Α-sialon phosphor, light-emitting device, and method for producing α-sialon phosphor

A low-defect α-sialon phosphor is produced using specialized manufacturing processes, ensuring stable light emission in high-temperature conditions, addressing the issue of characteristic changes in conventional phosphors for automotive LEDs.

JP2024146155AActive Publication Date: 2024-10-15DENKA CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023058890
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Conventional α-sialon phosphors used in white LEDs experience significant changes in light emission characteristics under high-temperature environments, making them unsuitable for automotive applications.

Method used

Development of an α-sialon phosphor with a low density of crystal defects, achieved through specific manufacturing processes including annealing in nitrogen and hydrogen atmospheres and acid treatment, to maintain luminescent properties in high-temperature conditions.

Benefits of technology

The α-sialon phosphor maintains stable light emission characteristics even in high-temperature environments, suitable for use in white LEDs for automotive applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146155000001_ABST
    Figure 2024146155000001_ABST
Patent Text Reader

Abstract

To provide an α-sialon phosphor whose luminescence properties hardly change even in high temperature environments when used as wavelength conversion members in white LEDs, for example.SOLUTION: An α-sialon phosphor contains elemental Eu and has crystal defect density of 1.0×1015 spins / g or less as spin density of signals in the vicinity of g=2 detected by the electron spin resonance measurement at 25°C. An α-sialon phosphor contains elemental Eu and has crystal defect density of 1.0×1015 spins / g or less as the spin density of signals in the vicinity of g=2 detected by the electron spin resonance measurement at 200°C.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an α-sialon phosphor, a light emitting device, and a method for producing an α-sialon phosphor. [Background technology]

[0002] Alpha-SiAlON phosphors activated with rare earth elements such as Eu can efficiently convert blue light into long-wavelength light, and are therefore used as wavelength conversion materials in white LEDs.

[0003] In α-type sialon phosphors, the Si-N bonds of α-type silicon nitride crystals are usually partially replaced with Al-N bonds and Al-O bonds, and in order to maintain electrical neutrality, certain elements (Ca, Li, Mg, Y, or lanthanide metals excluding La and Ce) are intercalated and dissolved between the crystal lattices. Fluorescence properties are expressed by making some of the intercalated and dissolved elements rare earth elements that become the emission center. Among them, α-type sialon phosphors in which Ca is solid-dissolved and part of it is replaced with Eu are excited relatively efficiently in a wide wavelength range from ultraviolet to blue, and emit yellow or orange light.

[0004] In order to further improve the fluorescent properties of α-sialon phosphors, various attempts have been proposed (for example, Patent Documents 1 to 3, etc.). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2009-96882 A [Patent Document 2] Patent No. 6667025 [Patent Document 3] Patent No. 6785333 Summary of the Invention [Problem to be solved by the invention]

[0006] It is conceivable that white LEDs using α-type SiAlON phosphors as wavelength conversion materials could be applied to in-vehicle applications. For in-vehicle applications, it is required that the various characteristics of white LEDs do not change even at high temperatures. However, as a result of the preliminary study by the present inventors, it became clear that white LEDs that use conventional α-SiAlON phosphors as wavelength conversion materials undergo large changes in their light emission characteristics in high-temperature environments.

[0007] The present invention has been made in view of the above circumstances. One of the objects of the present invention is to provide an α-SiAlON phosphor whose luminescence characteristics are unlikely to change even in a high-temperature environment when used as a wavelength conversion member for a white LED. [Means for solving the problem]

[0008] The present inventors have completed the invention provided below and have solved the above problems.

[0009] 1. An α-SiAlON phosphor containing Eu element, The density of crystal defects in the α-sialon phosphor is 1.0×10 as the spin density value of a signal near g=2 detected by electron spin resonance measurement at 25° C. 15 α-SiAlON phosphor with a spins / g or less. 2. An α-SiAlON phosphor containing Eu element, The density of crystal defects in the α-sialon phosphor is 1.0×10 as the spin density value of a signal near g=2 detected by electron spin resonance measurement at 200° C. 15 α-SiAlON phosphor with a spins / g or less. 3. 2. The α-sialon phosphor according to claim 1, The density of crystal defects in the α-sialon phosphor is 1.0×10 as the spin density value of a signal near g=2 detected by electron spin resonance measurement at 25° C. 15 α-SiAlON phosphor with a spins / g or less. 4. An α-sialon phosphor according to any one of 1. to 3., The density of crystal defects in the α-SiAlON phosphor is 1.0×10 as the spin density value of the signal near g=2 detected by electron spin resonance measurement at 300° C. 15 α-SiAlON phosphor with a spins / g or less. 5. An α-sialon phosphor according to any one of 1. to 4., The density of crystal defects in the α-sialon phosphor is 9.5×10 as the spin density value of the signal near g=2 detected by electron spin resonance measurement at 600° C. 15 α-SiAlON phosphor with a spins / g or less. 6. α-SiAlON phosphor according to any one of 1. to 5., An α-type SiAlON phosphor with an internal quantum efficiency of 87% or more at 200°C. 7. An α-sialon phosphor according to any one of 1. to 6., An α-type SiAlON phosphor with an internal quantum efficiency of 80% or more at 300℃. 8. An α-sialon phosphor according to any one of 1. to 7., An α-SiAlON phosphor with an internal quantum efficiency maintenance rate of 89% or more, expressed as {(internal quantum efficiency at 24°C) / (internal quantum efficiency at 300°C)}×100[%]. 9. 1. An α-sialon phosphor according to any one of 1. to 8., An α-SiAlON phosphor with an external quantum efficiency maintenance rate of 88% or more, expressed as {(external quantum efficiency at 24°C) / (external quantum efficiency at 300°C)}×100[%]. 10. A light-emitting element; A wavelength conversion section that includes the α-sialon phosphor according to any one of 1. to 9. and converts the wavelength of the light emitted from the light emitting element into a longer wavelength. A light emitting device comprising: 11. a firing step of obtaining a lump-shaped α-SiAlON phosphor containing Eu element by firing; a crushing step of crushing the aggregated α-sialon phosphor to obtain a powdered α-sialon phosphor; an N2 annealing step of annealing the powdered α-SiAlON phosphor in a nitrogen gas atmosphere at a temperature in the range of 1200°C to 1700°C for a time in the range of 5 hours to 30 hours; an H2 annealing step of annealing the powdered α-SiAlON phosphor in a hydrogen gas atmosphere at a temperature in the range of 1200°C to 1700°C for a time in the range of 5 hours to 30 hours; an acid treatment step of performing an acid treatment on the powdered α-SiAlON phosphor after the H2 annealing step using an acidic aqueous solution; A method for producing an α-sialon phosphor comprising the steps of: Effect of the Invention

[0010] A white LED using the α-sialon phosphor of the present invention as a wavelength conversion member is less likely to change in light emission characteristics even in a high-temperature environment. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic cross-sectional view showing an example of the structure of a light-emitting device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In the drawings, similar components are given similar symbols and descriptions thereof will be omitted as appropriate. In order to avoid complexity, when there are multiple identical components in the same drawing, only one of them may be labeled with a reference symbol, and not all of them. The drawings are for illustrative purposes only. The shapes and dimensional ratios of the components in the drawings do not necessarily correspond to the actual products.

[0013] In this specification, unless otherwise specified, the expression "X to Y" in the explanation of a numerical range means from X to Y. For example, "1 to 5% by mass" means "from 1% by mass to 5% by mass".

[0014] In this specification, the "α-type Sialon phosphor containing Eu element" may be simply referred to as the "α-type Sialon phosphor". In this specification, the term "signal near g=2" literally means a signal whose g value in electron spin resonance measurement is near 2. Specifically, near g=2 means g=2±0.02.

[0015] <α-type Sialon phosphor> The α-sialon phosphor of this embodiment contains Eu element, or in other words, is an Eu-activated α-sialon phosphor.

[0016] The α-sialon phosphor of this embodiment satisfies one or both of the following (1) and (2). (1) The density of crystal defects in the α-SiAlON phosphor of the present embodiment is, at 25° C., 1.0×10 as the spin density value of a signal near g=2 detected by electron spin resonance measurement. 15 This value can be up to 1.0×10 14 spins / g or more 8.0×10 14 spins / g or less, more preferably 1.0×10 13 spins / g or more 6.0×10 14 spins / g or less. (2) The density of crystal defects in the α-SiAlON phosphor of the present embodiment is, at 200° C., 1.0×10 as the spin density value of the signal near g=2 detected by electron spin resonance measurement. 15 This value can be up to 1.0×10 14 spins / g or more 8.0×10 14 spins / g or less, more preferably 1.0×10 13spins / g or more 6.0×10 14 spins / g or less.

[0017] The inventors have investigated the cause of the change in the luminescence characteristics in a high-temperature environment from various viewpoints. Through the investigation, the inventors have come to the conclusion that the value of the density of crystal defects obtained through electron spin resonance (ESR) measurement may be correlated with the degree of change in the luminescence characteristics. This is because the presence of crystal defects is generally considered to cause a decrease in the luminescence characteristics.

[0018] Based on the above idea, the present inventors have newly created an α-SiAlON phosphor with a sufficiently small density of crystal defects obtained through electron spin resonance (ESR) measurement at 25° C. and / or 200° C. Then, by using this new α-SiAlON phosphor as a wavelength conversion material for a white LED, it has been possible to manufacture a white LED whose light emission characteristics are unlikely to change even in a high-temperature environment.

[0019] A sufficiently small density of crystal defects at 200°C means that there are few crystal defects even in a high-temperature environment. If the density of crystal defects in a high-temperature environment is small, various characteristics are unlikely to change even in the high temperatures experienced when the device is mounted in a vehicle, and therefore the light-emitting characteristics are also unlikely to change. In addition, if the density of crystal defects is sufficiently small not only at 200° C. but also at 25° C., it is believed that there will be a corresponding tendency for the number of crystal defects to be reduced even in high-temperature environments. In other words, if the density of crystal defects is sufficiently small at 25° C., it is believed that the light-emitting properties will be less likely to change even in high-temperature environments.

[0020] The α-sialon phosphor of this embodiment can be manufactured through an appropriate manufacturing process. Specifically, the α-sialon phosphor of this embodiment can be manufactured through two annealing processes: an N2 annealing process in which the powdered α-sialon phosphor is annealed in a nitrogen gas atmosphere, and an H2 annealing process in which the powdered α-sialon phosphor is annealed in a hydrogen gas atmosphere. If the manufacturing method is inappropriate, the α-sialon phosphor of this embodiment may not be obtained. The details of the manufacturing method will be described later.

[0021] The α-sialon phosphor of this embodiment will be described further.

[0022] Phosphor composition The composition of the α-sialon phosphor of this embodiment is, for example, General formula: (M1 x ,M2 y ,EU z )(Si 12-(m+n) Al m+n )(O n N 16-n ) This can be shown as: In the above general formula: M1 is a monovalent Li element, M2 is one or more divalent elements selected from the group consisting of Mg, Ca, and lanthanide elements (excluding La and Ce); 0≦x<2.0, 0≦y<2.0, 0 <z≦0.5、0<x+y、0.3≦x+y+z≦2.0、0<m≦4.0、0<n≦3.0 It is.

[0023] The solid solution composition of an α-SiAlON phosphor is represented by x, y, and z in the above general formula, and m and n, which are determined by the accompanying Si / Al ratio and O / N ratio. In particular, when M2 contains Ca, the α-SiAlON phosphor is stabilized over a wide composition range, and by substituting a portion of it with Eu, which acts as the luminescence center, a phosphor is obtained that is excited by light in a wide wavelength range from ultraviolet to blue and emits visible light from yellow to orange.

[0024] In general, since an α-sialon phosphor has a second crystal phase different from that of an α-sialon phosphor and an amorphous phase that inevitably exists, it is not possible to strictly define the solid solution composition by composition analysis, etc. The crystal phase of an α-sialon phosphor is preferably an α-sialon single phase, and may contain aluminum nitride or its polytypoid as another crystal phase.

[0025] Phosphor properties The α-sialon phosphor is usually handled in the form of an α-sialon phosphor powder, which is a collection of α-sialon phosphor particles. The α-sialon phosphor particles often contain secondary particles formed by agglomerating a plurality of primary particles.

[0026] The median diameter (D 50 ) is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. The upper limit of the median diameter of the α-sialon phosphor powder is preferably 30 μm or less, more preferably 20 μm or less. The median diameter of the α-sialon phosphor powder is the dimension of the secondary particles. By making the median diameter of the α-sialon phosphor powder 5 μm or more, the transparency of the wavelength conversion member can be further improved. On the other hand, by making the median diameter of the α-sialon phosphor powder 30 μm or less, chipping can be suppressed when cutting the wavelength conversion member with a dicer or the like.

[0027] Here, the median diameter (D 50 ) means the median diameter in the volume-based cumulative fraction obtained by the laser diffraction scattering method in accordance with JIS R1629:1997. Incidentally, when the α-SiAlON phosphor powder contains secondary particles, the median diameter obtained by the laser diffraction scattering method reflects the size of the secondary particles.

[0028] The shape of the α-SiAlON phosphor particles is not particularly limited, and examples of the shape include a sphere, a cube, a columnar shape, and an amorphous shape.

[0029] -Various characteristics at various temperatures In addition to the above-mentioned density of crystal defects (spin density) at 25°C and 200°C, by designing an α-SiAlON phosphor to satisfy one or more of the characteristics described below, the performance of the α-SiAlON phosphor, especially at high temperatures, can sometimes be further improved.

[0030] The density of crystal defects in the α-sialon phosphor of this embodiment is preferably 1.0×10 or less as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 300° C. 15 spins / g or less, preferably 1.0×10 14 spins / g or more 1.0×10 15 spins / g or less, more preferably 4.0×10 14 spins / g or more 9.0×10 14 spins / g or less.

[0031] The density of crystal defects in the α-sialon phosphor of this embodiment is preferably 9.5×10 as the spin density value of a signal near g=2 detected by electron spin resonance measurement at 600° C. 15 spins / g or less, preferably 5.0×10 15 spins / g or more 9.5×10 15 spins / g or less, more preferably 7.5×10 15 spins / g or more 9.5×10 15 spins / g or less.

[0032] The internal quantum efficiency of the α-sialon phosphor of this embodiment at 200° C. is preferably 87% or more, and more preferably 88% or more. The closer this value is to 100%, the better, but in reality it is 95% or less or 93% or less.

[0033] The internal quantum efficiency of the α-sialon phosphor of this embodiment at 300° C. is preferably 80% or more, and more preferably 82% or more. The closer this value is to 100%, the better, but in reality it is 90% or less or 88% or less.

[0034] In the α-sialon phosphor of this embodiment, the internal quantum efficiency maintenance rate, expressed as {(internal quantum efficiency at 24°C) / (internal quantum efficiency at 300°C)}×100[%], is preferably 89% or more, more preferably 89% or more and 99% or less, and even more preferably 90% or more and 99% or less.

[0035] In the α-sialon phosphor of this embodiment, the external quantum efficiency maintenance rate, expressed as {(external quantum efficiency at 24°C) / (external quantum efficiency at 300°C)}×100[%], is preferably 88% or more, more preferably 88% or more and 99% or less, and even more preferably 89% or more and 97% or less.

[0036] <Light emitting device> FIG. 1 is a schematic cross-sectional view illustrating the structure of a light emitting device. As shown in FIG. 1, the light emitting device 100 includes a light emitting element 120, a heat sink 130, a case 140, a first lead frame 150, a second lead frame 160, bonding wires 170 and 172, and a composite body 40. The light emitting device 100 includes a light emitting element 120, a heat sink 130, a case 140, a first lead frame 150, a second lead frame 160, bonding wires 170 and 172, and a composite body 40.

[0037] The light emitting element 120 is mounted in a predetermined region on the upper surface of the heat sink 130. By mounting the light emitting element 120 on the heat sink 130, it is possible to improve the heat dissipation properties of the light emitting element 120. Note that a packaging substrate may be used instead of the heat sink 130.

[0038] The light emitting element 120 is a semiconductor element that emits excitation light. For example, an LED chip that emits light with a wavelength of 300 nm to 500 nm, which corresponds to near ultraviolet to blue light, can be used as the light emitting element 120. One electrode (not shown) disposed on the upper surface side of the light emitting element 120 is connected to the surface of the first lead frame 150 via a bonding wire 170 such as a gold wire. The other electrode (not shown) formed on the upper surface of the light emitting element 120 is connected to the surface of the second lead frame 160 via a bonding wire 172 such as a gold wire.

[0039] A generally funnel-shaped recess whose hole diameter gradually increases from the bottom surface toward the top is formed in the case 140. The light emitting element 120 is provided on the bottom surface of the recess. The wall surface of the recess surrounding the light emitting element 120 serves as a reflector.

[0040] The composite 40 is filled in the recess whose wall surface is formed by the case 140. The composite 40 is a wavelength conversion member that lengthens the wavelength of the excitation light emitted from the light emitting element 120. The composite of this embodiment is used as the composite 40, and the phosphor 1 of this embodiment is dispersed in a sealing material 30 such as a resin. The light emitting device 100 emits a mixed color of the light of the light emitting element 120 and the light generated from the phosphor 1 that is excited by absorbing the light of the light emitting element 120. It is preferable that the light emitting device 100 emits white light by mixing the light of the light emitting element 120 and the light generated from the phosphor 1.

[0041] Incidentally, examples of resins that can be used for the sealing material 30 in the composite 40 include transparent resins such as silicone resin, epoxy resin, and urethane resin. The composite 40 can be produced, for example, by adding the α-sialon phosphor of this embodiment to liquid resin or powdered glass or ceramics, mixing them uniformly, and then curing or sintering them by heat treatment.

[0042] In the light emitting device 100 of this embodiment, the above-mentioned α-sialon phosphor is used as the phosphor 1, thereby suppressing changes in the light emitting characteristics at high temperatures. Therefore, the light emitting device 100 is suitable for use in vehicles. However, just to be clear, the use of the light emitting device 100 is not limited to in-vehicle use. The light emitting device 100 can also be used for lighting applications other than in-vehicle use, display applications, and the like.

[0043] Incidentally, although a surface mount type light emitting device is illustrated in FIG. 1, the light emitting device is not limited to the surface mount type, and may be a bullet type, a COB (chip on board) type, or a CSP (chip scale package) type.

[0044] <Method of manufacturing α-SiAlON phosphor> The method for producing the α-sialon phosphor of the present embodiment is as follows: a firing step of obtaining a lump-shaped α-SiAlON phosphor containing Eu element by firing; a crushing step of crushing the aggregated α-sialon phosphor to obtain a powdered α-sialon phosphor; an N2 annealing step of annealing the powdered α-SiAlON phosphor in a nitrogen gas atmosphere at a temperature in the range of 1200°C to 1700°C for a time in the range of 5 hours to 30 hours; an H2 annealing step of annealing the powdered α-SiAlON phosphor in a hydrogen gas atmosphere at a temperature of 1200°C to 1700°C for a time period of 5 hours to 30 hours; an acid treatment step of performing an acid treatment on the powdered α-SiAlON phosphor after the H2 annealing step using an acidic aqueous solution; Includes.

[0045] In the method for producing an α-sialon phosphor of the present embodiment, the H2 annealing step is preferably carried out after the N2 annealing step. In addition, it is preferable to carry out an elutriation step in which the powdered α-sialon phosphor after the acid treatment step is classified by elutriation.

[0046] The above manufacturing method makes it possible to obtain α-SiAlON phosphors with particularly few crystal defects. Although the details are unclear, it is speculated that the combination of the N2 annealing process and the H2 annealing process is effective in reducing crystal defects.

[0047] The following provides additional information about each step.

[0048] · Firing process The firing step can be performed by referring to a conventional method for producing an α-SiAlON phosphor. To briefly explain an example, (i) first, raw materials (such as nitrides and oxides of each element) containing elements constituting an α-SiAlON phosphor containing Eu are mixed to obtain a mixture, and (ii) the mixture is filled in a boron nitride container and fired at 1650°C to 1950°C in a nitrogen atmosphere to obtain a lump-shaped α-SiAlON phosphor containing Eu element. For the firing process, reference can be made to, for example, paragraphs 0036 to 0044 and the examples of WO 2020 / 203483. In addition, reference can be made to the descriptions in other known documents.

[0049] Crushing process In the firing step, an α-sialon phosphor having an ingot-like outer shape is usually produced, and this ingot-like α-sialon phosphor is pulverized by a pulverizer such as a crusher, a mortar grinder, a ball mill, a vibration mill, or a jet mill to obtain a powdered α-sialon phosphor. By adjusting the degree of pulverization, it is possible to adjust the particle size distribution, such as the median size, of the α-sialon phosphor.

[0050] In addition to the pulverization step, a sieve classification step may be carried out. By carrying out the sieve classification step, the particle size distribution such as the median size can be adjusted more precisely. Alternatively, the crushed powdered α-sialon phosphor may be dispersed in an aqueous solution and allowed to stand for a certain period of time to remove particles that are small in size and do not settle easily. This allows the particle size distribution, such as the median size, to be adjusted more precisely.

[0051] ·N2 annealing process The temperature in the N2 annealing step may be 1200°C or higher and 1700°C or lower, and is preferably 1300°C or higher and 1600°C or lower. The duration of the N2 annealing step may be from 5 hours to 30 hours, and is preferably from 8 hours to 25 hours. The pressure in the N2 annealing step is not particularly limited, but is, for example, from 0.02 MPa·G to 0.9 MPa·G, and preferably from 0.02 MPa·G to 0.2 MPa·G.

[0052] The N2 annealing step may be performed in a mixed gas atmosphere of N2 and an inert gas other than N2 (such as a noble gas), but is preferably performed in a gas atmosphere consisting essentially of N2. Even in a mixed gas atmosphere, the ratio of N2 in the mixed gas is preferably more than 50 volume %, more preferably more than 75 volume %. This is believed to further reduce crystal defects in the α-SiAlON phosphor.

[0053] ·H2 annealing process The temperature of the H2 annealing step may be 1200°C or higher and 1700°C or lower, and is preferably 1300°C or higher and 1600°C or lower. The duration of the H2 annealing step may be from 5 hours to 30 hours, and is preferably from 8 hours to 25 hours. The pressure in the H2 annealing step is not particularly limited, but is, for example, from 0.02 MPa to 0.9 MPa, and preferably from 0.02 MPa to 0.1 MPa.

[0054] The H2 annealing step may be performed in a mixed gas atmosphere of H2 and an inert gas other than H2 (such as a noble gas), but is preferably performed in a gas atmosphere consisting essentially of H2. Even when performed in a mixed gas atmosphere, the ratio of H2 in the mixed gas is preferably more than 50 volume %, more preferably more than 75 volume %. This is believed to further reduce crystal defects in the α-SiAlON phosphor.

[0055] Acid treatment process In the acid treatment step, for example, a powdered α-sialon phosphor is placed in an acidic aqueous solution and stirred with a stirrer. The acidic aqueous solution may be an acidic aqueous solution containing one acid selected from acids such as hydrofluoric acid, nitric acid, and hydrochloric acid, or a mixed acid aqueous solution obtained by mixing two or more of the above acids. Among these, an aqueous hydrofluoric acid solution containing only hydrofluoric acid and an aqueous mixed acid solution obtained by mixing hydrofluoric acid and nitric acid are more preferred. The concentration of the original solution of the acidic aqueous solution is appropriately set depending on the strength of the acid used, but is preferably 0.7% to 100%, more preferably 0.7% to 40%. In addition, the temperature when carrying out the acid treatment is preferably 60°C to 90°C, and the reaction time (immersion time) is preferably 15 minutes to 80 minutes.

[0056] By stirring at high speed, the particle surface can be sufficiently treated with acid. Here, "high speed" depends on the stirring device used, but when a laboratory-level magnetic stirrer is used, the stirring speed is, for example, 400 rpm or more, and in reality, 400 rpm or more and 500 rpm or less. From the viewpoint of the normal purpose of stirring, which is to constantly supply fresh acid to the particle surface, a stirring speed of about 200 rpm is sufficient, but by stirring at high speed of 400 rpm or more, the particle surface can be sufficiently treated by physical action in addition to chemical action. By selecting appropriate stirring conditions, foreign matter and heterogeneous phases (which may cause a decrease in luminescence characteristics) on the phosphor surface can be sufficiently removed. As a result, it is believed that the crystal defects in the α-SiAlON phosphor as a whole are further reduced. As a result, it is believed that the change in luminescence characteristics in a high-temperature environment can be further reduced.

[0057] ·Classification process Some classification treatment may be performed to adjust the particle size distribution of the α-sialon phosphor. Classification may be performed under dry or wet conditions. Classification may be performed using various industrially used devices, such as a settling tank, a hydrocyclone, a centrifuge, a cyclone, and an air separator. Among these, elutriation classification using a settling tank is preferred, but the specific classification method is not limited to elutriation classification using a settling tank.

[0058] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES

[0059] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. It should be noted that the present invention is not limited to the Examples.

[0060] <Production of α-type Sialon phosphor> (Examples 1 and 2 and Comparative Example 1) An α-SiAlON phosphor was produced according to the following procedure. (1) Firing process In a glove box, the raw powder composition was 62.4 parts by mass of silicon nitride powder (Ube Industries, Ltd., E10 grade), 22.5 parts by mass of aluminum nitride powder (Tokuyama Corporation, E grade), 2.2 parts by mass of europium oxide powder (Shin-Etsu Chemical Co., Ltd., RU grade), and 12.9 parts by mass of calcium nitride powder (Kojundo Chemical Laboratory Co., Ltd.), and the raw powders were dry-blended and then passed through a nylon sieve with a mesh size of 250 μm to obtain a raw mixed powder. 120 g of the raw mixed powder was filled into a cylindrical boron nitride container with an internal volume of 0.4 liters and a lid (Denka Co., Ltd., N-1 grade). The raw material powder mixture was placed in a container and heated (fired) in an electric furnace with a carbon heater in a nitrogen atmosphere at atmospheric pressure for 16 hours at 1800°C. Since calcium nitride contained in the raw material powder mixture is easily hydrolyzed in air, the boron nitride container filled with the raw material powder mixture was removed from the glove box, quickly placed in the electric furnace, and immediately evacuated to prevent the calcium nitride from reacting. (2) Crushing process The fired product obtained in (1) above was crushed or pulverized in a mortar and passed through a sieve with 150 μm openings to obtain a phosphor powder. When the crystal phase of this phosphor powder was examined by powder X-ray diffraction measurement using CuKα radiation, the crystal phase present was found to be α-sialon. (3)N2 annealing process The powdered α-sialon phosphor obtained in the above-mentioned pulverization step (2) was placed in a boron nitride container and covered. This container was placed in a heating furnace and subjected to a heat treatment in a nitrogen gas atmosphere under the conditions described in the "N2 annealing" column in Table 1 below. After cooling, the orange powder collected from the container was passed through a sieve with 75 μm openings. This resulted in an N2 annealed phosphor powder. (4)H2 annealing process The N2-annealed phosphor powder of (3) above was placed in a boron nitride container and the lid was closed. This container was placed in a heating furnace and heated under a hydrogen gas atmosphere. The heating conditions were as shown in the "H2-annealed" column of Table 1 below. After cooling, the orange powder collected from the container was passed through a sieve with 75 μm openings. This yielded an H2-annealed phosphor powder. (5) Acid treatment process First, 50 mL of 50% hydrofluoric acid and 50 mL of 70% nitric acid were mixed to prepare a mixed stock solution. 300 mL of distilled water was added to this mixed stock solution to dilute the concentration of the mixed stock solution to 25%, and 400 mL of mixed acid aqueous solution was prepared. To this mixed acid solution, 30 g of the phosphor powder recovered after the H2 annealing step (4) above was added, and the mixed acid solution was kept at a temperature of 80° C. and stirred with a magnetic stirrer at a rotation speed of 450 rpm for 60 minutes. After the stirring was completed, the acid adhering to the phosphor was thoroughly washed off with distilled water. The washed phosphor powder was recovered by filtration and dried.

[0061] The particle size distribution of the dried phosphor powder was measured by a laser diffraction scattering method in accordance with JIS R1629:1997 using a Microtrac MT3300EX II (Microtrac Bell Corporation). Specifically, 0.5 g of powdered α-SiAlON phosphor was added to 100 cc of ion-exchanged water, and a dispersion was performed for 3 minutes using an Ultrasonic Homogenizer US-150E (Nihon Seiki Seisakusho Co., Ltd., tip size φ20 mm, Amplitude 100%, oscillation frequency 19.5 KHz, amplitude approximately 31 μm) to obtain a dispersion. This dispersion was set in an MT3300EX II to measure the particle size distribution. From the particle size distribution obtained, the median diameter D 50 asked for.

[0062] The conditions of the N2 annealing step and the H2 annealing step, and D 50 is shown in Table 1.

[0063] [Table 1]

[0064] <Electron spin resonance measurement> Electron spin resonance measurements were carried out as follows for the α-SiAlON phosphors of Examples 1 and 2 and Comparative Example 1. The densities of crystal defects in the α-SiAlON phosphors at 25°C, 200°C, 300°C and 600°C were calculated as the spin density values ​​of the signal near g=2.

[0065] (Measurement Procedure) The sample powder (approximately 60 mg) was placed in an ESR sample tube and set in the apparatus. Simulated air (flow rate: 20 mL min-1) was circulated through the sample tube, and ESR measurements were performed at room temperature (25°C) around g = 2. Then, the temperature was raised to 200°C at a rate of 30°C / min and held at that temperature for 30 min, after which ESR measurements were performed near g=2. After that, the temperature was increased to 300° C. at a rate of 30° C. / min and held at that temperature for 30 min, after which ESR measurements were performed near g=2. After that, the temperature was increased to 600°C at a rate of 30°C / min and held at that temperature for 30 min, after which ESR measurements were performed near g=2.

[0066] (Measurement equipment and conditions) The ESR device "EMXplus" manufactured by BRUKER and the high temperature cavity "ER4114HT" manufactured by BRUKER were used. The measurement conditions were as follows. Magnetic field sweep range: Around 3350~3550G Modulation: 100kHz, 5G Microwave: 9.67GHz, 1mW Sweep time: 80s x 4 times Time constant: 327.68ms Number of data points: 1000 points

[0067] (Analysis of measurement data) The ESR spectrum is usually observed as a first derivative curve in order to sensitively observe the unevenness of the electromagnetic wave absorption spectrum. Since the absorption intensity is proportional to the spin number, the ESR spectrum is integrated twice to convert the differential curve into an integral curve, and the spin number of the sample is quantified from the peak area ratio with a standard sample. Regarding the integration range, the straight lines passing around g = 2.0171 and g = 1.9838 in the first derivative curve were subtracted as the baseline, and the range of g = 2.0171 to 1.9838 was integrated. This gave the peak area derived from the sample around g = 2. For the analysis, BRUKER's ESR software "WinEPR" was used.

[0068] (Calculation of spin number and spin density) The number of spins of the sample at 25°C was calculated from the peak area ratio of a secondary standard sample (ion-implanted polyethylene film) with a known number of spins, which was measured separately. The number of spins of the sample was then divided by the mass of the sample used in the measurement (g) to calculate the number of spins of the sample per unit mass at 25°C (spin density [spins / g]). Incidentally, the spin number of the secondary standard sample (ion-implanted polyethylene film) was calculated from the peak area ratio to that of a primary standard sample (copper sulfate pentahydrate) with a known spin number, which was measured separately at 25°C by ESR. The number of spins of the sample at 200°C was calculated from the peak area ratio to that of a secondary standard sample (ion-implanted polyethylene film) in the same manner as for 25°C, and then the effect of the measurement temperature on the signal intensity was corrected by multiplying the measurement temperature ((273+200)[K]) by room temperature ((273+25)[K]) (Curie's law). The number of spins of the sample was then divided by the sample mass [g] used for the measurement to calculate the number of spins of the sample per unit mass at 200°C (spin density [spins / g]). Similarly, the spin density [spins / g] of the sample at 300°C was calculated. Incidentally, when performing temperature correction using Curie's law, the measurement temperature ((273+300)[K]) was multiplied by room temperature ((273+25)[K]). Similarly, the spin density [spins / g] of the sample at 600°C was calculated. Incidentally, when performing temperature correction using Curie's law, the measurement temperature ((273+600)[K]) was multiplied by room temperature ((273+25)[K]).

[0069] (supplement) The absorption intensity in the ESR spectrum changes depending on the measurement conditions, so the effects of the Q value of the resonator, receiver gain, number of integrations [times], modulation [G], conversion time [ms], microwave power [mW], inner diameter of the sample tube [mm], center position of the resonator [mm], length of the inserted sample [mm], and spin quantum number were appropriately corrected during analysis.

[0070] The results are shown in Table 2 below. The units of values ​​are spins / g.

[0071] [Table 2]

[0072] <Evaluation: Change in luminescence characteristics due to temperature> For the α-SiAlON phosphors of each of the Examples and Comparative Examples, the absorptance, internal quantum efficiency, external quantum efficiency, and their temperature dependences were determined using a spectrophotometer (QE-2100 manufactured by Otsuka Electronics Co., Ltd.) by subtracting the re-excitation fluorescence from the total fluorescence to perform re-excitation correction, and the absorptance, internal quantum efficiency, and external quantum efficiency were obtained.

[0073] The above-mentioned absorptance, internal quantum efficiency and external quantum efficiency were measured while changing the sample temperature from room temperature to 300° C., and the temperature changes of the internal quantum efficiency and external quantum efficiency were evaluated. As a quantitative indicator of temperature change, we calculated the internal quantum efficiency at each temperature relative to the value of the internal quantum efficiency at room temperature ("internal quantum efficiency maintenance rate"), and the external quantum efficiency at each temperature relative to the value of the external quantum efficiency at room temperature ("external quantum efficiency maintenance rate").

[0074] The above evaluation results are summarized in Tables 3, 4 and 5.

[0075] [Table 3]

[0076] [Table 4]

[0077] [Table 5]

[0078] As can be seen from the above table, the density of crystal defects at 25°C or 200°C is 1.0×10 15 In Comparative Example 1, in which the spins / g was larger than the spins / g, the internal quantum efficiency and external quantum efficiency were significantly decreased, especially at a high temperature of 300°C. On the other hand, the density of crystal defects at 25°C or 200°C is 1.0×10 15 In Examples 1 and 2, where the internal quantum efficiency and external quantum efficiency are less than spins / g, the decrease in the internal quantum efficiency and external quantum efficiency was suppressed even at high temperatures. In other words, the change in the luminescence characteristics was small even at high temperatures. It can be said that the phosphors of Examples 1 and 2 are suitable for use in vehicles. [Explanation of symbols]

[0079] 1. Phosphor 30 Encapsulating material 40 Complex 100 Light emitting device 120 Light emitting element 130 Heat sink 140 cases 150 First lead frame 160 Second lead frame 170 Bonding Wire 172 Bonding Wire

Claims

1. An α-SiAlON phosphor containing Eu, The density of crystal defects in the α-sialon phosphor is 1.0×10 or less as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 25° C. 15 The α-sialon phosphor has a density of 100000000000000 spins / g or less.

2. An α-SiAlON phosphor containing Eu element, The density of crystal defects in the α-sialon phosphor is 1.0×10 as the spin density value of a signal near g=2 detected by electron spin resonance measurement at 200° C. 15 The α-sialon phosphor has a density of 100000000000000 spins / g or less.

3. 3. The α-sialon phosphor according to claim 2, The density of crystal defects in the α-sialon phosphor is 1.0×10 or less as a spin density value of a signal near g=2 detected by electron spin resonance measurement at 25° C. 15 The α-sialon phosphor has a density of 100000000000000 spins / g or less.

4. The α-sialon phosphor according to any one of claims 1 to 3, The density of crystal defects in the α-sialon phosphor is 1.0×10 as the spin density value of a signal near g=2 detected by electron spin resonance measurement at 300° C. 15 The α-sialon phosphor has a density of 100000000000000 spins / g or less.

5. The α-sialon phosphor according to any one of claims 1 to 3, The density of crystal defects in the α-sialon phosphor is 9.5×10 as the spin density value of a signal near g=2 detected by electron spin resonance measurement at 600° C. 15 The α-sialon phosphor has a density of 100000000000000 spins / g or less.

6. The α-sialon phosphor according to any one of claims 1 to 3, An α-sialon phosphor having an internal quantum efficiency of 87% or more at 200°C.

7. The α-sialon phosphor according to any one of claims 1 to 3, An α-sialon phosphor having an internal quantum efficiency of 80% or more at 300°C.

8. The α-sialon phosphor according to any one of claims 1 to 3, An α-sialon phosphor having an internal quantum efficiency maintenance rate of 89% or more, expressed as {(internal quantum efficiency at 24° C.) / (internal quantum efficiency at 300° C.)}×100[%].

9. The α-sialon phosphor according to any one of claims 1 to 3, An α-sialon phosphor having an external quantum efficiency maintenance rate of 88% or more, expressed as {(external quantum efficiency at 24° C.) / (external quantum efficiency at 300° C.)}×100[%].

10. A light-emitting element; A wavelength conversion section that includes the α-sialon phosphor according to any one of claims 1 to 3 and converts the wavelength of light emitted from the light emitting element into a longer wavelength light; A light emitting device comprising:

11. a firing step of obtaining a lump-shaped α-SiAlON phosphor containing Eu element by firing; a crushing step of crushing the aggregated α-sialon phosphor to obtain a powdered α-sialon phosphor; The powdered α-SiAlON phosphor is annealed in a nitrogen gas atmosphere at a temperature of 1200° C. to 1700° C. for a time period of 5 hours to 30 hours. 2 An annealing step; The powdered α-SiAlON phosphor is annealed in a hydrogen gas atmosphere at a temperature of 1200° C. to 1700° C. for a time period of 5 hours to 30 hours. 2 An annealing step; The H 2 an acid treatment step of performing an acid treatment on the powdered α-SiAlON phosphor after the annealing step using an acidic aqueous solution; A method for producing an α-sialon phosphor comprising the steps of:

Citation Information

Patent Citations

  • Phosphor, production method thereof, and light emitting device

    JP2015224339A

  • Process for producing fluorescent substance and fluorescent substance produced thereby

    WO2011024296A1

  • Phosphor and method for producing the same

    JP2009096882A

  • Phosphor particles, composite, light-emitting device, and method for manufacturing phosphor particles

    JP6667025B1

  • Phosphor powder, composite and light-emitting device

    JP6785333B2