Lithium-ion battery positive electrode material precursor and preparation method therefor
By optimizing the XRD peak intensity ratio and grain size ratio of the precursor, the problems of low capacity and poor cycle performance of layered oxide cathode materials are solved, and cathode materials with high capacity and cycle stability are achieved. Layered oxides are achieved by controlling reaction parameters. Structural optimization.
Patent Information
- Application Number
- PCT/CN2023/085405
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-03
AI Technical Summary
Existing layered oxide cathode materials have low capacity and poor cycle performance, and the relationship between the microstructure of the precursor and the microstructure of the cathode material has not been effectively explained. There is no regular description of the peak intensity ratio and the structure of the precursor. .
Provides a lithium-ion battery cathode material precursor, whose general formula is NiaMnbMcNd(OH)e, with XRD peak intensity ratio I(101)/I(001) < 0.75 and grain size ratio D(102)/D(001 ) < 0.65, by controlling the feed speed and stirring speed of the reactor salt solution, alkaline solution and complexing agent solution to meet the specific reaction parameter formula, the layered structure and grain size ratio of the precursor can be optimized.
The cathode material obtained by sintering has an excellent layered structure, reduces crystal structure defects such as lithium and nickel mixing, displays higher discharge capacity and cycle stability, is simple to operate, has good product consistency, and is easy to be industrialized.
Smart Images

Figure CN2023085405_03102024_PF_FP_ABST
Abstract
Description
A lithium-ion battery positive electrode material precursor and preparation method Technical Field
[0001] The present invention belongs to the field of manufacturing positive electrode materials for lithium ion batteries, and particularly relates to a positive electrode material precursor for lithium ion batteries and a preparation method thereof, a positive electrode material for lithium ion batteries and a preparation method thereof, and a lithium ion battery positive electrode and a lithium ion battery comprising the positive electrode material. Background Art
[0002] Over the past three decades, lithium-ion batteries have seen increasing adoption due to their high energy density and flexible applicability. Over the years, the cathode materials used in lithium-ion batteries have evolved from the original lithium cobalt oxide to three main categories: olivine-structured materials such as lithium iron phosphate, layered oxide materials such as lithium nickel cobalt manganese oxide, and spinel-structured materials such as lithium nickel manganese oxide. Layered oxide cathode materials, in both power and non-power lithium-ion batteries, hold a significant position in the cathode material market due to their excellent cycling performance, high capacity, and high voltage.
[0003] Currently, the vast majority of layered oxide cathode materials are produced using a precursor route. The structure of the precursor is highly inherited across the structure of layered oxide cathode materials. In materials science, it's well known that structure determines performance. Therefore, the electrochemical performance of cathode materials is closely related to the structure of the precursor, which in turn is determined by the preparation technology used.
[0004] The structure of the precursor includes a macrostructure (hundreds of nanometers to micrometers) and a microstructure (subnanometer to tens of nanometers). From a microscopic point of view, the precursor belongs to the hexagonal crystal system, which is a layered compound formed by stacking MO layers arranged in order of MO octahedrons along the c-axis, and the layers are connected by hydrogen bonds. Among them, the metal elements and oxygen atoms are stacked hexagonally in their respective layers. In some well-developed crystals, two-dimensional wafers that are close to hexagons will be formed, but in actual precursors, the hexagonal shape of the two-dimensional wafer is affected by many factors and is not obvious enough. By gradually enlarging the microscopic scale, it can be observed that the two-dimensional wafers will be stacked in a manner that is close to parallel to each other to form primary particles. The primary particles are then stacked, crossed, and even entangled with each other in a relatively more disordered manner to form commercial precursor secondary particles.
[0005] There are many patents that explain the structure of the precursor from a macroscopic perspective.
[0006] In CN111653756B, a precursor is described, which includes secondary particles formed by the aggregation of multiple primary particles. The secondary particles include multiple loose layers and multiple dense layers alternately distributed from their own core to the outer surface, and the innermost part of the secondary particles is the loose layer and the outermost part is the dense layer. The patent also defines the thickness relationship between the loose layer and the dense layer.
[0007] CN114988495A describes a multi-element co-agglomerated precursor, consisting of 3-6 small particles agglomerated to form large, spherical particles. This co-agglomerated precursor can effectively reduce the firing temperature of single-crystal cathodes, saving production costs. It can also reduce crystal structure defects such as lithium-nickel intermixing, resulting in improved capacity, rate, and cycle performance.
[0008] In CN107342417B, a precursor material with filamentous primary particles is described, and the average particle size of the primary particles and the particle size range of the secondary particle agglomerates of the material are defined; CN105731553A and CN105355907A both mention the influence of the precursor primary particles on the performance of the finished product; CN105355907A proposes a precursor with an annual ring structure.
[0009] The above-mentioned existing technologies all explain their performance and impact on the positive electrode material from the aspects of the arrangement of primary particles, size (greater than 100 nanometers), looseness and density of secondary particles, but do not explain the more microscopic structure of the precursor. However, how the atoms that make up the precursor are arranged at the microscopic scale of sub-nanometer to nanometer level, and what arrangement rules are used, are what truly determine the structure and performance of the precursor. Just like a high-rise building, its stability is determined by how each brick and the reinforced concrete in it are laid, rather than by its external shape and the shape and size of the room.
[0010] A simplified diagram of the microstructure of the precursor and layered oxide cathode material is shown in Figure 1. In both the precursor and cathode material, the atoms in the transition metal (TM) and O layers, which form the main structural components, are packed in a hexagonal closest-packed arrangement, stacking layer by layer along the c-axis in the order O-TM-O…O-TM-O. The only difference is that in the precursor, there are two layers of H between adjacent O layers, which are omitted in Figure 1. In the cathode material, these two layers of H are replaced by a layer of Li ions, forming a tighter ionic bond between the layers. It is precisely because of this close microstructural connection that the precursor has a non-negligible influence on the structure of the cathode material, which in turn significantly affects its physical, chemical, and electrochemical properties.
[0011] XRD is often used to characterize the microstructure of crystals. In the precursor, the (001) and (101) crystal planes are of particular interest. In CN112777647A, a high nickel hydroxide with a narrow particle size distribution is provided. The D50 of the secondary particles of the high nickel hydroxide is 10-15 μm, and the diameter distance (D90-D10) / D50≤0.68. It is believed that controlling the ratio of (D90-D10) / D50 to no more than 0.68 can effectively fill and improve the compaction density of the positive electrode material. In this patent application, it is also mentioned that the peak intensity ratio of (001) and (101) is between 1.0-1.7. It is believed that the half-peak width ratio and peak area ratio corresponding to (001) and (101) can reflect the primary particle morphology and grain orientation of the precursor, which is related to the capacity, cycle and other electrical properties of the positive electrode material after sintering. CN113321245A introduces a nickel-cobalt-manganese hydroxide, which, by using a specific preparation method, achieves a higher XRD peak intensity ratio of I (101 / 001≥0.95). The patent application believes that a higher peak intensity ratio gives the precursor material better connectivity and permeability, facilitates full contact with the lithium source during sintering, and has higher reaction activity. CN113387399A introduces a high-nickel precursor, and defines the peak intensity ratio of the (101) peak to the (001) peak in the XRD diagram as I (101) / I (001) > 0.8. CN112151790B introduces a high-nickel precursor Ni x Co y Mn z (OH)2, and limit the XRD peak intensity ratio I101 / I001>1.2.
[0012] In the above-cited and other published but uncited prior art related to the peak intensity ratio of precursors, although most of them believe that a higher peak intensity ratio (generally greater than 0.8) is beneficial to the sintering and various electrochemical properties of the positive electrode material, no one has paid attention to the fact that a smaller peak intensity ratio has a more favorable effect on the material performance. No one has yet explained the relationship between the peak intensity ratio and the precursor structure from a microscopic perspective, nor has there been any regular explanation of the corresponding relationship between the precursor microstructure and the positive electrode material microstructure, let alone an explanation of the effect of the precursor grain size ratio on the positive electrode material. Therefore, the current low capacity and poor cycle performance of commercial layered oxide positive electrode materials still need to be solved from the perspective of precursors.
[0013] Summary of the Invention
[0014] In view of the deficiencies of the prior art, the object of the present invention is to provide a precursor of a lithium-ion battery cathode material and a preparation method thereof, a precursor of a lithium-ion battery cathode material and a preparation method thereof, a lithium-ion battery cathode material and a preparation method thereof, and a lithium-ion battery cathode and a lithium-ion battery including the cathode material. The cathode material of the lithium-ion battery prepared using this precursor has a high capacity and excellent cycling performance.
[0015] To achieve the above object of the invention, a first aspect of the present invention provides a precursor of a lithium-ion battery cathode material.
[0016] The precursor of the lithium-ion battery cathode material described in the present invention has the general formula Ni a Mn b M c N d (OH) e , where 0 < a ≤ 1, preferably 0.5 ≤ a < 1; 0 ≤ b ≤ 1, preferably 0 ≤ b ≤ 0.5; 0 ≤ c ≤ 1, preferably 0 ≤ c ≤ 0.5; 0 ≤ d ≤ 1, preferably 0 ≤ d ≤ 0.5; 1.8 ≤ e ≤ 2.2, a + b + c + d = 1, M is at least one selected from Co, Fe, Cu, Mo, W, Zn, Cr, and Ti, and N contains at least Al, S, Na, Ca, Mg, Mo, Nb, Zr, V, Sc, P, Sr, Ba, Cl, F, Si, Ge, B, C, or K. Wherein, the precursor of the lithium-ion battery cathode material is a layered structure and has an XRD peak intensity ratio I(101) / I(001) < 0.75 and a grain size ratio D(102) / D(001) < 0.65.
[0017] In the XRD pattern of the layered oxide cathode material, I(003) / I(104) is a parameter that has received wide attention. Generally, when I(003) / I(104) > 1.2, the material has a good layered structure. The (003) and (104) crystal planes of the cathode material have a strong inheritance relationship with the atomic arrangement and stacking mode of the precursor. Specifically, the (001) crystal plane of the precursor perpendicular to the c-axis directly corresponds to the (003) crystal plane of the cathode material. Although the (104) crystal plane of the cathode material is not directly corresponding to the (101) and (102) crystal planes of the precursor, it has a close relationship with both of these crystal planes and is affected by both of them. Therefore, smaller I(101) / I(001) and D(102) / D(001) values are beneficial for the cathode material to obtain a higher I(003) / I(104) value, maintain a better layered structure, and exhibit better capacity and cycling performance.
[0018] Preferably, the median particle size, i.e., D50, of the precursor of the lithium-ion battery cathode material described in the present invention is 3 - 11 μm.
[0019] Preferably, the lithium-ion battery cathode material precursor of the present invention is spherical, with the major axis of the spherical shape being x and the minor axis being y, then 1<major axis x / minor axis y<2.
[0020] Preferably, the cathode material precursor of the lithium-ion battery of the present invention is: Ni 0.5 Co 0.2 Mn 0.3 (OH)2、Ni 0.90 Co 0.05 Mn 0.05 (OH)2 or Ni 0.90 Co 0.08 Al 0.02 (OH)2、Ni 0.90 Mn 0.08 Cu 0.01 Mg 0.01 (OH)2 or Ni 0.80 Co 0.05 Mn 0.05 Fe 0.05 Zr 0.05 (OH)2.
[0021] To achieve the above-mentioned object of the invention, the second aspect of the present invention further provides a method for preparing a positive electrode material precursor for a lithium-ion battery, comprising the following steps:
[0022] S1) solution preparation step: providing a mixed salt solution comprising nickel salt, manganese salt, M salt and N salt, an alkaline solution and a complexing agent solution;
[0023] S2) Synthesis step: continuously adding the mixed salt solution, alkaline solution, and complexing agent solution to the reaction base solution, and controlling the reaction parameters until the precursor D50 slowly grows to the target particle size, wherein the reaction parameters must satisfy the formula:
[0024] Wherein, J value is between 1 and 13 (1≤J≤13), S is the stirring speed value of the stirring blade, in rpm; T is the reaction temperature value, in °C; V 盐 is the feed rate of the mixed salt solution, in L / h; V 碱 is the feed rate of alkaline solution, in L / h; V 络合剂 is the feeding rate of the complexing agent solution, in L / h; K is a fixed value, K=5000;
[0025] S3) Filtration and washing: performing solid-liquid separation on the mixture obtained in step S2, and washing the solid with a washing liquid;
[0026] S4) Drying: The wet solid obtained in step S3 is dried, demagnetized, sieved and packaged.
[0027] Preferably, the mixed salt solution, alkaline solution and complexing agent solution in step S1 are all aqueous solutions.
[0028] Preferably, in step S1 , the molar ratio of nickel ions: manganese ions: M ions: N ions is a:b:c:d.
[0029] Preferably, the total concentration of nickel ions, manganese ions, M ions, and N ions is 1 to 3 mol / L.
[0030] Preferably, the alkaline solution in step S1 is an alkali metal hydroxide solution, and more preferably, the alkaline solution is a NaOH solution.
[0031] Preferably, the concentration of the alkaline solution is 2 to 12 mol / L.
[0032] Preferably, the complexing agent solution in step S1 is selected from one or more of an aqueous ammonia solution, a urea solution, and a soluble ammonium salt solution.
[0033] Preferably, the concentration of the complexing agent solution is 4 to 12 mol / L.
[0034] Preferably, the D50 target particle size in step S2 is 3 to 11 μm, preferably 3 to 5 μm.
[0035] Preferably, the base liquid in step S2 is water or an ammonia solution.
[0036] Preferably, the J value in step S2 is 1-8.
[0037] Preferably, the washing in step S3 is performed until the content of the anion element in the mixed salt contained in the washed solid is less than 5000 ppm. For example, when the anion in the mixed salt is sulfate ion, the content of sulfur element is measured; when the anion in the mixed salt is chloride ion, the content of chloride element is measured.
[0038] Preferably, the drying temperature in step S4 is ≥100° C., and the drying time is ≥3 h.
[0039] According to a third aspect of the present invention, there is provided a method for preparing a positive electrode material for a lithium ion battery, comprising the following steps:
[0040] a1) mixing the lithium ion battery cathode material precursor of the present invention and a lithium source in a molar ratio of the precursor to the lithium element of 1:1.01-1.05;
[0041] a2) placing the mixture obtained in step a1) into a tube furnace and sintering it at 650-1000°C in an oxygen atmosphere to obtain the positive electrode material LiNi a Mnb M c N d O f , where 1.8≤f≤2.2.
[0042] Preferably, the lithium source is lithium carbonate or lithium hydroxide.
[0043] According to a fourth aspect of the present invention, a lithium ion battery positive electrode material is provided, which is LiNi a Mn b M c N d O f , wherein the definitions of M, N, a, b, c, d and f are the same as those above.
[0044] The lithium-ion battery positive electrode material is prepared according to the method for preparing a lithium-ion battery positive electrode material of the present invention.
[0045] Preferably, the positive electrode material of the lithium-ion battery is LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.90 Co 0.05 Mn 0.05 O2、LiNi 0.90 Co 0.08 Al 0.02 O2、LiNi 0.90 Mn 0.08 Cu 0.01 Mg 0.01 O2 or LiNi 0.80 Co 0.05 Mn 0.05 Fe 0.05 Zr 0.05 O2.
[0046] According to a fifth aspect of the present invention, a positive electrode of a lithium ion battery is provided, comprising the positive electrode material of the lithium ion battery according to the present invention.
[0047] According to a sixth aspect of the present invention, a lithium ion battery is provided, comprising the positive electrode according to the present invention.
[0048] The positive effects of the present invention are:
[0049] The present invention provides a positive electrode material precursor for a lithium-ion battery. When the precursor has an XRD peak intensity ratio I(101) / I(001) less than 0.75 and a grain size ratio D(102) / D(001) less than 0.65, the positive electrode material obtained by sintering has an excellent layered structure, reduces crystal structure defects such as lithium-nickel mixing, and exhibits higher discharge capacity and cycle stability compared with the prior art.
[0050] The present invention provides a simple and easy-to-operate method for preparing a precursor. By controlling the feed rate of the salt solution, alkaline solution, and complexing agent solution in the reactor, as well as the stirring speed and reaction temperature to satisfy a specific relationship, the metal salt solution, alkaline solution, and complexing agent solution in the reactor are uniformly mixed to cause a coprecipitation reaction. When the reaction process satisfies the parameter formula provided by the present invention, the growth dominant orientation of ions deposited on the crystal can be controlled, resulting in a result in which the (001) peak intensity has a certain advantage over the (101) peak intensity, and the (001) crystal plane size is also larger than the (102) crystal plane size to a certain extent, ultimately achieving I(101) / I(001)<0.75 and D(102) / D(001)<0.65. The method is simple to operate, the obtained product has good consistency, and is easy to promote industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 is a schematic diagram of the microstructure of the precursor and cathode materials.
[0052] FIG2 is a flow chart showing a method for preparing a cathode material precursor for a lithium-ion battery according to one embodiment of the present invention. DETAILED DESCRIPTION
[0053] Hereinafter, the present invention will be further described through examples, but the present invention is not limited to the examples.
[0054] The main raw material information is as follows:
[0055] Nickel sulfate hexahydrate NiSO4·6H2O, 262.85 g / mol, battery grade, Jinchuan Group;
[0056] Cobalt sulfate heptahydrate CoSO4·7H2O, 281.15 g / mol, battery grade, Huayou Cobalt;
[0057] Manganese sulfate monohydrate MnSO4·H2O, 169.016 g / mol, battery grade, Guizhou Dalong Huicheng New Materials Co., Ltd.
[0058] Lithium hydroxide monohydrate LiOH·H2O, 41.96 g / mol, Shandong Ruifu Lithium Industry Co., Ltd.
[0059] Lithium carbonate Li2CO3, 73.89 g / mol, Shandong Ruifu Lithium Industry Co., Ltd.
[0060] Sodium chloride NaCl, 58.44 g / mol, analytical grade, Shanghai Aladdin Biochemical Technology Co., Ltd.
[0061] Polyvinylidene fluoride (PVDF), analytical grade, Shanghai Aladdin Biochemical Technology Co., Ltd.
[0062] Nitromethylpyrrolidone (NMP), analytical grade, Shanghai Aladdin Biochemical Technology Co., Ltd.
[0063] Ammonia (25%-28%), analytical grade, Shanghai Aladdin Biochemical Technology Co., Ltd.
[0064] Liquid caustic soda (32%), analytical grade, Shanghai Aladdin Biochemical Technology Co., Ltd.
[0065] The main experimental and testing equipment information is as follows:
[0066] XRD: Malvern Panalytical Aeris X-ray benchtop diffractometer;
[0067] Electrochemical testing equipment: Shenzhen Xinwei button cell testing system;
[0068] Calcination equipment: Hefei Kejing tube furnace, model OTF-1500X;
[0069] 10m 3 Reactor complete equipment: customized complete equipment.
[0070] The particle size D50 test method is as follows:
[0071] The material powder was taken and tested using a Malvern Mastersizer 3000 laser particle size analyzer with a wet sampler to obtain particle size distribution data.
[0072] The XRD test method is as follows:
[0073] The precursor powder was subjected to back pressure tableting treatment, and powder XRD measurement was performed using a Malvern Panalytical Aeris XRD tester with a test angle 2θ of 10°-80°, a step length of 2θ=0.0108°, and a test time of 100 s per step.
[0074] The XRD spectrum obtained by the test was first subjected to the Default operation using HighScore software, automatically fitted twice, performed background correction, read the intensity of the corresponding peak, and calculated the grain size of the corresponding crystal plane.
[0075] The electrochemical performance test method is as follows:
[0076] The positive electrode material and lithium sheet obtained in the embodiment were used as the positive and negative active materials, respectively, to assemble button batteries; the positive electrode slurry in the positive electrode sheet was composed of the positive electrode active material, acetylene black (conductive agent) and PVDF (binder), and the mass ratio of the three was 80:12:8; the button battery testing system of Shenzhen Xinwei was used for testing, and the charge and discharge voltage was within a set voltage range, such as 3.0–4.5 V. The button batteries assembled with the positive electrode materials were subjected to electrochemical performance tests at room temperature. The mass specific capacity of the positive electrode material was tested at a current density of 0.02 A / g (0.1C), and then its 100-cycle cycle performance was tested at a current density of 0.2 A / g (1C), and its cycle retention rate was calculated.
[0077] Example 1
[0078] Nickel sulfate, cobalt sulfate and manganese sulfate are used as raw materials, the molar ratio of nickel, cobalt and manganese is 5:2:3, and deionized water is used to prepare the salt solution to a total metal concentration of 2.0 mol / L, marked as B1; 12 mol / L NaOH is used as the alkaline solution, marked as B2; 10 mol / L ammonia water is used as the complexing agent, marked as B3.
[0079] Solutions B1, B2, and B3 were added dropwise to the reactor simultaneously. The stirring speed in the reactor was controlled at 200 rpm, the reaction temperature was 60°C, the feed rate of B1 was set at 900 L / h, the feed rate of B2 was set at 300 L / h ± 10 L / h, and the feed rate of B2 was fine-tuned within the set range according to the pH value in the reactor. The feed rate of B3 was 36 L / h. At this point, the reaction parameters satisfied the formula:
[0080] Feed continuously, take out the slurry from the reactor every 5 hours to test the particle size, and stop feeding until the particle size of the precursor grows to 4±0.05μm. The slurry is filtered and washed until the sulfur content is less than 3000ppm, and then transferred to an oven for drying at 140℃ for 5 hours. After demagnetization, screening and packaging, the precursor product Ni is confirmed by ICP. 0.5 Co 0.2 Mn 0.3 (OH)2.
[0081] Take Ni 0.5 Co 0.2 Mn 0.3 (OH)2 and lithium carbonate were mixed evenly using a high-speed mixer according to the molar ratio of precursor to lithium element of 1:1.03. The mixture was put into a sagger and placed in a tube furnace. It was sintered at 920℃ for 12 hours in an oxygen atmosphere to obtain the positive electrode material LiNi 0.5 Co 0.2 Mn 0.3O2. The electrochemical specific capacity and cycle performance of the positive electrode material were then tested, and the data are shown in Table 1.
[0082] Example 2
[0083] Nickel sulfate, cobalt sulfate and manganese sulfate are used as raw materials, the molar ratio of nickel, cobalt and manganese is 5:2:3, and deionized water is used to prepare the salt solution to a total metal concentration of 2.0 mol / L, marked as B1; 12 mol / L NaOH is used as the alkaline solution, marked as B2; 10 mol / L ammonia water is used as the complexing agent, marked as B3.
[0084] Solutions B1, B2, and B3 were added dropwise to the reactor simultaneously. The stirring speed in the reactor was controlled at 100 rpm, the reaction temperature was 50°C, the feed rate of B1 was set at 900 L / h, the feed rate of B2 was set at 300 L / h ± 10 L / h, and the feed rate of B2 was fine-tuned within the set range according to the pH value in the reactor. The feed rate of B3 was 36 L / h. At this point, the reaction parameters satisfied the formula:
[0085] Feed continuously, take out the slurry from the reactor every 5 hours to test the particle size, and stop feeding until the particle size of the precursor grows to 4±0.05μm. The slurry is filtered and washed until the sulfur content is less than 3000ppm, and then transferred to an oven for drying at 140℃ for 5 hours. After demagnetization, screening and packaging, the precursor product Ni 0.5 Co 0.2 Mn 0.3 (OH)2.
[0086] Take Ni 0.5 Co 0.2 Mn 0.3 (OH)2 and lithium carbonate were mixed evenly using a high-speed mixer according to the molar ratio of precursor to lithium element of 1:1.03. The mixture was put into a sagger and placed in a tube furnace. It was sintered at 920℃ for 12 hours in an oxygen atmosphere to obtain the positive electrode material LiNi 0.5 Co 0.2 Mn 0.3 O2. The electrochemical specific capacity and cycle performance of the positive electrode material were then tested, and the data are shown in Table 1.
[0087] Example 3
[0088] Nickel sulfate, cobalt sulfate, and manganese sulfate were used as raw materials, with a molar ratio of nickel, cobalt, and manganese of 5:2:3. Deionized water was used to prepare the salt solution to a total metal concentration of 2.0 mol / L, labeled B1; 4 mol / L NaOH was used as the alkaline solution, labeled B2; and 6 mol / L ammonia water was used as the complexing agent, labeled B3.
[0089] Solutions B1, B2, and B3 were added dropwise to the reactor simultaneously. The stirring speed in the reactor was controlled at 100 rpm, the reaction temperature was 70°C, the feed rate of B1 was set at 900 L / h, the feed rate of B2 was set at 900 L / h ± 30 L / h, and the feed rate of B2 was fine-tuned within the set range according to the pH value in the reactor. The feed rate of B3 was 72 L / h. At this point, the reaction parameters satisfied the formula:
[0090] Feed continuously, take out the slurry from the reactor every 5 hours to test the particle size, and stop feeding until the particle size of the precursor grows to 4±0.05μm. The slurry is filtered and washed until the sulfur content is less than 3000ppm, and then transferred to an oven for drying at 140℃ for 5 hours. After demagnetization, screening and packaging, the precursor product Ni 0.5 Co 0.2 Mn 0.3 (OH)2.
[0091] Take Ni 0.5 Co 0.2 Mn 0.3 (OH)2 and lithium carbonate were mixed evenly using a high-speed mixer according to the molar ratio of precursor to lithium element of 1:1.03. The mixture was put into a sagger and placed in a tube furnace. It was sintered at 920℃ for 12 hours in an oxygen atmosphere to obtain the positive electrode material LiNi 0.5 Co 0.2 Mn 0.3 O2. The electrochemical specific capacity and cycle performance of the positive electrode material were then tested, and the data are shown in Table 1.
[0092] Example 4
[0093] Nickel sulfate, cobalt sulfate, and manganese sulfate were used as raw materials, with a molar ratio of nickel, cobalt, and manganese of 90:5:5. Deionized water was used to prepare the salt solution to a total metal concentration of 2.0 mol / L, labeled B1; 12 mol / L NaOH was used as the alkaline solution, labeled B2; and 10 mol / L ammonia water was used as the complexing agent, labeled B3.
[0094] Solutions B1, B2, and B3 were added dropwise to the reactor simultaneously. The stirring speed in the reactor was controlled at 350 rpm, the reaction temperature was set at 60°C, the feed rate of B1 was set at 500 L / h, the feed rate of B2 was set at 166±5 L / h, and the feed rate of B2 was fine-tuned within the set range according to the pH value in the reactor. The feed rate of B3 was set at 20 L / h. At this point, the reaction parameters satisfied the formula:
[0095] Feed continuously, take out the slurry from the reactor every 5 hours to test the particle size, and stop feeding until the particle size of the precursor grows to 10±0.05μm. The slurry is filtered and washed until the sulfur content is less than 3000ppm, and then transferred to an oven for drying at 140℃ for 5 hours. After demagnetization, screening and packaging, the precursor product Ni 0.90 Co 0.05 Mn 0.05 (OH)2.
[0096] Take Ni 0.90 Co 0.05 Mn 0.05 (OH)2 and LiOH·H2O were mixed evenly using a high-speed mixer according to the molar ratio of precursor to lithium element of 1:1.03. The mixture was put into a sagger and placed in a tube furnace. It was sintered at 720℃ for 12 hours in an oxygen atmosphere to obtain the positive electrode material LiNi 0.90 Co 0.05 Mn 0.05 O2. The electrochemical specific capacity and cycle performance of the positive electrode material were then tested, and the data are shown in Table 1.
[0097] Example 5
[0098] Nickel sulfate, cobalt sulfate and aluminum sulfate were used as raw materials, with a molar ratio of nickel, cobalt and aluminum of 90:8:2. Deionized water was used to prepare the salt solution to a total metal concentration of 2.0 mol / L, marked as B1; 4 mol / L NaOH was used as the alkaline solution, marked as B2; and 4 mol / L ammonia water was used as the complexing agent, marked as B3.
[0099] Solutions B1, B2, and B3 were added dropwise to the reactor simultaneously. The stirring speed in the reactor was controlled at 150 rpm, the reaction temperature was 50°C, the feed rate of B1 was set at 200 L / h, the feed rate of B2 was set at 200 ± 5 L / h, and the feed rate of B2 was fine-tuned within the set range according to the pH value in the reactor. The feed rate of B3 was 71 L / h. At this point, the reaction parameters satisfied the formula:
[0100] Feed continuously, take out the slurry from the reactor every 5 hours to test the particle size, and stop feeding until the particle size of the precursor grows to 10±0.05μm. The slurry is filtered and washed until the sulfur content is less than 3000ppm, and then transferred to an oven for drying at 140℃ for 5 hours. After demagnetization, screening and packaging, the precursor product Ni 0.90 Co 0.08 Al 0.02 (OH)2.
[0101] Take Ni0.90 Co 0.08 Al 0.02 (OH)2 and LiOH·H2O were mixed evenly using a high-speed mixer according to the molar ratio of precursor to lithium element of 1:1.03. The mixture was put into a sagger and placed in a tube furnace. It was sintered at 720℃ for 12 hours in an oxygen atmosphere to obtain the positive electrode material LiNi 0.90 Co 0.08 Al 0.02 O2. The electrochemical specific capacity and cycle performance of the positive electrode material were then tested, and the data are shown in Table 1.
[0102] Example 6
[0103] Nickel sulfate, manganese sulfate, copper sulfate, and magnesium sulfate were used as raw materials, with a molar ratio of nickel, manganese, copper, and magnesium of 90:8:1:1. Deionized water was used to prepare the salt solution to a total metal concentration of 2.0 mol / L, labeled B1; 10 mol / L NaOH was used as the alkaline solution, labeled B2; and 8 mol / L ammonia water was used as the complexing agent, labeled B3.
[0104] Solutions B1, B2, and B3 were added dropwise to the reactor simultaneously. The stirring speed in the reactor was controlled at 250 rpm, the reaction temperature was 50°C, the feed rate of B1 was set at 600 L / h, the feed rate of B2 was set at 240 ± 5 L / h, and the feed rate of B2 was fine-tuned within the set range according to the pH value in the reactor. The feed rate of B3 was 40 L / h. At this point, the reaction parameters satisfied the formula:
[0105] Feed continuously, take out the slurry from the reactor every 5 hours to test the particle size, and stop feeding until the particle size of the precursor grows to 10±0.05μm. The slurry is filtered and washed until the sulfur content is less than 3000ppm, and then transferred to an oven for drying at 140℃ for 5 hours. After demagnetization, screening and packaging, the precursor product Ni 0.90 Mn 0.08 Cu 0.01 Mg 0.01 (OH)2.
[0106] Take Ni 0.90 Mn 0.08 Cu 0.01 Mg 0.01 (OH)2 and LiOH·H2O were mixed evenly using a high-speed mixer according to the molar ratio of precursor to lithium element of 1:1.03. The mixture was put into a sagger and placed in a tube furnace. It was sintered at 710℃ for 12 hours in an oxygen atmosphere to obtain the positive electrode material LiNi 0.90 Mn 0.08 Cu0.01 Mg 0.01 O2. The electrochemical specific capacity and cycle performance of the positive electrode material were then tested, and the data are shown in Table 1.
[0107] Example 7
[0108] Nickel sulfate, cobalt sulfate, manganese sulfate, ferrous sulfate, and zirconium sulfate are used as raw materials, with a molar ratio of nickel, cobalt, manganese, iron, and zirconium of 80:5:5:5:5. Deionized water is used to prepare the salt solution to a total metal concentration of 2.0 mol / L, marked as B1; 10 mol / L NaOH is used as the alkaline solution, marked as B2; 8 mol / L ammonia water is used as the complexing agent, marked as B3.
[0109] Solutions B1, B2, and B3 were added dropwise to the reactor simultaneously. The stirring speed in the reactor was controlled at 250 rpm, the reaction temperature was 50°C, the feed rate of B1 was set at 600 L / h, the feed rate of B2 was set at 240 ± 5 L / h, and the feed rate of B2 was fine-tuned within the set range according to the pH value in the reactor. The feed rate of B3 was 40 L / h. At this point, the reaction parameters satisfied the formula:
[0110] Feed continuously, take out the slurry from the reactor every 5 hours to test the particle size, and stop feeding until the particle size of the precursor grows to 10±0.05μm. The slurry is filtered and washed until the sulfur content is less than 3000ppm, and then transferred to an oven for drying at 140℃ for 5 hours. After demagnetization, screening and packaging, the precursor product Ni 0.80 Co 0.05 Mn 0.05 Fe 0.05 Zr 0.05 (OH)2.
[0111] Take Ni 0.80 Co 0.05 Mn 0.05 Fe 0.05 Zr 0.05 (OH)2 and LiOH·H2O were mixed evenly using a high-speed mixer according to the molar ratio of precursor to lithium element of 1:1.03. The mixture was put into a sagger and placed in a tube furnace. It was sintered at 780℃ for 12 hours in an oxygen atmosphere to obtain the positive electrode material Li Ni 0.80 Co 0.05 Mn 0.05 Fe 0.05 Zr 0.05 O2. The electrochemical specific capacity and cycle performance of the positive electrode material were then tested, and the data are shown in Table 1.
[0112] Comparative Example 1
[0113] Nickel sulfate, cobalt sulfate and manganese sulfate are used as raw materials, with the ratio of nickel, cobalt and manganese being 5:2:3. Deionized water is used to prepare the salt solution to a total metal concentration of 2.0 mol / L, marked as B1; 12 mol / L NaOH is used as the alkaline solution, marked as B2; 10 mol / L ammonia water is used as the chelating agent, marked as B3.
[0114] Solutions B1, B2, and B3 were added dropwise to the reactor simultaneously. The stirring speed in the reactor was controlled at 400 rpm, the reaction temperature was 70°C, the feed rate of B1 was set at 900 L / h, the feed rate of B2 was set at 300 L / h ± 10 L / h, and the feed rate of B2 was fine-tuned within the set range according to the pH value in the reactor. The feed rate of B3 was 36 L / h. At this point, the reaction parameters satisfied the formula:
[0115] Feed continuously, take out the slurry from the reactor every 5 hours to test the particle size, and stop feeding until the particle size of the precursor grows to 4±0.05μm. The slurry is filtered and washed until the sulfur content is less than 3000ppm, and then transferred to an oven for drying at 140℃ for 5 hours. After demagnetization, screening and packaging, the precursor product Ni 0.5 Co 0.2 Mn 0.3 (OH)2.
[0116] Take Ni 0.5 Co 0.2 Mn 0.3 (OH)2 and lithium carbonate were mixed evenly using a high-speed mixer according to the molar ratio of precursor to lithium element of 1:1.03. The mixture was put into a sagger and placed in a tube furnace. It was sintered at 920℃ for 12 hours under an oxygen atmosphere to obtain 102g of positive electrode material LiNi 0.5 Co 0.2 Mn 0.3 O2. The electrochemical specific capacity and cycle performance of the positive electrode material were then tested, and the data are shown in Table 1.
[0117] Comparative Example 2
[0118] Nickel sulfate, cobalt sulfate and manganese sulfate are used as raw materials, with the ratio of nickel, cobalt and manganese being 5:2:3. Deionized water is used to prepare the salt solution to a total metal concentration of 2.0 mol / L, marked as B1; 4 mol / L NaOH is used as the alkaline solution, marked as B2; 10 mol / L ammonia water is used as the chelating agent, marked as B3.
[0119] Solutions B1, B2, and B3 were added dropwise to the reactor simultaneously. The stirring speed in the reactor was controlled at 100 rpm, the reaction temperature was 50°C, the feed rate of B1 was set at 900 L / h, the feed rate of B2 was set at 900 L / h ± 10 L / h, and the feed rate of B2 was fine-tuned within the set range according to the pH value in the reactor. The feed rate of B3 was 100 L / h. At this point, the reaction parameters satisfied the formula:
[0120] Feed continuously, take out the slurry from the reactor every 5 hours to test the particle size, and stop feeding until the particle size of the precursor grows to 4±0.05μm. The slurry is filtered and washed until the sulfur content is less than 3000ppm, and then transferred to an oven for drying at 140℃ for 5 hours. After demagnetization, screening and packaging, the precursor product Ni 0.5 Co 0.2 Mn 0.3 (OH)2.
[0121] Take Ni 0.5 Co 0.2 Mn 0.3 (OH)2 and lithium carbonate were mixed evenly using a high-speed mixer according to the molar ratio of precursor to lithium element of 1:1.03. The mixture was put into a sagger and placed in a tube furnace. It was sintered at 920℃ for 12 hours in an oxygen atmosphere to obtain the positive electrode material LiNi 0.5 Co 0.2 Mn 0.3 O2. The electrochemical specific capacity and cycle performance of the positive electrode material were then tested, and the data are shown in Table 1.
[0122] Comparative Example 3
[0123] Nickel sulfate, cobalt sulfate, and manganese sulfate are used as raw materials, with a nickel-cobalt-manganese ratio of 90:5:5. Deionized water is used to prepare the salt solution to a total metal concentration of 2.0 mol / L, marked as B1; 4 mol / L NaOH is used as the alkaline solution, marked as B2; 10 mol / L ammonia water is used as the chelating agent, marked as B3.
[0124] Solutions B1, B2, and B3 were added dropwise to the reactor simultaneously. The stirring speed in the reactor was controlled at 100 rpm, the reaction temperature was 50°C, the feed rate of B1 was set at 900 L / h, the feed rate of B2 was set at 900 L / h ± 10 L / h, and the feed rate of B2 was fine-tuned within the set range according to the pH value in the reactor. The feed rate of B3 was 100 L / h. At this point, the reaction parameters satisfied the formula:
[0125] Feed continuously, take out the slurry from the reactor every 5 hours to test the particle size, and stop feeding until the particle size of the precursor grows to 10±0.05μm. The slurry is filtered and washed until the sulfur content is less than 3000ppm, and then transferred to an oven for drying at 140℃ for 5 hours. After demagnetization, screening and packaging, the precursor product Ni 0.90 Co 0.05 Mn 0.05 (OH)2.
[0126] Take Ni 0.90 Co 0.05 Mn 0.05 (OH)2 and LiOH·H2O were mixed evenly using a high-speed mixer according to the molar ratio of precursor to lithium element of 1:1.03. The mixture was put into a sagger and placed in a tube furnace. It was sintered at 720℃ for 12 hours in an oxygen atmosphere to obtain the positive electrode material LiNi 0.90 Co 0.05 Mn 0.05 O2. The electrochemical specific capacity and cycle performance of the positive electrode material were then tested, and the data are shown in Table 1.
[0127] Comparative Example 4
[0128] Nickel sulfate, cobalt sulfate and aluminum sulfate are used as raw materials, with the ratio of nickel, cobalt and aluminum being 90:8:2. Deionized water is used to prepare the salt solution to a total metal concentration of 2.0 mol / L, marked as B1; 4 mol / L NaOH is used as the alkaline solution, marked as B2; 10 mol / L ammonia water is used as the complexing agent, marked as B3.
[0129] Solutions B1, B2, and B3 were added dropwise to the reactor simultaneously. The stirring speed in the reactor was controlled at 50 rpm, the reaction temperature was 50°C, the feed rate of B1 was set at 900 L / h, the feed rate of B2 was set at 900 L / h ± 10 L / h, and the feed rate of B2 was fine-tuned within the set range according to the pH value in the reactor. The feed rate of B3 was 100 L / h. At this point, the reaction parameters satisfied the formula:
[0130] Feed continuously, take out the slurry from the reactor every 5 hours to test the particle size, and stop feeding until the particle size of the precursor grows to 10±0.05μm. The slurry is filtered and washed until the sulfur content is less than 3000ppm, and then transferred to an oven for drying at 140℃ for 5 hours. After demagnetization, screening and packaging, the precursor product Ni 0.90 Co 0.08 Al 0.02 (OH)2.
[0131] Take Ni0.90 Co 0.08 Al 0.02 (OH)2 and LiOH·H2O were mixed evenly using a high-speed mixer according to the molar ratio of precursor to lithium element of 1:1.03. The mixture was put into a sagger and placed in a tube furnace. It was sintered at 720℃ for 12 hours in an oxygen atmosphere to obtain the positive electrode material LiNi 0.90 Co 0.08 Al 0.02 O2. The electrochemical specific capacity and cycle performance of the positive electrode material were then tested, and the data are shown in Table 1.
[0132] Table 1
[0133] As can be seen from Table 1:
[0134] In Examples 1-7, when the preparation parameters are according to the formula When calculated, its J value is between 1-13, the I(101) / I(001) peak intensity ratio of the obtained precursor is less than 0.75, the grain size ratio D(102) / D(001) is less than 0.65, and its 0.1C capacity and 1C cycle retention rate are maintained at a high level.
[0135] Comparing Example 1 and Comparative Example 1, when the J value is not in the range of 1 to 13, although in Comparative Example 1, the peak intensity ratio I(101) / I(001) is still less than 0.75, the grain size ratio D(102) / D(001) is greater than 0.65. At this time, the capacity and cycle of the sintered positive electrode material are poor.
[0136] Comparing Example 2 and Comparative Example 2, when the J value is not in the range of 1 to 13, in Comparative Example 1, the peak intensity ratio I(101) / I(001) is greater than 0.75, and the grain size ratio D(102) / D(001) is greater than 0.65. At this time, the capacity and cycle of the sintered positive electrode material are poor.
[0137] Comparing Example 4 and Comparative Example 3, when the J value is not in the range of 1 to 13, in Comparative Example 1, the peak intensity ratio I(101) / I(001) is greater than 0.75, and the grain size ratio D(102) / D(001) is greater than 0.65. At this time, the capacity and cycle of the sintered positive electrode material are poor.
[0138] Comparing Example 5 and Comparative Example 4, when the J value is not in the range of 1 to 13, in Comparative Example 1, the peak intensity ratio I(101) / I(001) is greater than 0.75, and the grain size ratio D(102) / D(001) is greater than 0.65. At this time, the capacity and cycle of the sintered positive electrode material are poor.
[0139] This shows that, through the precursor material provided by the present invention, when the peak intensity ratio I(101) / I(001) satisfies less than 0.75 and the grain size ratio D(102) / D(001) is less than 0.65, the electrochemical performance of the positive electrode material obtained by sintering the precursor is also significantly improved, the capacity is increased, and the cycle stability is enhanced. In addition, through the preparation method of the improved precursor of the present invention, when the reaction parameter J during the synthesis process is between 1 and 13, the precursor as described above can be obtained, and the performance of the positive electrode material obtained by sintering the precursor is significantly better than that of the precursor whose reaction parameter J is not in the range of 1 to 13.
[0140] Although the present invention has been described in detail through the above preferred embodiments, it should be understood that the above description is not intended to limit the present invention. Those skilled in the art will appreciate that, based on the teachings of this specification, modifications or adjustments may be made to the present invention. Such modifications or adjustments should also be within the scope defined by the claims of the present invention.
Claims
1. A lithium ion battery cathode material precursor having a general formula Ni a Mn b M c N d (OH) e , in, 0 <a≤1,0≤b≤1,0≤c≤1,0≤d≤1,1.8≤e≤2.2,a+b+c+d=1, M is at least one selected from Co, Fe, Cu, Mo, W, Zn, Cr and Ti, N contains at least Al, S, Na, Ca, Mg, Mo, Nb, Zr, V, Sc, P, Sr, Ba, Cl, F, Si, Ge, B, C or K, The lithium-ion battery positive electrode material precursor has a layered structure, an XRD peak intensity ratio of I(101) / I(001)<0.75, and a grain size ratio of D(102) / D(001)<0.
65.
2. [Corrected 05.05.2023 according to Rule 26] A lithium-ion battery cathode material precursor according to claim 1, wherein: The median particle size of the lithium ion battery positive electrode material precursor, i.e., D50, is 3 to 11 μm; Preferably, the lithium-ion battery positive electrode material precursor is spherical, with the major axis of the spherical shape being x and the minor axis being y, then 1<major axis x / minor axis y<2; Preferably, the lithium-ion battery cathode material precursor is: Ni 0.5 Co 0.2 Mn 0.3 (OH)2、Ni 0.90 Co 0.05 Mn 0.05 (OH)2、Ni 0.90 Co 0.08 Al 0.02 (OH)2、Ni 0.90 Mn 0.08 Cu 0.01 Mg 0.01 (OH)2 or Ni 0.80 Co 0.05 Mn 0.05 Fe 0.05 Zr 0.05 (OH)2.
3. A method for preparing a lithium ion battery positive electrode material precursor according to claim 1 or 2, comprising the following steps: S1) solution preparation step: providing a mixed salt solution containing nickel salt, manganese salt, M salt and N salt, an alkaline solution and a complexing agent solution; S2) Synthesis step: continuously adding the mixed salt solution, alkaline solution and complexing agent solution to the reaction base solution, and controlling the reaction parameters until the precursor D50 slowly grows to the target particle size, wherein the reaction parameters need to satisfy the formula: Wherein, J value is between 1 and 13, S is the stirring speed of the stirring blade, in rpm; T is the reaction temperature, in °C; V 盐 is the feed rate of the mixed salt solution, in L / h; V 碱 is the feed rate of alkaline solution, in L / h; V 络合剂 is the feeding rate of the complexing agent solution, in L / h; K is a fixed value, K=5000; S3) filtering and washing: performing solid-liquid separation on the mixture obtained in step S2, and washing the solid with a washing liquid; S4) Drying: Dry the wet solid obtained in step S3, demagnetize, sieve and package.
4. The method for preparing a positive electrode material precursor for a lithium ion battery according to claim 3, comprising the following steps: The mixed salt solution, alkaline solution and complexing agent solution in step S1 are all aqueous solutions; Preferably, the molar ratio of nickel ions: manganese ions: M ions: N ions in step S1 is a:b:c:d.
5. The method for preparing a positive electrode material precursor for a lithium ion battery according to claim 3, wherein: The total concentration of nickel ions, manganese ions, M ions, and N ions is 1 to 3 mol / L; Preferably, the alkaline solution in step S1 is an alkali metal hydroxide solution, more preferably, the alkaline solution is a NaOH solution; Preferably, the concentration of the alkaline solution is 2 to 12 mol / L; Preferably, the complexing agent solution in step S1 is selected from one or more of an aqueous ammonia solution, a urea solution, and a soluble ammonium salt solution; Preferably, the concentration of the complexing agent solution is 4-12 mol / L.
6. The method for preparing a positive electrode material precursor for a lithium ion battery according to any one of claims 3 to 5, wherein: The D50 target particle size in step S2 is 3 to 11 μm, preferably 3 to 5 μm; Preferably, the base liquid in step S2 is water or an ammonia solution; Preferably, the J value in step S2 is 1 to 8; Preferably, the washing in step S3 is performed until the content of the anion element in the mixed salt contained in the washed solid is less than 5000 ppm; Preferably, the drying temperature in step S4 is ≥100° C., and the drying time is ≥3 h.
7. A method for preparing a positive electrode material for a lithium ion battery, comprising the following steps: a1) mixing the lithium ion battery positive electrode material precursor according to claim 1 or 2 or the lithium ion battery positive electrode material precursor prepared according to any one of claims 3 to 4 with a lithium source at a molar ratio of the precursor to the lithium element of 1:1.01 to 1.05, preferably 1:1.03, a2) placing the mixture obtained in step a1) into a tube furnace and sintering at 650-1000°C in an oxygen atmosphere to obtain the positive electrode material LiNi a Mn b M c N d O f ,in, 1.8≤f≤2.2; Preferably, the lithium source is lithium carbonate or lithium hydroxide.
8. A lithium ion battery positive electrode material, which is LiNi a Mn b M c N d O f ; in, 0 <a≤1,0≤b≤1,0≤c≤1,0≤d≤1,1.8≤f≤2.2,a+b+c+d=1, M is at least one selected from Co, Fe, Cu, Mo, W, Zn, Cr and Ti, N contains at least Al, S, Na, Ca, Mg, Mo, Nb, Zr, V, Sc, P, Sr, Ba, Cl, F, Si, Ge, B, C or K, Preferably, the lithium ion positive electrode material is prepared according to the method for preparing a lithium ion battery positive electrode material according to claim 7; Preferably, the positive electrode material of the lithium-ion battery is LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.90 Co 0.05 Mn 0.05 O2、LiNi 0.90 Co 0.08 Al 0.02 O2、LiNi 0.90 Mn 0.08 Cu 0.01 Mg 0.01 O2 or LiNi 0.80 Co 0.05 Mn 0.05 Fe 0.05 Zr 0.05 O2. 9 . A positive electrode of a lithium ion battery, comprising the positive electrode material of a lithium ion battery according to claim 8 . 10 . A lithium ion battery comprising the positive electrode of the lithium ion battery according to claim 9 .
Citation Information
Patent Citations
Preparation method for lithium ion battery precursor with controllable particle size distribution
CN110739447A
Hollow core-shell structure precursor positive electrode material and preparation method thereof
CN111276680A
Narrow-particle-size-distribution high-nickel hydroxide and preparation method thereof
CN112777647A
Precursor, method for manufacturing precursor, positive electrode material, method for manufacturing positive electrode material, and lithium-ion secondary cell
CN113646929A
Method for reducing sulfur content of sulfate system lithium ion battery positive electrode material precursor
CN114684871A
Cited By
Positive electrode material precursor and preparation method thereof, positive electrode material, lithium ion battery and electric equipment
CN119330427A