Α-sialon phosphor, light-emitting device, and method for producing α-sialon phosphor

The α-sialon phosphor with low crystal defects, produced using a specific manufacturing process, addresses the temperature-induced instability in conventional phosphors, ensuring stable light emission and efficiency up to 300°C, suitable for vehicle-mounted applications.

WO2024203914A1PCT designated stage expired Publication Date: 2024-10-03DENKA CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011417
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional α-sialon phosphors used in white LEDs exhibit significant changes in light emission characteristics at high temperatures, making them unsuitable for vehicle-mounted applications where stability is crucial.

Method used

Development of an α-sialon phosphor with a low density of crystal defects, achieved through a manufacturing process involving firing, pulverizing, nitrogen annealing, hydrogen annealing, and acid treatment, which maintains luminescent properties even at elevated temperatures.

Benefits of technology

The resulting α-sialon phosphor maintains high internal and external quantum efficiencies and stable light emission characteristics up to 300°C, ensuring consistent performance in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011417_03102024_PF_FP_ABST
    Figure JP2024011417_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is α-sialon phosphor that contains elemental Eu and has a crystal defect density, as the signal spin density in the vicinity of g = 2 and as detected by the electron spin resonance measurement at 25°C, of 1.0 × 1015 spins / g or less. Also provided is α-sialon phosphor that contains elemental Eu and has a crystal defect density, as the signal spin density in the vicinity of g = 2 and as detected by the electron spin resonance measurement at 200°C, of 1.0 × 1015 spins / g or less.
Need to check novelty before this filing date? Find Prior Art

Description

α-type sialon phosphor, light-emitting device, and method for producing α-type sialon phosphor

[0001] The present invention relates to an α-sialon phosphor, a light-emitting device, and a method for producing the α-sialon phosphor.

[0002] An α-sialon phosphor activated with a rare earth element such as Eu can efficiently convert blue light into long wavelength light, and is therefore used as a wavelength conversion material for white LEDs.

[0003] α-SiAlON phosphors usually have a structure in which the Si-N bonds of α-SiN crystals are partially replaced with Al-N bonds and Al-O bonds, and in order to maintain electrical neutrality, specific elements (Ca, Li, Mg, Y, or lanthanide metals excluding La and Ce) intercalate and form a solid solution between the crystal lattice. Fluorescent properties are exhibited by using rare earth elements as the luminescence center as some of the intercalated and solid-solved elements. In particular, α-SiAlON phosphors in which Ca is solid-solved and part of it is substituted with Eu are excited relatively efficiently in a wide wavelength range from ultraviolet to blue, and emit yellow or orange light.

[0004] In order to further improve the fluorescent properties of α-sialon phosphors, various attempts have been proposed (for example, Patent Documents 1 to 3).

[0005] Japanese Patent Publication No. 2009-96882 Japanese Patent No. 6667025 Japanese Patent No. 6785333

[0006] It is conceivable that white LEDs using α-SiAlON phosphors as wavelength conversion materials could be applied to automotive applications. In automotive applications, it is required that the various characteristics of the white LEDs do not change even at high temperatures. However, preliminary studies by the present inventors have revealed that white LEDs using conventional α-SiAlON phosphors as wavelength conversion materials experience significant changes in their light-emitting characteristics in high-temperature environments.

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an α-sialon phosphor whose light-emitting properties are unlikely to change even in a high-temperature environment when used as a wavelength conversion member for a white LED.

[0008] The present inventors have completed the invention provided below and solved the above problems.

[0009] 1. An α-sialon phosphor containing Eu, wherein the density of crystal defects in the α-sialon phosphor is 1.0×10 as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 25°C. 15 2. An α-sialon phosphor containing Eu, wherein the density of crystal defects in the α-sialon phosphor is 1.0×10 or less as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 200°C. 15 3. The α-sialon phosphor according to 2., wherein the density of crystal defects in the α-sialon phosphor is 1.0×10 or less as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 25° C. 15 4. An α-sialon phosphor according to any one of 1. to 3., wherein the density of crystal defects in the α-sialon phosphor is 1.0×10 or less as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 300°C. 15 5. An α-sialon phosphor according to any one of 1. to 4., wherein the density of crystal defects in the α-sialon phosphor is 9.5×10 or less as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 600°C. 15spins / g or less. 6. An α-sialon phosphor according to any one of 1. to 5., having an internal quantum efficiency of 87% or more at 200°C. 7. An α-sialon phosphor according to any one of 1. to 6., having an internal quantum efficiency of 80% or more at 300°C. 8. An α-sialon phosphor according to any one of 1. to 7., having an internal quantum efficiency retention rate of 89% or more, expressed as {(internal quantum efficiency at 24°C) / (internal quantum efficiency at 300°C)}×100[%]. 9. An α-sialon phosphor according to any one of 1. to 8., having an internal quantum efficiency retention rate of 89% or more, expressed as {(internal quantum efficiency at 24°C) / (internal quantum efficiency at 300°C)}×100[%]. 10. An α-sialon phosphor according to any one of items 1. to 9., wherein the α-sialon phosphor has an external quantum efficiency maintenance rate of 88% or more, expressed by {(external quantum efficiency at 24°C) / (external quantum efficiency at 300°C)}×100[%]. 11. An α-sialon phosphor according to any one of items 1. to 9., wherein the composition is represented by the general formula: (M1 x , M2 y , Eu z ) (Si 12-(m+n) Al m+n ) (O n N 16-n 11. An α-sialon phosphor represented by the formula (1), wherein M1 is a monovalent Li element, M2 is one or more divalent elements selected from the group consisting of Mg, Ca, and lanthanide elements (excluding La and Ce), and 0≦x<2.0, 0≦y<2.0, 0<z≦0.5, 0<x+y, 0.3≦x+y+z≦2.0, 0<m≦4.0, 0<n≦3.0. 12. A light emitting device comprising: a light emitting element; and a wavelength conversion unit comprising the α-sialon phosphor according to any one of 1. to 10., which converts the wavelength of light emitted from the light emitting element to a longer wavelength. a firing step of obtaining a bulk α-sialon phosphor containing Eu element by firing; a crushing step of crushing the bulk α-sialon phosphor to obtain a powdered α-sialon phosphor; and a nitrogen gas annealing step of annealing the powdered α-sialon phosphor in a nitrogen gas atmosphere at a temperature of 1200°C to 1700°C for a time of 5 hours to 30 hours. 2an annealing step in which the powdered α-sialon phosphor is annealed in a hydrogen gas atmosphere at a temperature of 1200° C. to 1700° C. for a time period of 5 hours to 30 hours; 2 an annealing step; 2 an acid treatment step of performing an acid treatment on the powdered α-sialon phosphor after the annealing step using an acidic aqueous solution.

[0010] A white LED using the α-sialon phosphor of the present invention as a wavelength conversion member is less likely to change in light emission characteristics even in a high temperature environment.

[0011] FIG. 1 is a schematic cross-sectional view showing an example of the structure of a light-emitting device.

[0012] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. In the drawings, similar components are given similar reference numerals, and descriptions thereof will be omitted where appropriate. To avoid complexity, when multiple identical components appear in the same drawing, only one of the components may be given a reference numeral, and not all of the components may be given a reference numeral. The drawings are for illustrative purposes only. The shapes and dimensional ratios of each component in the drawings do not necessarily correspond to actual objects.

[0013] In this specification, unless otherwise specified, the expression "X to Y" in the description of a numerical range means at least X and at most Y. For example, "1 to 5% by mass" means "at least 1% by mass and at most 5% by mass."

[0014] In this specification, "α-sialon phosphor containing Eu element" may be simply referred to as "α-sialon phosphor." In this specification, "a signal near g = 2" literally means a signal where the g value in electron spin resonance measurement is near 2. Specifically, "near g = 2" means g = 2 ± 0.02.

[0015] <α-SiAlON Phosphor> The α-SiAlON phosphor of this embodiment contains Eu element, or in other words, is an Eu-activated α-SiAlON phosphor.

[0016] The α-sialon phosphor of this embodiment satisfies one or both of the following conditions (1) and (2): (1) The density of crystal defects in the α-sialon phosphor of this embodiment is 1.0×10 or less as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 25° C. 15 This value can be 1.0 x 10 14 spins / g or more 8.0×10 14 spins / g or less, more preferably 1.0 x 10 13 spins / g or more 6.0×10 14 (2) The density of crystal defects in the α-sialon phosphor of this embodiment is 1.0×10 or less as the spin density value of a signal near g=2 detected by electron spin resonance measurement at 200° C. 15 This value can be 1.0 x 10 14 spins / g or more 8.0×10 14 spins / g or less, more preferably 1.0 x 10 13 spins / g or more 6.0×10 14 spins / g or less.

[0017] The present inventors have investigated the causes of changes in luminescence characteristics under high temperature environments from various perspectives. Through their investigations, the inventors have concluded that the density of crystal defects obtained through electron spin resonance (ESR) measurements may be correlated with the degree of change in luminescence characteristics. This is because the presence of crystal defects is generally thought to result in a deterioration in luminescence characteristics.

[0018] Based on the above idea, the present inventors have newly produced an α-sialon phosphor with a sufficiently small density of crystal defects as determined through electron spin resonance (ESR) measurements at 25° C. and / or 200° C. Then, by using this new α-sialon phosphor as a wavelength conversion member for a white LED, it has been possible to manufacture a white LED whose light-emitting characteristics are unlikely to change even in a high-temperature environment.

[0019] A sufficiently small density of crystal defects at 200°C means that there are few crystal defects even in a high-temperature environment. If the density of crystal defects is small in a high-temperature environment, various properties are unlikely to change even at high temperatures when mounted on a vehicle, and therefore it is thought that the light-emitting properties are also unlikely to change. Furthermore, if the density of crystal defects is sufficiently small even at 25°C rather than 200°C, it is thought that there will be a corresponding tendency for there to be fewer crystal defects even in a high-temperature environment. In other words, if the density of crystal defects is sufficiently small at 25°C, it is thought that the light-emitting properties are unlikely to change even in a high-temperature environment.

[0020] The α-sialon phosphor of this embodiment can be manufactured through an appropriate manufacturing process. Specifically, the α-sialon phosphor in powder form is annealed in a nitrogen gas atmosphere. 2 The annealing step is a step of annealing the powdered α-SiAlON phosphor in a hydrogen gas atmosphere. 2 The α-sialon phosphor of this embodiment can be manufactured by performing two annealing steps, the first annealing step and the second annealing step. If the manufacturing method is inappropriate, the α-sialon phosphor of this embodiment may not be obtained. Details of the manufacturing method will be explained later.

[0021] The α-sialon phosphor of this embodiment will be described further.

[0022] Composition of Phosphor The composition of the α-sialon phosphor of this embodiment is, for example, a phosphor represented by the general formula: (M1 x , M2 y , Eu z ) (Si 12-(m+n) Al m+n ) (O n N 16-n In the above general formula, M1 is a monovalent Li element, M2 is one or more divalent elements selected from the group consisting of Mg, Ca, and lanthanide elements (excluding La and Ce), and 0≦x<2.0, 0≦y<2.0, 0<z≦0.5, 0<x+y, 0.3≦x+y+z≦2.0, 0<m≦4.0, 0<n≦3.0.

[0023] The solid solution composition of an α-sialon phosphor is represented by m and n, which are determined by x, y, and z in the above general formula, as well as the accompanying Si / Al ratio and O / N ratio. In particular, when M2 contains Ca, the α-sialon phosphor is stabilized over a wide composition range, and by substituting a portion of it with Eu, which acts as the luminescence center, a phosphor is obtained that is excited by light in a wide wavelength range from ultraviolet to blue, and emits visible light in yellow to orange.

[0024] Generally, since an α-sialon phosphor has a second crystalline phase different from that of the α-sialon phosphor and an amorphous phase that inevitably exists, it is not possible to strictly define the solid solution composition by composition analysis, etc. The crystalline phase of the α-sialon phosphor is preferably a single α-sialon phase, and may contain aluminum nitride or its polytypoid as another crystalline phase.

[0025] Properties of the phosphor α-SiAlON phosphors are usually handled in the form of α-SiAlON phosphor powder, which is an aggregate of α-SiAlON phosphor particles. α-SiAlON phosphor particles often contain secondary particles, which are aggregates of multiple primary particles.

[0026] The median diameter (D 50 The lower limit of the median diameter of the α-sialon phosphor powder is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. The upper limit of the median diameter of the α-sialon phosphor powder is preferably 30 μm or less, and more preferably 20 μm or less. The median diameter of the α-sialon phosphor powder is the size of the secondary particles. That is, D 50 is preferably 1 μm or more and 30 μm or less, more preferably 5 μm or more and 30 μm or less, and even more preferably 10 μm or more and 20 μm or less. By making the median diameter of the α-sialon phosphor powder 5 μm or more, the transparency of the wavelength conversion member can be further increased. On the other hand, by making the median diameter of the α-sialon phosphor powder 30 μm or less, it is possible to suppress chipping when cutting the wavelength conversion member with a dicer or the like.

[0027] Here, the median diameter (D 50) means the median diameter in the volume-based cumulative fraction obtained by the laser diffraction scattering method in accordance with JIS R1629: 1997. Incidentally, when the α-sialon phosphor powder contains secondary particles, the median diameter obtained by the laser diffraction scattering method reflects the size of the secondary particles.

[0028] The shape of the α-sialon phosphor particles is not particularly limited, and examples of the shape include spherical, cubic, columnar, and amorphous.

[0029] - Characteristics at various temperatures In addition to the density of crystal defects (spin density) at 25°C and 200°C described above, by designing an α-sialon phosphor to satisfy one or more of the characteristics described below, the performance of the α-sialon phosphor, especially at high temperatures, can sometimes be further improved.

[0030] The density of crystal defects in the α-sialon phosphor of this embodiment is preferably 1.0×10 as the spin density value of a signal near g=2 detected by electron spin resonance measurement at 300° C. 15 spins / g or less, more preferably 1.0 x 10 14 spins / g or more 1.0×10 15 spins / g or less, more preferably 4.0 x 10 14 spins / g or more 9.0×10 14 spins / g or less.

[0031] The density of crystal defects in the α-sialon phosphor of this embodiment is preferably 9.5×10 as the spin density value of a signal near g=2 detected by electron spin resonance measurement at 600° C. 15 spins / g or less, more preferably 5.0 x 10 15 spins / g or more 9.5×10 15 spins / g or less, more preferably 7.5 x 10 15 spins / g or more 9.5×10 15 spins / g or less.

[0032] The internal quantum efficiency of the α-sialon phosphor of this embodiment at 200°C is preferably 87% or more, more preferably 88% or more. The closer this value is to 100%, the better, but in reality it is 95% or less or 93% or less. In other words, the internal quantum efficiency at 200°C is preferably 87% or more and 95% or less, more preferably 88% or more and 93% or less.

[0033] The external quantum efficiency of the α-sialon phosphor of this embodiment at 300°C is preferably 80% or more, more preferably 82% or more. The closer this value is to 100%, the better, but in reality it is 90% or less or 88% or less. In other words, the external quantum efficiency at 200°C is preferably 80% or more and 90% or less, more preferably 82% or more and 88% or less.

[0034] In the α-sialon phosphor of this embodiment, the internal quantum efficiency retention rate, expressed as {(internal quantum efficiency at 24°C) / (internal quantum efficiency at 300°C)}×100[%], is preferably 89% or more, more preferably 89% or more and 99% or less, and even more preferably 90% or more and 99% or less.

[0035] In the α-sialon phosphor of this embodiment, the external quantum efficiency maintenance rate, expressed as {(external quantum efficiency at 24°C) / (external quantum efficiency at 300°C)}×100[%], is preferably 88% or more, more preferably 88% or more and 99% or less, and even more preferably 89% or more and 97% or less.

[0036] 1 is a schematic cross-sectional view illustrating the structure of a light emitting device 100. As shown in FIG. 1, the light emitting device 100 includes a light emitting element 120, a heat sink 130, a case 140, a first lead frame 150, a second lead frame 160, bonding wires 170 and 172, and a composite 40.

[0037] The light emitting element 120 is mounted in a predetermined region on the upper surface of the heat sink 130. Mounting the light emitting element 120 on the heat sink 130 can improve the heat dissipation properties of the light emitting element 120. Note that a packaging substrate may be used instead of the heat sink 130.

[0038] The light-emitting element 120 is a semiconductor element that emits excitation light. For example, an LED chip that emits light with a wavelength of 300 nm or more and 500 nm or less, which corresponds to near-ultraviolet to blue light, can be used as the light-emitting element 120. One electrode (not shown) disposed on the upper surface of the light-emitting element 120 is connected to the surface of the first lead frame 150 via a bonding wire 170 such as a gold wire. The other electrode (not shown) formed on the upper surface of the light-emitting element 120 is connected to the surface of the second lead frame 160 via a bonding wire 172 such as a gold wire.

[0039] A generally funnel-shaped recess whose diameter gradually increases from the bottom to the top is formed in the case 140. The light emitting element 120 is provided on the bottom of the recess. The wall of the recess surrounding the light emitting element 120 serves as a reflector.

[0040] The composite 40 is filled in the recess whose wall surface is formed by the case 140. The composite 40 is a wavelength conversion member that lengthens the wavelength of the excitation light emitted from the light emitting element 120. The composite of this embodiment is used as the composite 40, and the phosphor 1 of this embodiment is dispersed in a sealing material 30 such as a resin. The light emitting device 100 emits a mixed color of the light from the light emitting element 120 and the light generated from the phosphor 1 that is excited by absorbing the light from the light emitting element 120. It is preferable that the light emitting device 100 emits white light by mixing the light from the light emitting element 120 and the light generated from the phosphor 1.

[0041] Incidentally, examples of resins that can be used for the sealing material 30 in the composite 40 include transparent resins such as silicone resin, epoxy resin, and urethane resin. The composite 40 can be produced, for example, by adding the α-sialon phosphor of this embodiment to a liquid resin or powdered glass or ceramics, mixing them uniformly, and then curing or sintering them by heat treatment.

[0042] In the light emitting device 100 of this embodiment, the use of the above-mentioned α-sialon phosphor as the phosphor 1 suppresses changes in light emitting characteristics at high temperatures. Therefore, the light emitting device 100 is suitable for use in vehicles. However, just to be clear, the use of the light emitting device 100 is not limited to vehicle use. The light emitting device 100 can also be used for lighting applications other than vehicle use, display applications, etc.

[0043] Incidentally, although FIG. 1 illustrates a surface-mounted light-emitting device, the light-emitting device is not limited to the surface-mounted type, and may be a bullet type, a COB (chip-on-board) type, or a CSP (chip-scale package) type.

[0044] <Method for manufacturing α-sialon phosphor> The method for manufacturing an α-sialon phosphor of this embodiment includes: a firing step of obtaining a bulk α-sialon phosphor containing Eu element by firing; a crushing step of crushing the bulk α-sialon phosphor to obtain a powdered α-sialon phosphor; and a N annealing step of annealing the powdered α-sialon phosphor in a nitrogen gas atmosphere at a temperature of 1200° C. to 1700° C. for a time of 5 hours to 30 hours. 2 an annealing step in which the powdered α-sialon phosphor is annealed in a hydrogen gas atmosphere at a temperature of 1200° C. to 1700° C. for a time period of 5 hours to 30 hours; 2 Annealing step, and 2 and an acid treatment step of performing an acid treatment on the powdered α-sialon phosphor after the annealing step using an acidic aqueous solution.

[0045] In the method for producing an α-sialon phosphor of this embodiment, preferably, H 2 The annealing process is performed using N 2 It is carried out after the annealing step. It is also preferable to carry out an elutriation step in which the powdered α-sialon phosphor after the acid treatment step is classified by elutriation.

[0046] By the above-mentioned manufacturing method, it is possible to obtain an α-sialon phosphor with particularly few crystal defects. 2 Annealing process and H 2It is believed that the combination of the annealing process is effective in reducing crystal defects.

[0047] Below, we will provide additional information about each step.

[0048] Firing process The firing process can be carried out with reference to conventional methods for producing α-sialon phosphors. Briefly, one example is as follows: (i) first, raw materials (such as nitrides or oxides of each element) containing elements constituting an α-sialon phosphor containing Eu are mixed to obtain a mixture; (ii) the mixture is filled into a boron nitride container and fired in a nitrogen atmosphere at 1650°C or higher and 1950°C or lower, thereby obtaining a bulk α-sialon phosphor containing Eu. Regarding the firing process, for example, reference can be made to the descriptions in paragraphs 0036 to 0044 and the Examples of WO 2020 / 203483. Other known documents can also be used as references.

[0049] - Crushing process In the firing process, an α-sialon phosphor having an ingot-shaped outer shape is usually produced. This ingot-shaped α-sialon phosphor is crushed using a crusher, mortar crusher, ball mill, vibration mill, jet mill, or other crusher to obtain a powdered α-sialon phosphor. By adjusting the degree of crushing, it is possible to adjust the particle size distribution, such as the median diameter, of the α-sialon phosphor.

[0050] In addition to the pulverization step, a sieving step may be performed. By performing the sieving step, the particle size distribution, such as the median diameter, can be adjusted more precisely. Alternatively, a step may be performed in which the pulverized powdered α-sialon phosphor is dispersed in an aqueous solution and allowed to stand for a certain period of time to remove particles with small particle sizes that are difficult to settle. This allows the particle size distribution, such as the median diameter, to be adjusted more precisely.

[0051] ・N 2 Annealing process N 2 The temperature of the annealing step may be 1200°C or higher and 1700°C or lower, but is preferably 1300°C or higher and 1600°C or lower. 2The annealing step may be carried out for a period of 5 hours to 30 hours, preferably 8 hours to 25 hours. 2 The pressure in the annealing step is not particularly limited, but is, for example, 0.02 MPa·G or more and 0.9 MPa·G or less, and preferably 0.02 MPa·G or more and 0.2 MPa·G or less.

[0052] N 2 The annealing process is performed using N 2 And, N 2 The reaction may be carried out in an atmosphere of a mixture of inert gases (such as noble gases) other than N. 2 Even in a mixed gas atmosphere, the N in the mixed gas is 2 The ratio of is preferably more than 50% by volume, and more preferably more than 75% by volume, which is thought to further reduce crystal defects in the α-sialon phosphor.

[0053] ・H 2 Annealing process H 2 The temperature of the annealing step may be 1200°C or higher and 1700°C or lower, and preferably 1300°C or higher and 1600°C or lower. 2 The duration of the annealing step may be from 5 hours to 30 hours, and is preferably from 8 hours to 25 hours. 2 The pressure in the annealing step is not particularly limited, but is, for example, 0.02 MPa or more and 0.9 MPa or less, and preferably 0.02 MPa or more and 0.1 MPa or less.

[0054] H 2 The annealing process is performed using H 2 And, H 2 The reaction may be carried out in an atmosphere of a mixture of inert gases (such as noble gases) other than H. 2 Even when the reaction is carried out in a mixed gas atmosphere, the H 2 The ratio of is preferably more than 50% by volume, and more preferably more than 75% by volume, which is thought to further reduce crystal defects in the α-sialon phosphor.

[0055] Acid Treatment Step In the acid treatment step, for example, a powdered α-sialon phosphor is placed in an acidic aqueous solution and stirred using a stirrer. Examples of the acidic aqueous solution include an acidic aqueous solution containing one acid selected from acids such as hydrofluoric acid, nitric acid, and hydrochloric acid, or a mixed acid aqueous solution obtained by mixing two or more of the above acids. Among these, a hydrofluoric acid aqueous solution containing hydrofluoric acid alone and a mixed acid aqueous solution obtained by mixing hydrofluoric acid and nitric acid are more preferred. The concentration of the acidic aqueous solution is appropriately set depending on the strength of the acid used, but is preferably 0.7% to 100%, more preferably 0.7% to 40%. Furthermore, the temperature during the acid treatment is preferably 60°C to 90°C, and the reaction time (immersion time) is preferably 15 to 80 minutes.

[0056] High-speed stirring facilitates sufficient acid treatment of the particle surface. Here, "high speed" depends on the stirring device used. When using a laboratory-level magnetic stirrer, the stirring speed is, for example, 400 rpm or higher, and more practically, 400 rpm to 500 rpm. For the normal purpose of stirring, which is to constantly supply fresh acid to the particle surface, a stirring speed of approximately 200 rpm is sufficient. However, high-speed stirring at 400 rpm or higher facilitates sufficient treatment of the particle surface through physical action in addition to chemical action. By selecting appropriate stirring conditions, foreign matter and heterogeneous phases (which may result in a deterioration of the luminescence characteristics) on the phosphor surface are sufficiently removed. As a result, it appears that crystal defects in the α-sialon phosphor as a whole are further reduced. As a result, it is believed that changes in the luminescence characteristics under high-temperature environments can be further minimized.

[0057] Classification step: Some sort of classification process may be carried out to adjust the particle size distribution of the α-sialon phosphor. Classification may be carried out under dry conditions or wet conditions. Classification may also be carried out using various industrially used devices, such as a settling tank, a hydrocyclone, a centrifuge, a cyclone, or an air separator. Among these, elutriation classification using a settling tank is preferred, but the specific classification method is not limited to elutriation classification using a settling tank.

[0058] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations may be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of achieving the object of the present invention are included in the present invention.

[0059] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. However, it should be noted that the present invention is not limited to the Examples.

[0060] <Production of α-SiAlON Phosphor> (Examples 1 and 2 and Comparative Example 1) An α-SiAlON phosphor was produced according to the following procedure. (1) Firing Step In a glove box, the raw material powders were dry-blended with a composition of 62.4 parts by mass of silicon nitride powder (E10 grade, manufactured by Ube Industries, Ltd.), 22.5 parts by mass of aluminum nitride powder (E grade, manufactured by Tokuyama Corporation), 2.2 parts by mass of europium oxide powder (RU grade, manufactured by Shin-Etsu Chemical Co., Ltd.), and 12.9 parts by mass of calcium nitride powder (Kojundo Chemical Research Institute). The raw material powders were then passed through a nylon sieve with 250 μm openings to obtain a raw material mixed powder. 120 g of this raw material mixed powder was filled into a lidded cylindrical boron nitride container (N-1 grade, manufactured by Denka Company, Ltd.) with an internal volume of 0.4 liters. The raw material mixed powder was placed in a container and heated (fired) in an electric furnace equipped with a carbon heater in a nitrogen atmosphere at atmospheric pressure for 16 hours at 1800°C. Since calcium nitride contained in the raw material mixed powder is easily hydrolyzed in air, the boron nitride container filled with the raw material mixed powder was removed from the glove box, quickly placed in an electric furnace, and immediately evacuated to prevent reaction of calcium nitride. (2) Crushing step The fired product obtained in (1) above was crushed or pulverized appropriately in a mortar and passed through a sieve with 150 μm openings to obtain a phosphor powder. The crystalline phase of this phosphor powder was examined by powder X-ray diffraction measurement using CuKα radiation, and the crystalline phase present was found to be α-sialon. (3) N 2 Annealing Step The powdered α-sialon phosphor obtained in the crushing step (2) above was placed in a container made of boron nitride and the container was covered. The container was placed in a heating furnace and the "N" in Table 1 below was added. 2The powder was then subjected to a heat treatment in a nitrogen gas atmosphere under the conditions described in the "Annealing" section. After cooling, the orange powder recovered from the container was passed through a sieve with 75 μm openings. 2 The annealed phosphor powder was obtained. 2 Annealing step (3) N 2 The annealed phosphor powder was placed in a boron nitride container and covered with a lid. The container was placed in a heating furnace and heated in a hydrogen gas atmosphere. The heating conditions were as shown in Table 1 below. 2 After cooling, the orange powder recovered from the container was passed through a sieve with 75 μm openings. 2 An annealed phosphor powder was obtained. (5) Acid Treatment Step First, 50 mL of 50% hydrofluoric acid and 50 mL of 70% nitric acid were mixed to prepare a mixed solution. 300 mL of distilled water was added to this mixed solution to dilute the concentration of the mixed solution to 25%, and 400 mL of mixed acid aqueous solution was prepared. The H 2 30 g of the phosphor powder recovered after the annealing step was added, and the temperature of the mixed acid solution was kept at 80°C, and the solution was stirred for 60 minutes at a rotation speed of 450 rpm using a magnetic stirrer. After stirring, the acid adhering to the phosphor was thoroughly washed with distilled water. The washed phosphor powder was recovered by filtration and dried.

[0061] The particle size distribution of the dried phosphor powder was measured using a Microtrac MT3300EX II (Microtrac Bell Corporation) by a laser diffraction scattering method in accordance with JIS R1629:1997. Specifically, 0.5 g of powdered α-sialon phosphor was first added to 100 cc of ion-exchanged water, and a dispersion was performed for 3 minutes using an Ultrasonic Homogenizer US-150E (Nihon Seiki Seisakusho Co., Ltd., tip size φ20 mm, Amplitude 100%, oscillation frequency 19.5 kHz, amplitude approximately 31 μm) to obtain a dispersion. This dispersion was set in the MT3300EX II, and the particle size distribution was measured. From the obtained particle size distribution, the median diameter D 50 asked for.

[0062] N 2Annealing process and H 2 Annealing step conditions and D 50 is shown in Table 1.

[0063]

[0064] <Electron spin resonance measurement> Electron spin resonance measurement was carried out as follows for the α-sialon phosphors of Examples 1 and 2 and Comparative Example 1. Then, the densities of crystal defects in the α-sialon phosphors at 25°C, 200°C, 300°C and 600°C were determined as the spin density values ​​of the signal near g = 2.

[0065] (Measurement Procedure) A sample powder (approximately 60 mg) was placed in an ESR sample tube and set in the apparatus. Simulated air (flow rate: 20 mL min-1) was circulated through the sample tube, and ESR measurements were performed at room temperature (25 ° C) around g = 2. Thereafter, the temperature was increased to 200 ° C at a rate of 30 ° C / min, and after holding for 30 minutes, ESR measurements were performed around g = 2. Thereafter, the temperature was increased to 300 ° C at a rate of 30 ° C / min, and after holding for 30 minutes, ESR measurements were performed around g = 2. Thereafter, the temperature was increased to 600 ° C at a rate of 30 ° C / min, and after holding for 30 minutes, ESR measurements were performed around g = 2.

[0066] (Measurement device and measurement conditions) A BRUKER ESR device "EMXplus" and a BRUKER high-temperature cavity "ER4114HT" were used. The measurement conditions were as follows: Magnetic field sweep range: around 3350 to 3550 G Modulation: 100 kHz, 5 G Microwave: 9.67 GHz, 1 mW Sweep time: 80 s x 4 times Time constant: 327.68 ms Number of data points: 1000 points

[0067] (Analysis of Measurement Data) ESR spectra are usually observed as first-order differential curves in order to sensitively observe the unevenness of the electromagnetic wave absorption spectrum. Since the absorption intensity is proportional to the spin number, the ESR spectrum was integrated twice to convert the differential curve into an integral curve, and the spin number of the sample was quantified from the peak area ratio with that of a standard sample. Regarding the integration range, the straight lines passing through the vicinity of g = 2.0171 and g = 1.9838 in the first-order differential curve were subtracted as the baseline, and then the range of g = 2.0171 to 1.9838 was integrated. This determined the peak area derived from the sample near g = 2. For the analysis, the ESR software "WinEPR" manufactured by BRUKER was used.

[0068] (Calculation of spin number and spin density) The spin number [spins] of the sample at 25°C was determined from the peak area ratio of a secondary standard sample (ion-implanted polyethylene film) with a known spin number, which was separately subjected to ESR measurement. Furthermore, the spin number of the sample was divided by the sample mass [g] used in the measurement to determine the spin number of the sample per unit mass at 25°C (spin density [spins / g]). Incidentally, the spin number of the secondary standard sample (ion-implanted polyethylene film) was determined from the peak area ratio of a primary standard sample (copper sulfate pentahydrate) with a known spin number, which was separately subjected to ESR measurement at 25°C. The number of spins [spins] of the sample at 200°C was determined from the peak area ratio to that of a secondary standard sample (ion-implanted polyethylene film) in the same manner as at 25°C, and then corrected for the effect of measurement temperature on signal intensity by multiplying the result by the measurement temperature ((273 + 200) [K]) divided by room temperature ((273 + 25) [K]) (Curie's law). The number of spins of the sample was then divided by the sample mass [g] used for measurement to determine the number of spins of the sample per unit mass at 200°C (spin density [spins / g]). Similarly, the spin density [spins / g] of the sample at 300°C was determined. Incidentally, when performing temperature correction using Curie's law, the result was multiplied by the measurement temperature ((273 + 300) [K]) divided by room temperature ((273 + 25) [K]). Similarly, the spin density [spins / g] of the sample at 600°C was determined. Incidentally, when performing temperature correction using Curie's law, the measurement temperature ((273+600) [K]) was multiplied by room temperature ((273+25) [K]).

[0069] (Note) The absorption intensity in the ESR spectrum changes depending on the measurement conditions. Therefore, the influence of the Q value of the resonator, receiver gain, number of integrations [times], modulation [G], conversion time [ms], microwave power [mW], inner diameter of the sample tube [mm], center position of the resonator [mm], length of inserted sample [mm], and spin quantum number was appropriately corrected during analysis.

[0070] The results are shown in Table 2 below, where the units of values ​​are spins / g.

[0071]

[0072] <Evaluation: Change in luminescence characteristics due to temperature> For the α-sialon phosphors of each example and comparative example, the absorptance, internal quantum efficiency, external quantum efficiency, and their temperature dependencies were measured using a spectrophotometer (QE-2100 manufactured by Otsuka Electronics Co., Ltd.) and re-excitation correction was performed by subtracting the re-excitation fluorescence from the total fluorescence to determine the absorptance, internal quantum efficiency, and external quantum efficiency.

[0073] The above-mentioned absorptance, internal quantum efficiency, and external quantum efficiency were measured while changing the sample temperature from room temperature to 300° C., and the temperature changes in the internal quantum efficiency and external quantum efficiency were evaluated. As quantitative indicators of temperature changes, the internal quantum efficiency at each temperature relative to the value of the internal quantum efficiency at room temperature ("internal quantum efficiency maintenance rate"), and the external quantum efficiency at each temperature relative to the value of the external quantum efficiency at room temperature ("external quantum efficiency maintenance rate") were calculated.

[0074] The above evaluation results are summarized in Tables 3, 4 and 5.

[0075]

[0076]

[0077]

[0078] As can be seen from the above table, the density of crystal defects at 25°C or 200°C is 1.0 x 10 15 In Comparative Example 1, where the density of crystal defects was greater than 1.0 × 10 at 25°C or 200°C, the internal quantum efficiency and external quantum efficiency were significantly reduced, particularly at a high temperature of 300°C. 15 In Examples 1 and 2, where the luminous flux density was less than 1000 s / g, the decrease in the internal quantum efficiency and the external quantum efficiency was suppressed even at high temperatures. In other words, the change in the luminescence characteristics was small even at high temperatures. It can be said that the phosphors of Examples 1 and 2 are suitable for use in automobiles.

[0079] This application claims priority based on Japanese Patent Application No. 2023-058890, filed March 31, 2023, the disclosure of which is incorporated herein by reference in its entirety.

[0080] REFERENCE SIGNS LIST 1 Phosphor 30 Sealant 40 Composite 100 Light emitting device 120 Light emitting element 130 Heat sink 140 Case 150 First lead frame 160 Second lead frame 170 Bonding wire 172 Bonding wire

Claims

1. An α-SiAlON phosphor containing Eu, wherein the density of crystal defects in the α-SiAlON phosphor is 1.0×10 or less as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 25° C. 15 The α-sialon phosphor has a density of 100000000000000 spins / g or less.

2. An α-SiAlON phosphor containing Eu, wherein the density of crystal defects in the α-SiAlON phosphor is 1.0×10 or less as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 200° C. 15 The α-sialon phosphor has a density of 100000000000000 spins / g or less.

3. The α-SiAlON phosphor according to claim 2, wherein the density of crystal defects in the α-SiAlON phosphor is 1.0×10 or less as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 25° C. 15 The α-sialon phosphor has a density of 100000000000000 spins / g or less.

4. An α-SiAlON phosphor according to any one of claims 1 to 3, wherein the density of crystal defects in the α-SiAlON phosphor is 1.0×10 or less as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 300°C. 15 The α-sialon phosphor has a density of 100000000000000 spins / g or less.

5. An α-SiAlON phosphor according to any one of claims 1 to 3, wherein the density of crystal defects in the α-SiAlON phosphor is 9.5×10 or less as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 600°C. 15 The α-sialon phosphor has a density of 100000000000000 spins / g or less.

6. An α-SiAlON phosphor according to any one of claims 1 to 3, which has an internal quantum efficiency of 87% or more at 200°C.

7. An α-SiAlON phosphor according to any one of claims 1 to 3, which has an internal quantum efficiency of 80% or more at 300°C.

8. An α-SiAlON phosphor according to any one of claims 1 to 3, wherein the α-SiAlON phosphor has an internal quantum efficiency maintenance rate of 89% or more, expressed as {(internal quantum efficiency at 24°C) / (internal quantum efficiency at 300°C)}×100[%].

9. An α-SiAlON phosphor according to any one of claims 1 to 3, wherein the α-SiAlON phosphor has an external quantum efficiency maintenance rate of 88% or more, expressed as {(external quantum efficiency at 24°C) / (external quantum efficiency at 300°C)}×100[%].

10. The α-SiAlON phosphor according to any one of claims 1 to 3, wherein the composition is represented by the general formula: (M1 x , M2 y , Eu z ) (Si 12-(m+n) A m+n ) (O n N 16-n ), wherein in the general formula, M1 is a monovalent Li element, M2 is one or more divalent elements selected from the group consisting of Mg, Ca, and lanthanide elements (excluding La and Ce), and 0≦x<2.0, 0≦y<2.0, 0<z≦0.5, 0<x+y, 0.3≦x+y+z≦2.0, 0<m≦4.0, 0<n≦3.

0.

11. A light emitting device comprising: a light emitting element; and a wavelength conversion section that contains the α-sialon phosphor according to any one of claims 1 to 3 and converts the wavelength of light emitted from the light emitting element into a longer wavelength.

12. A firing step for obtaining a lump-shaped α-SiAlON phosphor containing Eu element by firing; a crushing step for crushing the lump-shaped α-SiAlON phosphor to obtain a powdered α-SiAlON phosphor; and a N annealing step for annealing the powdered α-SiAlON phosphor in a nitrogen gas atmosphere at a temperature range of 1200°C to 1700°C for a time range of 5 hours to 30 hours. 2 annealing the powdered α-SiAlON phosphor in a hydrogen gas atmosphere at a temperature in the range of 1200° C. to 1700° C. for a time in the range of 5 hours to 30 hours; 2 An annealing step; 2 an acid treatment step of performing an acid treatment on the powdered α-sialon phosphor after the annealing step using an acidic aqueous solution.

Citation Information

Patent Citations

  • Phosphor, production method thereof, and light emitting device

    JP2015224339A

  • Process for producing fluorescent substance and fluorescent substance produced thereby