Additive for rechargeable lithium battery, electrolyte including same and rechargeable lithium battery
A polymer shell with a melting point of 90°C to 120°C, surrounding a foaming agent, addresses the thermal stability and safety issues in lithium-ion batteries by preventing short circuits and maintaining resistance, thereby enhancing battery performance.
Patent Information
- Application Number
- KR1020220133893
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-10-18
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-10-18
AI Technical Summary
Lithium-ion batteries face issues with thermal stability and safety, particularly due to the decomposition of LiPF and the subsequent formation of Li2O, which can lead to the formation of Li2O, which can result in high-temperature performance degradation and vulnerability to safety issues.
The use of a polymer shell with a melting point of 90°C to 120°C, which surrounds a foaming agent, effectively prevents the decomposition of LiPF6 by releasing the foaming agent at high temperatures, thereby preventing short circuits and maintaining battery resistance.
The polymer shell effectively suppresses short circuits and maintains battery resistance, ensuring improved thermal stability and safety by releasing the foaming agent at high temperatures, thus enhancing the battery's safety and performance.
Smart Images

Figure 112022109532277-PAT00003_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to an additive for a lithium secondary battery, an electrolyte for a lithium secondary battery containing the same, and a lithium secondary battery. Background Technology
[0002] Lithium secondary batteries are rechargeable and have an energy density more than three times higher per unit weight than conventional lead-acid batteries, nickel-cadmium batteries, nickel-hydrogen batteries, and nickel-zinc batteries, and can be fast-charged. As a result, they are being commercialized for laptops, mobile phones, power tools, and electric bicycles, and research and development to further improve energy density is actively underway.
[0003] These lithium secondary batteries are used by injecting an electrolyte into a battery cell comprising a positive electrode containing a positive electrode active material capable of intercalating and deintercalating lithium, and a negative electrode containing a negative electrode active material capable of intercalating and deintercalating lithium.
[0004] In particular, the electrolyte uses an organic solvent in which lithium salts are dissolved, and this electrolyte is important in determining the stability and performance of the lithium secondary battery.
[0005] LiPF6, which is the most widely used lithium salt in electrolytes, has the problem of reacting with the organic solvent in the electrolyte to accelerate solvent depletion and generate a large amount of gas. When LiPF6 decomposes, it produces LiF and PF5, which causes electrolyte depletion in the battery and results in high-temperature performance degradation and vulnerability to safety issues.
[0006] Accordingly, there is a demand for an electrolyte with improved safety that does not degrade in performance even under high-temperature conditions. The problem to be solved
[0007] One embodiment provides an additive for a lithium secondary battery with improved thermal stability.
[0008] Another embodiment provides an electrolyte for a lithium secondary battery with improved lifespan characteristics, high-temperature safety, and high-temperature reliability by applying the above additive.
[0009] Another embodiment provides a lithium secondary battery comprising the above-mentioned electrolyte for the lithium secondary battery. means of solving the problem
[0010] An additive for a lithium secondary battery according to one embodiment comprises a core containing a foaming agent and a shell surrounding the core, wherein the shell comprises a polymer having a melting point of 90°C to 120°C.
[0011] The ratio of the thickness of the core to the thickness of the shell may be 1:1 to 4:1.
[0012] The core may have a thickness of 0.1㎛ to 2.0㎛, and the shell may have a thickness of 0.025㎛ to 0.5㎛.
[0013] The above blowing agent may include a glass blowing agent, a hydrocarbon compound, a hydrofluoroolefin (HFO) compound, or a combination thereof.
[0014] The above glass foaming agent may include silicon dioxide, sodium oxide, and water.
[0015] The glass foaming agent may comprise 60% to 70% by weight of silicon dioxide, 20% to 30% by weight of sodium oxide, and 5% to 20% by weight of water.
[0016] The above polymer may include poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), polyacrylic acid, polyethylene, poly(methyl methacrylate), polyalkylene oxide, polyalkylene succinate, or a combination thereof.
[0017] The above additive may be in the form of fibers formed using electrospinning.
[0018] According to another embodiment, an electrolyte for a lithium secondary battery is provided, comprising a non-aqueous organic solvent, a lithium salt, and the aforementioned additive for a lithium secondary battery.
[0019] The above-mentioned additive for a lithium secondary battery may be included in an amount of 0.1% to 10% by weight, 0.1% to 5.0% by weight, or 0.1% to 3.0% by weight based on the total weight of the electrolyte for the lithium secondary battery.
[0020] According to another embodiment, a lithium secondary battery is provided comprising: a positive electrode including a positive active material; a negative electrode including a negative active material; and the aforementioned electrolyte. Effects of the invention
[0021] The above-mentioned additive for lithium secondary batteries has excellent electrolyte impregnation properties and can maintain battery characteristics without an increase in battery resistance when applied to the electrolyte.
[0022] In addition, a lithium secondary battery containing an additive for a lithium secondary battery according to one embodiment suppresses the occurrence of a short circuit due to an increase in resistance above the battery operating temperature, and the safety of the battery can be improved. Brief explanation of the drawing
[0023] FIG. 1 is a cross-sectional view of an additive according to one embodiment. FIG. 2 is a schematic diagram illustrating a lithium secondary battery according to one embodiment. Specific details for implementing the invention
[0024] The following embodiments are described in detail so that those skilled in the art can easily implement them. However, the structure actually applied may be implemented in various different forms and is not limited to the embodiments described herein.
[0025] The thickness was enlarged in the drawing to clearly represent various layers and regions.
[0026] When a part such as a layer, membrane, region, or plate is said to be "on" another part, this includes not only the case where it is "directly on" the other part, but also the case where there is another part in between. Conversely, when a part is said to be "directly on" another part, it means that there is no other part in between.
[0027] In this specification, “at least one of A, B, or C”, “one of A, B, C, or a combination thereof”, and “one of A, B, C, and a combination thereof” mean each component and all combinations thereof (e.g., A; B; A and B; A and C; B and C; or A, B, and C).
[0028] In the following, "combination" includes two or more mixtures, mutual substitutions, and two or more stacked structures.
[0029] An additive for a lithium secondary battery according to one embodiment is described below with reference to FIG. 1.
[0030] FIG. 1 is a cross-sectional view of an additive according to one embodiment.
[0031] Referring to FIG. 1, an additive (1) according to one embodiment comprises a core (3) and a shell (5) surrounding the core (3). The core (3) comprises a foaming agent, and the shell (5) comprises a polymer having a melting point of 90°C to 120°C.
[0032] The above additive (1) does not increase the resistance of the battery when the battery is operated, thereby maintaining the battery characteristics. Since the melting point of the shell (5) has the above range, the shell (5) can be properly melted at high temperatures, and the foaming agent of the core (3) can be released in time, effectively suppressing the occurrence of a short circuit in the battery. In addition, since the core (3) contains a foaming agent, when the shell (5) of the additive melts at high temperatures, the foaming agent is released to the outside of the core (3) and swells, increasing the resistance of the battery and causing a voltage drop, thereby suppressing the occurrence of a short circuit in the battery.
[0033] The ratio of the thickness of the core (3) to the thickness of the shell (5) may be 1:1 to 4:1, for example 3:2, for example 2:1, for example 5:2, for example 3:1, and is not limited to these.
[0034] When the thickness ratio of the core (3) and the shell (5) is within the above range, the time required for the melting of the shell (5) and the release of the core material can be adjusted to an appropriate range, and the occurrence of electrode short circuits in high-temperature conditions can be effectively controlled. In addition, when the temperature is not high, the shell (5) is not easily damaged, thereby preventing unnecessary increase in battery resistance and deterioration of battery characteristics.
[0035] When the additive comprising the core (3) and shell (5) is in the form of a fiber, the “thickness of the core” refers to the straight-line length of a line segment extending from the center of the circle representing the cross-section of the fiber to a point on the circumference of the core, and the “thickness of the shell” refers to the straight-line length between the point where the line segment extending from the center of the circle representing the cross-section of the fiber to a point on the circumference of the shell meets the circumference of the core and the point where the line segment meets the circumference of the shell.
[0036] When the additive comprising the core (3) and shell (5) is spherical, the “thickness of the core” refers to the length of a line segment extending from the center of the sphere to a point on the surface of the core, and the “thickness of the shell” refers to the length between the point where the line segment extending from the center of the sphere to a point on the surface of the shell meets the surface of the core and the point where the line segment meets the surface of the shell.
[0037] The thickness of the core (3) may be 0.1㎛ to 2.0㎛, for example, 0.1㎛ to 1.5㎛, for example, 0.1㎛ to 1.2㎛, for example, 0.1㎛ to 1.0㎛, for example, 0.3㎛ to 2㎛, for example, 0.3㎛ to 1.5㎛, for example, 0.3㎛ to 1.2㎛, for example, 0.5㎛ to 1.0㎛, and is not limited thereto.
[0038] By having the core (3) have a thickness within the above range, the core material is released along with the melting of the shell (5) at the right time, thereby effectively controlling the occurrence of electrode short circuits, while simultaneously maintaining battery characteristics without reducing electrolyte impregnation and unnecessarily increasing battery resistance.
[0039] The blowing agent included in the core (3) may be a commonly used blowing agent, for example, a glass blowing agent, a hydrocarbon compound, a hydrofluoroolefin (HFO) compound, or a combination thereof.
[0040] The glass blowing agent may include silicon dioxide, sodium oxide, and water. The silicon dioxide may be included in an amount of 60% to 70% by weight, for example, 65% by weight, based on 100% by weight of the glass blowing agent, but is not limited thereto. The sodium oxide may be included in an amount of 20% to 30% by weight, for example, 25% by weight, based on 100% by weight of the glass blowing agent, but is not limited thereto. The water is the remaining component in the glass blowing agent excluding silicon dioxide and sodium oxide, and may be included in an amount of, for example, 5% to 20% by weight, for example, 10% by weight, but is not limited thereto.
[0041] The above hydrocarbon compound may include a hydrocarbon having 1 to 6 carbon atoms, and may include, for example, a chlorinated hydrocarbon compound, a non-chlorinated hydrocarbon compound, or a combination thereof.
[0042] The above hydrocarbon compound may include at least one selected from dichloroethane, propyl chloride, isopropyl chloride, butyl chloride, isobutyl chloride, pentyl chloride, isopentyl chloride, n-butane, isobutane, n-pentane, isopentane, cyclopentane, n-hexane, and combinations thereof, but is not limited thereto.
[0043] The above hydrofluoroolefin compound may include, for example, a chlorinated hydrofluoroolefin compound, a non-chlorinated hydrofluoroolefin compound, or all of these.
[0044] The above hydrofluoroolefin compounds may be of types known in the art, for example, trans 1-chloro-3,3,3-trifluoropropene (trans CF3CH=CClH), cis 1-chloro-3,3,3-trifluoropropene (cis CF3CH=CClH), trans 1-chloro-2,3,3-trifluoropropene (trans CHF2CF=CClH), cis 1-chloro-2,3,3-trifluoropropene (cis CHF2CF=CClH), trans 1-chloro-1,3,3-trifluoropropene (trans CHF2CH=CClF), cis 1-chloro-1,3,3-trifluoropropene (cis CHF2CH=CClF), trans 2-chloro-1,3,3-trifluoropropene (trans CHF2CCl=CHF), cis 2-chloro-1,3,3-trifluoropropene (cis CHF2CCl=CHF), trans 2-chloro-1,1,3-trifluoropropene (trans CH2FCCl=CF2), cis 2-chloro-1,1,3-trifluoropropene (cis CH2FCCl=CF2), trans 3-chloro-1,2,3-trifluoropropene (trans CHFClCF=CFH), cis 3-chloro-1,2,3-trifluoropropene (cis CHFClCF=CFH), trans 3-chloro-1,1,2-trifluoropropene (trans CH2ClCF=CF2), cis 3-chloro-1,1,2-trifluoropropene (cis CH2ClCF=CF2), trans 3-chloro-2,3,3-trifluoropropene (trans CF2ClCF=CH2), cis 3-chloro-2,3,3-trifluoropropene (cis Monochlorotrifluoropropene such as CF2ClCF=CH2); trifluoropropene such as 2,3,3-trifluoropropene (CHF2CF=CH2), 1,1,2-trifluoropropene (CH3CF=CF2), 1,1,3-trifluoropropene (CH2FCH=CF2), and 1,3,3-trifluoropropene (CHF2CH=CHF);Tetrafluoropropenes such as 1,2,3,3-tetrafluoro-1-propene, 2,3,3,3-tetrafluoro-1-propene, 1,3,3,3-tetrafluoro-1-propene, 1,1,2,3-tetrafluoro-1-propene, 1,1,3,3-tetrafluoro-1-propene, 1,2,3,3-tetrafluoro-1-propene; pentafluoropropenes such as 1,2,3,3,3-pentafluoro-1-propene, 1,1,3,3,3-pentafluoro-1-propene, 1,1,2,3,3-pentafluoro-1-propene; It may include at least one selected from hexafluorobutenes such as 2,3,3,4,4,4-hexafluoro-1-butene, 1,1,1,4,4,4-hexafluoro-2-butene, 1,3,3,4,4,4-hexafluoro-1-butene, 1,2,3,4,4,4-hexafluoro-1-butene, 1,2,3,3,4,4-hexafluoro-1-butene, 1,1,2,3,4,4-hexafluoro-2-butene, 1,1,1,2,3,4,4-hexafluoro-2-butene, 1,1,1,2,3,4,4-hexafluoro-2-butene, 1,1,1,2,3,4-hexafluoro-2-butene, 1,1,1,2,3,4,4-hexafluoro-1-butene, and combinations thereof.;
[0045] The thickness of the shell (5) may be 0.025㎛ to 0.5㎛, for example, 0.025㎛ to 0.45㎛, for example, 0.025㎛ to 0.4㎛, for example, 0.025㎛ to 0.35㎛, for example, 0.025㎛ to 0.3㎛, for example, 0.05㎛ to 0.5㎛, for example, 0.1㎛ to 0.5㎛, for example, 0.15㎛ to 0.5㎛, for example, 0.2㎛ to 0.5㎛, for example, 0.2㎛ to 0.45㎛, for example, 0.2㎛ to 0.4㎛, and is not limited thereto.
[0046] By having the shell (5) have a thickness within the above range, the occurrence of electrode short circuits can be effectively controlled by the timely melting of the shell (5) and release of the core material, while simultaneously maintaining battery characteristics by not unnecessarily increasing the battery resistance. In one embodiment, the shell (5) may include a polymer having a melting point of 90°C to 120°C, for example, the polymer may be a thermoplastic resin. Such a polymer has excellent ion conductivity and can melt at a specific temperature while remaining stable within the operating temperature range of the battery, thus contributing to the safety of the battery. In addition, the polymer included in the shell (5) can improve the wettability of the electrolyte.
[0047] For example, the thermoplastic resin may be poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), polyacrylic acid, polyethylene, poly(methyl methacrylate), polyalkylene oxide, polyalkylene succinate, or a combination thereof, and may be, for example, poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), poly(vinylidene fluoride-hexafluoropropylene)), polyalkylene oxide, polyalkylene succinate, or a combination thereof, but is not limited thereto.
[0048] The above polyalkylene oxide may be polyethylene oxide, polypropylene oxide, polybutylene oxide, polypentylene oxide, polyhexylene oxide, polyheptylene oxide, etc., and may be, for example, polyethylene oxide, polypropylene oxide, or polybutylene oxide, etc., and may be, for example, polyethylene oxide, polypropylene oxide, etc., but is not limited thereto.
[0049] The above polyalkylene succinate may be polyethylene succinate, polypropylene succinate, polybutylene succinate, polypentylene succinate, polyhexylene succinate, polyheptylene succinate, or polyoxylene succinate, etc., and may be, for example, polyethylene succinate, polypropylene succinate, or polybutylene succinate, etc., and may be, for example, polybutylene succinate, etc., but is not limited thereto.
[0050] The polymer included in the shell (5) may have a melting point of 90°C to 120°C, for example, the melting point of the polymer may be 90°C or higher, for example, 95°C or higher, for example, 100°C or higher, for example, the melting point of the polymer may be 120°C or lower, for example, 115°C or lower, for example, 110°C or lower, and is not limited thereto. By having the melting point of the polymer included in the shell (5) within the above range, the shell (5) is maintained stably within the operating temperature range during charging and discharging of the battery, so as not to increase the resistance of the battery, and the shell (5) can be properly melted at a high temperature of 100°C or higher, and the foaming agent of the core (3) is released in time so as to effectively suppress the occurrence of a short circuit in the battery.
[0051] The additive (1) may be in the form of a fiber formed by electrospinning, i.e., a fiber. When the additive is in the form of a fiber, the core material is effectively leached at high temperatures, and the battery resistance is rapidly increased, thereby effectively suppressing the short circuit phenomenon of the battery. In addition to the fiber form, the additive (1) may have a structure including a core (3) and a shell (5) surrounding it, and may be in the form of an amorphous, plate-like, spherical shape, etc., but is not limited to these.
[0052] When manufacturing the core-shell structured additive (1), the electrospinning process can be carried out by a known process taking into account the melting temperature of the foaming agent and the thermoplastic resin.
[0053] An electrolyte for a lithium secondary battery according to another embodiment comprises a non-aqueous organic solvent, a lithium salt, and the aforementioned additive.
[0054] The above additive (1) may be included in an amount of 0.1% to 10% by weight based on the total weight of the electrolyte for a lithium secondary battery. For example, the above additive may be included in an amount of 0.2% or more by weight based on the total weight of the electrolyte for a lithium secondary battery, for example, 0.3% or more by weight, 0.4% or more by weight, 0.5% or more by weight, 0.6% or more by weight, 0.7% or more by weight, 0.8% or more by weight, 0.9% or more by weight, or 1% or more by weight and 9.0% or less by weight, for example, 8.0% or less by weight, 7.0% or less by weight, 6.0% or less by weight, 5.0% or less by weight, 4.0% or less by weight, or 3.0% or less by weight, but is not limited thereto.
[0055] When the content of the additive (1) is within the above range, there is no increase in battery resistance at the battery operating temperature, thereby maintaining battery characteristics, and at temperatures above the battery operating temperature, the battery resistance is increased, thereby enabling the realization of a lithium secondary battery with improved safety.
[0056] The above-mentioned non-aqueous organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can move.
[0057] The above-mentioned non-aqueous organic solvent may be a carbonate-based, ester-based, ether-based, ketone-based, alcohol-based, or aprotic solvent.
[0058] The above carbonate-based solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. The above ester-based solvents may include methyl acetate, ethyl acetate, n-propyl acetate, t-butyl acetate, methylpropionate, ethylpropionate, propylpropionate, decanolide, mevalonolactone, caprolactone, etc. The above ether-based solvents may include dibutyl ether, tetraglame, deglame, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc. In addition, cyclohexanone, etc. may be used as the ketone-based solvent. In addition, ethyl alcohol, isopropyl alcohol, etc. may be used as the alcohol-based solvent, and as the aprotic solvent, nitriles such as R-CN (where R is a hydrocarbon group having 2 to 20 carbon atoms in a straight, branched, or ring structure and may include a double bond, a ring, or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, sulfolanes, etc. may be used.
[0059] The above-mentioned non-aqueous organic solvents may be used alone or in a mixture of one or more. When used in a mixture of one or more, the mixing ratio can be appropriately adjusted according to the desired battery performance, which is widely understood by those working in the field.
[0060] In addition, for the above carbonate-based solvent, it is preferable to use a mixture of cyclic carbonates and chain carbonates. In this case, using a mixture of cyclic carbonates and chain carbonates in a volume ratio of 1:1 to 1:9 can result in excellent performance of the electrolyte.
[0061] The above-mentioned non-aqueous organic solvent may further include an aromatic hydrocarbon organic solvent in addition to the carbonate-based solvent. In this case, the carbonate-based solvent and the aromatic hydrocarbon solvent may be mixed in a volume ratio of 1:1 to 30:1.
[0062] As the above aromatic hydrocarbon solvent, an aromatic hydrocarbon compound of the following chemical formula 1 may be used.
[0063] [Chemical Formula 1]
[0064]
[0065] In the above chemical formula 1, R 201 to R 206 The groups may be identical or different from each other and may be hydrogen, halogen, alkyl groups having 1 to 10 carbon atoms, haloalkyl groups, or a combination thereof.
[0066] Specific examples of the above aromatic hydrocarbon solvents include benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorotoluene, 2,3-difluorotoluene, 2,4-difluorotoluene. 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, and combinations thereof are selected.
[0067] The above electrolyte may further include vinylene carbonate, vinyl ethylene carbonate, or an ethylene-based carbonate compound of the following chemical formula 2 as a life-enhancing additive to improve battery life.
[0068] [Chemical Formula 2]
[0069]
[0070] In the above chemical formula 2, R 207 and R 208 The groups are identical or different from each other and are selected from hydrogen, halogen groups, cyano groups (CN), nitro groups (NO2), or fluorinated C1 to C5 alkyl groups, and the R 207 and R 208 At least one of the following is selected from a halogen group, a cyano group (CN), a nitro group (NO2), and a fluorinated alkyl group having 1 to 5 carbon atoms, provided that R207 and R 208 Not all of it is hydrogen.
[0071] Representative examples of the above-mentioned ethylene-based carbonate compounds include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, or fluoroethylene carbonate. When using more of these lifespan-enhancing additives, the amount used can be appropriately controlled.
[0072] The above lithium salt is a material that is dissolved in a non-aqueous organic solvent and acts as a source of lithium ions within the battery, enabling the operation of a basic lithium secondary battery and facilitating the movement of lithium ions between the positive and negative electrodes.
[0073] Representative examples of the above lithium salts include LiPF6, LiBF4, LiDFOP, LiDFOB, LiPO2F2, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide (LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2)(where x and y are natural numbers, for example, integers from 1 to 20), LiCl, LiI, or LiB(C2O4)2 (one or more selected from lithium bis(oxalato) borate (LiBOB).
[0074] It is preferable to use a lithium salt concentration within the range of 0.1M to 2.0M. When the lithium salt concentration falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0075] The above additives and electrolytes can be applied to lithium secondary batteries.
[0076] A lithium secondary battery according to one embodiment will be described below with reference to FIG. 2.
[0077] A lithium secondary battery according to one embodiment comprises a positive electrode (114) comprising a positive electrode active material; a negative electrode (112) comprising a negative electrode active material; and the aforementioned electrolyte.
[0078] Lithium secondary batteries can be classified into lithium-ion batteries, lithium-ion polymer batteries, and lithium polymer batteries depending on the type of separator and electrolyte used; classified into cylindrical, prismatic, coin, and pouch types depending on their shape; and divided into bulk and thin-film types depending on their size. Since the structures and manufacturing methods of these batteries are widely known in this field, a detailed description is omitted.
[0079] Here, a cylindrical lithium secondary battery is described as an example of a lithium secondary battery. FIG. 2 schematically illustrates the structure of a lithium secondary battery according to one embodiment. Referring to FIG. 2, a lithium secondary battery (100) according to one embodiment comprises a battery cell including a positive electrode (114), a negative electrode (112) positioned opposite the positive electrode (114), a separator (113) disposed between the positive electrode (114) and the negative electrode (112), and an electrolyte (not shown) impregnating the positive electrode (114), the negative electrode (112), and the separator (113); a battery container (120) containing the battery cell; and a sealing member (140) sealing the battery container (120). The positive electrode comprises a positive current collector and a positive active material layer positioned on the positive current collector, and the positive active material layer comprises a positive active material.
[0080] As the above-mentioned positive electrode active material, a compound capable of reversible intercalation and deintercalation of lithium (a lithated intercalation compound) may be used. Specifically, at least one type of composite oxide of lithium and a metal including cobalt, manganese, nickel, or a combination thereof may be used.
[0081] A composite oxide in which a portion of the metal is substituted with a metal other than another metal may be used, or at least one phosphate compound of the composite oxide selected from, for example, LiFePO4, LiCoPO4, or LiMnPO4 may be used, or a composite oxide having a coating layer on its surface may be used, or a composite oxide having a coating layer may be mixed and used. The coating layer may include at least one coating element compound selected from the oxide of the coating element, the hydroxide of the coating element, the oxyhydroxide of the coating element, the oxycarbonate of the coating element, or the hydroxycarbonate of the coating element. The compound forming the coating layer may be amorphous or crystalline. As the coating element included in the coating layer, Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof may be used. For the coating layer formation process, any coating method may be used as long as the above-mentioned compounds are coated using these elements in a manner that does not adversely affect the physical properties of the cathode active material (e.g., spray coating, immersion method, etc.). Since this is a matter that is well understood by those skilled in the field, a detailed explanation will be omitted.
[0082] The positive active material may be one or more of the lithium complex oxides represented by, for example, Chemical Formula 3 below.
[0083] [Chemical Formula 3]
[0084] Li x M 1 y M 2 z M 3 1-y-z O2
[0085] In the above chemical formula 3,
[0086] 0.5≤x≤1.8, 0 <y≤1, 0≤z≤1, 0≤y+z≤1, M 1 , M2 and M 3 Each may be independently selected from metals such as Ni, Co, Mn, Al, Sr, Mg, or La, and combinations thereof.
[0087] In one embodiment, the positive active material is LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi a Mn b Co c O2(a+b+c=1), LiNi a Mn b Co c Al d O2(a+b+c+d=1) or LiNi e Co f Al g It may be at least one type selected from O2(e+f+g=1).
[0088] For example, the above LiNi a Mn b Co c O2(a+b+c=1), LiNi a Mn b Co c Al d O2(a+b+c+d=1) and LiNi e Co f Al g The positive active material selected in O2(e+f+g=1) may be a high nickel (high Ni) based positive active material.
[0089] For example, the above LiNi a Mn b Co c O2(a+b+c=1) and LiNi a Mn b Co c Al d In the case of O2(a+b+c+d=1), the nickel content may be 60% or more (a ≥ 0.6), and more specifically, 80% or more (a ≥ 0.8).
[0090] For example, the above LiNi e Co f Al gIn the case of O2 (e+f+g=1), the nickel content may be 60% or more (e ≥ 0.6), and more specifically, 80% or more (e ≥ 0.8).
[0091] The content of the above positive active material may be 90% to 98% by weight based on the total weight of the positive active material layer.
[0092] The above positive active material layer may optionally include a conductive material and a binder. In this case, the content of the conductive material and the binder may each be 1.0 weight% to 5.0 weight% with respect to the total weight of the positive active material layer.
[0093] The above conductive material is used to impart conductivity to the positive electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or conductive materials including mixtures thereof.
[0094] The above binder serves to adhere the positive active material particles well to each other and also to adhere the positive active material well to the current collector. Representative examples include polyvinyl alcohol, carboxymethylcellulose, hydroxypropylcellulose, diacetylcellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited to these.
[0095] Al may be used as the anode current collector, but is not limited to these.
[0096] The above cathode includes a cathode active material layer comprising a cathode current collector and a cathode active material formed on the cathode current collector.
[0097] The above-mentioned negative electrode active material includes a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.
[0098] As a material capable of reversibly intercalating / deintercalating the above lithium ions, any carbon-based negative electrode active material commonly used in lithium secondary batteries can be used, and representative examples include crystalline carbon, amorphous carbon, or a combination thereof. Examples of the above crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the above amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0099] As the above lithium metal alloy, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn may be used.
[0100] Materials capable of doping and undoping the above lithium include Si, Si-C composites, SiOx (0 < x < 2), Si-Q alloys (wherein Q is an element selected from alkali metals, alkaline earth metals, group 13 elements, group 14 elements, group 15 elements, group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO2, Sn-R (wherein R is an element selected from alkali metals, alkaline earth metals, group 13 elements, group 14 elements, group 15 elements, group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), and at least one of these may also be mixed with SiO2.
[0101] As the above elements Q and R, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof may be used.
[0102] Examples of the above transition metal oxides include vanadium oxide, lithium vanadium oxide, or lithium titanium oxide.
[0103] In a specific embodiment, the cathode active material may be a Si-C composite comprising a Si-based active material and a carbon-based active material.
[0104] In the above Si-C composite, the average particle size of the Si-based active material may be 50 nm to 200 nm. When the average particle size of the Si-based active material falls within the above range, volume expansion occurring during charging and discharging can be suppressed, and the disruption of the conductive path due to particle fragmentation during charging and discharging can be prevented.
[0105] The above Si-based active material may be included in an amount of 1 to 60 weight% based on the total weight of the Si-C composite, for example, 3 It may be included in an amount of up to 60 weight%.
[0106] In another specific embodiment, the cathode active material may further include crystalline carbon together with the aforementioned Si-C composite.
[0107] When the above-mentioned cathode active material includes a Si-C composite and crystalline carbon together, the Si-C composite and crystalline carbon may be included in the form of a mixture, in which case the Si-C composite and crystalline carbon may be included in a weight ratio of 1:99 to 50:50. More specifically, the Si-C composite and crystalline carbon may be included in a weight ratio of 5:95 to 20:80.
[0108] The above crystalline carbon may include, for example, graphite, and more specifically, may include natural graphite, artificial graphite, or a mixture thereof.
[0109] The average particle size of the crystalline carbon above may be 5 μm to 30 μm.
[0110] In this specification, the average particle size may be the particle size (D50) at 50% by volume ratio in the cumulative size-distribution curve.
[0111] The above Si-C composite may further include a shell surrounding the surface of the Si-C composite, and the shell may include amorphous carbon. The amorphous carbon may include soft carbon, hard carbon, mesophase pitch carbide, calcined coke, or a mixture thereof.
[0112] The above amorphous carbon may be included in an amount of 1 to 50 parts by weight, for example, 5 to 50 parts by weight, or 10 to 50 parts by weight, per 100 parts by weight of carbon-based active material.
[0113] The content of the negative electrode active material in the above negative electrode active material layer may be 95% to 99% by weight with respect to the total weight of the negative electrode active material layer.
[0114] In one embodiment, the negative electrode active material layer comprises a binder and may optionally further comprise a conductive material. The content of the binder in the negative electrode active material layer may be 1% to 5% by weight based on the total weight of the negative electrode active material layer. Additionally, when further comprising a conductive material, the negative electrode active material may be used in an amount of 90% to 98% by weight, the binder in an amount of 1% to 5% by weight, and the conductive material in an amount of 1% to 5% by weight.
[0115] The above binder serves to effectively bond the negative electrode active material particles to each other and also to effectively bond the negative electrode active material to the current collector. As the binder, a water-insoluble binder, a water-soluble binder, or a combination thereof may be used.
[0116] Examples of the above-mentioned water-insoluble binders include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or combinations thereof.
[0117] Examples of the above water-soluble binders include rubber-based binders or polymer resin binders. The above rubber-based binder may be selected from styrene-butadiene rubber, acrylated styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, and combinations thereof. The above polymer resin binder may be selected from polytetrafluoroethylene, ethylene-propylene copolymer, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene-propylene-diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.
[0118] When a water-soluble binder is used as the above-mentioned cathode binder, a cellulose-based compound capable of imparting viscosity may be further included as a thickener. As the above-mentioned cellulose-based compound, one or more types such as carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, or alkali metal salts thereof may be mixed and used. As the above-mentioned alkali metal, Na, K, or Li may be used. The content of such thickener may be 0.1 to 3 parts by weight per 100 parts by weight of the cathode active material.
[0119] The above conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed. Examples include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fibers; metal-based materials such as metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or conductive materials including mixtures thereof.
[0120] As the above-mentioned cathode current collector, a material selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof may be used.
[0121] Depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. The separator may be a porous substrate; or a composite porous substrate.
[0122] The porous substrate is a substrate containing pores through which lithium ions can move. The porous substrate may be, for example, polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof, and a mixed multilayer film such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may be used.
[0123] The above-described composite porous substrate may be in the form of a porous substrate and a functional layer located on the porous substrate. The functional layer may be at least one of, for example, a heat-resistant layer and an adhesive layer, from the perspective of enabling additional functional addition; for example, the heat-resistant layer may comprise a heat-resistant resin and optionally a filler. Additionally, the adhesive layer may comprise an adhesive resin and optionally a filler. The filler may be an organic filler or an inorganic filler.
[0124] The additive for a lithium secondary battery according to one embodiment may be included in the electrolyte as described above, and may also be applied to the current collector, electrode tab, separator, etc. of the lithium secondary battery.
[0125] When the above additive is applied to a current collector or an electrode tab, the additive may be coated onto the uncoated portion of the current collector or the electrode tab by a coating solution dispersed in a suitable solvent. When the above additive is applied to a separator, the additive may be included in the separator components, or a coating solution in which the additive is dispersed in a suitable solvent may be coated onto at least one surface of the separator.
[0126] The embodiments of the present invention described above will be explained in more detail through the following examples. However, the following examples are for illustrative purposes only and do not limit the scope of the present invention.
[0128] Manufacturing of additives
[0129] Synthesis Example 1
[0130] A polymer solution containing 1 wt% of a foaming agent (SMG-200B, Hanmir Co.) and 10 wt% of poly(vinylidene fluoride hexafluoropropylene) (PVDF-HFP) was prepared, and a fiber-shaped additive was manufactured by electrospinning such that the ratio of the thickness of the core to the shell was 1:1.
[0132] Synthesis Example 2
[0133] A polymer solution containing 2 wt% of a foaming agent (SMG-200B, Hanmir Co.) and 10 wt% of poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP) was prepared, and a fiber-shaped additive was manufactured by electrospinning such that the thickness of the core and shell was 2:1.
[0135] Synthesis Example 3
[0136] A polymer solution containing 4 wt% of a foaming agent (SMG-200B, Hanmir Co.) and 10 wt% of poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP) was prepared, and a fiber-shaped additive was manufactured by electrospinning such that the thickness of the core and shell was 4:1.
[0138] Synthesis Example 4
[0139] A fiber-shaped additive was prepared using the same method as Synthesis Example 1 above, except that the thickness of the core and shell was electrospun to be 1:2.
[0141] Synthesis Example 5
[0142] A fiber-shaped additive was prepared using the same method as Synthesis Example 1 above, except that the thickness of the core and shell was electrospun to be 5:1.
[0144] Comparative Synthesis Example 1
[0145] A fiber-shaped additive was prepared in the same manner as in Synthesis Example 1, except that a polymer solution containing polyethylene glycol (PEG) was used instead of poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP).
[0147] Comparative Synthesis Example 2
[0148] A fiber-shaped additive was prepared in the same manner as in Synthesis Example 1, except that a polymer solution containing polypropylene (PP) was used instead of poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP).
[0150] manufacturing of lithium secondary batteries
[0151] Example 1
[0152] A lithium secondary battery was manufactured using LiCoO2 as the positive electrode, artificial graphite as the negative electrode, and an electrolyte having the following composition.
[0153] (Electrolyte composition)
[0154] Salt: LiPF61.3 M
[0155] Solvent: Ethylene carbonate: Propylene carbonate: Ethyl propionate: Propyl propionate (volume ratio of EC:PC:EP:PP = 15:15:25:45)
[0156] Additive: 3 parts by weight of fluoroethylene carbonate, 2 parts by weight of the additive prepared according to Synthesis Example 1 (provided that in the above electrolyte composition, “parts by weight” refers to the relative weight of the additive to 100 parts by weight of the total electrolyte (lithium salt and non-aqueous organic solvent).)
[0158] Example 2
[0159] A lithium secondary battery was manufactured in the same manner as in Example 1, except that 1.5 parts by weight of the additive prepared according to Synthesis Example 2 were used instead of the additive prepared from Synthesis Example 1.
[0161] Example 3
[0162] A lithium secondary battery was manufactured in the same manner as in Example 1, except that 1.25 parts by weight of the additive prepared according to Synthesis Example 3 was used instead of the additive prepared from Synthesis Example 1.
[0164] Comparative Example 1
[0165] A lithium secondary battery was manufactured in the same manner as in Example 1, except that the additive prepared from Synthesis Example 1 was not used.
[0167] Comparative Example 2
[0168] A lithium secondary battery was manufactured in the same manner as in Example 1, except that 0.1 parts by weight of a foaming agent (SMG-200B, Hanmir Co.) was used instead of the additive prepared from Synthesis Example 1.
[0170] Comparative Example 3
[0171] A lithium secondary battery was manufactured in the same manner as in Example 1, except that 1 part by weight of a foaming agent (SMG-200B, Hanmir Co.) was used instead of the additive prepared from Synthesis Example 1.
[0173] Comparative Example 4
[0174] A lithium secondary battery was manufactured in the same manner as Example 1, except that 2 parts by weight of the additive prepared according to Comparative Synthesis Example 1 were used instead of the additive prepared from Synthesis Example 1.
[0176] Comparative Example 5
[0177] A lithium secondary battery was manufactured in the same manner as in Example 1, except that 2 parts by weight of the additive prepared according to Comparative Synthesis Example 2 were used instead of the additive prepared from Synthesis Example 1.
[0179] Evaluation 1: Dose Retention Rate Evaluation
[0180] For the lithium secondary batteries according to Examples 1 to 3 and Comparative Examples 1 to 5, the delta OCV (Δ OCV) was measured after charging at 0.5C / 4.4V 0.05C Cut-off and storing at 60°C for 4 weeks, and the results are shown in Table 1 below. A small Δ OCV value indicates excellent capacity retention.
[0181] 60℃ High Temperature Storage (After 4 weeks) Δ OCV(V) Example 1 0.23 Example 2 0.21 Example 3 0.29 Comparative Example 3 0.42 Comparative Example 4 0.39
[0182] Referring to Table 1 above, the lithium secondary batteries according to Examples 1 to 3 show a smaller △OCV value during high-temperature storage evaluation compared to the lithium secondary batteries according to Comparative Examples 3 and 4. Thus, it can be seen that the lithium secondary batteries according to the examples have a better cell capacity retention rate at high temperatures compared to the lithium secondary batteries according to the comparative examples.
[0184] Assessment 2: Heat Exposure Assessment
[0185] Lithium secondary batteries according to Examples 1 to 3 and Comparative Examples 1 to 5 were placed in a chamber, and the temperature was increased from room temperature (25℃) at a rate of 5±2℃ per minute. Changes in the lithium secondary batteries were observed while maintaining the temperature for about 1 hour. The above process was performed twice, and the results are shown in Table 2 below.
[0186] Heat exposure temperature 130℃ 132℃ 134℃ 136℃ 1 time 2nd time 1 time 2nd time 1 time 2nd time 1 time 2nd time Example 1 OK OK OK OK OK OK OK OK Example 2 OK OK OK OK OK OK OK OK Example 3 OK OK OK OK OK OK OK OK Comparative Example 1 NG NG - - - - - - Comparative Example 2 NG NG - - - - - - Comparative Example 5 NG NG - - - - - -
[0187] In Table 2 above, “NG” means that a thermal runaway phenomenon was observed at the exposure temperature, and “OK” means that there was no thermal runaway phenomenon at the exposure temperature. Also, “-” means that a thermal exposure evaluation was not performed.
[0188] In Examples 1 to 3, when exposed to high temperatures, the shell of the additive according to one embodiment melts, and the foaming agent contained in the core is released, causing the volume of the foaming agent to increase and a rapid increase in battery resistance to occur; consequently, no thermal runaway phenomenon is observed even in high-temperature thermal exposure evaluations up to 136°C. On the other hand, in Comparative Examples 1, 2, and 5, a thermal runaway phenomenon is observed when exposed to a temperature of 130°C. This is interpreted as the thermal runaway phenomenon occurring because there is no device to control the short circuit between electrodes at high temperatures when the additive according to the present invention is not included or when a small amount of foaming agent is added.
[0189] Thus, it can be seen that the lithium secondary battery according to the embodiment maintains battery characteristics within the battery operating temperature range compared to the lithium secondary battery according to the comparative example, while exhibiting superior safety at high temperatures.
[0190] Although preferred embodiments of the present invention have been described in detail above, the scope of the invention is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concept of the invention as defined in the claims below also fall within the scope of the present invention. Explanation of the symbols
[0192] 100: Lithium secondary battery 112: Cathode 113: Separator 114: Bipolar 120: Battery container 140: Encapsulated member
Claims
Claim 1 An additive for a lithium secondary battery comprising a core including a foaming agent and a shell surrounding the core, wherein the shell comprises a polymer having a melting point of 90°C to 120°C, and the polymer comprises poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), polyacrylic acid, polyethylene, poly(methyl methacrylate), polyalkylene oxide, polyalkylene succinate, or a combination thereof. Claim 2 An additive for a lithium secondary battery according to claim 1, wherein the ratio of the thickness of the core to the thickness of the shell is 1:1 to 4:
1. Claim 3 An additive for a lithium secondary battery according to claim 1, wherein the core has a thickness of 0.1 μm to 2.0 μm and the shell has a thickness of 0.025 μm to 0.5 μm. Claim 4 In claim 1, the blowing agent is an additive for a lithium secondary battery comprising a glass blowing agent, a hydrocarbon compound, a hydrofluoroolefin (HFO) compound, or a combination thereof. Claim 5 In paragraph 4, the glass foaming agent is an additive for a lithium secondary battery comprising silicon dioxide, sodium oxide, and water. Claim 6 In claim 4, the glass foaming agent is an additive for a lithium secondary battery comprising 60% to 70% by weight of silicon dioxide, 20% to 30% by weight of sodium oxide, and 5% to 20% by weight of water. Claim 7 delete Claim 8 In claim 1, the additive is an additive for a lithium secondary battery in the form of a fiber formed using electrospinning. Claim 9 An electrolyte for a lithium secondary battery comprising a non-aqueous organic solvent, a lithium salt, and an additive for a lithium secondary battery according to any one of claims 1 to 6 and 8. Claim 10 In claim 9, the lithium secondary battery electrolyte is a lithium secondary battery electrolyte containing 0.1% to 10% by weight based on the total weight of the lithium secondary battery electrolyte. Claim 11 In claim 9, the lithium secondary battery electrolyte is a lithium secondary battery electrolyte containing 0.1% to 5.0% by weight based on the total weight of the lithium secondary battery electrolyte. Claim 12 In claim 9, the lithium secondary battery electrolyte is a lithium secondary battery electrolyte containing 0.1% to 3.0% by weight based on the total weight of the lithium secondary battery electrolyte. Claim 13 A lithium secondary battery comprising: a positive electrode comprising a positive active material; a negative electrode comprising a negative active material; and the electrolyte of claim 9.
Citation Information
Patent Citations
Electrolyte for lithium secondary battery and lithium secondary battery containing the same
KR1020170116710A
Fire Extinguishing Systems For Energy Storage System
KR102330073B1