Sodium battery and electric device
By designing the pore structure of the negative electrode active material layer in sodium batteries and using an electrolyte containing M elements to regulate the N/P ratio, the cycle performance and safety problems caused by negative electrode sodium in traditional sodium batteries are solved, and high energy is achieved Improved density and safety performance.
Patent Information
- Application Number
- PCT/CN2024/074782
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-01-31
- Filing Date
- 2024-01-30
- Publication Date
- 2024-11-21
AI Technical Summary
Traditional sodium batteries have reduced circulation performance and safety problems due to negative sodium analysis, and the volume and mass of the negative electrode materials account for a large proportion, which limits the energy density of sodium batteries and cannot meet the market's demand for energy density.
By designing the negative electrode active material layer with pore structure and adding compounds containing M elements to the electrolyte, the N/P ratio is controlled to be less than 1, ensuring that the sodium metal deposited in the negative electrode participates in the cycle during the charging process, increasing the energy density, and passing through the electrolyte The additives in the process guide the sodium metal to uniformly deposit in the negative electrode pore structure to avoid the formation of sodium dendrites and improve circulation and safety performance.
It significantly improves the energy density and cycling performance of sodium batteries, reduces the volume and mass proportion of the negative electrode material, enhances the safety performance of the battery, and achieves higher endurance and comprehensive electrochemical performance.
Smart Images

Figure CN2024074782_21112024_PF_FP_ABST
Abstract
Description
Sodium batteries and electrical equipment
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on January 31, 2023, with application number 202310118805.5 and application name “Sodium Battery and Electrical Equipment”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present application relates to the field of battery technology, and in particular to sodium batteries and electrical equipment. Background Art
[0003] In order to avoid the reduction of sodium battery cycle performance and battery safety issues caused by sodium precipitation in the negative electrode, traditional sodium batteries make the effective capacity of the negative electrode greater than that of the positive electrode. However, the mass specific capacity and volume specific capacity of the negative electrode material are generally lower than those of the positive electrode material. Therefore, the volume and mass proportion of the negative electrode material in traditional sodium batteries is relatively large, which greatly limits the energy density of the sodium battery and cannot fully meet the current market demand for the energy density of sodium batteries.
[0004] Summary of the Invention
[0005] In view of this, the present application provides a sodium battery and electrical equipment. The effective capacity of the negative electrode of this sodium battery is smaller than that of the positive electrode, and sodium metal deposition occurs at the negative electrode during charging. However, through special structural design and electrolyte composition design, the sodium metal deposited at the negative electrode can fully participate in the subsequent cycle process, contributing to the reversible capacity, significantly improving the energy density of the battery, and providing high battery safety performance.
[0006] In a first aspect, the present application provides a sodium battery, comprising:
[0007] positive electrode;
[0008] a negative electrode, the negative electrode comprising a negative electrode active material layer, the negative electrode active material layer having a porous structure;
[0009] a separator disposed between the positive electrode and the negative electrode; and
[0010] An electrolyte, wherein the electrolyte includes an additive, wherein the additive includes at least one compound containing an M element, wherein the M element includes one or more of K, Rb, Cs, and Mg;
[0011] Wherein, the N / P ratio of the sodium battery is less than 1.
[0012] By designing and achieving a battery with an N / P ratio of less than 1, the volume and mass proportion of the negative electrode material in the battery can be reduced, thereby increasing the battery's energy density. Furthermore, the negative electrode active material layer has pores that can accommodate the sodium metal deposited at the negative electrode during charging. This sodium metal will be preferentially discharged during subsequent cycles, contributing to the reversible capacity. Furthermore, the addition of the aforementioned metal salts to the electrolyte facilitates the uniform and efficient deposition of sodium metal within the pore structure of the negative electrode, preventing the formation of sodium dendrites, thereby improving the long-term cycle performance and safety of the sodium battery.
[0013] In some embodiments, 0.4≤N / P<1.
[0014] In some embodiments, 0.5≤N / P≤0.7.
[0015] In some embodiments, the N / P ratio of the sodium battery is controlled by adjusting the ratio of the amount of the positive electrode active material to the amount of the negative electrode active material in the positive electrode.
[0016] In some embodiments, the compound containing element M includes a salt of element M, which salt includes at least one of hexafluorophosphate of element M, bisfluorosulfonyl imide salt of element M, bis(trifluoromethylsulfonyl)imide salt of element M, tetrafluoroborate of element M and nitrate of element M.
[0017] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the additive in the electrolyte is 1%-15%.
[0018] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the additive in the electrolyte is 3%-10%.
[0019] In some embodiments, the electrolyte includes a solvent, and the solvent includes at least one of a non-halogenated ether solvent and a fluorinated ether solvent.
[0020] In some embodiments, the solvent includes a fluoroether solvent.
[0021] In some embodiments, the concentration of sodium salt in the electrolyte is 0.5 mol / L-2 mol / L.
[0022] In some embodiments, the concentration of sodium salt in the electrolyte is 0.6 mol / L-1.2 mol / L.
[0023] In some embodiments, the porosity of the negative electrode active material layer is in the range of 10% to 60%.
[0024] In some embodiments, the porosity of the negative electrode active material layer is in the range of 30%-55%.
[0025] In some embodiments, the negative electrode active material layer includes the negative electrode active material, and the negative electrode active material includes one or more of a carbon-based material, a metal oxide, and a phosphorus-based material.
[0026] In some embodiments, the negative electrode active material includes a carbon-based material.
[0027] In some embodiments, the negative electrode active material includes hard carbon and / or soft carbon.
[0028] In some embodiments, the D50 of the negative active material in the sodium battery is in the range of 2 μm to 10 μm.
[0029] In some embodiments, the positive electrode active material of the sodium battery includes one or more of a layered transition metal oxide, a polyanion compound, and a Prussian blue-based material.
[0030] The second aspect of the present application provides an electrical device comprising the sodium battery provided in the first aspect of the present application. Due to the use of the sodium battery as a power source, the electrical device can have a longer endurance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] FIG1 is a simplified structural design diagram of a sodium battery according to an embodiment.
[0032] Description of reference numerals:
[0033] 10 - sodium battery, 11 - positive electrode, 12 - negative electrode, 121 - negative electrode active material layer, 122 - pores, 13 - separator, 14 - electrolyte. DETAILED DESCRIPTION
[0034] As shown in FIG1 , an embodiment of the present application provides a sodium battery 10, comprising a positive electrode 11, a negative electrode 12, a separator 13 disposed between the positive electrode 11 and the negative electrode 12, and an electrolyte 14; the negative electrode 12 comprises a negative electrode active material layer 121, and the negative electrode active material layer 121 has a porous structure;
[0035] The sodium battery 10 has an N / P ratio of less than 1; the electrolyte includes an additive, the additive includes at least one compound containing an M element, and the M element includes one or more of K, Rb, Cs, and Mg.
[0036] It should be noted that the N / P ratio of the sodium battery 10 in this application can be calculated as "negative electrode reversible surface capacity / positive electrode reversible surface capacity × 100%." Generally, the reversible surface capacity can be calculated as "areal density of active material × gram capacity of active material." The N / P ratio of the sodium battery 10 in this application is less than 1, specifically meaning that, at least when the positive electrode releases its full capacity, the amount of sodium ions that the negative electrode can accept is less than the amount of sodium ions released by the positive electrode during charging. Compared with traditional batteries, the sodium battery 10 provided by the present application reduces the amount of negative electrode material while keeping the amount of positive electrode material unchanged, thereby improving the energy density of the sodium battery; at the same time, the active material layer 121 of the negative electrode 12 has pores 122. During the charging process of the battery, the "excess" sodium ions released by the positive electrode can be deposited in the pore structure of the negative electrode and converted into sodium element, and this part of the "precipitated sodium" is active sodium, which can exert its capacity. That is to say, at least when the state of charge of the sodium battery is 100%, sodium element is deposited in the pore structure of the negative electrode active material layer; in addition, the theoretical specific capacity of sodium element is significantly higher than that of general negative electrode active materials (for example, hard carbon, etc.), so the energy density of the battery is further improved. And K + , Rb + 、Cs + and Mg 2+ It can be adsorbed on the surface of sodium element during the sodium metal deposition process. The accumulation of positive ions on the surface of sodium element can effectively reduce the overpotential of sodium metal deposition, prevent the uneven deposition of sodium ions, avoid the deposition of sodium element on the negative electrode surface, inhibit the formation of sodium dendrites, and promote the uniform deposition of sodium element into active sodium in the pores of the negative electrode active material layer, thereby improving the cycle performance and safety performance of the battery.
[0037] It can be understood that as the amount of negative electrode material used decreases, the thickness of the negative electrode can also be reduced accordingly, thereby effectively reducing the internal resistance of the negative electrode; at the same time, the electrical conductivity of sodium element is relatively high, and after it is deposited on the negative electrode, it can also improve the electrical conductivity of the negative electrode, thereby helping to improve the rate performance of the battery.
[0038] In the present application, illustratively, the N / P ratio of the sodium battery 10 may be 0.3, 0.35, 0.4, 0.45, 0.5, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 0.97, 0.99, etc.
[0039] In this application, taking the negative electrode active material of the sodium battery 10 as an example, the negative electrode active material is converted into Na x C n , and sodium element is deposited in the negative electrode active material layer.
[0040] In some embodiments of the present application, the compound containing the M element includes but is not limited to the salt of the M element, and the salt includes but is not limited to at least one of the hexafluorophosphate of the M element, the bisfluorosulfonyl imide salt of the M element, the bis(trifluoromethylsulfonyl)imide salt of the M element, the tetrafluoroborate of the M element, and the nitrate of the M element. Specifically, the cesium salt includes but is not limited to one or more of cesium hexafluorophosphate, cesium bisfluorosulfonyl imide, bis(trifluoromethylsulfonyl imide), cesium tetrafluoroborate, and cesium nitrate. Exemplarily, the potassium salt includes but is not limited to one or more of potassium hexafluorophosphate, potassium bisfluorosulfonyl imide, potassium nitrate, bis(trifluoromethylsulfonyl imide), and potassium tetrafluoroborate. Rubidium salt includes but is not limited to one or more of rubidium hexafluorophosphate, rubidium bisfluorosulfonyl imide, rubidium nitrate, bis(trifluoromethylsulfonyl imide), and rubidium tetrafluoroborate. The magnesium salt includes, but is not limited to, one or more of magnesium hexafluorophosphate, magnesium bis(fluorosulfonyl imide), magnesium bis(trifluoromethylsulfonyl imide), magnesium tetrafluoroborate, magnesium nitrate, and the like.
[0041] Generally, the negative electrode 12 includes a negative electrode current collector and a negative electrode active material layer 121 disposed on at least one surface of the negative electrode current collector. The negative electrode material layer contains a negative electrode active material, and optionally a conductive agent and a binder. Similarly, the positive electrode 11 includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector. The positive electrode active material layer contains a positive electrode active material, and optionally a conductive agent and a binder.
[0042] In some embodiments of the present application, 0.4≤N / P<1. For example, the N / P of the sodium battery 10 can be 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 0.97, etc. This helps to ensure that the amount of negative electrode active material is sufficient, which can not only achieve normal battery performance, but also control the amount of sodium precipitation in the negative electrode during subsequent cycles within a more reasonable range, fully reducing the risk of sodium dendrites forming on the negative electrode that affect the battery cycle performance and service life, and maximizing the safety of the battery.
[0043] In some embodiments of the present application, 0.5≤N / P≤0.7. For example, the N / P ratio of the sodium battery 10 can be 0.5, 0.52, 0.55, 0.6, 0.65, 0.68, 0.7, and the like. It is understandable that the theoretical specific capacity of sodium is much higher than that of the commonly used negative electrode active materials for sodium batteries. Considering this perspective alone, the lower the N / P ratio of the sodium battery, the better the improvement in the energy density of the sodium battery. However, a very low N / P ratio of a sodium battery can also affect other battery properties. During charging, more sodium metal will be deposited on the negative electrode, resulting in more side reactions and sodium dendrites, faster battery capacity decay, and difficulty achieving an optimal cycle life. Currently, no one has yet found a balance in the impact of the N / P ratio of sodium batteries on various factors. After theoretical derivation and extensive experiments, the applicant discovered that controlling the N / P ratio of the battery within the above range can significantly improve the battery's energy density while ensuring the battery's cycle life, resulting in a sodium battery with the best overall electrochemical performance.
[0044] In some embodiments of the present application, the N / P ratio of the battery can be controlled by adjusting the ratio of the amount of positive electrode active material to the amount of negative electrode active material in the positive electrode. Taking into account the different specific capacity performances of different positive and negative electrode active materials, those skilled in the art can make adjustments based on actual production conditions. Generally, the N / P ratio can be calculated by "reversible surface capacity of the negative electrode / reversible surface capacity of the positive electrode × 100%". Generally, the reversible surface capacity can be calculated by "areal density of active material × gram capacity of active material". Taking the above-mentioned sodium battery 10 where the negative electrode active material is a hard carbon material as an example, the reversible surface capacity of the negative electrode of the sodium battery is "areal density of hard carbon × gram capacity of hard carbon".
[0045] In some embodiments of the present application, the porosity of the negative electrode active material layer 121 is in the range of 10%-60%. For example, the porosity of the negative electrode active material layer can be 10%, 15%, 20%, 25%, 30%, 32.5%, 35%, 37.5%, 38%, 39%, 40%, 45%, 50%, 55%, 60%, etc. In some specific embodiments, the porosity of the negative electrode active material layer can be in the range of 30%-55%. Controlling the porosity of the negative electrode active material layer within the above range can not only reserve sufficient space to accommodate the deposited sodium element, and ensure that the sodium element is deposited in the pore structure to the greatest extent, so as to fully improve the final battery cycle performance and extend the battery cycle life, but also ensure that the negative electrode has a large compaction density, which can further ensure that the battery has both high energy density and good cycle performance. In the present application, the porosity of the negative electrode active material layer may be calculated as follows: pore volume of the negative electrode active material layer / total volume of the negative electrode×100%. Specifically, the porosity may be measured using mercury intrusion porosimetry.
[0046] In some embodiments of the present application, the pores in the negative electrode active material layer are primarily formed by the arrangement of negative electrode active material particles, conductive agents, binders, and other substances, and may also include pores within the negative electrode active material particles (e.g., hard carbon) themselves. It should be noted that the porosity measured by mercury intrusion porosimetry only includes pores formed by the arrangement of negative electrode active material particles, conductive agents, binders, and other substances. It is understandable that even if the pores within the hard carbon itself are not included in the measurement using the mercury intrusion porosimetry method, a small amount of active sodium may be deposited within the pore structure of the hard carbon material itself.
[0047] In some embodiments of the present application, the D50 of the negative electrode active material particles is within the range of 2μm-10μm. For example, the D50 of the negative electrode active material can be 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, etc. Controlling the D50 of the negative electrode active material particles within the above range is conducive to forming a sufficient number of pore structures with appropriate pore sizes in the negative electrode, and is also conducive to obtaining a negative electrode with a high compaction density.
[0048] In some embodiments of the present application, the negative electrode active material layer includes a negative electrode active material, which includes but is not limited to one or more of carbon-based materials, metal oxides, and phosphorus-based materials. Phosphorus-based materials include but are not limited to one or more of phosphides and phosphorus-carbon materials. In some specific embodiments, the negative electrode active material includes a carbon-based material. In some specific examples, the negative electrode active material includes but is not limited to hard carbon and / or soft carbon. Hard carbon and soft carbon are currently the materials with the greatest commercial potential among negative electrode materials for sodium batteries.
[0049] In some embodiments of the present application, the positive electrode active material is not limited to one or more of layered transition metal oxides, polyanion compounds and Prussian blue materials. The chemical formula of the layered transition metal oxide can be Na x AO2, wherein A is not limited to one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, 0<x≤1. The polyanionic compound includes one or more of sodium vanadium trifluorophosphate Na3V2(PO4)2F3, sodium vanadium fluorophosphate NaVPO4F, sodium vanadium phosphate Na3V2(PO4)3, Na4Fe3(PO4)2P2O7, NaFePO4, Na3V2(PO4)3. The Prussian blue compound can be expressed as Na y E1E2(CN)6, wherein E1 and E2 independently include one or more of Fe, Mn, Co, Ni, Cu, Zn, Cr, Ti, V, Zr and Ce, wherein 0<y≤2.
[0050] In some embodiments of the present application, the mass percentage of the additive in the electrolyte 14 is in the range of 1%-15% based on the total mass of the electrolyte 14. For example, the mass percentage of the additive in the electrolyte can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, etc.
[0051] In some embodiments of the present application, the mass percentage of the additive in the electrolyte 14 is within the range of 3%-10% based on the total mass of the electrolyte 14. For example, the mass percentage of the additive in the electrolyte can be 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc. By controlling the content of the additive within the above range, there can be sufficient M ions in the electrolyte to induce the uniform deposition of sodium ions in the pore structure of the negative electrode to achieve the effect of inhibiting the growth of sodium dendrites, without affecting the transport and deposition of sodium ions in the electrolyte, and without affecting the performance of the SEI film, so that the comprehensive electrochemical performance of the final sodium battery can be better.
[0052] In some embodiments of the present application, the electrolyte 14 includes a solvent, and the above-mentioned solvent includes at least one of a non-halogenated ether solvent and a fluoroether solvent. Among them, the non-halogenated ether solvent includes but is not limited to one or more of diethylene glycol dimethyl ether, ethylene glycol dimethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol monomethyl ether and tetraethylene glycol dimethyl ether. In some specific embodiments, the non-halogenated ether solvent is diethylene glycol dimethyl ether, which is more conducive to improving the energy density and cycle performance of the battery. The fluoroether solvent includes but is not limited to 1,1,2,2,-tetrafluoroethyl ether, 1,1,2,2,-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, hexafluoroisopropyl ether, tetrafluoroethyl tetrafluoropropyl ether, 2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, difluoromethyl-2,2,3,3-tetrafluoropropyl ether, 2,2,3,3 ,3-pentafluoropropyl methyl ether, 1,1,2,3,3,3-hexafluoropropyl ethyl ether, 1,1,2,3,3,3-pentafluoropropyl difluoromethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether, bis(2,2,2-trifluoroethyl) ether and bis(2,2-difluoroethyl) ether. Compared with the carbonate solvents commonly used in the prior art, ether solvents are more friendly to carbon-based negative electrode materials and have stronger compatibility. They can effectively inhibit the consumption of active sodium during the cycle process; and the solid electrolyte interface (SEI) film formed on the negative electrode surface is thinner, which is beneficial to ensuring the cycle performance of the battery, and is also beneficial to promoting the diffusion rate of Na+, thereby improving the rate performance of the battery. In some specific embodiments, the solvent includes a fluoroether solvent. Fluorinated ether solvents can also be used as diluents for electrolytes. The introduction of fluorine atoms can effectively improve the oxidative stability of ether molecules. The presence of fluorine in the SEI film can also effectively improve its structural stability, thereby significantly improving the cycle stability of the battery. At the same time, fluorine can also promote the attachment of M ions to the surface of sodium elements, which can better promote the deposition of sodium elements in the pores of the negative electrode active material layer. In addition, the local strong polarity of the fluorinated end group can improve the ionic conductivity of the electrolyte, construct a local super-concentrated electrolyte, and promote the conversion of sodium elements deposited at the negative electrode into Na+ during the discharge process. In some specific embodiments, the conversion rate of sodium elements deposited at the negative electrode during a single discharge process can be greater than 99%. In some specific embodiments, the solvent includes both non-halogenated ether solvents and fluorinated ether solvents, and the mixed use of the electrolyte has a better effect.
[0053] In some embodiments of the present application, the sodium salt concentration in the electrolyte 14 is 0.5 mol / L-2 mol / L. For example, the sodium salt concentration in the electrolyte can be 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1.0 mol / L, 1.1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L, etc. In some specific embodiments, the sodium salt concentration in the electrolyte is 0.6 mol / L-1.2 mol / L. Among them, the sodium salt includes but is not limited to one or more of sodium hexafluorophosphate, sodium perchlorate, sodium bisfluorosulfonyl imide, sodium bisfluorosulfonyl imide, sodium bistrifluoromethanesulfonyl imide, sodium trifluoromethanesulfonate, sodium tetrafluoroborate, sodium difluorophosphate, sodium tetraphenylborate and sodium chloride.
[0054] The present application also provides an electrical device including the sodium battery 10. The electrical device may be a vehicle, an energy storage device, or an electronic device. The vehicle may be a pure electric vehicle, a hybrid electric vehicle, or the like; the electronic device may be a consumer electronics product, or the like.
[0055] The technical solution of this application is described in detail below with multiple embodiments.
[0056] Example 1
[0057] (1) Preparation of negative electrode: The negative electrode active material - hard carbon (gram capacity of 320 mAh / g), conductive agent (specifically Super-P), binder - sodium carboxymethyl cellulose (CMC), binder - styrene-butadiene rubber (SBR) emulsion (solid content of SBR emulsion is 40%) are mixed in water at a mass ratio of 95:1.5:1.5:5 to prepare negative electrode slurry. The negative electrode active material is coated with a coating machine at a surface density of 9.75 mg / cm 2 , coating width 200mm, apply negative electrode slurry on the surface of negative electrode current collector (specifically aluminum foil) and dry it, then pass the cold press to press the coated electrode at 1.0g / cm 3 The negative electrode was cold pressed according to the designed compaction density, cut and cut to obtain the final negative electrode, wherein the porosity of the negative electrode active material layer was 40.1%;
[0058] (2) Preparation of positive electrode: positive electrode active material - NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 The O2 material (with a gram capacity of 130 mAh / g), a binder - polyvinylidene fluoride (PVDF), and a conductive agent (specifically Super-P) were mixed uniformly in a solvent (specifically N-methylpyrrolidone) at a mass ratio of 96:2:2 to prepare a positive electrode slurry. The positive electrode active material surface density was 40 mg / cm using an extrusion coater. 2, the coating width is 200mm. The positive electrode slurry is coated on the surface of the positive electrode collector (specifically aluminum foil) and dried, and then the coated electrode is pressed by a cold press at 3.0g / cm 3 The designed compact is cold pressed, cut and prepared to obtain the final positive electrode.
[0059] (3) Preparation of electrolyte: Dissolve 1 mol of sodium salt NaPF6 in 1 L of solvent diethylene glycol dimethyl ether to obtain a 1 mol / L NaPF6 organic solution, and then add 3 wt.% of additive CsPF6 to obtain an electrolyte.
[0060] (4) The negative electrode prepared in step (1), the positive electrode prepared in step (2), and a separator (specifically a polypropylene / polyethylene composite separator) are stacked in sequence so that the separator separates the positive and negative electrodes, and wound into a dry battery cell. After welding and aluminum-plastic film packaging, the electrolyte prepared in step (3) is injected, and then vacuum-sealed. After being left at 60° C. for 48 h, pressurized at 45° C., vented, repackaged, and capacity divided, a soft-pack sodium battery with a capacity of 30 Ah is obtained. The electrolyte injection amount is set at 3.5 g / Ah.
[0061] The N / P ratio of the prepared sodium battery was 0.6.
[0062] Example 2
[0063] The difference from Example 1 is that the amount of the negative electrode active material - hard carbon is adjusted so that the N / P ratio of the sodium battery is 0.5 and the porosity of the negative electrode active material layer is 45.2%.
[0064] Example 3
[0065] The difference from Example 1 is that the amount of the negative electrode active material - hard carbon is adjusted so that the N / P ratio of the sodium battery is 0.7 and the porosity of the negative electrode active material layer is 40.6%.
[0066] Example 4
[0067] The difference from Example 1 is that the amount of the negative electrode active material - hard carbon is adjusted so that the N / P ratio of the sodium battery is 0.4 and the porosity of the negative electrode active material layer is 54.0%.
[0068] Example 5
[0069] The difference from Example 1 is that the amount of the negative electrode active material, hard carbon, is adjusted so that the N / P ratio of the sodium battery is 0.95. The porosity of the active material layer is 30.5%.
[0070] Example 6
[0071] The difference from Example 1 is that the porosity of the negative electrode material layer is adjusted so that the porosity of the negative electrode active material layer is 8%.
[0072] Example 7
[0073] The difference from Example 1 is that the porosity of the negative electrode material layer is adjusted so that the porosity of the negative electrode active material layer is 20%.
[0074] Example 8
[0075] The difference from Example 1 is that the additive added to the electrolyte is replaced by MgNO3 instead of CsPF6.
[0076] Example 9
[0077] The difference from Example 1 is that the additive added to the electrolyte is replaced by RbNO3 instead of CsPF6.
[0078] Example 10
[0079] The difference from Example 1 is that the additive added to the electrolyte is replaced by KPF6 instead of CsPF6.
[0080] Example 11
[0081] The only difference from Example 1 is that the content of the additive in the electrolyte is 11 wt.%.
[0082] Example 12
[0083] The difference from Example 1 is that the sodium salt in the electrolyte is replaced by NaClO4 instead of NaPF6.
[0084] Example 13
[0085] The difference from Example 1 is that the electrolyte solvent is replaced by ethylene glycol dimethyl ether instead of diethylene glycol dimethyl ether.
[0086] Example 14
[0087] The difference from Example 1 is that the electrolyte solvent is replaced by 1,1,2,2,-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether instead of diethylene glycol dimethyl ether.
[0088] Example 15
[0089] The difference from Example 1 is that the electrolyte solvent is replaced by diethylene glycol dimethyl ether with diethylene glycol dimethyl ether: 1,1,2,2,-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether in a volume ratio of 4:6.
[0090] In order to highlight the beneficial effects of the embodiments of the present application, the following comparative examples are provided.
[0091] Comparative Example 1
[0092] The only difference from Example 1 is that the electrolyte does not contain additives.
[0093] Comparative Example 2
[0094] The only difference from Example 1 is that the amount of the negative electrode active material is adjusted so that the N / P ratio of the battery is 1.1.
[0095] Comparative Example 3
[0096] The only difference from Example 1 is that the amount of the negative electrode active material is adjusted so that the N / P ratio of the battery is 1.1, and the electrolyte does not contain any additives.
[0097] Electrochemical performance tests were performed on the sodium batteries of the above embodiments and comparative examples.
[0098] (1) Cycling performance: Each sodium battery was subjected to charge and discharge cycle tests at 25°C with a current rate of 0.33C and a voltage range of 2.0V-4.0V. During charging, the battery was first charged at a constant current of 0.33C to a cutoff voltage of 4.0V, and then charged at a constant voltage to a cutoff current of 0.05C. During discharge, the battery was discharged at a constant current of 0.33C to 2.0V. The first-cycle discharge capacity of each battery and the capacity retention rate after 500 cycles were recorded. The first-cycle discharge capacity is equal to the ratio of the first-cycle discharge capacity of each sodium battery to the mass of the positive electrode active material in the battery; the capacity retention rate after 500 cycles is equal to the ratio of the discharge capacity after 500 cycles to the first-cycle discharge capacity. The results are summarized in Table 1.
[0099] In addition, the discharge curves of each battery obtained by the above-mentioned 0.1C constant current charge and discharge were integrated and divided by the first cycle discharge capacity to obtain the average voltage of each battery, that is, the charge and discharge voltage platform. The weight energy density of each sodium battery was then calculated according to the following formula:
[0100] Gravimetric energy density = fractional capacity × average voltage platform / battery weight. The results are summarized in Table 1.
[0101] Table 1 Summary of electrochemical performance test results of sodium batteries in various embodiments and comparative examples
[0102] It can be seen from the results in Table 1 that the weight energy density of the batteries of the embodiments of the present application is significantly higher than that of the comparative example batteries 2-3, and under the same N / P ratio, the cycle performance of the battery of Example 1 is significantly better than that of the battery of Comparative Example 1, which fully demonstrates the superiority of the batteries of the embodiments of the present application. Comparing the batteries of the embodiments, it can be found that when the N / P ratio of the battery is controlled within the range of 0.5-0.7, the comprehensive electrochemical performance of the battery is better; comparing the data of Example 1 and Examples 6-7, it can be found that when other conditions remain unchanged, when the porosity of the negative electrode active material layer is within the preferred range of this application, the 500-cycle capacity retention rate of the battery is significantly higher, and the weight energy density of the battery is also maintained at a high level (Example 1); when the additive content is within the preferred range of this application, the performance of the battery is also better; when the electrolyte solvent is selected or contains a fluoroether solvent, it can also further enhance the electrochemical performance of the battery and further enhance the capacity cycle retention rate of the battery.
[0103] In the description of this specification, “a plurality of” means at least two, for example, two, three, etc., unless otherwise clearly defined.
[0104] The above is an exemplary embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made thereto without departing from the principles of the present application. These improvements and modifications are also considered to be within the scope of protection of the present application.
Claims
1. A sodium battery (10), It is characterized in that include: Anode (11); A negative electrode (12), the negative electrode (12) comprising a negative electrode active material layer (121), the negative electrode active material layer (121) having a pore (122) structure; a separator (13), the separator (13) being disposed between the positive electrode (11) and the negative electrode (12); and An electrolyte (14), wherein the electrolyte (14) comprises an additive, wherein the additive comprises at least one compound containing an M element, wherein the M element comprises one or more of K, Rb, Cs and Mg; Wherein, the N / P ratio of the sodium battery (10) is less than 1.
2. The sodium battery (10) according to claim 1, It is characterized in that 0.4≤N / P<1.
3. The sodium battery (10) according to claim 1 or 2, It is characterized in that 0.5≤N / P≤0.
7.
4. The sodium battery (10) according to any one of claims 1 to 3, wherein the N / P ratio of the sodium battery (10) is regulated by regulating the ratio of the amount of the positive electrode active material in the positive electrode (11) to the amount of the active material in the negative electrode (12).
5. The sodium battery (10) according to any one of claims 1 to 4, It is characterized in that The compound containing element M includes a salt of element M, and the salt includes at least one of hexafluorophosphate of element M, bisfluorosulfonyl imide salt of element M, bis(trifluoromethylsulfonyl)imide salt of element M, tetrafluoroborate of element M and nitrate of element M.
6. The sodium battery (10) according to any one of claims 1 to 5, It is characterized in that Based on the total mass of the electrolyte (14), the mass percentage of the additive in the electrolyte (14) is 1%-15%.
7. The sodium battery (10) according to any one of claims 1 to 6, It is characterized in that Based on the total mass of the electrolyte (14), the mass percentage of the additive in the electrolyte (14) is 3%-10%.
8. The sodium battery (10) according to any one of claims 1 to 7, It is characterized in that The electrolyte (14) includes a solvent, and the solvent includes at least one of a non-halogenated ether solvent and a fluorinated ether solvent.
9. The sodium battery (10) according to claim 8, It is characterized in that The solvent includes a fluoroether solvent.
10. The sodium battery (10) according to any one of claims 1 to 9, It is characterized in that The sodium salt concentration in the electrolyte is 0.5 mol / L-2 mol / L.
11. The sodium battery (10) according to claim 10, It is characterized in that The sodium salt concentration in the electrolyte is 0.6 mol / L-1.2 mol / L.
12. The sodium battery (10) according to any one of claims 1 to 11, It is characterized in that The porosity of the negative electrode active material layer (121) is in the range of 10% to 60%.
13. The sodium battery (10) according to claim 12, It is characterized in that The porosity of the negative electrode active material layer (121) is in the range of 30%-55%.
14. The sodium battery (10) according to any one of claims 1 to 13, It is characterized in that The negative electrode active material layer (121) includes a negative electrode active material, and the negative electrode active material includes one or more of a carbon-based material, a metal oxide, and a phosphorus-based material.
15. The sodium battery (10) according to claim 14, It is characterized in that The negative electrode active material includes a carbon-based material.
16. The sodium battery (10) according to claim 14 or 15, It is characterized in that The negative electrode active material includes hard carbon and / or soft carbon.
17. The sodium battery (10) according to any one of claims 1 to 16, It is characterized in that The D50 of the negative electrode active material in the sodium battery (10) is in the range of 2 μm-10 μm.
18. The sodium battery (10) according to any one of claims 1 to 17, It is characterized in that The positive electrode active material of the sodium battery (10) comprises one or more of layered transition metal oxides, polyanion compounds and Prussian blue materials.
19. An electrical device, It is characterized in that The electrical equipment comprises the sodium battery (10) according to any one of claims 1 to 18.