weight or less.

[0069] The amount of endothermic material contained in the conductive layer (13) is such that the sum of the amount of endothermic material contained in the positive active material layer (12) and the amount of endothermic material contained in the conductive layer (13) is 1 part by weight or more and 30 parts by weight or less when the total weight of the positive active material layer (12) is 100 parts by weight. In this embodiment, the endothermic material may be contained in both the positive active material layer (12) and the conductive layer (13), or the endothermic material may be contained only in the conductive layer (13).

[0070] In this embodiment as well, similar to the previously described embodiment, a sufficient heat-absorbing effect can be obtained by making the content of the heat-absorbing material 1 part by weight or more when the total weight of the positive active material layer (12) is 100 parts by weight. In addition, by making the content of the heat-absorbing material 30 parts by weight or less, the thickness of the conductive layer (13) can be suppressed while maintaining the conductivity of the conductive layer (13), and the volume of the all-solid-state secondary battery (1) can be suppressed from increasing. Meanwhile, the thickness of the conductive layer is preferably in the range of 0.5 μm or more and 10 μm or less, and more preferably 1 μm or more and 5 μm or less. In this embodiment, the conductive layer (13) containing the heat-absorbing material is a layer that exhibits a heat-absorbing effect, so it may be called a heat-absorbing layer.

[0071] <5-2. Method for manufacturing an all-solid-state secondary battery according to a second embodiment of the present invention>

[0072] Next, a method for manufacturing an all-solid-state secondary battery (1) according to a second embodiment will be described. In the process of manufacturing the positive electrode layer (10) of the method for manufacturing an all-solid-state secondary battery (1) according to a first embodiment, a slurry formed by adding a material constituting the conductive layer (13) (conductive material, heat-absorbing material, binder, etc.) to a non-polar solvent is applied onto a positive electrode current collector (11) and dried to form the conductive layer (13). A slurry for forming the positive electrode active material layer (12) is applied onto the conductive layer (13), dried to form the positive electrode active material layer (12), and the positive electrode layer (10) is manufactured by applying pressure. The other processes can be manufactured in the same manner as in the first embodiment to produce the all-solid-state secondary battery (1).

[0073] <5-3. Composition of an all-solid-state secondary battery according to the third embodiment of the present invention>

[0074] In the above-described embodiment, an all-solid-state secondary battery (1) having a positive electrode layer (10), a negative electrode layer (20), and a solid electrolyte layer (30) each as one layer was described, but, for example, as shown in FIG. 3, a solid electrolyte layer (30) may be placed on both sides of the positive electrode layer (10), and a negative electrode layer (20) may be placed on the outside of these solid electrolyte layers (30) to form an all-solid-state secondary battery (1).

[0075] In the case of an all-solid-state secondary battery (1) with such a configuration, a conductive layer (13) may be installed between the positive current collector (11) and the positive active material layer (12). This conductive layer (13) does not necessarily have to be formed on both sides of the positive current collector (11), and as shown in FIG. 3, the conductive layer (13) may be formed on one side of the positive current collector (11). Additionally, the positive active material layer (12) and / or the conductive layer (13) of this all-solid-state secondary battery (1) may contain an endothermic material.

[0076] Although preferred embodiments of the present invention have been described in detail above with reference to the attached drawings, the present invention is not limited to these examples.

[0077] It is clear to those skilled in the art to which the present invention pertains that various modifications or variations can be made within the scope of the technical concept described in the claims, and these are also naturally understood to fall within the technical scope of the present invention.

[0078] The following describes embodiments of the all-solid-state secondary battery according to the present invention in more detail, but the present invention is not limited to these embodiments.

[0079] (Example 1)

[0080] [Formation of the bipolar layer]

[0081] LiNi as a positive electrode active material 0.8 Co 0.15 Al 0.05O2(NCA) ternary powder, Li2S-P2S5 (80:20 mol%) amorphous powder as a sulfide-based solid electrolyte, and vapor-grown carbon fiber powder as a positive electrode conductive material (conductivity aid) are weighed in a weight ratio of 60:35:5 and mixed using a rotating mixer. Additionally, 5 parts by weight of lithium carbonate are weighed for every 100 parts by weight of this mixture and added to the mixture, then mixed using a rotating mixer. Subsequently, a dehydrated xylene solution in which SBR is dissolved is added as a binder so that it is 5.0% by weight relative to the total weight of the mixture containing the endothermic material, thereby producing a primary mixture. Since the solid components excluding solvents such as the dehydrated xylene solution in this primary mixture will have the same mass as the positive electrode active material layer, the positive electrode active material layer in this embodiment will contain 4.5% by weight of the endothermic material (lithium carbonate) relative to the entire positive electrode active material layer.

[0082] In addition, a second mixture is produced by adding an appropriate amount of dehydrated xylene for viscosity adjustment to this first mixture. Furthermore, to improve the dispersibility of the mixture, zirconia balls with a diameter of 5 mm are introduced into the second mixture such that the space, the mixture, and the zirconia balls each occupy 1 / 3 of the total volume of the mixing container. The third mixture produced by this is introduced into a rotating mixer and stirred at 3000 rpm for 3 minutes to produce an anode active material layer coating solution.

[0083] Next, an aluminum foil current collector with a thickness of 20 μm was prepared as the positive current collector, the positive current collector was mounted on a desktop screen printer, and a positive active material layer coating solution was applied onto a sheet using a metal mask with a diameter of 2.0 cm × 2.0 cm and a thickness of 150 μm. After that, the sheet coated with the positive active material layer coating solution was dried on a hot plate at 60°C for 30 minutes, and then vacuum dried at 80°C for 12 hours. Accordingly, a positive active material layer was formed on the positive current collector. The total thickness of the positive current collector and the positive active material layer after drying was approximately 165 μm.

[0084] [Formation of the cathode layer]

[0085] Graphite powder (vacuum dried at 80°C for 24 hours) as the negative electrode active material and PVDF as a binder are weighed in a weight ratio of 95.0:5.0. Then, this material and an appropriate amount of N-methyl-2-pyrrolidone (hereinafter NMP) are fed into a rotating mixer, stirred at 3000 rpm for 3 minutes, and then degassed for 1 minute to produce a negative electrode active material layer coating solution. Next, a copper foil current collector with a thickness of 16 μm is prepared as a negative electrode current collector, and the negative electrode active material layer coating solution is applied onto the copper foil current collector using a blade. The thickness of the negative electrode active material layer coating solution on the copper foil current collector is approximately 150 μm. The sheet coated with the negative electrode active material layer coating solution is placed in a dryer heated to 80°C and dried for 15 minutes. Additionally, the sheet after drying is vacuum dried at 80°C for 24 hours. Accordingly, a negative electrode layer is produced. The thickness of the cathode layer is approximately 140 μm.

[0086] [Formation of Solid Electrolyte Layer]

[0087] A primary mixture is prepared by adding a dehydrated xylene solution in which SBR is dissolved to Li2S-P2S5 (80:20, molar ratio) amorphous powder as a sulfide-based solid electrolyte, such that the SBR content is 2.0 wt% relative to the total weight of the mixture. Additionally, a secondary mixture is prepared by adding an appropriate amount of dehydrated xylene to the primary mixture to adjust the viscosity. Furthermore, to improve the dispersibility of the mixture, zirconia balls with a diameter of 5 mm are introduced into the secondary mixture such that the space, the mixture, and the zirconia balls each occupy 1 / 3 of the total volume of the mixing container. The tertiary mixture produced by this process is introduced into a rotating mixer and stirred at 3000 rpm for 3 minutes to produce an electrolyte layer coating solution. A cathode layer is mounted on a desktop screen printer, and the electrolyte layer coating solution is applied onto the cathode active material layer using a 500 μm metal mask. After that, the sheet coated with the electrolyte layer solution is dried on a hot plate at 40°C for 10 minutes, and then vacuum dried at 40°C for 12 hours. Accordingly, a solid electrolyte layer is formed on the cathode layer. The total thickness of the solid electrolyte layer after drying is approximately 300 μm.

[0088] [Creation of All-Solid State Batteries]

[0089] A sheet composed of a negative electrode layer and a solid electrolyte layer is cut into 3.5 cm × 3.5 cm and an anode layer into 3.0 cm × 3.0 cm using a Thomson blade, and these are bonded together by a dry lamination method using a roll press with a roll thickness of 150 μm to produce a single cell of an all-solid-state battery. The layer thickness of the single cell is approximately 400 μm.

[0090] [Encapsulation of All-Solid State Batteries]

[0091] The generated single cell is placed in an aluminum laminate film equipped with terminals, vacuumed to 100 Pa using a vacuum pump, and then packed by heat sealing. The total thickness of the all-solid-state battery is approximately 600 μm.

[0092] [Battery Characteristics Evaluation]

[0093] The capacity (mAh) of a single cell is measured using a charge / discharge evaluation device (TOSCAT-3100) manufactured by Toyo System. The charge / discharge is performed under conditions of 60°C. The cell is charged to 4.20V with a current of 0.1mA and discharged to 2.50V with a current of 0.1mA to determine the capacity of the single cell.

[0094] [Heating Test]

[0095] After charging the all-solid-state battery to 4.20V, it is stored in a constant temperature bath at 80°C for 24 hours. The change in thickness of the battery is measured before and after storage. In the case of the type of battery enclosed in a laminated bag as described in this embodiment, the ratio of change in thickness represents the ratio of change in the total volume of the battery.

[0096] [DSC Test]

[0097] The battery is charged to 4.20V, and a sample for DSC is prepared in a glove box in an Ar atmosphere in the following order. A single cell is removed from the outer laminated bag and a hole of φ 2.5mm is made in a mold. It is placed in a SUS sample pan, a cover is set, and the opening is sealed by joining with a press machine. The sample for DSC prepared in this way is measured using a DSC measuring device (DSC7000X) manufactured by Hitachi High-Tech Science. Measurements are taken from room temperature to 500℃, and the cumulative heat capacity is estimated. When the cumulative heat capacity of Comparative Example 1 is set to 100%, the ratio of change in cumulative heat capacity in each evaluation example is estimated as the reduction rate.

[0098] (Example 2)

[0099] In the formation of the positive electrode layer, the amount of lithium carbonate added to the positive electrode active material layer is 10 parts by weight per 100 parts by weight of the mixture forming the positive electrode active material layer, except that it is the same as Example 1.

[0100] (Example 3)

[0101] In the formation of the positive electrode layer, the amount of lithium carbonate added to the positive electrode active material layer is 1 part by weight per 100 parts by weight of the mixture forming the positive electrode active material layer, except that it is the same as Example 1.

[0102] (Example 4)

[0103] In the formation of the anode layer, the amount of lithium carbonate added to the anode layer is 25 parts by weight per 100 parts by weight of the mixture forming the anode active material layer, except that it is the same as Example 1.

[0104] (Example 5)

[0105] In the formation of the anode layer, lithium carbonate is not added to the anode active material layer, but is added to the conductive layer formed between the anode current collector and the anode active material layer. A specific manufacturing method is described below. Acetylene black, lithium carbonate, and acid-modified PVDF are weighed in a weight ratio of 30:40:30 as the conductive material of the conductive layer and as a binder, respectively. Then, these materials and an appropriate amount of NMP are fed into a rotating mixer and stirred at 3000 rpm for 5 minutes to produce a conductive layer coating solution. Subsequently, an aluminum foil with a thickness of 20 μm is mounted on a desktop screen printer, and the conductive layer coating solution is applied onto the aluminum foil using a 400 mesh screen. Afterward, the aluminum foil coated with the conductive layer coating solution is vacuum dried at 80°C for 12 hours. Accordingly, a conductive layer is formed over the anode current collector. The thickness of the conductive layer after drying is 15 μm. This conductive layer is adjusted so that the lithium carbonate content in the conductive layer is 5 parts by weight per 100 parts by weight of the mixture forming the positive electrode active material layer. A positive electrode layer is formed by applying a positive electrode active material layer coating solution, which is the same as in Example 1 except that it does not contain lithium carbonate, onto the conductive layer formed in this way and drying it. The sequence after the formation of the negative electrode layer is the same as in Example 1.

[0106] (Example 6)

[0107] The conductive layer is the same as Example 5, except that the content of lithium carbonate in the conductive layer is adjusted to 25 parts by weight per 100 parts by weight of the mixture forming the positive electrode active material layer.

[0108] (Example 7)

[0109] The process of forming the anode layer is the same as Example 5, except that the anode active material layer coating solution is applied and dried on the side opposite to the side where the conductive layer of the anode current collector is formed.

[0110] (Example 8)

[0111] The conductive layer is the same as Example 7, except that the content of lithium carbonate in the conductive layer is adjusted to 25 parts by weight per 100 parts by weight of the mixture forming the positive active material layer.

[0112] (Example 9)

[0113] The formation of the anode layer is the same as Example 1, except that aluminum hydroxide is contained in the anode active material layer instead of lithium carbonate.

[0114] (Example 10)

[0115] In the formation of the anode layer, the content of aluminum hydroxide in the anode active material layer is 10 parts by weight per 100 parts by weight of the mixture forming the anode active material layer, except that it is the same as Example 9.

[0116] (Example 11)

[0117] In the formation of the anode layer, the content of aluminum hydroxide in the anode active material layer is 1 part by weight per 100 parts by weight of the mixture forming the anode active material layer, except that it is the same as Example 9.

[0118] (Comparative Example 1)

[0119] In the formation of the anode layer, it is the same as Example 1 except that lithium carbonate is not added to the anode active material layer.

[0120] (Comparative Example 2)

[0121] The method is the same as Example 1, except that lithium carbonate is not contained in the positive active material layer, and in the formation of the negative active material layer, 5 parts by weight (i.e., the same amount as used in Example 1) of lithium carbonate is contained in the negative active material layer per 100 parts by weight of the mixture forming the positive active material layer.

[0122] (Comparative Example 3)

[0123] The method is the same as Example 1, except that lithium carbonate is not contained in the positive active material layer, and in the formation of the solid electrolyte layer, 5 parts by weight of lithium carbonate (i.e., the same amount as used in Example 1) is contained in the solid electrolyte layer per 100 parts by weight of the mixture forming the positive active material layer.

[0124] (Comparative Example 4)

[0125] It is the same as Comparative Example 2, except that aluminum hydroxide is contained in the negative electrode active material layer instead of lithium carbonate.

[0126] (Comparative Example 5)

[0127] It is the same as Comparative Example 3, except that aluminum hydroxide is contained in the solid electrolyte layer instead of lithium carbonate.

[0128] (Comparative Example 6)

[0129] In the formation of the positive electrode layer, the content of lithium carbonate in the positive electrode active material layer is 0.3 parts by weight per 100 parts by weight of the mixture forming the positive electrode active material layer, except that it is the same as Example 1.

[0130] (Reference Example 1)

[0131] This reference example involves incorporating an endothermic material into a secondary battery of a liquid system. Specific experimental methods are described below.

[0132] [Formation of the bipolar layer]

[0133] NCA ternary powder as a positive electrode active material and acetylene black as a conductivity aid are weighed and mixed in a weight ratio of 97:3. Additionally, 1 part by weight of lithium carbonate is weighed for every 100 parts by weight of the mixture and added to the mixture and mixed. Subsequently, an NMP solution in which PVdF is dissolved as a binder is added to the mixture such that the PVdF content is 3.0% by weight relative to the total weight of the mixture to produce a first mixture. Furthermore, a second mixture is produced by adding an appropriate amount of NMP to the first mixture to adjust the viscosity. The second mixture produced by this is fed into a rotating mixer and stirred at 2000 rpm for 3 minutes to produce a positive electrode active material layer coating liquid. Next, an aluminum foil current collector with a thickness of 20 μm is prepared as the positive current collector, the positive current collector is mounted on a desktop screen printer, and a positive active material layer coating liquid is applied onto a sheet using a metal mask with a diameter of 2.0 cm × 2.0 cm and a thickness of 150 μm. Afterward, the sheet coated with the positive active material layer coating liquid is dried on a hot plate at 100°C for 30 minutes, and then vacuum dried at 180°C for 12 hours. Accordingly, a positive active material layer is formed on the positive current collector. The total thickness of the positive current collector and the positive active material layer after drying is approximately 120 μm. Pressure molding is performed on the laminate formed in this way using a roll press machine to create a positive layer. A hole is punched in this positive layer using a 3.0 cm × 3.0 cm Thomson blade.

[0134] [Formation of the cathode layer]

[0135] Graphite powder (vacuum dried at 80°C for 24 hours) as the negative electrode active material and PVdF as a binder are weighed in a weight ratio of 95.0:5.0. Then, these materials and an appropriate amount of NMP are fed into a rotating mixer, stirred at 3000 rpm for 3 minutes, and then degassed for 1 minute to produce a negative electrode active material layer coating solution. Subsequently, a copper foil current collector with a thickness of 16 μm is prepared as the negative electrode current collector, and the negative electrode active material layer coating solution is applied onto the copper foil current collector using a blade. The thickness of the negative electrode active material layer coating solution on the copper foil current collector is approximately 150 μm. The sheet coated with the negative electrode active material layer coating solution is placed in a drying oven heated to 80°C and dried for 15 minutes. Furthermore, the sheet after drying is vacuum dried at 80°C for 24 hours. Accordingly, a negative electrode layer is produced. The thickness of the negative electrode layer is approximately 140 μm. Pressure molding is performed on the cathode layer using a roll press. A hole is punched in the cathode layer using a 3.5 cm × 3.5 cm Thomson blade.

[0136] [Production of Liquid System Lithium-ion Secondary Batteries]

[0137] A porous polyethylene film (thickness 12 μm) is used as the separator. An electrode structure is manufactured by placing the separator between the positive and negative electrode layers. This electrode structure is placed into an aluminum laminate film equipped with terminals. Lithium hexafluorophosphate (LiPF6) is dissolved to a concentration of 1.3 mol / L in a non-aqueous solvent in which ethylene carbonate and dimethyl carbonate are mixed in a volume ratio of 3:7 to prepare an electrolyte. The prepared electrolyte is injected into the aluminum laminate film to impregnate the separator. After vacuuming to 100 Pa using a vacuum pump, heat sealing is performed and the battery is packed. Accordingly, a liquid system lithium-ion secondary battery is produced.

[0138] The evaluation results of Examples 1 to 11, Comparative Examples 1 to 6, and Reference Examples described above are shown in Table 1 below.

[0139] Sample No. endothermic substances Layer containing endothermic substances Content of endothermic substance (parts by weight) Cell capacity (mAh) Change in thickness after storage at 80℃ DSC heating value (J / cm2) Reduction rate (%) Example 1 lithium carbonate positive active material layer 5 20.3 0.6 53748 17% Example 2 lithium carbonate positive active material layer 10 19.4 0.6 43094 33% Example 3 lithium carbonate positive active material layer 1 19.9 1.0 61145 5% Example 4 lithium carbonate positive active material layer 25 16.5 1.0 11135 83% Example 5 lithium carbonate Challenge stratification 5 19.8 0.4 52274 19% Example 6 lithium carbonate Challenge stratification 25 19.8 0.6 14225 78% Example 7 lithium carbonate Conductive layer on the back of the positive current collector 5 20.5 0.6 52177 19% Example 8 lithium carbonate Conductive layer on the back of the positive current collector 25 20.3 0.6 12890 80% Example 9 aluminum hydroxide positive active material layer 5 19.7 0.8 54800 15% Example 10 aluminum hydroxide positive active material layer 10 19.4 0.4 45199 30% Example 11 aluminum hydroxide positive active material layer 1 20.3 0.6 62481 3% Comparative Example 1 doesn't exist - - 19.8 0.6 64401 - Comparative Example 2 lithium carbonate cathode active material layer 5 19.8 0.6 64404 1% Comparative Example 3 lithium carbonate solid electrolyte layer 5 20.2 0.4 65244 -1% Comparative Example 4 aluminum hydroxide cathode active material layer 5 20.1 0.6 64998 -1% Comparative Example 5 aluminum hydroxide solid electrolyte layer 5 19.2 0.8 64744 -1% Comparative Example 6 lithium carbonate positive active material layer 0.3 19.4 0.4 63197 1% Reference Example 1 lithium carbonate positive active material layer 1 19.4 32 -

[0140] Meanwhile, the content of the endothermic material listed in Table 1 represents the amount of the endothermic material added per 100 parts by weight of the mixture for the positive electrode active material layer before the addition of the binder. Through the results of Table 1, it can be seen that Examples 1 to 11, in which the positive electrode layer contains at least 1 part by weight of lithium carbonate or aluminum hydroxide as an endothermic material per 100 parts by weight of the positive electrode active material layer, exhibit a clearly higher endothermic effect compared to Comparative Examples 1 to 6. Furthermore, it can be seen that the endothermic material can sufficiently exhibit an endothermic effect even when contained in the conductive layer of the positive electrode layer. Consequently, in Examples 1 to 11, it is possible to manufacture an all-solid-state secondary battery capable of sufficiently suppressing rapid heat generation.

[0141] In addition, it can be seen that if the content of the endothermic material contained in the anode layer is 30 parts by weight or less per 100 parts by weight of the anode active material layer, the charging capacity of the anode layer can be sufficiently maintained. On the other hand, although not described in the above-mentioned examples, when the endothermic material was contained in an amount of about 50 parts by weight per 100 parts by weight of the anode active material layer, the battery did not operate. This is thought to be due to the excessively high proportion of the endothermic material that does not contribute to lithium-ion conductivity or electron conductivity in the anode active material layer.

[0142] In the all-solid-state batteries of the examples and comparative examples described here, the change in thickness indicates a change in volume. As can be seen from the results in Table 1, when placed under an environment of 80°C, the change in thickness is less than 1% compared to the case at room temperature (25°C), indicating that there is almost no change. On the other hand, in the lithium-ion secondary battery of the liquid system of the reference example, even when the lithium carbonate content is 1 part by weight per 100 parts by weight of the positive electrode active material layer, it can be seen that the change in volume at 80°C is 32%, which is very large. From these results, it can be seen that in the secondary battery of the liquid system, the decomposition reaction of the endothermic material occurs vigorously even at a low temperature of about 80°C, whereas in the all-solid-state secondary battery according to the present invention, the endothermic effect is sufficiently exhibited even when the temperature becomes higher than 80°C, and the decomposition of the endothermic material is relatively slow up to a temperature of about 80°C, thereby suppressing deformation of the battery due to volume expansion. Explanation of the symbols

[0143] 1, 1a: All-solid-state secondary battery 10: Anode layer 11: Positive current collector 12: Positive active material layer 13: Challenge Stratum 20: Cathode layer 21: Cathode current collector 22: Cathode active material layer 30: Solid electrolyte layer

Claims

Claim 1 A solid-state secondary battery comprising a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein the positive electrode layer comprises a plate-shaped positive electrode current collector, a positive electrode active material layer located on the positive electrode current collector, and a conductive layer containing a conductive material, a binder, and a heat-absorbing material that absorbs heat through a decomposition reaction, wherein the conductive layer is disposed on at least one surface of the positive electrode current collector, wherein the content of the conductive material in the conductive layer is 6 wt% or more and 54 wt% or less, the content of the heat-absorbing material is 24 wt% or more and 81 wt% or less, and the content of the binder is 10 wt% or more and 40 wt% or less, wherein the content of the heat-absorbing material contained in the conductive layer is 1 wt% or more and 30 wt% or less when the total weight of the positive electrode active material layer is 100 wt%, and the heat-absorbing material is lithium carbonate. Claim 2 A solid-state secondary battery according to claim 1, wherein the conductive layer is disposed between the positive current collector and the positive active material layer, disposed on one side of the positive current collector where the positive active material layer is not located, or disposed on both of these. Claim 3 delete Claim 4 delete Claim 5 delete Claim 6 A solid-state secondary battery according to claim 1, wherein the solid electrolyte layer contains a sulfide-based solid electrolyte. Claim 7 A solid-state secondary battery according to claim 1, further comprising an outer body that accommodates the anode layer, the cathode layer, and the solid electrolyte layer inside, wherein the outer body is of the film type. Claim 8 In claim 7, an all-solid-state secondary battery in which the difference between the volume inside the outer body at 80°C and the volume at 25°C is within 5% of the volume at 25°C.

Citation Information

Patent Citations

  • Positive electrode, power storage device and method for manufacturing positive electrode

    JP2015219999A

  • All-solid battery

    JP2018116810A

  • Coated active material and lithium solid state battery

    US20140087270A1