Method of fabricating a device having a passivating layer

TWI945294BActive Publication Date: 2026-11-11MICROSOFT TECHNOLOGY LICENSING LLC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
TW111138209
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-11-10
Filing Date
2022-10-07
Publication Date
2026-11-11
Estimated Expiration
2042-10-06

AI Technical Summary

Technical Problem

Existing methods for fabricating semiconductor-superconductor hybrid structures face challenges in maintaining the integrity of the interface between components due to contamination and damage during post-manufacturing processes, particularly affecting materials like lead which are fragile and susceptible to water vapor.

Method used

A method involving the formation of a patterned layer on a substrate using a stencil mask under vacuum conditions, followed by the in-situ deposition of a passivation layer, such as aluminum oxide, to protect the structure from contamination and damage during subsequent processing.

Benefits of technology

This approach maintains the quality of the interface between semiconductor and superconductor components by preventing contamination and degradation, ensuring reliable performance of quantum computing components like semiconductor-superconductor hybrid structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure TWG2TB001920039_001
    Figure TWG2TB001920039_001
  • Figure TWG2TB001920039_002
    Figure TWG2TB001920039_002
  • Figure TWG2TB001920039_003
    Figure TWG2TB001920039_003
Patent Text Reader

Abstract

A method of manufacturing an element includes: depositing a material onto the surface of a substrate via a stencil photomask to form a patterned layer of the material on the surface; and forming a passivation layer on the patterned layer and the surface; wherein the method is performed in a sealing apparatus and the substrate is held under vacuum until the passivation layer has been formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to a method for manufacturing components with a passivation layer. Prior Technology

[0002] Under suitable conditions, semiconductor nanowires, which are similar to superconductors, could potentially carry the topological phases of matter. This makes them promising candidates for building blocks in fault-tolerant quantum computers.

[0003] The topological phase itself manifests as a pair of Majorana zero modes (MZMs) at the nanowire tip. Along the body of the wire, away from the tip, gaps exist in the single-electron spectrum. Experiments typically use tunneling spectroscopy at the nanowire tip to detect the zero-bias peak (ZBP) in the tunneling conductance.

[0004] By forming such nanowire networks and introducing topological states into parts of the network, it becomes possible to generate qubits that can be used for quantum computing purposes. A qubit is an element that can be measured with two possible outcomes, but at any given time (when not being measured), it is actually in a quantum superposition of two states corresponding to different outcomes.

[0005] Nanowires can take the form of elongated segments of semiconductor materials, with their length being many times greater than their width and thickness. Nanowires are quasi-one-dimensional systems. Superconducting layers are conventionally arranged on at least a portion of nanowires.

[0006] Another system for generating MZMs is a semiconductor nanowire based on a two-dimensional electron gas (2DEG), which is closely coupled to a conventional superconductor. Superconductors are typically grown as part of an epitaxial 2D wafer stack, but can also be deposited after material growth during fabrication. This material platform possesses considerable spin-orbit coupling and a large electron g-factor, which are key factors in the formation of topological states.

[0007] To induce the topological phase, the device is cooled to the temperature at which superconductors (such as aluminum) exhibit superconducting behavior. The superconductor induces a proximity effect in adjacent semiconductors, thereby causing the semiconductor region near the interface with the superconductor to also exhibit superconducting properties; that is, a superconducting pairing gap is induced in the adjacent semiconductors. When a magnetic field is applied, a micro-Zoom (MZM) is formed at both ends of the semiconductor-superconductor mixture.

[0008] The role of a magnetic field is to enhance spin degeneracy in semiconductors. In the context of quantum systems, degeneracy refers to the situation where different quantum states have the same energy level. Enhancing degeneracy means making these states adopt different energy levels. Spin degeneracy refers to the situation where different spin states have the same energy level. Spin degeneracy can be enhanced by a magnetic field, resulting in energy level splitting between electrons with different spin polarizations. This is known as the Zeeman effect. The Zeeman energy, the magnitude of the energy level splitting, should be at least as large as the superconducting gap to close the negligible superconducting gap and reopen the topological gap in the system.

[0009] Induced MZM may also involve modulating the electrostatic potential of charge carriers in nanowires by using electrostatic gates. An electrostatic potential is applied using gate electrodes. Applying an electrostatic potential can manipulate the number of charge carriers in the conduction band or valence band of a semiconductor device.

[0010] The properties of hybrid structures depend heavily on the quality of the interface between the semiconductor and superconductor components. Significant advances in materials science have been made in achieving initial coupling between semiconductors and superconductors. One hybrid platform is aluminum grown on indium arsenide.

[0011] Kanne et al. (Nature Nanotechnology, Vol. 16, pp. 776-781) described the growth of lead (Pb) on vapor-liquid-solid nanowires. Lead possesses a much larger superconducting gap than aluminum, making it an attractive candidate material for inclusion in hybrid structures. However, lead films are fragile and therefore susceptible to damage from numerous post-fabrication processes. Summary of the Invention

[0012] In one embodiment, a method for manufacturing a component is provided. The method includes: depositing a material onto a surface of a substrate via a stencil photomask to form a patterned layer of the material on the surface; and forming a passivation layer on the patterned layer and the surface. The method is performed in a sealing apparatus, and the substrate is held under vacuum until the passivation layer has been formed.

[0013] By keeping this substrate under vacuum, contamination and damage to its surface can be avoided. Furthermore, since the stencil mask is used to pattern the deposited material, there is no need to form a photomask on this substrate or perform in-situ etching. This method can be performed at low temperatures, thus preventing degradation of the substrate and the patterned layer.

[0014] This summary is provided to introduce some concepts in a simplified form, which will be further described in the embodiments below. This summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to limit the scope of the claimed subject matter. The claimed subject matter is also not limited to embodiments that address any or all of the shortcomings pointed out herein. Simple Explanation of the Diagram

[0015] To aid in understanding the embodiments of this disclosure and to show how these embodiments can be implemented, reference is made to the accompanying drawings by way of example only, wherein: Figure 1 is a flowchart outlining the method for manufacturing the component; Figures 2A to 2C are schematic cross-sectional views of the workpiece obtained in each step of the method in Figure 1; and Figure 3 is a block diagram of an example device used to perform this method. Implementation

[0016] The verb "include" is used in this text as a shorthand for "includes or consists of". In other words, although the verb "includes" is intended to be an open term, it is explicitly considered that this term should be replaced with the closed term "consisting of", specifically in the context of its use in relation to chemical ingredients.

[0017] Directional terms such as "top," "bottom," "left," "right," "above," "below," "horizontal," and "vertical" are used here for ease of description and in relation to the orientation shown in the relevant diagrams. For the avoidance of any doubt, these terms are not intended to limit orientation within an external frame of reference.

[0018] As used herein, the term "superconductor" refers to a material that becomes superconducting when cooled to a temperature below its critical temperature Tc. The use of this term is not intended to limit the temperature of the device.

[0019] A nanowire is a slender component with a width in the nanometer range and an aspect ratio of at least 100, at least 500, or at least 1000. Typical examples of nanowires have widths ranging from 10 to 500 nm, depending on the case, from 50 to 100 nm or 75 to 125 nm. The length is typically on the order of micrometers, for example, at least 1 μm or at least 10 μm.

[0020] A "semiconductor-superconductor hybrid structure" comprises a semiconductor component and a superconductor component, configured such that the superconductor component can induce superconductivity in the semiconductor component via a proximity effect under specific operating conditions. Specifically, this term refers to a structure capable of exhibiting topological behavior, such as Majorana zero modes or other excitations useful for quantum computing applications. Operating conditions generally include cooling the structure to a temperature below the critical temperature of the superconductor component, applying a magnetic field to the structure, and applying electrostatic gate to the structure. Generally, at least a portion of the semiconductor component is in close contact with the superconductor component. For example, the superconductor component can be epitaxially grown on the semiconductor component. However, certain element structures with one or more other components between the semiconductor and superconductor components have been proposed.

[0021] The difference between a "topological insulator-superconductor hybrid structure" and a semiconductor-superconductor hybrid structure is that the semiconductor components are replaced by topological insulator components. Electrostatic gates are typically not required in topological insulator-superconductor hybrid structures. Furthermore, a magnetic field is usually not required because spin momentum locking provides spin polarization.

[0022] As used herein, “vacuum” refers to an environment with a gas pressure less than or equal to 1 x 10⁴ Pa. “Medium vacuum” refers to an environment with a gas pressure in the range of 3 kPa to 0.1 Pa. “Ultra-high vacuum” refers to an environment with a pressure less than or equal to 100 nanopascals.

[0023] This document provides a method for manufacturing an element comprising a patterned thin film on a substrate. The thin film is patterned in situ using a stencil mask or the like, rather than by using in-situ etching or stripping. A passivation layer is then formed in situ on the thin film. By patterning the film and forming the passivation layer in situ, an initial interface between the thin film and the substrate is obtained. The passivation layer protects the surface of the thin film and the substrate from damage during any subsequent post-manufacturing operations, specifically during any post-manufacturing etching process. Furthermore, in some embodiments, this method can be performed at low temperatures to prevent the thin film from dehydrating from the substrate.

[0024] Although this method will be described with particular reference to the fabrication of a semiconductor-superconductor hybrid structure, in which the substrate comprises a semiconductor and the patterned layer comprises a superconductor, this method can be applied to the fabrication of other combinations of materials and other components. The patterned layer may comprise any thin film or combination of thin films that can be grown on the substrate, such as superconductors, semiconductors, metals and / or ferromagnets.

[0025] An example method will now be described with reference to FIG. 1 and FIGS. 2A to 2C. FIG. 1 is a flowchart outlining the method, and FIGS. 2A to 2C show the workpieces obtained at various stages of the method.

[0026] In block 101, a patterned layer of material is formed on a substrate by depositing the material onto the substrate via a template mask. This operation is shown in FIG. 2A.

[0027] The nature of the substrate 210 is not particularly limited. The substrate 210 generally comprises at least one wafer, i.e., a piece of single-crystal material. The wafer provides a physical support and a growth medium for other components. The wafer typically comprises a high-bandgap semiconductor material. Examples of wafer materials include indium phosphide, indium antimonide, indium arsenide, gallium arsenide, gallium phosphide, and silicon.

[0028] The substrate 210 may include semiconductor components.

[0029] For example, the semiconductor components may include nanowires. The nanowires may be selective-area-grown (''SAG'') nanowires. A plurality of such nanowires may be present, and the nanowires may be arranged in a network.

[0030] The nanowires may comprise III-V semiconductor materials, specifically materials of formula 1: where x ranges from 0 to 1. In other words, the nanowires may comprise indium antimonide (x = 0), indium arsenide (x = 1), or a ternary mixture comprising 50% indium by mole and variable proportions of arsenic and antimony (0 < x < 1).

[0031] Another useful class of semiconductor materials is II-VI semiconductor materials. Examples of II-VI semiconductor materials include cadmium telluride, mercury telluride, lead telluride, and tin telluride.

[0032] The semiconductor components may include semiconductor heterostructures configured to accommodate a two-dimensional electron gas (''2DEG'') or a two-dimensional hole gas (''2DHG''). The semiconductor heterostructure comprises a quantum well disposed between a lower barrier and an upper barrier. The quantum well comprises a material different from the materials of the lower barrier and the upper barrier. The materials of the lower barrier and the upper barrier may be selected independently of each other.

[0033] There are no particular restrictions on the configuration of the lower and upper barriers, provided that these layers allow charge carriers (electrons or holes) to be trapped in quantum wells. The lower barrier may comprise one or more layers of one or more different materials. The upper barrier may comprise one or more layers of one or more different materials. Constructing barriers from multiple layers can provide defect filtering, i.e., reduce the influence of dislocations in the crystalline structure of the materials used.

[0034] Quantum wells may contain a layer of semiconductor material with a relatively small band gap compared to the materials of the lower and upper barriers. For example, Odoh and Njapba, "A Review of Semiconductor Quantum Well Devices," Advances in Physics Theories and Applications, Vol. 46, 2015, pp. 26-32; and S. Kasap and P. Capper (eds.), Springer Handbook of Electronic and Photonic Materials, DOI 10.1007 / 978-3-319-48933-9_40, describe illustrative materials for forming quantum wells.

[0035] As an alternative to semiconductor components, or in addition to semiconductor components, the substrate may include topological insulator components. A topological insulator is a material having a conductive surface and an electrically insulating body. A useful class of topological insulator materials is defined by Equation 2: Where y is in the range of 0 to 1. Specifically, y can be in the range of 0.5 to 1, 0.6 to 0.9, or 0.8 to 0.9.

[0036] The substrate can be fabricated in the same equipment used to perform this method. Substrate fabrication may include cleaning the wafer to remove adsorbed contaminants. Substrate fabrication may include growing any semiconductor components and / or topological insulator components on the wafer. For example, growth can be controlled by using a stencil photomask. By fabricating the substrate in the same equipment, exposure to the open atmosphere is avoided. This prevents contamination of the substrate surface and / or avoids chemical degradation of the materials used, thereby improving the quality of the finished device. The characteristics of semiconductor-superconductor hybrid devices are particularly sensitive to the interface quality between the semiconductor and superconductor components.

[0037] There are no particular limitations on the properties of the material used to form the patterned layer 220, provided that the material can be deposited on the substrate 210.

[0038] The patterned layer can be made of metal.

[0039] Metals can be superconductors. Examples of superconducting metals include aluminum and lead. Both aluminum and lead have good compatibility with the semiconductor materials of Formula 1.

[0040] The metal can be a common metal. For example, common metals can be used to form electrical connectors or contact pads. Examples of common metals include titanium and gold. Another example is a chromium / gold double layer.

[0041] Lead can be particularly useful in certain implementations due to its very large superconducting gap Δ. Therefore, hybrid elements incorporating lead can have large topological gaps. This means that Majorana zero modes formed in such elements are better protected against thermal changes, allowing for more reliable quantum computing. Water corrodes lead, and lead films are easily damaged by water vapor. A passivation layer formed later in this method protects the lead layer from damage.

[0042] In examples where the substrate includes a topological insulator, the topological insulator is a tellurium compound, specifically a compound of formula 2, and the material may be palladium. It has been reported that when palladium is deposited on the compound of formula 2, a superconducting compound PdTe 2 is formed at the interface between the palladium layer and the topological insulator.

[0043] The patterned layer can be made of a ferromagnetic insulator, such as materials selected from EuS, EuO, GdN, Y3Fe5O12, Bi3Fe5O12, YFeO3, Fe2O3, Fe3O4, Sr2CrReO6, CrBr3 / CrI3, and YTiO3. Specifically, the ferromagnetic insulator material can be EuS or EuO. These materials can be deposited at low temperatures.

[0044] The patterned layer may be made of a barrier material as described in US 2021 / 0126181 A1. Examples of barrier materials include those of Formula 3: Where z is in the range of 0.05 to 1.

[0045] Other examples of barrier materials include those in Equation 4: Where n is in the range of 0.04 to 0.9.

[0046] When a ferromagnetic insulating layer or barrier layer is present, the patterned layer 220 typically also includes a superconducting material layer.

[0047] The patterned layer 220 may be made of a composite oxide. The composite oxide is a compound of oxygen and at least two other elements. An example of a composite oxide is strontium titanate (SrTiO3). SrTiO3 can accommodate a high-density two-dimensional electron gas and possesses useful magnetic properties.

[0048] While this example illustrates a single patterned layer 220, methods involving the formation of two or more patterned layers are also considered. Depending on the design of the component to be manufactured, different stencils may be used for each layer. Using individually selected stencils allows for the deposition of different materials at different locations on the substrate, thus allowing for further freedom in component design.

[0049] When this method is used to manufacture hybrid components, the patterning layer may include: A semiconductor or topological insulating layer, if not pre-prepared as a substrate; Depending on the circumstances, a layer of ferromagnetic insulator or barrier material; and Superconductor material layer.

[0050] When this method is used to form a layer of superconducting material, two or more different superconductors can be deposited. For example, an aluminum layer can be deposited first, followed by a lead layer deposited on top of the aluminum layer. As described in WO 2021 / 113746 A1, this improves the coupling between the lead layer and the substrate.

[0051] As shown in Figure 2A, the patterned material layer 220 is deposited via an opening in the stencil mask 328. Material flux F1, such as a material bundle from an evaporator, passes through the opening and reaches the surface of the substrate.

[0052] The use of stencils allows for the patterning of layers without applying a resist to the substrate surface, as in comparative techniques such as stripping or etching lithography. Therefore, patterning is achieved within a growth chamber in which the layers are fabricated. The substrate is not exposed to an open atmosphere, and the substrate surface remains in its initial state. This allows for the acquisition of higher quality components.

[0053] During the deposition of the patterned layer, the substrate can be maintained at a temperature below or equal to 273 K (0°C), for example, in the range of 50 to 100 K. If the temperature of the metal film is too high, it may dehydrate from the substrate. As used herein, dehydration refers to the process of a continuous film breaking into isolated blocks. It has been found that applying a passivation layer to the metal film at low temperatures can reduce dehydration and allow the device to withstand higher temperatures during subsequent processing steps.

[0054] Patterned layers are formed using directional deposition processes (typically physical deposition processes). Specifically, patterned layers can be formed by evaporation, or, where appropriate, by molecular beam epitaxy. For many materials, physical deposition onto low-temperature substrates (e.g., substrates at 0°C or lower) is possible.

[0055] After the patterned layer is formed, a passivation layer is formed on the patterned layer and on the substrate surface. In this example, the passivation layer is an aluminum oxide layer formed in two operations.

[0056] In block 102, an aluminum layer is formed on the patterned layer and on the substrate surface. This operation is shown in Figure 2B.

[0057] An aluminum layer 230 is deposited over the entire surface of the substrate 210 and is covered by a patterned layer. This can be referred to as "global deposition". The deposition may involve growing the aluminum layer by molecular beam epitaxy.

[0058] The aluminum layer 230 can be fabricated in the same growth chamber as the patterned layer. To achieve this, the stencil mask 328 can be moved away from the substrate so as not to interfere with the aluminum flux F2. For example, the stencil mask can be rotated to a vertical position, placed to one side, or removed from the growth chamber via a gas chamber.

[0059] Alternatively, the aluminum layer 230 can be fabricated in different growth chambers of a sealed apparatus. In such embodiments, the substrate moves between two growth chambers while being held in a vacuum, preferably an ultra-high vacuum. The growth chambers may be coupled together via valves and, where appropriate, via a buffer chamber that acts as a gas sac.

[0060] In embodiments where aluminum layers are grown using a directional deposition process, the patterned layer may project shadows onto portions of the substrate surface. In other words, the patterned layer can block the deposition material bundle. The aluminum layer may therefore have an uneven thickness. If the thickness of the patterned layer 220 is greater than about 10 nm, shadows can be observed.

[0061] To reduce the effects of shading, the orientation of the aluminum beam relative to the substrate surface can be changed during layer growth. The substrate can be moved, for example, rotated or tilted. The beam source is movable. Depending on the situation, multiple material beams can be applied simultaneously or sequentially from multiple different directions.

[0062] The thickness of the aluminum layer 230 can be less than or equal to 3 nm, for example, in the range of 2 to 3 nm. An aluminum layer with a thickness of about 3 nm or less can be easily and completely oxidized by exposure to oxygen.

[0063] During aluminum deposition, the substrate temperature can be maintained at or below 273 K (0°C), for example, in the range of 50 to 100 K. As mentioned above, maintaining the substrate at a low temperature helps prevent the patterned layer from desiccating from the substrate. It can be assumed that the substrate temperature is equal to the temperature of the sample stage holding the substrate.

[0064] Aluminum layers are typically formed using physical deposition processes. Specifically, aluminum layers can be formed by evaporation, or, depending on the circumstances, by molecular beam epitaxy. Aluminum evaporates at relatively low temperatures, and physical deposition of aluminum on low-temperature substrates has been found to be quite effective.

[0065] Subsequently, in block 103, aluminum layer 230 is oxidized. This transforms the aluminum layer into a passivation layer 240 of aluminum oxide, as shown in Figure 2C.

[0066] Oxidation may involve exposing the aluminum layer to oxygen. The oxygen pressure can be in the range of 0.1 to 10 Pa, for example, 0.5 to 1.5 Pa. Exposing the aluminum to oxygen at a pressure of about 1 Pa provides a convenient route for oxidation.

[0067] The degree of oxidation can be controlled by selecting the oxygen pressure and the oxidation temperature. Typically, complete oxidation of the aluminum layer 230 deposited in operation 102 is desired. When exposed to oxygen, aluminum undergoes self-limiting oxidation. As an example, when aluminum is exposed to the atmosphere, an aluminum oxide layer with a depth of approximately 3 nm is formed.

[0068] Oxidation typically begins shortly after the deposition of the aluminum layer 230 is completed, while the substrate remains at a low temperature (e.g., below 273 K, and possibly below 200 K). For example, oxidation may begin within an hour of deposition completion, within 30 minutes, further within 10 minutes, and further within 5 minutes. Because the substrate remains in a vacuum, heat transfer to the substrate is generally slow, due to the near absence of conduction or convection.

[0069] Keeping the substrate at a low temperature until the aluminum layer is at least partially oxidized may help prevent dehydration.

[0070] During the oxidation process, the substrate temperature can be raised because it protects the patterned layer from dehydration once the initial oxide layer is formed. The initial substrate temperature may be in the range of 50 to 100 K. The final temperature may be as high as 303 K (30°C). Allowing for higher temperatures increases the depth of aluminum oxide oxidation.

[0071] Forming an aluminum layer, followed by an in-situ aluminum oxide layer, allows for the formation of a passivation layer without exposing the substrate to high temperatures. This enables the passivation of temperature-sensitive films.

[0072] Once formed, the passivated aluminum oxide layer 240 protects the patterned layer 220 and the substrate 210, including any semiconductor or topological insulator components. This allows for post-manufacturing operations without damaging the patterned layer or the substrate, or degrading the interface between the patterned layer and the substrate.

[0073] Various modifications can be made to the example methods.

[0074] Although the example described uses an aluminum oxide passivation layer, passivation layers formed of other materials may also be used.

[0075] For example, block 102 can be modified to include in-situ deposition of a dielectric material layer on the substrate. In such embodiments, the operation of block 103 is omitted. If the patterned layer and the substrate are not temperature-sensitive, atomic layer deposition of the dielectric material can be performed. Atomic layer deposition generally involves heating the substrate to a temperature of at least 350 K.

[0076] In another example, a different metal can be used to replace the aluminum layer formed at block 102. At block 103, any suitable reagent (not necessarily oxygen) can be used to convert the metal into a passivating material.

[0077] An example device 300 for implementing this method will now be described with reference to Figure 3. Figure 3 is a block diagram of this device.

[0078] The apparatus 300 includes a set of vacuum chambers 310, 320, and 330. These vacuum chambers are referred to as working chambers. Each vacuum chamber is connected to a buffer chamber 350 via its respective gate valve 314, 324, and 334. This allows a substrate to move between the vacuum chambers without exposure to the open atmosphere. By connecting the working chambers via the buffer chambers, unwanted transfer of reagents between the working chambers is prevented.

[0079] In this example, the first working chamber 310 may be configured to allow the fabrication of semiconductor components on the wafer and is in communication with a material source 312 to provide semiconductor material or a suitable precursor thereof for deposition on the wafer.

[0080] The second working chamber 320 is configured to allow the operation of blocks 102 and 103 in Figure 1. The second working chamber may be a molecular beam epitaxy chamber. The second working chamber 320 is configured to provide an ultra-high vacuum environment.

[0081] In this example, the second working chamber 320 is connected to two material sources 322 and 323. The first material source 322 may be an evaporator for providing a material such as lead to be deposited in the patterned layer. The second material source 323 may be an evaporator for providing a material, such as aluminum, for forming the passivation layer.

[0082] A cooling plate 326 for cooling the substrate is disposed in the second working chamber 320. The cooling plate may include one or more tubes, and liquid nitrogen may be pumped through the tubes to cool the substrate.

[0083] The substrate can be mounted on a sample carrier. The sample carrier can be configured to act as a heat sink, i.e., contain a material with a relatively high specific heat capacity. This may help keep the substrate at a low temperature when it moves between chambers.

[0084] A stencil mask 328 is also arranged in the second working chamber. The stencil mask can be moved using a manipulator, allowing it to be positioned on the substrate as needed. The stencil mask is used to pattern material layers, as described with reference to block 101 in Figure 1.

[0085] The third working chamber 330 in this example is configured as an oxidation chamber for the alumina layer, as described with reference to block 103 in Figure 1. A third vacuum chamber is connected to an oxygen supply 332. The third vacuum chamber and the oxygen supply 332 can be configured together to provide an environment with an oxygen pressure of 0.1 to 10 Pa, or 0.5 to 5 Pa depending on the situation. A cooling plate 336 is provided in this chamber for controlling the substrate temperature during oxidation.

[0086] Various modifications can be made to the sample device.

[0087] This device may include two separate working chambers, each used to manufacture the patterned layer and the aluminum layer.

[0088] In variants where materials other than alumina are used as the passivation layer, the oxide chamber 330 can be omitted.

[0089] The device may include additional chambers for fabricating substrates.

[0090] It should be understood that the above embodiments are described only by way of examples.

[0091] More generally, according to one embodiment disclosed herein, a method for manufacturing an element is provided. This method includes depositing material onto a substrate surface via a stencil photomask to form a patterned layer of material on the surface; and forming a passivation layer on the patterned layer and the surface. This method is performed in a sealing apparatus, and the substrate is held under vacuum until after the passivation layer has been formed.

[0092] This method is particularly suitable for manufacturing quantum computer components.

[0093] For example, this device may include a semiconductor-superconductor hybrid structure and / or a topological insulator-superconductor hybrid structure. Because this method allows for an initial interface between the patterned layer and the substrate, it allows for higher quality hybrid structures. The passivation layer also provides good protection for the hybrid structure during any post-manufacturing processing, such as the addition of gate electrodes.

[0094] This component may include superconducting circuitry. This component may include one or more Josephson junctions.

[0095] By maintaining the substrate under vacuum, contamination of the substrate surface can be avoided. Damage to materials that might be chemically degraded by air or water vapor can also be prevented. Vacuum can be an environment with a gas pressure less than or equal to 1 x 10⁴ Pa. Deposition operations are typically performed under ultra-high vacuum. Oxidation operations can be performed under medium vacuum.

[0096] Since the stencil mask is used to pattern the deposited material, there is no need to form a photomask on the substrate. Etching is also avoided. This prevents degradation and / or contamination of the patterned layer and the substrate surface.

[0097] Patterned and passivation layers are formed without applying resist to the substrate. Patterned and passivation layers are formed without etching. Patterned and passivation layers are formed without electron beam lithography. Patterned and passivation layers are formed without a stripping process.

[0098] Patterned layers can be formed by physical deposition (e.g., evaporation) of materials.

[0099] Passivation layers can be formed by physical deposition (e.g., evaporation). Passivation layers can be formed by physical deposition of a precursor (e.g., aluminum), followed by in-situ conversion (e.g., oxidation) of the precursor into a passivating material (e.g., aluminum oxide). Using physical deposition allows the substrate to be kept at low temperatures during this process.

[0100] Forming a passivation layer may include forming an aluminum layer on a patterned layer and a surface; and an aluminum oxide layer to form the passivation layer. The aluminum layer can be deposited by evaporation. For example, the aluminum layer can be grown on the patterned layer and the substrate surface by molecular beam epitaxy. Advantageously, aluminum can evaporate at relatively low temperatures. This allows the substrate to be kept at a low temperature during the formation of the aluminum layer, which helps prevent the patterned layer from desiccating from the substrate. Oxidation of the aluminum layer can also be performed at low temperatures.

[0101] The alumina layer may contain oxygen exposed to pressures ranging from 0.1 Pa to 3 kPa, or, where appropriate, from 0.1 Pa to 10 Pa, and further, where appropriate, from 0.5 Pa to 5 Pa. An environment with gas pressures ranging from 0.1 Pa to 3 kPa is considered a moderate vacuum. Oxidation can be carried out at temperatures below or equal to 30°C.

[0102] Oxidation of the aluminum layer can be performed at a low substrate temperature. During oxidation, the substrate temperature may rise. The initial substrate temperature can range from 50 to 150 K. During oxidation, the final substrate temperature is typically less than or equal to 30°C (303 K), and, in some cases, less than or equal to 0°C (273 K). Keeping the substrate at a low temperature until the aluminum layer is at least partially oxidized prevents dehydration of the patterned layer.

[0103] The thickness of the aluminum layer can be less than or equal to 3 nm, and depending on the circumstances, less than or equal to 2 nm. For example, the thickness of the aluminum layer can be in the range of 1 to 3 nm, and depending on the circumstances, 1 to 2 nm.

[0104] The supply direction of the material forming the passivation layer can be changed during the formation of the passivation layer. For example, this method can be further included by rotating and / or tilting the substrate during the formation of the passivation layer. This allows for the acquisition of a passivation layer with a more uniform thickness.

[0105] The patterned layer can be made of a superconducting material. Superconducting materials can be selected from lead and aluminum.

[0106] The superconducting gap of lead is approximately six times the size of that of aluminum. A large superconducting gap is a desirable characteristic for superconducting components of hybrid devices. However, lead films are highly susceptible to damage and can be corroded, for example, by water. This method allows for the in-situ formation of a passivation layer on the lead. The passivation layer can, for example, protect the lead layer during any post-manufacturing process.

[0107] It has been reported that aluminum is tightly coupled to the semiconductor material of Formula 1. The strength of the coupling can vary depending on the thickness of the aluminum layer, which can range from, for example, 4 to 10 nm. When exposed to high temperatures, the film may easily dehydrate. The method presented herein can be performed at low temperatures, which can reduce or avoid dehydration.

[0108] The formation of a patterned layer may include growing a patterned layer by molecular beam epitaxy.

[0109] Both the patterning layer and the passivation layer can be applied in the same vacuum chamber. This reduces the risk of contaminating the patterning layer and the substrate surface.

[0110] Alternatively, the patterned layer may be formed in the first vacuum chamber of the sealing device, and this method may further include transferring the substrate from the first vacuum chamber to the second vacuum chamber after the patterned layer is formed and before the passivation layer is formed.

[0111] There are no particular limitations on the thickness of the patterned layer. Because this method can be performed without exposing the substrate to high temperatures, it is particularly useful for thin patterned layers that may easily dehydrate when exposed to excessive heat. For example, the patterned layer may have a thickness of less than or equal to 10 nm, and, depending on the case, less than or equal to 5 nm.

[0112] Before the passivation layer is formed, the substrate can be kept at a temperature below or equal to 273 K (0°C). Specifically, the substrate can be kept at a temperature in the range of 50 to 100 K. Keeping the substrate at a low temperature, at least until after the passivation layer is deposited, prevents the patterned layer from dehydrating.

[0113] A patterned layer can be formed when the substrate is at a temperature in the range of 50 to 100 K. An aluminum layer can be deposited when the substrate is at a temperature in the range of 50 to 100 K. An aluminum layer can be oxidized when the substrate is at a temperature less than or equal to 273 K.

[0114] The substrate may include semiconductor components. For example, the substrate may include a wafer and semiconductor components disposed on the wafer.

[0115] In embodiments where semiconductor components are present, this method may further include fabricating the semiconductor components in a sealing apparatus prior to forming the patterned layer. This avoids contamination of the semiconductor component surface, thereby allowing for a better interface to be formed between the semiconductor component and the patterned layer to be formed. A stencil mask can be used to control the growth of the semiconductor component.

[0116] Semiconductor components may contain one or more nanowires. The nanowires may be SAG nanowires.

[0117] Semiconductor components may include heterostructures configured to accommodate two-dimensional electron gases or two-dimensional hole gases. The heterostructure may include quantum well layers disposed between two barrier layers.

[0118] Semiconductor components may contain materials of Formula 1: Where x is in the range of 0 to 1. This material may be indium arsenide (x=1). Other examples of materials of Formula 1 include those in the range of 0 to 0.7, or 0.01 to 0.7, or 0.35 to 0.45.

[0119] As an alternative to semiconductor components, or in addition to semiconductor components, the substrate may comprise a topological insulator. Without the desire to be bound by theory, computationally useful excitations (e.g., Majorana zero modes) can be induced in a topological insulator-superconductor hybrid device without requiring electrostatic gate control of the topological insulator.

[0120] Examples of topological insulator materials include HgTe, Bi₂Te₃, Bi₂Se₃, Sb₂Te₃, CsPbI₃, and CsSnI₃. Topological insulator materials can be tellurium compounds, such as those of Formula 2: Where y is in the range of 0 to 1, or, depending on the situation, 0.5 to 1, 0.6 to 0.9, or 0.8 to 0.9.

[0121] In embodiments where the topological insulator is a tellurium compound, particularly in embodiments where the topological insulator is a compound of formula 2, the patterned layer can be made of palladium. Depositing palladium on such a material can result in the formation of a superconducting layer of PdTe2 at the interface with the topological insulator material.

[0122] After the passivation layer is formed, the substrate can be removed from the self-sealing equipment. The passivation layer protects the patterned layer and substrate surface from degradation by air or water vapor. Post-manufacturing processes can then be performed. For example, gate electrodes can be added to components. The passivation layer protects the patterned layer and substrate surface from damage during post-manufacturing processes. For example, the passivation layer protects the patterned layer and substrate surface from damage by any post-manufacturing etching processes.

[0123] Once the disclosure herein is presented, other variations or use cases of the disclosed technology may become apparent to those skilled in the art. The scope of this disclosure is not limited to the described embodiments, but only to the claims of the appended invention applications.

[0124] 101: Square 102: Square 103: Square 210:Substrate 220: Patterned layer 230: Aluminum layer 240: Passivation layer 300: Equipment 310: Vacuum chamber 312: Material Source 314: Gate valve 320: Vacuum chamber 322: Material Source 323: Material Source 324: Gate valve 326: Cooling plate 328: Template Photomask 330: Vacuum chamber 332: Oxygen Supply Unit 334: Gate valve 336: Cooling plate 350: Buffer Chamber F1: Material Flux F2: Flux

[0125] Domestic storage information (please note in order of storage institution, date, and number) none Overseas storage information (please note in the order of storage country, institution, date, and number) none

Claims

1. A method of manufacturing an element, the method comprising the steps of: depositing a material onto a surface of a substrate via a template photomask to form a patterned layer of the material on the surface; and forming a passivation layer on the patterned layer and the surface; wherein the method is performed in a sealed apparatus and the substrate is held under a vacuum until the passivation layer has been formed; wherein the substrate is held at a temperature less than or equal to 0°C.

2. The method as described in claim 1, wherein the step of forming the passivation layer comprises the following steps: forming an aluminum layer on the patterned layer and the surface; and oxidizing the aluminum layer to form the passivation layer.

3. The method as described in claim 2, wherein the thickness of the aluminum layer is in the range of 1 to 3 nm.

4. The method as described in any one of claims 1 to 3, wherein the step of forming the patterned layer comprises the step of growing the patterned layer by molecular beam epitaxy.

5. The method as described in any one of claims 1 to 3, wherein the steps of forming the patterned layer and forming the passivation layer are performed in the same vacuum chamber.

6. The method of any one of claims 1 to 3, wherein the patterned layer is formed in a first vacuum chamber of the sealing device, and the method further comprises the step of transferring the substrate from the first vacuum chamber to a second vacuum chamber after the patterned layer is formed and before the passivation layer is formed.

7. The method as described in any one of claims 1 to 3, further comprising the step of rotating and / or tilting the substrate during the formation of the passivation layer.

8. The method as described in claim 7, wherein the substrate is maintained at a temperature in the range of 50 to 100 K.

9. The method as described in any one of claims 1 to 3, wherein the thickness of the patterned layer is less than or equal to 10 nm, or, where appropriate, less than or equal to 5 nm.

10. The method as described in any one of claims 1 to 3, wherein the material is a superconducting material.

11. The method as described in claim 10, wherein the superconducting material is selected from lead and aluminum.

12. The method as described in any one of claims 1 to 3, wherein the substrate includes a semiconductor component.

13. The method as described in claim 12, further comprising the step of: fabricating the semiconductor component in the sealing apparatus prior to forming the patterned layer.

14. The method as described in claim 12, wherein the semiconductor component comprises one or more nanowires.

15. The method as described in claim 12, wherein the semiconductor component comprises a heterostructure configured to accommodate a two-dimensional electron gas or a two-dimensional hole gas.

16. The method as described in claim 12, wherein the semiconductor component comprises a material of formula 1: where x is in the range of 0 to 1.

17. The method as described in any one of claims 1 to 3, wherein the substrate includes a topological insulator.

18. The method as described in claim 17, wherein the topological insulator is a tellurium compound.

19. The method as described in claim 18, wherein the topological insulator is a material of formula 2: where y is in the range of 0.6 to 0.

9.

20. The method as described in claim 17, wherein the material of the patterned layer is palladium.

Citation Information

Patent Citations

  • Method for the in situ production of Majorana material superconductor hybrid networks and to a hybrid structure which is produced using the method

    US11088312B2

  • Semiconductor device and channel structure thereof

    US20160093745A1

  • Method for the in situ production of majorana material superconductor hybrid networks and to a hybrid structure which is produced using the method

    US20200044137A1