Photosensitive composition for hologram recording, hologram recording medium, polymer, large capacity memory, optical element, ar light guide plate, and ar glasses
The photosensitive composition of monofunctional and polyfunctional photopolymerizable monomers addresses stability and noise issues in hologram recording, achieving high refractive index modulation and transparency for improved hologram recording media in AR glasses and optical materials.
Patent Information
- Application Number
- PCT/JP2024/012676
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Current hologram recording materials face challenges with refractive index modulation stability, noise from phosphor by-products, and limited transparency due to fluorescence and yellowing issues, which affect recording density and storage stability, especially in applications like AR glasses and optical materials.
A photosensitive composition combining a monofunctional and polyfunctional photopolymerizable monomer, represented by specific molecular formulas, which enhances transparency, polymerization ease, chemical stability, and suppresses fluorescence, achieving high refractive index modulation and improved storage stability.
The composition enables high-transparency, low-fluorescence hologram recording media with enhanced diffraction properties and long-term storage stability, suitable for AR glasses and optical components, by improving refractive index modulation and reducing noise and yellowing issues.
Smart Images

Figure JP2024012676_03102024_PF_FP_ABST
Abstract
Description
Photosensitive composition for hologram recording, hologram recording medium, polymer, large-capacity memory, optical element, AR light guide plate, and AR glass
[0001] The present invention relates to a photosensitive composition for hologram recording, which comprises a combination of at least two different photopolymerizable monomers and a photopolymerization initiator, and has high transparency, ease of polymerization, and excellent chemical stability. The present invention also relates to a hologram recording medium, a polymer, an optical material, an optical component, a large-capacity memory, an optical element, an AR light guide plate, and an AR glass, which use the photosensitive composition for hologram recording.
[0002] Large-capacity memories using photopolymerizable holographic materials have been the subject of much research. When holographic recording materials are irradiated with interference fringes resulting from the interference of light, photopolymerization occurs at different rates in bright areas with high light intensity and dark areas with low light intensity, resulting in the formation of a refractive index modulation structure accompanied by the diffusion and migration of materials with different refractive indices. Holographic memories used for the long-term storage of large amounts of data are strongly required to be able to record holograms at a high recording density (S / N) and to have a refractive index modulation structure that is stable over a long period of time (hereinafter referred to as archival property).
[0003] For example, as described in Patent Document 1, photocompositions containing photopolymerization initiators typically form phosphors after exposure and curing. It is known that photopolymerizable hologram recording materials also produce phosphors as by-products of the recording material when a refractive index modulation structure is formed by hologram recording. These phosphors cause noise during hologram recording, resulting in a decrease in recording density (S / N), posing a major technical challenge.
[0004] In recent years, research into using hologram recording materials in Augmented Reality (AR) glasses has been in full swing worldwide. AR glasses, which use optical elements with recorded holograms as light guide plates for image display, are required to be able to display images output from a projector for a long period of time while achieving high color reproducibility and low power consumption. Therefore, there is a strong demand for hologram recording materials that achieve a high refractive index modulation (Δn), reduce optical noise such as fluorescence, and have excellent archival properties. The refractive index modulation (Δn) is widely used as an indicator of the diffraction efficiency and diffraction characteristics of holograms, and it is generally believed that the higher the Δn value, the better the hologram characteristics.
[0005] Patent Document 2 discloses that a hologram composition containing fluorinated urethane as a plasticizer and combining different polymerizable monomers can achieve a high Δn value. However, it is unclear whether a composition that does not contain fluorinated urethane can achieve a large refractive index modulation amount Δn, and the archival stability of Δn and suppression of fluorescence phenomenon are not clearly stated.
[0006] Patent Document 3 describes that a composition containing a copolymer having a monofunctional photopolymerizable monomer characterized by a styrene-type vinyl monomer and a bifunctional monomer as structural units can provide a hologram recording material with high sensitivity and high archival stability. However, polymers obtained from styrene-type vinyl monomers contain benzyl positions that are easily oxidized. For this reason, there are always concerns about the poor weather resistance and coloration, typically yellowing, of optical materials using these polymers.
[0007] Patent Document 4 exemplifies a composition comprising a combination of at least two cationically polymerizable monomers, including a monofunctional photopolymerizable monomer and a polyfunctional photopolymerizable monomer, a photocationic polymerization initiator, a polymerization inhibitor, and a binder resin, as a recording material exhibiting an extremely high Δn value. However, while this composition is a hologram recording composition with excellent diffraction characteristics, the polymerizable monomer used has a dinaphthothiophene structure. Therefore, it is inherently prone to yellowing, and its use in optical materials requiring high transparency in the visible light region is severely limited.
[0008] Japanese Patent No. 4185939 Special Publication No. 2013-510204 International Publication No. 2008 / 123094 International Publication No. 2018 / 043593
[0009] An object of the present invention is to provide a photosensitive composition for hologram recording that is useful as a hologram recording medium, optical material, or optical component, and that has high transparency, easy polymerization, high chemical stability, excellent archival properties, and low fluorescence.
[0010] The present inventors have found that by introducing a specific molecular structure into at least two different photopolymerizable monomers, which are a combination of a monofunctional photopolymerizable monomer and a polyfunctional photopolymerizable monomer, it is possible to achieve high transparency, easy polymerization, and high chemical stability, while improving archival stability and suppressing fluorescence. Specifically, it has been found that a high-performance holographic recording medium can be obtained by using a composition containing at least a monofunctional or polyfunctional photopolymerizable monomer represented by the following formula (1-1) or (1-2):
[0011] The gist of the present invention lies in the following.
[0012] [1] A photosensitive composition for hologram recording, comprising a photopolymerization initiator and at least two different photopolymerizable monomers, which are a combination of a monofunctional photopolymerizable monomer and a polyfunctional photopolymerizable monomer, wherein at least one of the photopolymerizable monomers is a compound selected from the group consisting of a compound represented by the following formula (1-1) and a compound represented by the following formula (1-2):
[0013]
[0014] [In formula (1-1), A 1 represents a photopolymerizable group. 1 represents a single bond or an optionally branched divalent linking group. 1 represents a fused aromatic ring group which may have a substituent. 1 is an integer from 2 to 5, and a plurality of R 1 may be the same or different. 1 The benzene ring having A 1 -L 1 -O, and R1 In addition to the above, it may further have a substituent.]
[0015] [In formula (1-2), A 2 represents a photopolymerizable group. 2 represents a single bond or an optionally branched divalent linking group. 2 represents a fused aromatic ring group which may have a substituent. 2 is an integer of 2 to 4, and a plurality of R 2 may be the same or different. n represents an integer of 2 to 4. When n is 2, X represents a single bond or a divalent group selected from the group consisting of structures represented by the following formulas (1a) to (1g). When n is 3, X represents a trivalent organic group. When n is 4, X represents a carbon atom or a silicon atom. When a plurality of A exists in formula (1-2), 2 , L 2 , R 2 , m 2 may be the same or different. 2 The benzene ring having A 2 -L 2 -O, R 2 and X may further have a substituent.]
[0016]
[0017] [In formula (1a), R 3 and R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.] [2] The photosensitive composition for hologram recording according to [1], wherein n is 2. [3] The m 1 and m 2 [4] The photosensitive composition for hologram recording according to [1] or [2], wherein each of A is 2 or 3. 1 and A 2 [5] The photosensitive composition for hologram recording according to any one of [1] to [3], wherein R is a (meth)acryloyl group or an allyl group. 1 and R 2The photosensitive composition for hologram recording according to any one of [1] to [4], wherein the fused aromatic ring is any one of a naphthalene ring, a phenanthrene ring, a dibenzothiophene ring, and a thianthrene ring. [6] The photosensitive composition for hologram recording according to any one of [1] to [5], wherein at least one of the monofunctional photopolymerizable monomers contains a compound represented by formula (1-1) and at least one of the polyfunctional photopolymerizable monomers contains a compound represented by formula (1-2). [7] A holographic recording medium comprising the photosensitive composition for hologram recording according to any one of [1] to [6]. [8] A polymer obtained by polymerizing the photosensitive composition for hologram recording according to any one of [1] to [6]. [9] An optical material comprising the polymer according to [8].
[10] An optical part comprising the polymer according to [8].
[11] A large-capacity memory comprising the holographic recording medium according to [7].
[12] An optical element obtained by holographic recording in the holographic recording medium according to [7].
[13] An AR light guide plate (wave guide plate) including the optical element according to
[12] .
[14] AR glasses including the optical element according to
[12] .
[0018] The present invention provides a photosensitive composition for hologram recording that is useful as a hologram recording material and has high transparency, high solubility, easy polymerization, low fluorescence, and excellent chemical stability and archival properties. The photosensitive composition for hologram recording of the present invention is particularly useful as a reactive composition used in hard coat layers of optical lenses and optical components, and in hologram recording media. Use of the photosensitive composition for hologram recording of the present invention makes it possible to realize optical materials or optical components that have high light transmittance, high chemical stability, and excellent processability while suppressing the fluorescence phenomenon.
[0019] FIG. 1 is a schematic diagram showing an outline of the configuration of an apparatus used for holographic recording.
[0020] The present invention will be described in detail below with reference to the following embodiments. The present invention is not limited to the following embodiments, and various modifications can be made within the scope of the present invention.
[0021] In the present invention, "(meth)acrylate" is a general term for acrylate and methacrylate. "(meth)acryloyl group" is a general term for acryloyl group and methacryloyl group. The same applies to "(meth)acryloyloxy group" and "(meth)acrylic".
[0022] In the present invention, the term "aromatic ring" is a general term for "aromatic hydrocarbon ring" and "aromatic heterocyclic ring". Similarly, the term "aromatic ring group" is a general term for "aromatic hydrocarbon group" and "aromatic heterocyclic group". In the present invention, the term "optionally has a substituent" means that the group may have one or more substituents.
[0023] 1. Composition of the Present Invention The photosensitive composition for hologram recording of the present invention (hereinafter may be referred to as "the composition of the present invention") is a photosensitive composition comprising a photopolymerization initiator and at least two different photopolymerizable monomers that are a combination of a monofunctional photopolymerizable monomer and a polyfunctional photopolymerizable monomer, wherein at least one of the photopolymerizable monomers is a compound selected from the group consisting of a compound represented by the following formula (1-1) (hereinafter may be referred to as "compound (1-1)") and a compound represented by the following formula (1-2) (hereinafter may be referred to as "compound (1-2)").
[0024]
[0025] [In formula (1-1), A 1 represents a photopolymerizable group. 1 represents a single bond or an optionally branched divalent linking group. 1 represents a fused aromatic ring group which may have a substituent. 1 is an integer from 2 to 5, and a plurality of R 1 may be the same or different. 1 The benzene ring having A 1 -L 1 -O, and R 1 In addition to the above, it may further have a substituent.]
[0026]
[0027] [In formula (1-2), A 2represents a photopolymerizable group. 2 represents a single bond or an optionally branched divalent linking group. 2 represents a fused aromatic ring group which may have a substituent. 2 is an integer of 2 to 4, and a plurality of R 2 may be the same or different. n represents an integer of 2 to 4. When n is 2, X represents a single bond or a divalent group selected from the group consisting of structures represented by the following formulas (1a) to (1g). When n is 3, X represents a trivalent organic group. When n is 4, X represents a carbon atom or a silicon atom. When a plurality of A exists in formula (1-2), 2 , L 2 , R 2 , m 2 may be the same or different. 2 The benzene ring having A 2 -L 2 -O, R 2 and X may further have a substituent.]
[0028]
[0029] [In formula (1a), R 3 and R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0030] The photosensitive composition for hologram recording of the present invention provides a hologram recording medium that is highly transparent, has low fluorescence, and has excellent diffraction properties that can be used stably for a long period of time.
[0031] Hereinafter, compound (1-1) and compound (1-2) will be collectively referred to as "compound (1)."
[0032] 1-1. Photopolymerizable Monomers As described above, the at least two different photopolymerizable monomers contained in the photosensitive composition for hologram recording of the present invention are a monofunctional photopolymerizable monomer and a polyfunctional photopolymerizable monomer. When the composition of the present invention contains two photopolymerizable monomers, the photosensitive composition for hologram recording contains one monofunctional photopolymerizable monomer and one polyfunctional photopolymerizable monomer. When the composition of the present invention contains three or more photopolymerizable monomers, the composition contains one monofunctional photopolymerizable monomer and one polyfunctional photopolymerizable monomer, and the other one or more photopolymerizable monomers may be either monofunctional photopolymerizable monomers or polyfunctional photopolymerizable monomers. However, the photosensitive composition for hologram recording of the present invention always contains compound (1) as a photopolymerizable monomer.
[0033] Among the compounds (1), the compound (1-1) is a monofunctional photopolymerizable monomer, and the compound (1-2) is a polyfunctional photopolymerizable monomer.
[0034] In a first preferred embodiment of the photosensitive composition for hologram recording of the present invention, among the at least two different photopolymerizable monomers obtained by combining a monofunctional photopolymerizable monomer and a polyfunctional photopolymerizable monomer, the polyfunctional photopolymerizable monomer is compound (1). In this case, the shrinkage upon curing tends to be low, which is preferred. In a second preferred embodiment of the photosensitive composition for hologram recording of the present invention, among the at least two different photopolymerizable monomers obtained by combining a monofunctional photopolymerizable monomer and a polyfunctional photopolymerizable monomer, the monofunctional photopolymerizable monomer is compound (1). In this case, the viscosity of the composition tends to be low, which is preferred, and therefore the processability is excellent. In a particularly preferred embodiment of the photosensitive composition for hologram recording of the present invention, among the at least two different photopolymerizable monomers obtained by combining a monofunctional photopolymerizable monomer and a polyfunctional photopolymerizable monomer, both the monofunctional photopolymerizable monomer and the polyfunctional photopolymerizable monomer are compound (1). That is, the monofunctional photopolymerizable monomer is a compound represented by formula (1-1) and the polyfunctional photopolymerizable monomer is a compound represented by formula (1-2). In this case, a high refractive index modulation amount Δn can be realized, which is preferable.
[0035] The content of compound (1) in the composition of the present invention is preferably 1% by mass or more and 99% by mass or less, and more preferably 5% by mass or more and 95% by mass or less, relative to the total solid content of the composition of the present invention. If the content of compound (1) is less than 1% by mass, the effect of using compound (1) is not fully exhibited. If the content of compound (1) exceeds 99% by mass, the curing rate tends to decrease.
[0036] The composition of the present invention may contain a photopolymerizable monomer other than compound (1), as described below. In this case, the total content of compound (1) and the photopolymerizable monomer other than compound (1) is as described below.
[0037] The content ratio of the monofunctional photopolymerizable monomer to the polyfunctional photopolymerizable monomer contained in the composition of the present invention is not particularly limited, but it is preferable that the monofunctional photopolymerizable monomer and the polyfunctional photopolymerizable monomer account for 10 to 99 mol % and 1 to 90 mol %, respectively, relative to the total (100 mol %) of the monofunctional photopolymerizable monomer and the polyfunctional photopolymerizable monomer. It is more preferable that the monofunctional photopolymerizable monomer and the polyfunctional photopolymerizable monomer account for 30 to 97 mol % and 3 to 70 mol %, respectively, and it is even more preferable that the monofunctional photopolymerizable monomer and the polyfunctional photopolymerizable monomer account for 50 to 95 mol % and 5 to 50 mol %. When the content of the monofunctional photopolymerizable monomer is equal to or less than the upper limit of the above range and the content of the polyfunctional photopolymerizable monomer is equal to or greater than the lower limit of the above range, the hologram recording storability is good, which is preferable. When the content of the monofunctional photopolymerizable monomer is equal to or greater than the lower limit of the above range and the content of the polyfunctional photopolymerizable monomer is equal to or less than the upper limit of the above range, the viscosity of the composition is less likely to increase, which is preferable.
[0038] 1-2-1. Structure of Compound (1) Compound (1-1) contains a photopolymerizable group A 1 is a single bond to the oxygen atom or a linking group L 1 and a benzene ring (hereinafter sometimes referred to as a "phenoxy ring" or a "phenoxy skeleton") substituted via a fused aromatic ring group R 1 Similarly, the compound (1-2) is characterized by having a partial structure in which two or more photopolymerizable groups A 2 is a single bond to the oxygen atom or a linking group L 2and a benzene ring (hereinafter sometimes referred to as a "phenoxy ring" or a "phenoxy skeleton") substituted via a fused aromatic ring group R 2 It is characterized by having a partial structure in which two or more of the following are bonded.
[0039] In hologram materials, high-refractive-index polymerizable monomers are often used to improve the refractive index modulation amount Δn, and organic compounds having aromatic ring groups are sometimes used to improve the refractive index. However, organic compounds having highly planar aromatic ring groups generally have poor solubility in various solvents, making them difficult to use as high-concentration solutions that achieve high refractive indexes or high Δn values. Even if a high-concentration solution can be prepared, the high crystallinity of the organic compound poses a problem of prone to precipitation from the storage solution over time. In particular, aromatic organic compounds used in optical materials with a refractive index exceeding 1.65 have multiple aromatic rings as substituents, and their solubility in various solvents tends to decrease as their molecular weight increases.
[0040] Compound (1) contains a large number of fused aromatic ring groups R 1 , R 2 This compound is characterized by having a phenoxy skeleton as a partial structure in which the substituents R are densely connected. This creates a molecular twist between the substituents on the phenoxy skeleton, which can significantly reduce the crystallinity of compound (1). In particular, the compound has a high refractive index due to the condensed aromatic ring group R 1 , R 2 The more the number of substitutions, the higher the refractive index of the compound (1) and the larger the molecular weight, but the symmetry and planarity of the entire molecule also tend to decrease, and high solubility in solvents can be realized. 1 , A 2 In the case of (meth)acryloyl groups, the concentration of (meth)acrylic groups in the monomer is relatively low, which makes it very useful as a hologram recording material with little shrinkage during curing.
[0041] In addition, the linking group L 1 , L 2 The photopolymerizable group A 1 , A 2 The linking group L is attached to an appropriate position away from a high refractive index site with large steric hindrance. 1 , L2 By bonding the compound (1) via the photopolymerizable group A, the flexibility of the compound (1) can be significantly improved. 1 , A 2 This allows the resulting polymer to have a high refractive index and improved chemical stability. 1 , A 2 However, a large number of condensed aromatic ring groups R 1 , R 2 The phenoxy skeleton substituted with a linking group L 1 , L 2 Since the bond is via the photopolymerization initiator, the fluorescence phenomenon caused by the photopolymerization initiator can be suppressed, thereby achieving low fluorescence.
[0042] 1-2-2. Regarding formulas (1-1) and (1-2) L 1 , L 2 represents a single bond or an optionally branched divalent linking group. 1 , L 2 may have an oxygen atom, a sulfur atom, or a nitrogen atom which may have a substituent. 2 There are multiple L 2 may be the same or different.
[0043] L 1 , L 2 As the linking group constituting L, an aliphatic hydrocarbon group which may have a substituent is preferred from the viewpoint of ease of synthesis and availability. The number of carbon atoms in the aliphatic hydrocarbon group (not including the number of carbon atoms in the substituent) is preferably 1 to 8. When the number of carbon atoms in the aliphatic hydrocarbon group is 8 or less, the refractive index of compound (1) is less likely to decrease, and the viscosity is reduced due to the small molecular weight, which tends to improve processability. 1 , L 2 The aliphatic hydrocarbon group constituting the photopolymerizable group A may be either a cyclic aliphatic hydrocarbon group or a chain aliphatic hydrocarbon group, or a combination of these structures. 1 , A 2 From the viewpoint of reducing peripheral steric hindrance, a chain aliphatic hydrocarbon group is preferred.
[0044] L 1 , L 2From the viewpoint of imparting high solubility to various media to compound (1), L is preferably a linking group having an oxygen atom, a sulfur atom, or a nitrogen atom which may have a substituent. These linking groups may have a substituent, and preferably have a carbon number (not including the carbon number of the substituent) of 1 to 8. When the carbon number of the linking group is 8 or less, the refractive index of compound (1) is less likely to decrease, and the viscosity is reduced due to the small molecular weight, which tends to improve processability. 1 , L 2 The linking group constituting the photopolymerizable group A may be either a cyclic linking group or a chain linking group, or these structures may be combined. 1 , A 2 From the viewpoint of reducing peripheral steric hindrance, a chain linking group is preferred.
[0045] L 1 , L 2 The chain linking group having an oxygen atom, a sulfur atom, or a nitrogen atom which may have a substituent, which constitutes the group, is —CH 2 CH 2 OCH 2 CH 2 -, -CH 2 CH 2 OCH 2 CH 2 OCH 2 CH 2 -, -CH 2 CH 2 SCH 2 CH 2 -, -CH 2 CH 2 (CO)-, -CH 2 CH 2 CH 2 (CO)-, -CH 2 CH 2 CH 2 CH 2 (CO)-, -CH 2 CH 2 CH 2 CH 2 CH 2 (CO)-, -CH 2 CH 2 OCH 2 CH 2 (CO)-, -CH 2 CH 2 NH(CO)-, -CH2 CH 2 CH 2 NH(CO)-、-CH 2 CH 2 CH 2 CH 2 NH(CO)-、-CH 2 CH 2 OCH 2 CH 2 NH(A)-、-OCH 2 CH 2 -、-OCH 2 CH 2 OCH 2 CH 2 -、-OCH 2 CH 2 OCH 2 CH 2 OCH 2 CH 2 -、-OCH 2 CH 2 SCH 2 CH 2 -、-OCH 2 CH 2 (CO)-、-OCH 2 CH 2 CH 2 (CO)-、-OCH 2 CH 2 CH 2 CH 2 (CO)-、-OCH 2 CH 2 CH 2 CH 2 CH 2 (CO)-、-OCH 2 CH 2 OCH 2 CH 2 (CO)-、-OCH 2 CH 2 NH(A)-、-OCH 2 CH 2 CH 2 NH(A)-、-OCH 2 CH 2 CH 2 CH 2 NH(A)-、-OCH 2 CH 2 OCH 2 CH 2NH(CO)- and the like.
[0046] L 1 , L 2 From the viewpoint of a high refractive index, it is preferable that L 1 , L 2 The ring contained in the cyclic group constituting L may have a monocyclic structure or a condensed ring structure. 1 , L 2 The number of rings contained in L is preferably 1 to 4, more preferably 1 to 3, and even more preferably 1 or 2. 1 , L 2 The ring contained in L does not necessarily need to be aromatic, but it is preferably an aromatic hydrocarbon ring in order to maintain a high refractive index while keeping the size of the ring in the entire molecule small. 1 , L 2 Examples of the aromatic hydrocarbon ring constituting the formula (I) include a benzene ring, an indene ring, a naphthalene ring, an azulene ring, a fluorene ring, an acenaphthylene ring, an anthracene ring, a phenanthrene ring, and a pyrene ring.
[0047] Linking group L 1 , L 2 may have a substituent. 1 , L 2 Examples of the substituent that may be substituted include a halogen atom (a chlorine atom, a bromine atom, an iodine atom), a hydroxyl group, a mercapto group, an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a phenyl group, a mesityl group, a tolyl group, a naphthyl group, a cyano group, an acetyloxy group, an alkylcarbonyloxy group having 2 to 9 carbon atoms, an alkoxycarbonyl group having 2 to 9 carbon atoms, a sulfamoyl group, an alkylsulfamoyl group having 2 to 9 carbon atoms, an alkylcarbonyl group having 2 to 9 carbon atoms, a phenethyl group, a hydroxyethyl group, an acetylamido group, a dialkylaminoethyl group having an alkyl group having 1 to 4 carbon atoms bonded thereto, a trifluoromethyl group, an alkylthio group having 1 to 8 carbon atoms, an aromatic ring thio group having 6 to 10 carbon atoms, and a nitro group.
[0048] 1-2-3. R in formulas (1-1) and (1-2) 1 , R 2 About R 1 , R 2represents a fused aromatic ring group which may have a substituent. The fused aromatic ring of the fused aromatic ring group is roughly classified into a fused aromatic hydrocarbon ring and a fused aromatic heterocycle.
[0049] Examples of the fused aromatic hydrocarbon ring include a naphthalene ring, a phenanthrene ring, a perylene ring, a tetracene ring, a pyrene ring, a benzpyrene ring, a chrysene ring, a triphenylene ring, an acenaphthene ring, a fluoranthene ring, a fluorene ring, and an anthracene ring.
[0050] R 1 , R 2 From the viewpoint of ease of synthesis and availability, the fused aromatic hydrocarbon ring constituting R is preferably a naphthalene ring, a phenanthrene ring, a pyrene ring, or a fluorene ring. 1 , R 2 The fused aromatic hydrocarbon ring constituting the formula (I) is more preferably a naphthalene ring, a phenanthrene ring, or a fluorene ring.
[0051] R 1 , R 2 As the fused aromatic heterocycle constituting the compound (1), a fused sulfur-containing aromatic heterocycle is preferred because it tends to increase the refractive index of compound (1). The fused sulfur-containing aromatic heterocycle has at least a sulfur atom as a heteroatom constituting the fused aromatic heterocycle. In addition to the sulfur atom, the heteroatom may have an oxygen atom, a nitrogen atom, or both an oxygen atom and a nitrogen atom. From the viewpoints of avoiding coloration and ensuring solubility, the number of heteroatoms constituting the fused sulfur-containing aromatic heterocycle is preferably 1 to 3, more preferably 1 to 2.
[0052] Examples of the fused sulfur-containing aromatic heterocycle include fused aromatic heterocycles containing one sulfur atom, such as a benzothiophene ring, a dibenzothiophene ring, a benzonaphthothiophene ring, a dinaphthothiophene ring, a naphthothiophene ring, a dinaphthothiophene ring, and a dibenzothiopyran ring; fused aromatic heterocycles containing two or more sulfur atoms, such as a thianthrene ring; and fused aromatic heterocycles containing two or more heteroatoms, such as a benzothiazole ring, a naphthothiazole ring, a phenothiazine ring, a thiazoloimidazole ring, a thiazolopyridine ring, a thiazolopyridazine ring, a thiazolopyrimidine ring, a dioxazolopyrazine ring, a thiazolopyrazine ring, a thiazolooxazole ring, a dibenzobenzothiophene ring, a thienoxazole ring, a thienothiadiazole ring, and a thiazolothiadiazole ring.
[0053] The number of rings constituting the fused sulfur-containing aromatic heterocycle is preferably 2 to 8, more preferably 2 to 6, and from the viewpoint of facilitating raw material availability and synthesis, particularly preferably 2 to 5. In particular, from the viewpoints of achieving a high refractive index and low coloration, the fused sulfur-containing aromatic heterocycle is preferably a benzothiazole ring, a dibenzothiophene ring, a benzothiophene ring, a benzonaphthothiophene ring, or a thianthrene ring.
[0054] R 1 , R 2 From the viewpoint of ease of synthesis, the fused aromatic heterocycle constituting the above may be a fused nitrogen-containing aromatic heterocycle. The fused nitrogen-containing aromatic heterocycle has at least a nitrogen atom as a heteroatom constituting the fused aromatic heterocycle. In addition to the nitrogen atom, the heteroatom may have an oxygen atom, a sulfur atom, or both an oxygen atom and a sulfur atom. From the viewpoint of avoiding coloration, the number of heteroatoms constituting the fused nitrogen-containing aromatic heterocycle is preferably 1 to 3, and more preferably 1 to 2.
[0055] Examples of the fused nitrogen-containing aromatic heterocycle include fused aromatic heterocycles containing one nitrogen atom, such as an indole ring, a carbazole ring, a benzocarbazole ring, a dibenzocarbazole ring, a quinoline ring, an isoquinoline ring, a benzoxazole ring, a naphthoxazole ring, a benzothiazole ring, a naphthothiazole ring, a phenoxazine ring, a phenothiazine ring, a thienoxazole ring, a thiazolooxazole ring, an oxazolooxazole ring, a furothiazole ring, a thienothiazole ring, and a thiazolothiazole ring. Rings include fused aromatic heterocycles containing two or more nitrogen atoms, such as a benzimidazole ring, an oxazoloimidazole ring, an oxazolopyridine ring, an oxazolopyridazine ring, an oxazolopyrimidine ring, an oxazolopyrazine ring, a quinolinoxazole ring, a dioxazolopyrazine ring, a thiazoloimidazole ring, a thienothiadiazole ring, a thiazolothiadiazole ring, a thiazolopyridine ring, a thiazolopyridazine ring, a thiazolopyrimidine ring, a thiazolopyrazine ring, and a quinolinothiazole ring.
[0056] The number of rings constituting the fused nitrogen-containing aromatic heterocycle is preferably 2 to 8, more preferably 2 to 6, and from the viewpoint of facilitating raw material availability and synthesis, particularly preferably 2 to 5. In particular, from the viewpoints of achieving a high refractive index and low coloration, the fused nitrogen-containing aromatic heterocycle is preferably a carbazole ring, a benzocarbazole ring, a dibenzocarbazole ring, a quinoline ring, an isoquinoline ring, a benzoxazole ring, a benzothiazole ring, a benzimidazole ring, or a thiadiazole ring, and more preferably a carbazole ring, a benzocarbazole ring, a dibenzocarbazole ring, a benzoxazole ring, a benzothiazole ring, a benzimidazole ring, or a thiadiazole ring.
[0057] R 1 , R 2The fused aromatic heterocycle constituting the compound (1) may be a fused oxygen-containing aromatic heterocycle. The fused oxygen-containing aromatic heterocycle tends to improve the heat resistance and weather resistance of the polymer containing compound (1). The fused oxygen-containing aromatic heterocycle has at least an oxygen atom as a heteroatom constituting the fused aromatic heterocycle. In addition to the oxygen atom, the heteroatom may have a nitrogen atom, a sulfur atom, or both a nitrogen atom and a sulfur atom. From the viewpoint of ensuring heat resistance, the number of oxygen atoms constituting the fused oxygen-containing aromatic heterocycle is preferably 1 to 3, more preferably 1 to 2.
[0058] Examples of the fused oxygen-containing aromatic heterocycle include fused aromatic heterocycles containing one oxygen atom such as a benzofuran ring, a dibenzofuran ring, a naphthofuran ring, a benzonaphthofuran ring, a dinaphthofuran ring, a phenoxazine ring, an oxazole ring, an isoxazole ring, a benzoxazole ring, a benzisoxazole ring, a naphthoxazole ring, a thienoxazole ring, a thiazolooxazole ring, an oxazoloimidazole ring, and a furothiazole ring; and fused aromatic heterocycles containing two or more oxygen atoms such as a dibenzodioxin ring, an oxazolooxazole ring, and a dioxazolopyrazine ring.
[0059] The number of rings constituting the fused oxygen-containing aromatic heterocycle is preferably 2 to 8, more preferably 2 to 6, and from the viewpoint of facilitating raw material availability and synthesis, particularly preferably 2 to 5. In particular, from the viewpoints of achieving a high refractive index and low coloration, the fused oxygen-containing aromatic heterocycle is preferably a dibenzofuran ring, a benzonaphthofuran ring, a dinaphthofuran ring, an oxazole ring, an isoxazole ring, a benzoxazole ring, a benzisoxazole ring, or a naphthoxazole ring, and more preferably a dibenzofuran ring, a benzonaphthofuran ring, a dinaphthofuran ring, or a benzoxazole ring.
[0060] These R 1 , R 2The fused aromatic ring constituting the formula (I) may have a substituent. Examples of the substituent include a halogen atom such as chlorine, bromine, or iodine, an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, an alkynyl group having 2 to 8 carbon atoms, an alkoxyl group, a cyano group, an acetyloxy group, an alkylcarbonyloxy group having 2 to 9 carbon atoms, an alkoxycarbonyl group having 2 to 9 carbon atoms, a sulfamoyl group, an alkylsulfamoyl group having 2 to 9 carbon atoms, an alkylcarbonyl group having 2 to 9 carbon atoms, a phenethyl group, a hydroxyethyl group, an acetylamido group, a dialkylaminoethyl group formed by bonding alkyl groups having 1 to 4 carbon atoms, a trifluoromethyl group, an alkylthio group having 1 to 8 carbon atoms, an aromatic ring thio group having 6 to 10 carbon atoms, and a nitro group. Among these, preferred are alkyl groups having 1 to 8 carbon atoms, alkoxy groups having 1 to 8 carbon atoms, alkylthio groups having 1 to 8 carbon atoms, aromatic ring thio groups having 6 to 10 carbon atoms, cyano groups, acetyloxy groups, alkylcarboxyl groups having 2 to 8 carbon atoms, sulfamoyl groups, alkylsulfamoyl groups having 2 to 9 carbon atoms, and nitro groups.
[0061] These R 1 , R 2 From the viewpoint of increasing the refractive index of compound (1), the fused aromatic ring constituting the compound (1) preferably further has a group containing an aromatic ring as a substituent. 1 , R 2 In addition to the fused aromatic rings constituting R, examples of the aromatic rings include a benzene ring, a furan ring, a thiophene ring, a pyrrole ring, and a pyridine ring. 1 , R 2 The substituent may be directly bonded to the fused aromatic ring constituting R at any position, or may be bonded via an oxygen atom, a sulfur atom, or a nitrogen atom which may have a substituent, or may be bonded via an arbitrary linking group. 1 , R 2 It is more preferable that the aromatic ring contained in the substituent is directly bonded to the fused aromatic ring constituting R. In addition, by making the aromatic ring contained in this substituent a sulfur-containing aromatic heterocycle, the refractive index of compound (1) tends to be higher. The definition of a sulfur-containing aromatic heterocycle is 1 , R 2The sulfur-containing aromatic heterocycle is more preferably a fused sulfur-containing aromatic heterocycle, and particularly preferably a benzothiazole ring, a dibenzothiophene ring, a benzothiophene ring, a benzonaphthothiophene ring, a dinaphthothiophene ring, or a thianthrene ring.
[0062] R 1 , R 2 The number of aromatic rings which the aryl group has as a substituent is not particularly limited, but from the viewpoints of ease of synthesis and solubility, 1 to 4 is preferred, and 1 or 2 is more preferred.
[0063] R 1 , R 2 From the viewpoint of achieving both a high refractive index and high solubility in various media, the fused aromatic ring which may have a substituent constituting R is preferably a naphthalene ring, a fluorene ring, a thianthrene ring, a phenanthrene ring, or a dibenzothiophene ring, more preferably a dibenzothiophene ring or a phenanthrene ring, and among these, a naphthalene ring, a phenanthrene ring, a dibenzothiophene ring, or a thianthrene ring is preferred. 1 , R 2 The fused aromatic rings constituting the formula (I) may have two or more rings selected from the above-mentioned fused aromatic hydrocarbon ring, fused sulfur-containing aromatic heterocycle, fused nitrogen-containing aromatic heterocycle, and fused oxygen-containing aromatic heterocycle.
[0064] R 1 , R 2 As described below, 1 2 to 4 m 2 is 3 to 4, so there are multiple R 1 , R 2 may be the same or different.
[0065] 1-2-4. m in formulas (1-1) and (1-2) 1 , m 2 About m 1 represents an integer of 2 to 5. 2 represents an integer of 2 to 4. 1 , m 2 For example, from the viewpoint of ease of synthesis of compound (1) and ease of availability of raw materials, 1is preferably 2 or 3, and more preferably 3. 2 is preferably 2 or 3.
[0066] In formula (1-2), n is an integer of 2 to 4, and (R 2 ) m2 There are multiple (R 2 ) m2 R 2 and m 2 may be the same or different.
[0067] 1-2-5. Regarding n and X in formula (1-2), n represents an integer of 2 to 4. When n is 2, X represents a single bond or a divalent group selected from the group consisting of structures represented by the following formulas (1a) to (1g). When n is 3, X represents a trivalent organic group. When n is 4, X represents a carbon atom or a silicon atom.
[0068]
[0069] [In formula (1a), R 3 and R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0070] From the viewpoint of ease of synthesis of the compound (1-2) and ease of availability of raw materials, n is preferably an integer of 2 to 3, and more preferably 2.
[0071] When n is 2, X is preferably a single bond, or a divalent oxygen atom or sulfur atom from the viewpoint of increasing the refractive index of the compound (1-2). When X is a single bond, it is more preferable from the viewpoint of the chemical stability of the intermediate compound. Furthermore, from the viewpoints of inhibiting coloration of the compound (1-2), ease of synthesis, and ease of raw material availability, X is preferably a dimethylmethylene group (R 3 , R 4 In particular, X is a methyl group), a phthalidenylene group (the above formula (1d)), and a sulfonyl group (the above formula (1f)) are preferred. When n is 3, from the viewpoint of easy availability of raw materials, X is preferably a methylmethine group or a methine group. When n is 4, from the viewpoint of compound stability, X is preferably a carbon atom.
[0072] 1-2-6. A in formulas (1-1) and (1-2) 1 , A 2 About A 1 , A 2 represents a photopolymerizable group. The photopolymerizable group is a group that is polymerizable by a photopolymerization initiator, and examples thereof include an oxiranyl group, an oxetanyl group, a vinyl group, an allyl group, and a (meth)acryloyl group. Of these, an allyl group and a (meth)acryloyl group are preferred from the viewpoint of ease of synthesis, and a (meth)acryloyl group is particularly preferred from the viewpoint of high reactivity.
[0073] Compound (1-2) contains A 2 There are multiple A 2 may be the same or different.
[0074] 1-2-7. R of the phenoxy ring in compound (1) 1 , R 2 and the substituents other than X The phenoxy ring in compound (1) is 1 The phenoxy ring in compound (2) may have a substituent other than R 2 and may have a substituent other than X.
[0075] Examples of the substituent that the phenoxy ring may have include a halogen atom such as fluorine, chlorine, bromine, or iodine, an alkyl group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, an alkynyl group having 2 to 8 carbon atoms, an alkoxyl group, a cyano group, an acetyloxy group, an alkylcarbonyloxy group having 2 to 9 carbon atoms, an alkoxycarbonyl group having 2 to 9 carbon atoms, a sulfamoyl group, an alkylsulfamoyl group having 2 to 9 carbon atoms, an alkylcarbonyl group having 2 to 9 carbon atoms, a phenethyl group, a hydroxyethyl group, an acetylamido group, a dialkylaminoethyl group formed by bonding alkyl groups having 1 to 4 carbon atoms, a trifluoromethyl group, an alkylthio group having 1 to 8 carbon atoms, an aromatic ring thio group having 6 to 10 carbon atoms, and a nitro group.
[0076] From the viewpoint of ease of synthesis, the phenoxy ring is R 1 Or R 2and X. On the other hand, from the viewpoint of improving the refractive index and solubility, the phenoxy ring preferably has, as a substituent, an alkyl group having 1 to 8 carbon atoms, an alkoxyl group having 1 to 8 carbon atoms, an alkylthio group having 1 to 8 carbon atoms, an aromatic ring thio group having 6 to 10 carbon atoms, a cyano group, an acetyloxy group, an alkylcarboxyl group having 2 to 8 carbon atoms, a sulfamoyl group, an alkylsulfamoyl group having 2 to 9 carbon atoms, or a nitro group.
[0077] 1-2-8. Molecular Weight of Compound (1) From the viewpoint of maintaining a low viscosity of the composition of the present invention and maintaining good processability, the molecular weight of compound (1) is preferably 2,500 or less, more preferably 2,200 or less, and even more preferably 2,000 or less. From the viewpoint of reducing the shrinkage rate during polymerization, the molecular weight of compound (1) is preferably 500 or more, more preferably 600 or more, and even more preferably 700 or more. In particular, the molecular weight of compound (1-1), which is a monofunctional photopolymerizable monomer, is preferably 2,000 or less, more preferably 1,800 or less, and even more preferably 1,500 or less, and is preferably 500 or more, more preferably 600 or more, and even more preferably 700 or more. The molecular weight of compound (1-2), which is a polyfunctional photopolymerizable monomer, is preferably 2,500 or less, more preferably 2,200 or less, and even more preferably 2,000 or less, and is preferably 500 or more, more preferably 600 or more, and even more preferably 700 or more.
[0078] 1-2-9. Relationship between molecular structure and physical properties of compound (1) Compound (1) has a highly planar fused aromatic ring group R 1 , R 2 By bonding two or more of these to the phenoxy skeleton, a phenoxy ring and a fused aromatic ring group R 1 , R 2 In particular, the fused aromatic ring group R 1 , R 2However, in the case of fused aromatic ring groups that have a substituent or ring structure at the ortho position of the linkage to the phenoxy ring, such as 9-naphthalenyl, 9-phenanthrenyl, 1-thianthrenyl, 4-dibenzofuranyl, and 4-dibenzothiophenyl groups, the dihedral angle tends to be larger. This allows for high solubility in various media while suppressing aggregation of the high refractive index structure, making it suitable for use as a polymerizable monomer with an ultra-high refractive index.
[0079] The above molecular twisting is also due to the condensed aromatic ring group R 1 , R 2 This has the effect of suppressing excessive conjugation elongation between the phenoxy ring and the compound (1), thereby suppressing the shift in the absorption wavelength of the compound (1) to longer wavelengths, thereby achieving, for example, the realization of a colorless and transparent optical material in the visible light region and improving the stability of the compound against heating, light irradiation, oxidation, etc.
[0080] Furthermore, in the development of high refractive index materials, it is very important to improve the electron density per volume in the monomer and polymer, that is, to shorten the intermolecular distance in order to improve the refractive index. 1 , R 2 By introducing a linker of an appropriate molecular length into the high refractive index structure of the above, it is thought that the intermolecular distance may be shortened compared to a derivative without a linker due to molecular interactions such as van der Waals forces and hydrogen bonds, which may lead to an even higher refractive index of the same high refractive index structure.
[0081] Furthermore, as mentioned in the background art above, it is known that in photocompositions, as polymerization progresses due to exposure, fluorescent substances derived from the photopolymerization initiator are by-produced. This is thought to be due to the molecular structure introduced into the photopolymerization initiator so that it can be activated by irradiated light, which easily absorbs ultraviolet and visible light. After activation and decomposition due to exposure, the absorption structure of these photopolymerization initiators is mainly incorporated into the polymer terminals, but since molecular motion is extremely slow in a medium where curing has progressed compared to a solution state, overlap between absorption structures due to π-π interactions and the like can be stabilized. As a result, it is generally thought that as polymerization and curing progress, stronger fluorescence phenomena are exhibited. The photopolymerizable group A of compound (1) 1 , A2 As described above, R 1 , R 2 is bonded to the substituted phenoxy skeleton via the linking group L. 1 , A 2 is a fused aromatic ring substituent R 1 , R 2 The photopolymerization initiator activated by exposure and the photopolymerizable group A of the compound (1) are in an environment where the photopolymerization initiator is spatially covered with the photopolymerizable group A of the compound (1). 1 , A 2 When the compound (1) is bonded to the polymer, the absorption structure derived from the photopolymerization initiator incorporated at the polymer end is 1 , R 2 The condensed aromatic rings of the compound (1) tend to shield the absorbing structures, inhibiting the intermolecular interaction between the absorbing structures. This is thought to be why the composition of the present invention containing the compound (1) as a photopolymerizable monomer can suppress the fluorescence phenomenon caused by the photopolymerization initiator.
[0082] In the composition of the present invention, in which monofunctional and polyfunctional photopolymerizable monomers are mixed, the activated photopolymerization initiator forms the photopolymerizable group A under various environments. 1 , A 2 It is thought that the overlap between the absorption structures of the photopolymerization initiators due to π-π interactions and the like is greatly reduced because the photopolymerization initiators can bond with the π-π interactions.
[0083] 1-2-10. Exemplary Compounds of Compound (1) Specific examples of compound (1) are shown below. Compound (1) contained in the photosensitive composition of the present invention is not limited to these examples as long as it does not depart from the gist of the composition. In the following, Et represents an ethyl group.
[0084]
[0085]
[0086]
[0087]
[0088] 1-2-11. Method for synthesizing compound (1) Compound (1) can be synthesized by combining various known methods. For example, compound (1) can be synthesized by reacting a compound represented by the following formula (2) (hereinafter sometimes referred to as "compound (2)") with a compound having a group capable of reacting with a hydroxy group.
[0089]
[0090] [In formula (2), R represents R in formula (1-1) 1 and R in formula (1-2) 2 m corresponds to m in formula (1-1). 1 and m in formula (1-2) 2 When compound (1-1) is produced, na represents 1, and when compound (1-2) is produced, na represents an integer of 2 to 4. When compound (1-1) is produced, Xa represents a hydrogen atom or R 1 In the case of producing compound (1-2), this corresponds to X in formula (1-2). The same applies to the following reaction formulas.]
[0091] An example of the synthesis of compound (1) will be described below.
[0092]
[0093] [In the above reaction formula, L represents L in the formula (1-1) 1 and L in the formula (1-2). 2 A corresponds to A in the formula (1-1). 1 and A in the formula (1-2). 2 Y represents a leaving group such as a halogen atom, a sulfonic acid group such as a methanesulfonic acid group, a tosylic acid group, or a trifluoromethanesulfonic acid group, a carboxyl group, a dimethylpyrazolyl group, or a 1-methylpropylideneaminooxy group. L' and A' represent precursor structures that become L and A, respectively, through chemical reactions. In the following reaction formulas, the same symbols represent the same things.]
[0094] For example, the compound (1) may be a compound represented by the formula (1-1) or (1-2) containing a photopolymerizable group A 1 , A2 is a (meth)acryloyl group. Compound (1A) can be produced by reacting the hydroxyl group of compound (2) with a (meth)acrylate reagent having a polymerizable group represented by formula (i) (hereinafter, may be referred to as (meth)acrylate reagent (i)).
[0095] Examples of the (meth)acrylating reagent (i) include alkylating reagents such as 2-methanesulfonylethyl (meth)acrylate, glycidyl (meth)acrylate, and 2,3-dibromopropyl acrylate.
[0096] Examples of the (meth)acrylating reagent (i) include isocyanates such as 2-acryloyloxyethyl isocyanate, 2-methacryloyloxyethyl isocyanate, 2-(2-methacryloyloxyethyloxy)ethyl isocyanate, and 1,1-(bisacryloyloxymethyl)ethyl isocyanate, and carbonylating reagents such as 2-[(3,5-dimethylpyrazolyl)carbonylamino]ethyl methacrylate and 2-[0-(1'-methylpropylideneamino)carboxyamino]ethyl methacrylate.
[0097] Furthermore, compound (1A) can also be produced by subjecting a compound represented by formula (3) (hereinafter, sometimes referred to as “compound (3)”), which is obtained by reacting compound (2) with a compound having a linking group represented by formula (ii), to a polymerizable group-forming reaction with a (meth)acryloylating reagent represented by formula (iii).
[0098] The reaction of the active hydrogen of the hydroxyl group in formula (2) with the reagents represented by (i) and (ii) and the reaction of compound (3) with the reagent represented by formula (iii) can be carried out by known methods. For example, compound (1A) can be obtained by reacting compound (2) with an isocyanate in the presence of a basic compound.
[0099] The basic compound may be one or more organic basic compounds (triethylamine, diisopropylethylamine, 1,1,3,3-tetramethylguanidine, diazabicycloundecene, diazabicyclononene, pyridine, imidazole, etc.), or one or more inorganic basic compounds (sodium carbonate, potassium carbonate, sodium hydride, potassium hydride, potassium tert-butoxide, etc.), or a combination of one or more organic basic compounds and one or more inorganic basic compounds.
[0100] In the reaction of compound (2) with the reagents represented by formulas (i) and (ii), and in the reaction of compound (3) with the reagent represented by formula (iii), it is preferable to use an organic solvent. Examples of organic solvents include dichloromethane, tetrahydrofuran (THF), dimethoxyethane, toluene, and N,N-dimethylformamide (DMF). One type of organic solvent may be used, or two or more types may be used in combination.
[0101] In the production of compound (1A), it is preferable to purify the reaction product (crude product) obtained in the synthesis reaction. By purifying and removing impurities, low coloration can be achieved. Known methods can be applied as the purification method. For example, purification can be performed by extraction, column chromatography, recrystallization, distillation, etc. These purification methods may be performed alone or in combination.
[0102] When the compound (1A) is a solid at room temperature, it is preferable to use a recrystallization method, since colored substances can be easily removed to a high degree.
[0103] Examples of recrystallization solvents include aliphatic hydrocarbons such as n-pentane, n-hexane, and n-heptane, alicyclic hydrocarbons such as cyclopentane and cyclohexane, aromatic hydrocarbons such as toluene, ethylbenzene, xylene, and mesitylene, halogenated hydrocarbons such as methylene chloride, chloroform, and 1,2-dichloroethane, ethers such as diethyl ether, diisopropyl ether, tetrahydrofuran, t-butyl methyl ether, and 1,4-dioxane, ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, esters such as ethyl acetate, n-butyl acetate, and propylene glycol monomethyl ether acetate, nitriles such as acetonitrile and propionitrile, alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, 2-butanol, t-butanol, 2-methoxyethanol, 2-butoxyethanol, and propylene glycol monomethyl ether, glycols such as ethylene glycol and diethylene glycol, and water. These solvents may be used alone or in combination of two or more.
[0104] Compound (2) and intermediate compound (3), which are raw materials used in the production of compound (1A), can be produced by the following reaction.
[0105]
[0106] [In the above reaction formula, Q represents a leaving group such as a halogen atom or a trifluoromethanesulfonic acid group. R-M represents an organometallic reagent that can react with Q to form a carbon-carbon bond, such as an organolithium reagent, organomagnesium reagent, organozinc reagent, organocerium reagent, organosilicon reagent, organoboron reagent, or organotin reagent, or an aromatic ring compound that directly utilizes a carbon-hydrogen bond to undergo a cross-coupling reaction.]
[0107] For example, compound (2) can be synthesized by simultaneously or sequentially linking multiple fused aromatic ring groups R to a compound represented by formula (5) (hereinafter sometimes referred to as "compound (5)"), which is obtained by reacting compound (4) with a compound having a linking group represented by formula (ii), through a linking reaction with an organic reagent represented by formula (iv).
[0108] 2. Photosensitive Composition for Hologram Recording of the Present Invention The photosensitive composition for hologram recording of the present invention contains a photopolymerization initiator. 1 , A 2 undergoes a polymerization reaction to obtain the polymer of the present invention. The composition of the present invention may contain a photopolymerizable monomer other than compound (1). The composition of the present invention, which is a photosensitive composition for hologram recording, is preferably a photocomposition containing a matrix resin, a radical scavenger, and other additives in addition to the photopolymerizable monomer and photopolymerization initiator. The composition of the present invention used as a material for hologram recording media will be described in detail below.
[0109] 2-1. Photopolymerization initiator The photopolymerization initiator contained in the composition of the present invention may be a photoradical polymerization initiator, a photocationic polymerization initiator, etc. Examples of photopolymerization initiators described below include those generally referred to as polymerization catalysts.
[0110] The content of the photopolymerization initiator in the composition of the present invention is preferably 0.5 μmol / g or more, more preferably 1 μmol / g or more, in terms of molar amount per unit weight of the composition. The content of the photopolymerization initiator in the composition of the present invention is preferably 100 μmol / g or less, more preferably 50 μmol / g or less, in terms of molar amount per unit weight of the composition.
[0111] If the content of the photopolymerization initiator is too low, the amount of radicals generated will be small. This may slow down the photopolymerization rate and reduce the recording sensitivity of the holographic recording medium. If the content of the photopolymerization initiator is too high, the radicals generated by light irradiation may recombine with each other or undergo disproportionation. This may reduce the contribution to photopolymerization and also reduce the recording sensitivity of the holographic recording medium. When two or more photopolymerization initiators are used in combination, it is preferable that the total amount of the initiators satisfy the above range.
[0112] 2-1-1. Photoradical Polymerization Initiator Any known photoradical polymerization initiator can be used as the photoradical polymerization initiator that assists in the polymerization of the composition of the present invention. Examples include azo compounds, azide compounds, organic peroxides, organic borates, bisimidazole derivatives, titanocene compounds, iodonium salts, organic thiol compounds, halogenated hydrocarbon derivatives, acetophenones, benzophenones, hydroxybenzenes, thioxanthones, anthraquinones, ketals, acylphosphine oxides, sulfone compounds, carbamic acid derivatives, sulfonamides, triarylmethanols, and oxime esters. Among these, titanocene compounds, acylphosphine oxide compounds, and oxime ester compounds are preferred as photoradical polymerization initiators because they undergo polymerization reactions with light in the visible range. Benzophenones, acylphosphine oxide compounds, and oxime ester compounds are preferred from the standpoints of compatibility, availability, and the like.
[0113] When a titanocene compound is used as a photoradical polymerization initiator, the type thereof is not particularly limited, and can be appropriately selected from various titanocene compounds described in, for example, JP-A-59-152396 and JP-A-61-151197.
[0114] Specific examples of titanocene compounds include dicyclopentadienyl-Ti-dichloride, dicyclopentadienyl-Ti-bis-phenyl, dicyclopentadienyl-Ti-bis-2,3,4,5,6-pentafluorophenyl-1-yl, dicyclopentadienyl-Ti-bis-2,3,5,6-tetrafluorophenyl-1-yl, dicyclopentadienyl-Ti-bis-2,4,6-trifluorophenyl-1-yl, and dicyclopentadienyl-Ti-bis-2,6-difluorophenyl-1-yl. , dicyclopentadienyl-Ti-bis-2,4-difluorophenyl-1-yl, dimethylcyclopentadienyl-Ti-bis-2,3,4,5,6-pentafluorophenyl-1-yl, dimethylcyclopentadienyl-Ti-bis-2,3,5,6-tetrafluorophenyl-1-yl, dimethylcyclopentadienyl-Ti-bis-2,6-difluorophenyl-1-yl, dicyclopentadienyl-Ti-bis-2,6-difluoro-3-(pyr-1-yl)-phenyl-1-yl, and the like.
[0115] Specific examples of the acylphosphine oxide compound include a monofunctional initiator having only one photocleavage site per molecule, and a bifunctional initiator having two photocleavage sites per molecule.
[0116] Examples of the monofunctional initiator include triphenylphosphine oxide, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and 2,6-dichlorobenzoyldiphenylphosphine oxide.
[0117] Examples of the bifunctional initiator include bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, and bis(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide.
[0118] Specific examples of the oxime ester compound include 1-[4-(phenylthio)-2-(O-benzoyloxime)]-1,2-octanedione, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime)ethanone, 4-(acetoximino)-5-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-5-oxopentanoate, 1-(9-ethyl-6-cyclohexanoyl-9H-carbazol-3-yl)-1-(O-acetyloxime)methyl glutarate, 1-(9-ethyl-9H-carbazol-3-yl)-1-(O-acetyloxime)methyl glutarate, and 1-(9-ethyl-9H-carbazol-3-yl)-1-(O-acetyloxime)-3-methylbutanoic acid.
[0119] Specific examples of preferred photoradical polymerization initiators include benzophenone, 2,4,6-trimethylbenzophenone, methyl orthobenzoylbenzoate, 4-phenylbenzophenone, t-butylanthraquinone, 2-ethylanthraquinone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, oligo{2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone}, benzyl dimethyl ketal, 1-hydroxycyclohexyl phenyl ketone, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-( 4-morpholinophenyl)-butanone-1, diethylthioxanthone, isopropylthioxanthone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropan-1-one and methylbenzoyl formate, 1-[4-(phenylthio)-2-(O-benzoyloxime)]-1,2-octanedione, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime)ethanone, and the like.
[0120] These photoradical polymerization initiators may be used either alone or as a mixture of two or more kinds in any combination and ratio.
[0121] 2-1-2. Photocationic Polymerization Initiator The photocationic polymerization initiator in the present invention is an initiator that generates cationic species by light. The photocationic polymerization initiator is not particularly limited as long as it is a compound that generates cationic species by light irradiation, but onium salts are generally well known.
[0122] Examples of onium salts include diazonium salts of Lewis acids, iodonium salts of Lewis acids, and sulfonium salts of Lewis acids. Specific examples include phenyldiazonium salt of boron tetrafluoride, diphenyliodonium salt of phosphorus hexafluoride, diphenyliodonium salt of antimony hexafluoride, tri-4-methylphenylsulfonium salt of arsenic hexafluoride, and tri-4-methylphenylsulfonium salt of antimony tetrafluoride. Aromatic sulfonium salts are preferably used.
[0123] Specific examples of the photocationic polymerization initiator include S,S,S',S'-tetraphenyl-S,S'-(4,4'-thiodiphenyl)disulfonium bishexafluorophosphate, diphenyl-4-phenylthiophenylsulfonium hexafluorophosphate, diphenyl-4-phenylthiophenylsulfonium hexafluoroantimonate, etc. Examples include UVI-6992 (trade name) manufactured by Dow Chemical, CPI-100P (trade name) manufactured by San-Apro, CPI-101A (trade name) manufactured by San-Apro, CPI-200K (trade name) manufactured by San-Apro, and Omnicat 270 (trade name) manufactured by IGM Resins.
[0124] These cationic photopolymerization initiators may be used either alone or as a mixture of two or more kinds in any combination and ratio.
[0125] The amount of the cationic photopolymerization initiator in the composition of the present invention is preferably 0.02 parts by mass or more and 20 parts by mass or less, more preferably 0.1 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the total of all cationic photopolymerizable compounds in the composition. If the amount of the cationic photopolymerization initiator is less than 0.02 parts by mass, a sufficient reaction does not occur. If the amount of the cationic photopolymerization initiator added exceeds 20 parts by mass, it becomes difficult to achieve both a good pot life and a good polymerization rate.
[0126] When using a cationic photopolymerization initiator, a cationic photopolymerization sensitizer can also be used in combination. A cationic photopolymerization sensitizer is a formulation in which, when the light emitted from a light source used in cationic photopolymerization does not match well with the absorption wavelength of the cationic photopolymerization initiator, the cationic photopolymerization sensitizer is used in combination to efficiently transfer the energy of the irradiated light to the cationic photopolymerization initiator. Known examples of cationic photopolymerization sensitizers include phenolic compounds such as methoxyphenol (Japanese Patent Laid-Open No. 5-230189), thioxanthone compounds (Japanese Patent Laid-Open No. 2000-204284), and dialkoxyanthracene compounds (Japanese Patent Laid-Open No. 2000-119306).
[0127] The cationic photopolymerization sensitizer is usually used in an amount of 0.2 to 5 parts by mass, preferably 0.5 to 1 part by mass, per part by mass of the cationic photopolymerization initiator. If the amount of cationic photopolymerization sensitizer is too small, the sensitization effect may be difficult to achieve. If the amount of cationic photopolymerization sensitizer is too large, the physical properties of the polymer may be reduced.
[0128] 2-2. Photopolymerizable Monomer Other than Compound (1) The composition of the present invention may contain a photopolymerizable monomer other than Compound (1) (hereinafter, may be referred to as a “concomitant monomer”).
[0129] Examples of the co-monomer other than compound (1) include a photocationic polymerizable monomer, a photoradical polymerizable monomer, etc. These co-monomers may be used alone or in any combination and ratio of two or more.
[0130] When only a monofunctional photopolymerizable monomer is used as compound (1), the co-monomer includes a polyfunctional photopolymerizable monomer other than compound (1). The co-monomer is preferably a trifunctional or higher functional monomer, since it can significantly improve the recording storability of holograms. On the other hand, it is preferable to use a bifunctional monomer in combination, since it can suppress the curing shrinkage of the recording material. When only a polyfunctional photopolymerizable monomer is used as compound (1), the composition of the present invention includes a co-monomer of a monofunctional photopolymerizable monomer, since it can improve moldability. When a monofunctional photopolymerizable monomer and a polyfunctional photopolymerizable monomer are used as compound (1), the co-monomer may be either a monofunctional photopolymerizable monomer or a polyfunctional photopolymerizable monomer.
[0131] When the composition of the present invention contains a co-monomer other than compound (1), the content thereof is preferably 0.1 mass% or more and 90 mass% or less, and more preferably 0.3 mass% or more and 80 mass% or less, relative to the total solid content of the composition of the present invention. If the content of the co-monomer is less than 0.1 mass%, the effect of imparting properties by its addition is not fully exhibited. If the content of the co-monomer exceeds 90 mass%, problems such as impairing the effect of compound (1) in suppressing the fluorescence phenomenon tend to occur.
[0132] The content of the photopolymerizable monomer in the composition of the present invention may be any content as long as it does not contradict the gist of the present invention. However, based on the molar amount per unit mass of the composition, the content of all photopolymerizable monomers including compound (1) is preferably 5 μmol / g or more, more preferably 10 μmol / g or more, and even more preferably 100 μmol / g or more. The content of all photopolymerizable monomers is preferably 1000 μmol / g or less, more preferably 800 μmol / g or less, and even more preferably 500 μmol / g or less. When the content of the photopolymerizable monomer is equal to or greater than the above lower limit, sufficient diffraction efficiency can be obtained in the holographic recording medium. When the content of the copolymerizable monomer is equal to or less than the above upper limit, compatibility with the resin matrix in the recording layer is maintained, and shrinkage of the recording layer due to recording tends to be kept low.
[0133] <Photocationically polymerizable monomer> Examples of photocationically polymerizable co-monomers include compounds having an oxirane ring, styrene and its derivatives, vinylnaphthalene and its derivatives, vinyl ethers, N-vinyl compounds, compounds having an oxetane ring, etc. Among these, it is preferable to use at least a compound having an oxetane ring, and it is further preferable to use a compound having an oxirane ring in combination with a compound having an oxetane ring.
[0134] The compound having an oxirane ring may be a prepolymer containing two or more oxirane rings in one molecule. Examples of such prepolymers include alicyclic polyepoxies, polyglycidyl esters of polybasic acids, polyglycidyl ethers of polyhydric alcohols, polyglycidyl ethers of polyoxyalkylene glycols, polyglycidyl ethers of aromatic polyols, hydrogenated compounds of polyglycidyl ethers of aromatic polyols, urethane polyepoxy compounds, and epoxidized polybutadienes.
[0135] Examples of styrene and its derivatives include styrene, p-methylstyrene, p-methoxystyrene, β-methylstyrene, p-methyl-β-methylstyrene, α-methylstyrene, p-methoxy-β-methylstyrene, and divinylbenzene.
[0136] Examples of vinylnaphthalene and its derivatives include 1-vinylnaphthalene, α-methyl-1-vinylnaphthalene, β-methyl-1-vinylnaphthalene, 4-methyl-1-vinylnaphthalene, and 4-methoxy-1-vinylnaphthalene.
[0137] Examples of vinyl ethers include isobutyl ether, ethyl vinyl ether, phenyl vinyl ether, p-methylphenyl vinyl ether, and p-methoxyphenyl vinyl ether.
[0138] Examples of the N-vinyl compound include N-vinylcarbazole, N-vinylpyrrolidone, N-vinylindole, N-vinylpyrrole, and N-vinylphenothiazine.
[0139] Examples of compounds having an oxetane ring include various known oxetane compounds described in JP-A Nos. 2001-220526 and 2001-310937.
[0140] These photocationically polymerizable co-monomers may be used either alone or as a mixture of two or more kinds in any combination and ratio.
[0141] <Photoradically polymerizable monomer> The photoradically polymerizable co-monomer is a compound having one or more ethylenically unsaturated double bonds in one molecule, and examples thereof include (meth)acrylic acid esters, (meth)acrylamides, vinyl esters, and styrenes.
[0142] Examples of (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, (n- or i-)propyl (meth)acrylate, (n-, i-, sec- or t-)butyl (meth)acrylate, amyl (meth)acrylate, adamantyl (meth)acrylate, chloroethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxypentyl (meth)acrylate, cyclohexyl (meth)acrylate, allyl (meth)acrylate, trimethylolpropane mono(meth)acrylate, pentaerythritol mono(meth)acrylate, benzyl (meth)acrylate, methoxybenzyl (meth)acrylate, chlorobenzyl (meth)acrylate, hydroxybenzyl (meth)acrylate, Dimethyl (meth)acrylate, hydroxyphenethyl (meth)acrylate, dihydroxyphenethyl (meth)acrylate, furfuryl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, phenyl (meth)acrylate, hydroxyphenyl (meth)acrylate, chlorophenyl (meth)acrylate, sulfamoylphenyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, 2-(hydroxyphenylcarbonyloxy)ethyl (meth)acrylate, phenol EO-modified (meth)acrylate, phenylphenol EO-modified (meth)acrylate, paracumylphenol EO-modified (meth)acrylate, nonylphenol EO-modified (meth)acrylate, N-acryloyloxyethyl hexahydrophthalimide, bisphenol F EO-modified diacrylate, bisphenol A EO-modified diacrylate, dibromophenyl (meth)acrylate, tribromophenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl acrylate, tricyclodecane dimethylol di(meth)acrylate, bisphenoxyethanol fluorene di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate,Examples include dipentaerythritol hexa(meth)acrylate. Here, "EO" means "ethylene oxide."
[0143] Examples of (meth)acrylamides include (meth)acrylamide, N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-butyl(meth)acrylamide, N-benzyl(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, N-phenyl(meth)acrylamide, N-tolyl(meth)acrylamide, N-(hydroxyphenyl)(meth)acrylamide, N-(sulfamoylphenyl)(meth)acrylamide, N-(phenylsulfonyl)(meth)acrylamide, N-(tolylsulfonyl)(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-methyl-N-phenyl(meth)acrylamide, and N-hydroxyethyl-N-methyl(meth)acrylamide.
[0144] Examples of vinyl esters include vinyl acetate, vinyl butyrate, vinyl benzoate, vinyl benzoate, vinyl t-butylbenzoate, vinyl chlorobenzoate, vinyl 4-ethoxybenzoate, vinyl 4-ethylbenzoate, vinyl 4-methylbenzoate, vinyl 3-methylbenzoate, vinyl 2-methylbenzoate, vinyl 4-phenylbenzoate, and vinyl pivalate.
[0145] Examples of styrenes include styrene, p-acetylstyrene, p-benzoylstyrene, 2-butoxymethylstyrene, 4-butylstyrene, 4-sec-butylstyrene, 4-tert-butylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, dichlorostyrene, 2,4-diisopropylstyrene, dimethylstyrene, p-ethoxystyrene, 2-ethylstyrene, 2-methoxystyrene, 4-methoxystyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, p-methylstyrene, p-phenoxystyrene, p-phenylstyrene, and divinylbenzene.
[0146] These photoradical polymerizable co-monomers may be used either alone or as a mixture of two or more kinds in any combination and ratio.
[0147] Any of the photocationically polymerizable co-monomers and photoradical polymerizable co-monomers exemplified above may be used, or two or more of them may be used in combination. For example, for high refractive index optical lenses and holographic recording media, it is preferable to use a photoradical polymerizable co-monomer as the other photopolymerizable monomer to be used in combination with compound (1) because it is unlikely to inhibit the reaction of forming a resin matrix.
[0148] 2-3. Solvent The composition of the present invention may contain a solvent to adjust the viscosity.
[0149] Specific examples of the solvent may be selected depending on the physical properties of the composition, and include alcohols such as ethanol, propanol, isopropanol, ethylene glycol, and propylene glycol; aliphatic hydrocarbons such as hexane, pentane, and heptane; alicyclic hydrocarbons such as cyclopentane and cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and chloroform; chain ethers such as dimethyl ether and diethyl ether; cyclic ethers such as dioxane and tetrahydrofuran; esters such as methyl acetate, ethyl acetate, butyl acetate, ethyl lactate, and ethyl butyrate; ketones such as acetone, ethyl methyl ketone, methyl isobutyl ketone, and cyclohexanone; Examples of organic solvents include cellosolves such as ethyl cellosolve and butyl cellosolve; carbitols such as methyl carbitol, ethyl carbitol and butyl carbitol; propylene glycol monoalkyl ethers such as propylene glycol monomethyl ether, propylene glycol monoethyl ether and propylene glycol mono-n-butyl ether; glycol ether esters such as ethylene glycol monomethyl ether acetate and propylene glycol monomethyl ether acetate; N,N-dimethylformamide, N,N-dimethylacetamide, etc.), sulfoxides (amides such as dimethyl sulfoxide; nitriles such as acetonitrile and benzonitrile; and N-methylpyrrolidone.
[0150] These solvents can be used alone or in combination. Depending on the polymerization method (emulsion polymerization, suspension polymerization, etc.), water can also be used.
[0151] When a solvent (or dispersion medium) is used, there is no particular limitation on the amount thereof, and it may be adjusted to obtain a composition with a suitable viscosity depending on the polymerization method, processing method, and application.
[0152] 2-4. Matrix Resin The composition of the present invention preferably contains a matrix resin. In particular, the matrix resin constituting the recording layer of the holographic recording medium is an organic substance that does not undergo significant chemical or physical changes upon irradiation with light, and is mainly composed of a polymer of an organic compound.
[0153] Since the matrix resin constitutes the composition of the present invention together with the polymerizable compound described above and the photopolymerization initiator described below, it is strongly required that the matrix resin have excellent compatibility with the polymerizable compound, photopolymerization initiator, etc. Poor compatibility between the matrix resin and the other components described above creates an interface between the materials, causing light to refract or reflect at the interface, resulting in leakage of light to unwanted areas. This can lead to distortion or breakage of interference fringes, resulting in recording in inappropriate areas and resulting in degradation of information. The compatibility between the matrix resin and the other components described above can be evaluated based on the scattered light intensity obtained by placing a detector in a direction different from that of the transmitted light relative to the sample, as described, for example, in Japanese Patent No. 3737306.
[0154] The matrix resin of the composition of the present invention may be a resin that is composed of a plurality of materials that are soluble in a solvent and that are three-dimensionally crosslinked after being formed into a usable state in the composition. Examples of such a resin include thermoplastic resins, thermosetting resins, and photocurable resins, which are described below.
[0155] Three-dimensionally crosslinked resins are solvent-insoluble and are the result of a reaction and curing process between a polymerizable compound that is liquid at room temperature and a compound reactive with the polymerizable compound. The three-dimensionally crosslinked resin acts as a physical barrier, suppressing volumetric changes during recording. That is, after recording, the recording layer tends to expand in bright areas and contract in dark areas, resulting in unevenness on the surface of the holographic recording medium. To suppress this volumetric change, it is more preferable to use a composition containing a three-dimensionally crosslinked resin matrix for the recording layer. Among these, thermosetting resins are preferred as matrix resins in terms of adhesion to the support. Resin materials that can be used as matrix resins are described in detail below.
[0156] 2-4-1. Thermoplastic Resin Specific examples of thermoplastic resin materials include chlorinated polyethylene, polymethyl methacrylate resin (PMMA), copolymers of methyl methacrylate and other alkyl acrylate esters, copolymers of vinyl chloride and acrylonitrile, polyvinyl acetate resin (PVAC), polyvinyl alcohol, polyvinyl formal, polyvinylpyrrolidone, cellulose resins such as ethyl cellulose and nitrocellulose, polystyrene resins, polycarbonate resins, etc. These may be used alone or in combination of two or more.
[0157] There are no particular restrictions on the solvent for these thermoplastic resins as long as it dissolves them. Examples of the solvent include ketones such as acetone and methyl ethyl ketone, esters such as butyl acetate and propylene glycol methyl ether acetate, aromatic hydrocarbons such as toluene and xylene, ethers such as tetrahydrofuran and 1,2-dimethoxyethane, and amides such as N,N-dimethylacetamide and N-methylpyrrolidone. These may be used alone or in combination of two or more.
[0158] 2-4-2. Thermosetting Resin When using a thermosetting resin as the matrix resin, the curing temperature varies depending on the type of crosslinking agent and catalyst.
[0159] Typical examples of functional group combinations that cure at room temperature include epoxy and amine, epoxy and thiol, and isocyanate and amine. Typical examples of combinations that use a catalyst include epoxy and phenol, epoxy and acid anhydride, and isocyanate and polyol.
[0160] The former is simple because it reacts immediately upon mixing, but when molding, such as in holographic recording media, adjustments are difficult due to the limited time available. The latter allows for flexible control of the curing temperature and curing time by appropriately selecting the type and amount of catalyst used, making it suitable for curing while molding, such as in holographic recording media. A wide variety of resin raw materials, from low molecular weight to high molecular weight, are commercially available, so they can be selected while maintaining compatibility with polymerizable reactive compounds and photoinitiators, adhesion to the substrate, and other properties. Each raw material is explained below. Each raw material may be used alone or in combination of two or more types.
[0161] <Epoxy> Examples of the epoxy include polyglycidyl ether compounds of polyols such as (poly)ethylene glycol, (poly)propylene glycol, (poly)tetramethylene glycol, trimethylolpropane, and glycerin; alicyclic epoxy compounds having a cyclic aliphatic group with a 4- to 7-membered ring such as 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate and 3,4-epoxy-1-methylcyclohexyl-3,4-epoxy-1-methylhexanecarboxylate; bisphenol A type epoxy compounds, hydrogenated bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, and phenol or cresol novolac type epoxy compounds.
[0162] The epoxy preferably has two or more epoxy groups in one molecule, but the type is not particularly limited. If the number of epoxy groups is small, the hardness required for the matrix may not be obtained. There is no particular upper limit on the number of epoxy groups in one molecule, but it is usually 8 or less, and preferably 4 or less. If the number of epoxy groups is too large, it may take a long time to consume the epoxy groups, and the formation of the matrix resin may take too long.
[0163] <Amine> The amine may be one containing a primary amino group or a secondary amino group. Examples of such amines include aliphatic polyamines such as ethylenediamine, diethylenetriamine, and derivatives thereof, alicyclic polyamines such as isophoronediamine, menthanediamine, N-aminoethylpiperazine, and derivatives thereof, aromatic polyamines such as m-xylylenediamine, diaminodiphenylmethane, and derivatives thereof, polyamides such as condensates of dicarboxylic acids such as dimer acid with the above-mentioned polyamines, imidazole compounds such as 2-methylimidazole and derivatives thereof, and other compounds such as dicyandiamide and adipic dihydrazide.
[0164] <Thiol> Examples of thiols include thiol compounds such as dithiols such as 1,3-butanedithiol, 1,4-butanedithiol, 2,3-butanedithiol, 1,2-benzeneedithiol, 1,3-benzeneedithiol, 1,4-benzeneedithiol, 1,10-decanedithiol, 1,2-ethaneedithiol, 1,6-hexaneedithiol, and 1,9-nonanedithiol, and polythiols such as Thiokol (manufactured by Toray Fine Chemicals Co., Ltd.) and jER Cure QX40 (manufactured by Mitsubishi Chemical Corporation). Of these, commercially available fast-curing polythiols such as jER Cure QX40 are preferably used.
[0165] <Phenol> Examples of phenol include bisphenol A, novolac-type phenolic resins, and resol-type phenolic resins.
[0166] <Acid Anhydride> Examples of the acid anhydride include monofunctional acid anhydrides such as phthalic anhydride, tetrahydrophthalic anhydride and derivatives thereof, and difunctional acid anhydrides such as pyromellitic anhydride, benzophenonetetracarboxylic anhydride and derivatives thereof.
[0167] <Amount of amine, thiol, phenol, or acid anhydride used> The amount of amine, thiol, phenol, or acid anhydride used is, in terms of the ratio to the number of moles of epoxy groups, usually 0.1 equivalents or more, preferably 0.7 equivalents or more, and usually 2.0 equivalents or less, preferably 1.5 equivalents or less. If the amount of amine, thiol, phenol, or acid anhydride used is too small or too large, the number of unreacted functional groups will be large, and storage stability may be impaired.
[0168] <Polymerization Initiator for Thermosetting Resin> As a catalyst for curing a thermosetting resin, an anionic polymerization initiator or a cationic polymerization initiator can be used depending on the curing temperature and curing time.
[0169] Anionic polymerization initiators generate anions upon exposure to heat or active energy rays. Examples include amines. Examples of amines include amino group-containing compounds such as dimethylbenzylamine, dimethylaminomethylphenol, and 1,8-diazabicyclo[5.4.0]undecene-7, and derivatives thereof; imidazole compounds such as imidazole, 2-methylimidazole, and 2-ethyl-4-methylimidazole, and derivatives thereof. These can be used alone or in combination depending on the curing temperature and curing time.
[0170] The cationic polymerization initiator generates cations when exposed to heat or active energy rays. Examples include aromatic onium salts. Specific examples include SbF 6 -, BF 4 -, AsF 6 -, PF 6 -, CF 3 SO 3 -, B (C 6 F 5 ) 4 Examples of suitable compounds include compounds comprising an anion component such as - and an aromatic cation component containing an atom such as iodine, sulfur, nitrogen, or phosphorus. Among these, diaryliodonium salts and triarylsulfonium salts are preferred. These can be used alone or in combination depending on the curing temperature and curing time.
[0171] The amount of these thermosetting resin polymerization initiators used is usually 0.001% by mass or more, preferably 0.01% by mass or more, and usually 50% by mass or less, preferably 10% by mass or less, based on the matrix resin. If the amount of these thermosetting resin polymerization initiators used is too small, the concentration of the thermosetting resin polymerization initiator will be too low. As a result, the polymerization reaction may take too long. On the other hand, if the amount of thermosetting resin polymerization initiator used is too large, the polymerization reaction may not undergo a continuous ring-opening reaction.
[0172] <Isocyanate> The isocyanate is preferably one having two or more isocyanate groups per molecule, but the type is not particularly limited. If the number of isocyanate groups per molecule is small, the hardness required for a matrix resin may not be obtained. The upper limit of the number of isocyanate groups per molecule is not particularly limited, but is usually 8 or less, and preferably 4 or less. If the number of isocyanate groups per molecule is too large, it may take a long time to consume the isocyanate groups, and the formation of the matrix resin may take too long. The upper limit of the number of isocyanate groups per molecule is not particularly limited, but is usually about 20 or less.
[0173] Examples of isocyanates include aliphatic isocyanates such as hexamethylene diisocyanate, lysine methyl ester diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate; alicyclic isocyanates such as isophorone diisocyanate and 4,4'-methylenebis(cyclohexyl isocyanate); aromatic isocyanates such as tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate, and naphthalene-1,5'-diisocyanate; and oligomers thereof, of which 3 to 7 monomers are preferred.
[0174] Other examples include reaction products of the above-mentioned isocyanates with water, polyhydric alcohols such as trimethylolethane and trimethylolpropane, and polymers of hexamethylene diisocyanate or derivatives thereof.
[0175] The molecular weight of the isocyanate is preferably 100 to 50,000 in number average molecular weight, more preferably 150 to 10,000, and even more preferably 150 to 5,000. If the number average molecular weight is too small, the crosslinking density increases, which can lead to an excessively high hardness of the matrix resin and a decrease in recording speed. If the number average molecular weight is too large, the compatibility with other components decreases or the crosslinking density decreases, which can lead to an excessively low hardness of the matrix resin and the loss of recorded content.
[0176] <Polyol> Examples of polyols include polypropylene polyol, polycaprolactone polyol, polyester polyol, and polycarbonate polyol.
[0177] (Polypropylene Polyol) Polypropylene polyol is obtained by reacting propylene oxide with a diol or a polyhydric alcohol. Examples of diols or polyhydric alcohols include ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, decamethylene glycol, polyethylene glycol, and polytetramethylene glycol. Commercially available polypropylene polyols include Sannix GP-400 and GP-1000 (all manufactured by Sanyo Chemical Industries, Ltd., trade names), and Adeka Polyether G400, G700, and G1500 (all manufactured by ADEKA Corporation, trade names).
[0178] (Polycaprolactone polyol) Polycaprolactone polyol is obtained by reacting a lactone with a diol or a polyhydric alcohol. Examples of lactones include α-caprolactone, β-caprolactone, γ-caprolactone, ε-caprolactone, α-methyl-ε-caprolactone, and β-methyl-ε-caprolactone.
[0179] Examples of diols or polyhydric alcohols include ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, decamethylene glycol, polyethylene glycol, and polytetramethylene glycol.
[0180] Commercially available polycaprolactone polyols obtained by the reaction of ε-caprolactone include PLACCEL 205, PLACCEL 205H, PLACCEL 205U, Examples of such products include PLACCEL 205UT, PLACCEL 210, PLACCEL 210N, PLACCEL 210CP, PLACCEL 220, PLACCEL 230, PLACCEL 230N, PLACCEL 240, PLACCEL 220EB, PLACCEL 220EC, PLACCEL 303, PLACCEL 305, PLACCEL 308, PLACCEL 309, PLACCEL 312, PLACCEL 320, PLACCEL 401, PLACCEL L205AL, PLACCEL L212AL, PLACCEL L220AL, PLACCEL L320AL, PLACCEL T2103, PLACCEL T2205, PLACCEL P3403, and PLACCEL 410 (all of which are trade names manufactured by Daicel Corporation).
[0181] (Polyester Polyol) Examples of polyester polyols include those obtained by polycondensing a dicarboxylic acid or an anhydride thereof with a polyol.
[0182] Examples of dicarboxylic acids include succinic acid, adipic acid, sebacic acid, azelaic acid, dimer acid, maleic anhydride, isophthalic acid, terephthalic acid, and trimellitic acid.
[0183] Examples of polyols include ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, decamethylene glycol, polyethylene glycol, and polytetramethylene glycol.
[0184] Examples of polyester polyols include polyethylene adipate, polybutylene adipate, polyhexamethylene adipate, etc. Commercially available polyester polyols include the ADEKA New Ace F series, ADEKA New Ace Y series, and ADEKA New Ace NS series (trade names, manufactured by ADEKA Corporation), and Kuraray Polyol N-2010, P-4011, and P-1020 (trade names, all manufactured by Kuraray Co., Ltd.).
[0185] (Polycarbonate Polyol) Examples of polycarbonate polyols include those obtained by a dealcoholization condensation reaction between glycols and dialkyl carbonates (e.g., dimethyl carbonate, diethyl carbonate, etc.), those obtained by a dephenolation condensation reaction between glycols and diphenyl carbonates, and those obtained by a glycol removal condensation reaction between glycols and carbonates (e.g., ethylene carbonate, diethyl carbonate, etc.).
[0186] Examples of glycols include aliphatic diols such as 1,6-hexanediol, diethylene glycol, propylene glycol, 1,4-butanediol, 3-methyl-1,5 pentanediol, and neopentyl glycol, and alicyclic diols such as 1,4-cyclohexanediol and 1,4-cyclohexanedimethanol.
[0187] Examples of polycarbonate polyols include poly(hexamethylene carbonate) polyol obtained by the condensation reaction of 1,6-hexanediol and diethyl carbonate, poly(pentylene carbonate) obtained by the condensation reaction of pentanediol and diethyl carbonate, and poly(butylene carbonate) obtained by the condensation reaction of 1,4-butanediol and diethyl carbonate.
[0188] Commercially available polycarbonate polyols include Placcel CD CD205, Placcel CD CD210, Placcel CD CD220 (all trade names manufactured by Daicel Corporation), Duranol T5651, Duranol T5652, Duranol T5650J (all trade names manufactured by Asahi Kasei Corporation), and the like.
[0189] (Molecular Weight of Polyol) The molecular weight of the polyol described above is preferably 100 to 50,000 in number average molecular weight, more preferably 150 to 10,000, and even more preferably 150 to 5,000. If the number average molecular weight is too small, the crosslinking density increases, which may cause the matrix resin to have too high hardness, resulting in a decrease in recording speed. If the number average molecular weight is too large, the compatibility with other components may decrease or the crosslinking density may decrease, which may cause the matrix resin to have too low hardness, resulting in the erasure of recorded content.
[0190] <Other Components> The matrix resin in the present embodiment may contain other components in addition to the above-described components, as long as it does not go against the spirit of the present invention.
[0191] Examples of such other components include compounds having a hydroxyl group, such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, decamethylene glycol, trimethylolpropane, polyethylene glycol, and polytetramethylene glycol, which are used for the purpose of changing the physical properties of the matrix resin.
[0192] <Urethane Polymerization Catalyst> A suitable urethane polymerization catalyst may be included to promote the reaction between the isocyanate and the polyol.
[0193] Examples of urethane polymerization catalysts include onium salts such as bis(4-t-butylphenyl)iodonium perfluoro-1-butanesulfonate, bis(4-t-butylphenyl)iodonium p-toluenesulfonate, bis(4-t-butylphenyl)iodonium trifluoromethanesulfonate, (4-bromophenyl)diphenylsulfonium triflate, (4-t-butylphenyl)diphenylsulfonium trifluoromethanesulfonate, diphenyliodonium perfluoro-1-butanesulfonate, (4-fluorophenyl)diphenylsulfonium trifluoromethanesulfonate, diphenyl-4-methylphenylsulfonium trifluoromethanesulfonate, triphenylsulfonium trifluoromethanesulfonate, and bis(alkylphenyl)iodonium hexafluorophosphonic acid; zinc chloride, tin chloride, iron chloride, aluminum chloride, and BF 3protonic acids such as hydrochloric acid and phosphoric acid; amines such as trimethylamine, triethylamine, triethylenediamine, dimethylbenzylamine, and diazabicycloundecene; imidazoles such as 2-methylimidazole, 2-ethyl-4-methylimidazole, and 1-cyanoethyl-2-undecylimidazolylium trimellitate; bases such as sodium hydroxide, potassium hydroxide, and potassium carbonate; tin catalysts such as dibutyltin laurate, dioctyltin laurate, and dibutyltin octoate; bismuth catalysts such as tris(2-ethylhexanoate)bismuth and tribenzoyloxybismuth; and zirconium catalysts such as tetrakis(ethylacetoacetate)zirconium, 1,1'-isopropylidene zirconocene dichloride, and tetrakis(2,4-pentanedionato)zirconium.
[0194] Among these, bismuth catalysts and zirconium catalysts are preferred for improving storage stability.
[0195] The bismuth catalyst is not particularly limited as long as it is a catalyst containing bismuth element and is a compound that promotes the reaction between isocyanate and polyol. Examples of the bismuth catalyst include tris(2-ethylhexanoate)bismuth, tribenzoyloxybismuth, bismuth triacetate, tris(dimethyldicarbamate)bismuth, bismuth hydroxide, triphenylbismuth(V) bis(trichloroacetate), tris(4-methylphenyl)oxobismuth(V), and triphenylbis(3-chlorobenzoyloxy)bismuth(V).
[0196] Among these, trivalent bismuth compounds are preferred from the viewpoint of catalytic activity, and bismuth carboxylate, a compound represented by the general formula Bi(OCOR) 3 (R is a linear or branched alkyl group, a cycloalkyl group, or a substituted or unsubstituted aromatic group) is more preferred. The above bismuth catalysts may be used alone or in any combination and ratio of two or more.
[0197] The zirconium catalyst is not particularly limited as long as it is a catalyst containing zirconium element and is a compound that promotes the reaction of isocyanate and polyol. Examples thereof include cyclopentadienyl zirconium trichloride, decamethyl zirconocene dichloride, 1,1'-dibutyl zirconocene dichloride, 1,1'-isopropylidene zirconocene dichloride, tetrakis(2,4-pentanedionato)zirconium, tetrakis(trifluoro-2,4-pentanedionato)zirconium, tetrakis(hexafluoro-2,4-pentanedionato)zirconium, zirconium butoxide, zirconium Examples of the zirconium oxide include barium zirconium oxide, calcium zirconium oxide, zirconium bromide, zirconium chloride, zirconium fluoride, zirconium dichloride (indenyl) and zirconium carbonate.
[0198] Among these, compounds having an organic ligand are preferred in terms of compatibility with other components, and are more preferred than compounds having an alkoxide or acetylacetonate (2,4-pentanedionato) structure. Any one of the above zirconium compounds may be used alone, or two or more may be used in any combination and ratio.
[0199] The bismuth-based catalyst and the zirconium-based catalyst may be used alone or in combination.
[0200] The amount of the urethane polymerization catalyst used is, in terms of the ratio to the matrix resin, usually 0.0001% by mass or more, preferably 0.001% by mass or more, and usually 10% by mass or less, preferably 5% by mass or less. If the amount of the urethane polymerization catalyst used is too small, curing may take too long. If the amount of the urethane polymerization catalyst used is too large, it may be difficult to control the curing reaction.
[0201] Although the composition can be cured at room temperature by using a urethane polymerization catalyst, it may also be cured at elevated temperatures, preferably between 40°C and 90°C.
[0202] 2-4-3. Photocurable resins When using photocurable resins as the matrix resin, they must be cured using a photoinitiator for the matrix resin that is appropriate for the wavelength used. Since curing during light irradiation can cause problems with molding and adhesion, it is desirable for the curing reaction to be stable around room temperature, which is the temperature at which the resin is primarily worked. Given this, catalytic curing using a photoinitiator for the matrix resin is the preferred choice.
[0203] Generally, when a matrix resin photoinitiator is irradiated with light, it generates either a cationic or anionic active substrate. Therefore, it is considered best to select a material that undergoes curing with these active substrates and then cure it to form a matrix resin.
[0204] Examples of functional groups that react with cations such as protons include epoxy groups and oxetanyl groups. Specific examples of compounds containing these include polyglycidyl ether compounds of polyols such as (poly)ethylene glycol, (poly)propylene glycol, (poly)tetramethylene glycol, trimethylolpropane, and glycerin, which have an epoxy group; alicyclic epoxy compounds having a 4- to 7-membered cyclic aliphatic group such as 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate and 3,4-epoxy-1-methylcyclohexyl-3,4-epoxy-1-methylhexanecarboxylate; bisphenol A epoxy compounds, hydrogenated bisphenol A epoxy compounds, bisphenol F epoxy compounds, and phenol or cresol novolac epoxy compounds. Examples of compounds containing an oxetanyl group include 2-ethyl-2-oxetanyl ether of bisphenol A and 1,6-bis(2-ethyl-2-oxetanyloxy)hexane. (Note that the term "(poly)ethylene glycol" refers to both "ethylene glycol" and its polymer, "polyethylene glycol.")
[0205] Examples of functional groups that react with anions include epoxy groups and episulfide groups. Specific examples of compounds having an episulfide group include phenyl episulfide and diepisulfide methyl ether of bisphenol A.
[0206] The amount of the matrix resin photoinitiator used when photocuring the matrix resin described above is typically 0.01% by mass or more, preferably 0.1% by mass or more, and typically 1% by mass or less, preferably 0.5% by mass or less, relative to the polymerizable compound. If the amount of matrix resin photoinitiator used is too small, curing may take too long. If the amount of matrix resin photoinitiator used is too large, it may be difficult to control the curing reaction.
[0207] In particular, when used as a hologram recording material, light is also irradiated during recording, so it is important that the wavelength during curing is different from the wavelength during recording. The wavelength difference is at least 10 nm, preferably 30 nm. The selection of a photoinitiator for the matrix resin can generally be predicted from the absorption wavelength of the initiator.
[0208] 2-4-4. Matrix Resin Content The matrix resin content in the composition of the present invention may be any content as long as it does not deviate from the spirit of the present invention. For example, when an isocyanate and a polyol are used as the matrix resin, the total content thereof is usually 0.1% by mass or more, preferably 10% by mass or more, more preferably 35% by mass or more, and usually 99.9% by mass or less, preferably 99% by mass or less. By setting this content to be equal to or greater than the above-mentioned lower limit, it becomes easier to form a recording layer.
[0209] In this case, the ratio of the number of isocyanate-reactive functional groups in the polyol to the number of isocyanate groups in the isocyanate is preferably 0.1 or more, more preferably 0.5 or more, and usually 10.0 or less, preferably 2.0 or less. When this ratio is within the above range, there are fewer unreacted functional groups, and storage stability is improved.
[0210] In the composition of the present invention, the content of the urethane polymerization catalyst is preferably determined in consideration of the reaction rate of the isocyanate and the polyol, and is preferably 5% by mass or less, more preferably 4% by mass or less, even more preferably 1% by mass or less, and is preferably 0.003% by mass or more.
[0211] 2-5. Radical Scavenger In hologram recording, a radical scavenger may be added to accurately fix the interference light intensity pattern as a polymer distribution in the hologram recording medium. The radical scavenger preferably has both a functional group that captures radicals and a reactive group that is covalently fixed to the matrix resin. An example of a functional group that captures radicals is a stable nitroxyl radical group.
[0212] 2-5-1. Types of Radical Scavenger Reactive groups that can be covalently bonded to a matrix resin include hydroxyl groups, amino groups, isocyanate groups, and thiol groups. Examples of such radical scavengers include 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl free radical (TEMPOL), 3-hydroxy-9-azabicyclo[3.3.1]nonane N-oxyl, 3-hydroxy-8-azabicyclo[3.2.1]octane N-oxyl, and 5-HO-AZADO: 5-hydroxy-2-azatricyclo[3.3.1.1]octane N-oxyl. 3,7 ] decane N-oxyl.
[0213] 2-5-2. Content of Radical Scavenger Any one of the above-mentioned various radical scavengers may be used alone, or two or more may be used in any combination and ratio. The content of the radical scavenger in the composition of the present invention, in terms of molar amount per unit weight of the composition, is preferably 0.5 μmol / g or more, more preferably 1 μmol / g or more, and is preferably 100 μmol / g or less, more preferably 50 μmol / g or less.
[0214] If the content of the radical scavenger is too low, the radical scavenging efficiency will be low, and the polymer with a low degree of polymerization will diffuse, tending to result in an increase in components that do not contribute to signals. If the content of the radical scavenger is too high, the polymerization efficiency of the polymer will be reduced, tending to make it impossible to record signals. When two or more radical scavengers are used in combination, it is preferable that the total amount thereof satisfies the above range.
[0215] 2-6. Other Components The composition of the present invention may contain other components in addition to the components described above, provided that the other components do not deviate from the spirit of the present invention.
[0216] Other components include plasticizers, dispersants, leveling agents, antifoaming agents, adhesion promoters, any organic or inorganic fillers, diffusing agents, wavelength converting materials such as pigments, and for controlling the recording reaction, chain transfer agents, polymerization terminators (polymerization inhibitors), compatibilizers, reaction aids, sensitizers, etc. Examples of additives that may be required to improve other properties include preservatives, stabilizers, antioxidants, UV absorbers, light stabilizers, etc. These components may be used alone or in any combination and ratio of two or more.
[0217] <Antioxidant and Light Stabilizer> The composition of the present invention preferably contains an antioxidant and a light stabilizer in order to improve the heat yellowing resistance and weather resistance of the resulting polymer.
[0218] Specific examples of the antioxidant include phenolic antioxidants such as 2,6-di-t-butylphenol, 2,6-di-t-butyl-p-cresol, n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, triethylene glycol bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]; and triphenyl phosphite, trisisodecyl phosphite, isodecyl diphenyl phosphite, 2-ethylhexyl diphenyl phosphite, Examples of phosphorus-based antioxidants include tetra(C12-C15 alkyl)-4,4'-isopropylidene diphenyl diphosphite, tris(nonylphenyl)phosphite, tristridecyl phosphite, 2,4,8,10-tetra-tert-butyl-6-[(2-ethylhexan-1-yl)oxy]-12H-dibenzo[d,g][1,3,2]dioxaphosphocin, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 3,9-dioctadecan-1-yl-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, and tris(2,4-di-t-butylphenyl)phosphite. These can be used alone or in combination of two or more.
[0219] As the antioxidant, it is preferable to use a phenolic antioxidant in combination with a phosphorus-based antioxidant. A preferred combination of a phenolic antioxidant and a phosphorus-based antioxidant is a combination of at least one selected from tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane and n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate as the phenolic antioxidant and tris(2,4-di-t-butylphenyl)phosphite as the phosphorus-based antioxidant.
[0220] The content of the antioxidant in the composition of the present invention is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and even more preferably 0.1 to 2 parts by mass, per 100 parts by mass of the total amount of the composition, in order to improve the heat yellowing resistance of the resulting polymer.
[0221] As the light stabilizer, a hindered amine light stabilizer (HALS) is preferably used. Specific examples of HALS include 2,2,6,6-tetramethyl-4-piperidinyl stearate, 2,2,6,6-tetramethyl-4-piperidyl methacrylate, 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, bis(2,2,6,6-tetramethyl-1-undecyloxypiperidin-4-yl)carbonate, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate, and ADK STAB L. A-68 (manufactured by ADEKA Corporation), Adekastab LA-63P (manufactured by ADEKA Corporation), butane-1,2,3,4-tetracarboxylic acid tetrakis(1,2,2,6,6-pentamethyl-4-piperidinyl), 1,2,3,4-butanetetracarboxylic acid tetrakis(2,2,6,6-tetramethyl-4-piperidinyl), TINUVIN 111FDL, TINUVIN 123, TINUVIN 144, TINUVIN 152, TINUVIN 249, TINUVIN 292, TINUVIN 5100 (all manufactured by BASF), and the like. These may be used alone or in combination of two or more.
[0222] The content of the light stabilizer in the composition of the present invention is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and even more preferably 0.1 to 2 parts by mass, per 100 parts by mass of the total amount of the composition, in terms of improving the heat yellowing resistance and weather resistance of the resulting polymer.
[0223] The antioxidants and light stabilizers may be used either alone or in combination of two or more thereof.
[0224] <Sensitizer> A compound that controls the excitation of the photopolymerization initiator can be added to the composition of the present invention. Examples of such compounds include a sensitizer and a sensitization aid.
[0225] The sensitizer can be selected from various known sensitizers. Generally, colored compounds such as dyes are often used as sensitizers to absorb visible and ultraviolet laser light. When used in holographic recording media, the sensitizers vary depending on the wavelength of the laser light used for recording and the type of initiator used. In systems using green lasers, specific examples of preferred sensitizers include those described in JP-A-5-241338, JP-A-2-69, JP-B-2-55446, etc. In systems using blue lasers, specific examples of preferred sensitizers include those described in JP-A-2000-10277, JP-A-2004-198446, etc. These sensitizers may be used alone or in any combination and ratio of two or more.
[0226] When the resulting holographic recording medium is required to be colorless and transparent, it is preferable to use a cyanine dye as a sensitizer. Cyanine dyes are generally easily decomposed by light, so post-exposure is performed. That is, by leaving the holographic recording medium under room light or sunlight for several hours to several days, the cyanine dye in the holographic recording medium is decomposed and no longer absorbs in the visible range, resulting in a colorless and transparent holographic recording medium.
[0227] The amount of sensitizer needs to be increased or decreased depending on the thickness of the recording layer to be formed, but it is preferable that the ratio to the photopolymerization initiator described above in 2-1 is usually 0.01% by mass or more, preferably 0.1% by mass or more, and usually 10% by mass or less, preferably 5% by mass or less. If the amount of sensitizer used is too small, the initiation efficiency may decrease, and recording may take a long time. If the amount of sensitizer used is too large, the absorption of light used for recording and reproduction may increase, making it difficult for light to reach the depth direction. When two or more sensitizers are used in combination, the total amount thereof should be within the above range.
[0228] <Plasticizer> The composition of the present invention may contain a plasticizer in order to improve reaction efficiency and adjust the physical properties of the recording layer of the holographic recording medium.
[0229] Examples of the plasticizer include phthalates such as dioctyl phthalate, diisononyl phthalate, diisodecyl phthalate, and diundecyl phthalate; adipates such as bis(2-ethylhexyl) adipate, diisononyl adipate, and di-n-butyl adipate; sebacates such as dioctyl sebacate and dibutyl sebacate; phosphates such as tricresyl phosphate; citric acid esters such as acetyl tributyl citrate; trimellitates such as trioctyl trimellitate; epoxidized soybean oil, chlorinated paraffin, alkoxylated (poly)alkylene glycol esters such as acetoxymethoxypropane; and terminally alkoxylated polyalkylene glycols such as dimethoxypolyethylene glycol.
[0230] It is also possible to use a plasticizer containing a fluorine element, such as those exemplified in Japanese Patent No. 6069294. Examples of the plasticizer containing a fluorine element include 2,2,2-trifluoroethyl butylcarbamate, bis(2,2,2-trifluoroethyl)-(2,2,4-trimethylhexane-1,6-diyl)biscarbamate, bis(2,2,2-trifluoroethyl)-[4-({[(2,2,2-trifluoroethoxy)carbonyl]amino}-methyl)octane-1,8-diyl]biscarbamate, 2,2,3,3,4,4,5,5,6,6,7,7,8,8,9,9-hexadecafluorononyl butylcarbamate, and 2,2,2-trifluoroethyl phenylcarbamate.
[0231] These plasticizers are typically used in an amount of 0.01% by mass to 50% by mass, preferably 0.05% by mass to 20% by mass, based on the total solid content of the composition of the present invention. If the plasticizer content is less than this range, the effects of improving reaction efficiency and adjusting physical properties will not be achieved. If the plasticizer content is too high, the transparency of the recording layer will decrease and the plasticizer will bleed out significantly.
[0232] <Leveling Agent> A leveling agent can be used in the composition of the present invention. Examples of leveling agents include sodium polycarboxylates, ammonium polycarboxylates, amine polycarboxylates, silicon-based leveling agents, acrylic leveling agents, ester compounds, ketone compounds, and fluorine compounds. Any one of these may be used alone, or two or more may be used in any combination and ratio.
[0233] <Chain Transfer Agent> A chain transfer agent can be used in the composition of the present invention. Examples of the chain transfer agent include phosphinates such as sodium phosphite and sodium hypophosphite, mercaptans such as mercaptoacetic acid, mercaptopropionic acid, 2-propanethiol, 2-mercaptoethanol, and thiophenol, aldehydes such as acetaldehyde and propionaldehyde, ketones such as acetone and methyl ethyl ketone, halogenated hydrocarbons such as trichloroethylene and perchloroethylene, terpenes such as terpinolene, α-terpinene, β-terpinene, and γ-terpinene, 1,4-cyclohexadiene, 1,4-cycloheptadiene, 1,4-cyclooctadiene, and 1,4-heptadiene. non-conjugated dienes such as thiadiene, 1,4-hexadiene, 2-methyl-1,4-pentadiene, 3,6-nonanedien-1-ol, and 9,12-octadecadienol; linolenic acids such as linoleic acid, γ-linolenic acid, methyl linolenate, ethyl linolenate, isopropyl linolenate, and linoleic acid anhydride; linoleic acids such as linoleic acid, methyl linoleate, ethyl linoleate, isopropyl linoleate, and linoleic acid anhydride; eicosapentaenoic acids such as eicosapentaenoic acid and ethyl eicosapentaenoate; and docosahexaenoic acids such as docosahexaenoic acid and ethyl docosahexaenoate.
[0234] The amount of these additives used is usually 0.001% by mass or more, preferably 0.01% by mass or more, and usually 30% by mass or less, preferably 15% by mass or less, more preferably 10% by mass or less, and particularly preferably 5% by mass or less, relative to the total solid content of the composition of the present invention. When two or more additives are used in combination, the total amount thereof should satisfy the above range.
[0235] 2-7. Method for producing photosensitive composition for hologram recording The composition of the present invention may be produced by mixing the respective components, or by mixing the components other than the photopolymerization initiator in advance and adding the photopolymerization initiator immediately before the photopolymerization reaction. The method for producing a composition containing a photopolymerizable monomer, a matrix resin, and a photopolymerization initiator is not particularly limited, and the order of mixing can also be adjusted as appropriate. When the composition contains components other than those described above, the respective components may be mixed in any combination and order.
[0236] The composition of the present invention, which uses an isocyanate and a polyol as the matrix resin, can be obtained, for example, by the following method, but the present invention is not limited to this. A photoreactive composition (liquid A) is obtained by mixing a photopolymerizable monomer, a photopolymerization initiator, and all other components except the isocyanate and urethane polymerization catalyst. A mixture of the isocyanate and the urethane polymerization catalyst is obtained as liquid B. The photoreactive composition (liquid A) can also be obtained by mixing a photopolymerizable monomer and a photopolymerization initiator with all other components except the isocyanate.
[0237] It is preferable to dehydrate and degas each liquid. If dehydration and degassing are insufficient, bubbles may form during the production of the holographic recording medium, making it impossible to obtain a uniform recording layer. During this dehydration and degassing process, heating and decompression may be performed as long as the components are not damaged.
[0238] The preparation of the composition by mixing liquid A and liquid B is preferably carried out immediately before molding the holographic recording medium. In this case, conventional mixing techniques can also be used. When mixing liquid A and liquid B, degassing may be carried out as necessary to remove residual gas. Furthermore, liquid A and liquid B are preferably subjected to a filtration process to remove foreign matter and impurities, either individually or after mixing. In this case, it is more preferable to filter each liquid separately.
[0239] An isocyanate-functional prepolymer obtained by reacting an isocyanate having an excess of isocyanate groups with a polyol can also be used as the matrix resin. Furthermore, an isocyanate-reactive prepolymer obtained by reacting an isocyanate with a polyol having an excess of isocyanate-reactive functional groups can also be used as the matrix resin.
[0240] 3. Method for Polymerizing the Composition of the Present Invention The method for polymerizing the composition of the present invention is not particularly limited, but includes a method of polymerizing by irradiating with active energy rays and a method of polymerizing by heating together with irradiating with active energy rays.
[0241] 3-1. Photopolymerization initiation method (active energy rays) When the composition of the present invention is photopolymerized, it is carried out by irradiating it with active energy rays. The active energy rays used are preferably electron beams or light in the wavelength range from ultraviolet to infrared. As the light source, for example, if the active energy rays are ultraviolet rays, an ultra-high pressure mercury light source or a metal halide light source can be used. If they are visible light, a metal halide light source or a halogen light source can be used. If they are infrared rays, a halogen light source can be used. In addition to these, light sources such as lasers and LEDs can also be used.
[0242] The amount of active energy ray irradiation is appropriately set depending on the type of light source, the thickness of the coating film, etc., but is preferably set appropriately so that the reaction rate of the total amount of polymerizable functional groups of compound (1) and other polymerizable compounds is 80% or more, more preferably 90% or more. The reaction rate is calculated from the change in absorption peak intensity of the polymerizable functional groups before and after the reaction using infrared absorption spectroscopy. After polymerization by irradiation with active energy rays, the polymerization may be further promoted by heat treatment or annealing treatment as needed. The heating temperature in this case is preferably in the range of 80 to 200°C. The heating time is preferably in the range of 10 to 60 minutes.
[0243] 3-2. Photopolymerization initiation method (heating in combination) When heat treatment is used in combination for photopolymerization of the composition of the present invention, the heating temperature is preferably in the range of 80 to 200°C, more preferably 100 to 150°C. If the heating temperature is lower than 80°C, a longer heating time is required, which tends to be uneconomical. If the heating temperature is higher than 200°C, not only is the energy cost high but the heating time and cooling time are long, which tends to be uneconomical.
[0244] 4. Polymer The polymer of the present invention obtained by polymerizing the composition of the present invention will be described below.
[0245] 4-1. Refractive Index Generally, because the overall density increases through the polymerization reaction, the refractive index of the polymer tends to be higher than that of its precursor, the photopolymerizable monomer. By using a monomer with a high refractive index and allowing the polymerization reaction to proceed sufficiently, the refractive index of the resulting polymer can be increased. For this reason, it is considered important to improve the refractive index of the polymer by designing the molecular structure of the monomer.
[0246] The refractive index shows a large value when evaluated with irradiation light of a short wavelength, but a sample that shows a relatively large refractive index at a short wavelength also shows a relatively large refractive index at a long wavelength, and this relationship is not reversed. Therefore, by evaluating and comparing the refractive index at a constant wavelength, it is possible to compare the intrinsic refractive index of the material. In the present invention, the value at an irradiation light wavelength of 587 nm was used as the standard.
[0247] The refractive index of the composition of the present invention and the polymer of the present invention is preferably 1.60 or more, more preferably 1.63 or more, particularly preferably 1.65 or more, and most preferably 1.67 or more. There is no upper limit to the refractive index of the compound (1) and the polymer of the present invention, but it is usually 2.0 or less.
[0248] When the composition of the present invention and the polymer of the present invention are used as recording layer materials for holographic recording media, the refractive index of compound (1) and the polymer of the present invention is usually in the range of 1.65 or more and 1.78 or less, preferably 1.77 or less. If the refractive index is less than 1.65, the diffraction efficiency is low and the multiplicity is insufficient. If the refractive index is more than 1.78, the difference in refractive index with the matrix resin becomes too large, resulting in increased scattering and reduced transmittance, requiring greater energy for recording and reproduction.
[0249] 4-2. Glass Transition Temperature The glass transition temperature of the polymer of the present invention is preferably 90°C or higher, more preferably 100°C or higher, even more preferably 110°C or higher, particularly preferably 120°C or higher, and is preferably 250°C or lower, more preferably 220°C or lower, and even more preferably 200°C or lower. If the glass transition temperature is below this range, the optical properties may change from the designed values under the usage environment, and the practically required heat resistance may not be satisfied. If the glass transition temperature is above this range, the processability of the polymer may decrease, and a molded product with a good appearance and high dimensional accuracy may not be obtained. Furthermore, the polymer may become brittle, reducing the mechanical strength and making the molded product less easy to handle.
[0250] 5. Optical Materials and Optical Components The composition and polymer of the present invention have properties such as high transparency, high refractive index, ease of polymerization, ease of processability, high chemical stability, archival properties, and low fluorescence, and can therefore be applied to various optical materials and optical components.
[0251] Examples of optical materials include optical overcoats, hard coating agents, adhesives for optical components, resins for optical fibers, and acrylic resin modifiers.
[0252] Examples of optical components include lenses, filters, diffraction gratings, prisms, light guides, cover glass for display devices, photosensors, photoswitches, LEDs, light-emitting elements, optical waveguides, light splitters, optical fiber adhesives, display element substrates, color filter substrates, touch panel substrates, polarizing plates, display backlights, light guide plates, anti-reflection films, viewing angle expansion films, optical recording, optical shaping, and optical relief printing.
[0253] These layers can also be used as, for example, protective films for displays.
[0254] Among these, the composition and polymer of the present invention, due to their high refractive index, are particularly suitable for use in plastic lenses, including imaging lenses for cameras (such as vehicle-mounted cameras, digital cameras, PC cameras, mobile phone cameras, and surveillance cameras), eyeglass lenses, light beam focusing lenses, and light diffusing lenses.
[0255] Lenses using the composition and polymer of the present invention can be subjected to physical or chemical treatments such as surface polishing, antistatic treatment, hard coating treatment, antireflective coating treatment, dyeing treatment, etc., in order to improve the lenses, for example, to prevent reflection, to impart high hardness, to improve abrasion resistance, to improve chemical resistance, to impart antifogging properties, or to impart fashionability, as required.
[0256] 6. Holographic Recording Medium The holographic recording medium of the present invention using the composition of the present invention comprises a recording layer and, if necessary, a support or other layers. Typically, the holographic recording medium has a support, and the recording layer and other layers are laminated on this support to form the holographic recording medium. If the recording layer or other layers have the strength and durability required for the medium, the holographic recording medium does not need to have a support. Examples of other layers include a protective layer, a reflective layer, an anti-reflection layer (anti-reflection film), etc.
[0257] 6-1. Recording Layer The recording layer of the holographic recording medium of the present invention is a layer formed from the composition of the present invention, and is the layer on which information is recorded. Information is usually recorded as a hologram. As will be described later in the section on recording method, the polymerizable compound (hereinafter referred to as polymerizable monomer) contained in the recording layer undergoes a chemical change, such as polymerization, in part upon holographic recording. Therefore, in the holographic recording medium after recording, part of the polymerizable monomer is consumed, and exists as a reacted compound, such as a polymer.
[0258] There are no particular limitations on the thickness of the recording layer, and it may be appropriately determined taking into consideration the recording method, etc. The thickness of the recording layer is preferably 1 μm or more, more preferably 10 μm or more, and preferably 1 cm or less, and even more preferably 3 mm or less. By setting the thickness of the recording layer to the above-mentioned lower limit or more, the selectivity of each hologram tends to be high during multiplexed recording in the holographic recording medium, and the degree of multiplexed recording tends to be high. By setting the thickness of the recording layer to the above-mentioned upper limit or less, it becomes possible to uniformly mold the entire recording layer, and multiplexed recording tends to be possible with uniform diffraction efficiency of each hologram and a high S / N ratio.
[0259] The shrinkage rate of the recording layer due to exposure during recording and reproduction of information is preferably 0.25% or less from the viewpoint of recording reproducibility.
[0260] 6-2. Support There are no particular limitations on the details of the support, and any support can be used as long as it has the strength and durability required for the holographic recording medium. There are no limitations on the shape of the support, but it is usually formed into a flat plate or film. There are also no limitations on the material that makes up the support, and it may be transparent or opaque.
[0261] Examples of transparent materials for the support include organic materials such as acrylic, polyethylene terephthalate, polyethylene naphthoate, polycarbonate, polyethylene, polypropylene, amorphous polyolefin, polystyrene, polycycloolefin, cellulose acetate, etc., and inorganic materials such as glass, silicon, quartz, etc. Among these, polycarbonate, acrylic, polyester, amorphous polyolefin, glass, etc. are preferred, and polycarbonate, acrylic, amorphous polyolefin, polycycloolefin, and glass are particularly more preferred.
[0262] Examples of opaque support materials include metals such as aluminum, and the above-mentioned transparent supports coated with metals such as gold, silver, and aluminum, or dielectrics such as magnesium fluoride and zirconium oxide.
[0263] The thickness of the support is not particularly limited, but is preferably in the range of 0.05 mm to 1 mm. If the thickness of the support is equal to or greater than the lower limit, the mechanical strength of the hologram recording medium can be ensured and warping of the substrate can be prevented. If the thickness of the support is equal to or less than the upper limit, advantages such as increased light transmittance and reduced weight and cost of the hologram recording medium can be obtained.
[0264] The surface of the support may be subjected to a surface treatment. This surface treatment is usually performed to improve the adhesion between the support and the recording layer. Examples of surface treatments include subjecting the support to a corona discharge treatment or forming an undercoat layer on the support in advance. Examples of compositions for the undercoat layer include halogenated phenols, partially hydrolyzed vinyl chloride-vinyl acetate copolymers, polyurethane resins, etc.
[0265] The surface of the support may be treated for purposes other than improving adhesion. Examples of such treatments include a reflective coating treatment for forming a reflective coating layer made of a metal such as gold, silver, or aluminum, and a dielectric coating treatment for forming a dielectric layer made of magnesium fluoride, zirconium oxide, or the like. These layers may be formed as a single layer or as two or more layers.
[0266] These surface treatments may be performed for the purpose of controlling the gas and moisture permeability of the substrate. For example, the reliability of the holographic recording medium can be improved by providing the supports sandwiching the recording layer with a function of suppressing the gas and moisture permeability.
[0267] The support may be provided on either the upper or lower side of the recording layer of the holographic recording medium of the present invention, or on both sides. When supports are provided on both the upper and lower sides of the recording layer, at least one of the supports is configured to be transparent so as to transmit active energy rays (excitation light, reference light, reproduction light, etc.).
[0268] In the case of a holographic recording medium having a support on one or both sides of the recording layer, a transmission or reflection hologram can be recorded. In the case of a support having a reflective property on one side of the recording layer, a reflection hologram can be recorded.
[0269] The support may be provided with a pattern for data addressing. In this case, there is no limitation on the patterning method. For example, the support itself may be provided with unevenness, a pattern may be formed on the reflective layer described later, or a combination of these methods may be used.
[0270] 6-3. Protective Layer The protective layer is a layer for preventing deterioration of the recording and reproduction characteristics of the recording layer. There are no restrictions on the specific configuration of the protective layer, and any known protective layer can be applied. For example, a layer made of a water-soluble polymer, organic / inorganic material, etc. can be formed as the protective layer.
[0271] The position where the protective layer is formed is not particularly limited. The protective layer may be formed, for example, on the surface of the recording layer, between the recording layer and the support, or on the outer surface side of the support. The protective layer may also be formed between the support and another layer.
[0272] 6-4. Reflective Layer The reflective layer is formed when the holographic recording medium is configured to be a reflective type. In the case of a reflective type holographic recording medium, the reflective layer may be formed between the support and the recording layer, or may be formed on the outer surface of the support. Usually, the reflective layer is preferably located between the support and the recording layer. Any known reflective layer can be used, and for example, a thin metal film or the like can be used.
[0273] 6-5. Antireflection Film For both transmission and reflection holographic recording media, an antireflection film may be provided on the side where the information light, reference light, and reproduction light enter and exit, or between the recording layer and the support. The antireflection film improves the light utilization efficiency and suppresses noise generation. Any known antireflection film can be used.
[0274] 6-6. Manufacturing Method of Holographic Recording Medium There are no limitations on the manufacturing method of the holographic recording medium of the present invention. For example, the holographic recording medium can be manufactured by applying the composition of the present invention onto a support without a solvent to form a recording layer. In this case, any method can be used as the coating method. Specific examples include spraying, spin coating, wire bar coating, dipping, air knife coating, roll coating, blade coating, doctor roll coating, etc.
[0275] When forming a recording layer, particularly when forming a thick recording layer, a method of molding in a mold or a method of applying the composition to a release film and punching out a mold can be used. The recording layer can also be produced by preparing a coating liquid containing the composition of the present invention containing a solvent, applying this to a support, and drying it to form a recording layer. In this case, any coating method can be used. For example, the same method as described above can be used.
[0276] There are no limitations on the solvent used in the coating solution, and examples thereof are also given in the section 2-3. Solvent. It is usually preferable to use a solvent that has sufficient solubility for the components used, provides good coating properties, and does not attack supports such as resin substrates. One solvent may be used alone, or two or more solvents may be used in any combination and ratio. There are no limitations on the amount of solvent used. However, in terms of coating efficiency and handleability, it is preferable to prepare a coating solution with a solids concentration of about 1 to 100% by mass.
[0277] Examples of the solvent include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and methyl amyl ketone; aromatic solvents such as toluene and xylene; alcohol-based solvents such as methanol, ethanol, propanol, n-butanol, heptanol, hexanol, diacetone alcohol, and furfuryl alcohol; ketone alcohol-based solvents such as diacetone alcohol and 3-hydroxy-3-methyl-2-butanone; ether-based solvents such as tetrahydrofuran and dioxane; halogen-based solvents such as dichloromethane, dichloroethane, and chloroform; cellosolve-based solvents such as methyl cellosolve, ethyl cellosolve, butyl cellosolve, methyl cellosolve acetate, and ethyl cellosolve acetate; propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and propylene glycol Examples of suitable solvents include propylene glycol solvents such as cholesteryl monobutyl ether acetate and dipropylene glycol dimethyl ether; ester solvents such as ethyl acetate, butyl acetate, amyl acetate, butyl acetate, ethylene glycol diacetate, diethyl oxalate, ethyl pyruvate, ethyl-2-hydroxybutyrate ethyl acetoacetate, methyl lactate, ethyl lactate, methyl 2-hydroxyisobutyrate, and methyl 3-methoxypropionate; perfluoroalkyl alcohol solvents such as tetrafluoropropanol, octafluoropentanol, and hexafluorobutanol; highly polar solvents such as dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide; chain hydrocarbon solvents such as n-hexane and n-octane; cyclic hydrocarbon solvents such as cyclohexane, methylcyclohexane, ethylcyclohexane, dimethylcyclohexane, n-butylcyclohexane, tert-butylcyclohexane, and cyclooctane; and mixed solvents thereof.
[0278] Examples of methods for producing a holographic recording medium include a method in which a thermally melted composition is applied to a support, and then cooled and solidified to form a recording layer; a method in which a liquid composition is applied to a support, and then thermally polymerized to harden the composition to form a recording layer; and a method in which a liquid composition is applied to a support, and then photopolymerized to harden the composition to form a recording layer.
[0279] The holographic recording medium thus produced can be in the form of a free-standing slab or disc and can be used in three-dimensional image display devices, diffractive optical elements, large-capacity memories, and other applications. In particular, the holographic recording medium of the present invention, which uses the composition of the present invention, has high refractive index modulation and is also useful as an AR glass light guide plate (waveguide plate). Here, AR is an abbreviation for augmented reality.
[0280] 6-7. Uses of Holographic Recording Medium <Large Capacity Memory Use> Information is written (recorded) and read (reproduced) to the holographic recording medium of the present invention by irradiation with light.
[0281] When recording information, light capable of causing a chemical change in the polymerizable monomer, that is, its polymerization and concentration change, is used as object light (also called recording light).
[0282] For example, when recording information as a volume hologram, an object beam and a reference beam are irradiated onto the recording layer, causing the object beam and the reference beam to interfere with each other in the recording layer. This causes the polymerizable monomer in the recording layer to polymerize and change in concentration, resulting in interference fringes that cause a refractive index difference in the recording layer. The interference fringes recorded in the recording layer are then recorded as a hologram in the recording layer.
[0283] To reconstruct a volume hologram recorded in a recording layer, a predetermined reconstruction beam (usually a reference beam) is irradiated onto the recording layer. The irradiated reconstruction beam is diffracted in accordance with the interference fringes. This diffracted beam contains the same information as that in the recording layer, and so the information recorded in the recording layer can be reconstructed by reading the diffracted beam with an appropriate detection means.
[0284] The wavelength ranges of the object light, the reproduction light, and the reference light are arbitrary depending on the application, and may be in the visible light range or the ultraviolet range. Among these lights, preferred examples include ruby, glass, Nd-YAG, and Nd-YVO 4 diode lasers such as GaAs, InGaAs, and GaN; gas lasers such as helium-neon, argon, krypton, excimer, and CO2; and lasers with excellent monochromaticity and directivity, such as dye-containing dye lasers.
[0285] There is no limitation on the irradiation dose of the object beam, the reproduction beam, and the reference beam, and the irradiation dose can be any as long as recording and reproduction are possible. If the irradiation dose is extremely low, the chemical change of the polymerizable monomer may be incomplete, and the heat resistance and mechanical properties of the recording layer may not be fully exhibited. Conversely, if the irradiation dose is extremely high, the components of the recording layer (components of the composition of the present invention) may be deteriorated. Therefore, the object beam, the reproduction beam, and the reference beam are usually set to 0.1 J / cm or less depending on the composition of the composition of the present invention used to form the recording layer, the type and amount of the photopolymerization initiator, etc. 2 Above, 20J / cm 2 Irradiate within the following range:
[0286] Hologram recording methods include polarization collinear hologram recording, reference beam incident angle multiplexing hologram recording, etc. When the hologram recording medium of the present invention is used as a recording medium, good recording quality can be achieved with any of these recording methods.
[0287] <Application to AR Glass Light Guide Plate (Application to AR Glass Light Guide Plate)> A volume hologram is recorded on the holographic recording medium of the present invention in the same manner as in the case of the large-capacity memory application described above.
[0288] For a volume hologram recorded in the recording layer, a predetermined reproduction light is irradiated onto the recording layer. The irradiated reproduction light is diffracted in accordance with the interference fringes. In this case, even if the wavelength of the reproduction light does not match the wavelength of the recording light, diffraction occurs as long as the interference fringes and the Bragg condition are met. Therefore, by recording corresponding interference fringes according to the wavelength and incident angle of the reproduction light to be diffracted, diffraction can be caused for reproduction light over a wide wavelength range. This allows the display color gamut of AR glasses to be expanded.
[0289] By recording the corresponding interference fringes according to the wavelength and diffraction angle of the reconstructed light, it is possible to guide the reconstructed light incident from outside the hologram recording medium into the hologram recording medium, to reflect, split, expand, or reduce the reconstructed light that has been guided inside the hologram recording medium, or to emit the reconstructed light that has been guided inside the hologram recording medium to the outside of the hologram recording medium, thereby widening the viewing angle of the AR glasses.
[0290] The wavelength ranges of the object light and the reproduction light are arbitrary depending on the respective applications, and may be either the visible light range or the ultraviolet range. Among these light sources, the aforementioned laser and the like are preferred. The reproduction light is not limited to the laser and the like, and display devices such as a liquid crystal display (LCD) and an organic electroluminescence display (OLED) are also preferred.
[0291] There is no limitation on the irradiation dose of the object beam, the reproduction beam, and the reference beam, and the irradiation dose can be any as long as recording and reproduction are possible. If the irradiation dose is extremely low, the chemical change of the polymerizable monomer may be incomplete, and the heat resistance and mechanical properties of the recording layer may not be fully exhibited. Conversely, if the irradiation dose is extremely high, the components of the recording layer (components of the composition of the present invention) may be deteriorated. Therefore, the object beam, the reproduction beam, and the reference beam are usually set to 0.1 J / cm or less depending on the composition of the composition of the present invention used to form the recording layer, the type and amount of the photopolymerization initiator, etc. 2 Above, 20J / cm 2 Irradiate within the following range:
[0292] 6-8. Performance index of holographic recording media The performance of a holographic recording media is indexed by total Δn, which is calculated using the sum of the diffraction efficiencies across the entire multiplexed recording. In the case of a transmission hologram, the diffraction efficiency of the hologram is given by the ratio of the intensity of diffracted light to the sum of the intensity of transmitted light and the intensity of diffracted light. From the obtained diffraction efficiency, Δn is calculated using the following equation based on Coupled Wave Theory (H. Kogelnik, The Bell System Technical Journal (1969), 48, 2909-2947), and the sum across the entire multiplexed recording is taken as total Δn.
[0293]
[0294] where η is the diffraction efficiency, T is the thickness of the medium, λ is the wavelength of the reference light, and θ is the angle of incidence of the reference light.
[0295] In the case of large-capacity memory, a higher total Δn is preferable because it means that more information can be stored per unit volume.In the case of AR glasses, a higher total Δn is preferable because it allows the projected image from the projector to be delivered to the pupil brightly, reduces power consumption, and widens the viewing angle.
[0296] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples as long as it does not deviate from the gist of the invention.
[0297] [Raw Materials Used] The raw materials for the compositions used in the Examples and Comparative Examples are as follows.
[0298] <Isocyanate> Duranate (registered trademark) TSS-100: hexamethylene diisocyanate-based polyisocyanate (NCO 17.6%) (manufactured by Asahi Kasei Corporation)
[0299] <Polyol> Placcel PCL-205U: Polycaprolactone diol (molecular weight 530) (manufactured by Daicel Corporation) Placcel PCL-305: Polycaprolactone triol (molecular weight 550) (manufactured by Daicel Corporation)
[0300] <Photopolymerization initiator> HLI02: 1-(9-ethyl-6-cyclohexanoyl-9H-carbazol-3-yl)-1-(O-acetyloxime)methyl glutarate
[0301] <Radical Scavenger> TEMPOL: 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl free radical (Tokyo Chemical Industry Co., Ltd.)
[0302] <Urethane polymerization catalyst> Octylic acid solution of tris(2-ethylhexanoate)bismuth (active ingredient amount: 56% by mass)
[0303] Example 1 Preparation of Compound M-1 Compound M-1 was prepared by the following synthesis method.
[0304]
[0305] 2,4,6-Tribromophenol (2.3 g), phenanthrene-9-boronic acid (5.8 g), and sodium carbonate (3.5 g) were dissolved in 100 mL of dioxane and 25 mL of water, and the solution was degassed by passing nitrogen gas through it. 10 mg of dichlorobis[di-t-butyl(p-dimethylaminophenyl)phosphino]palladium(II) was added to the reaction solution, and nitrogen gas was passed through it for an additional 5 minutes. The reaction solution was heated under a nitrogen atmosphere and stirred under reflux for 5 hours. After cooling to room temperature, 100 mL of ethyl acetate and 50 mL of water were added, and the mixture was separated. The resulting organic layer was washed with an aqueous sodium bicarbonate solution. After drying the organic layer, the resulting solid was washed with hexane. The solid was dried in a vacuum dryer, yielding 4.4 g of crude compound S-1.
[0306] The NMR measurement data of the compound S-1 was as follows: 1 H-NMR (400MHz, CDCl 3 , δ, ppm) 8.84-8.66 (Ar, 6H), 8.32 (dd, Ar, 1H), 8.11 (dd, Ar, 1H), 8.07 (d d, Ar, 1H), 8.04-7.86 (Ar, 8H), 7.75-7.57 (Ar, 12H), 5.18-5.13 (OH, 1H)
[0307] Compound S-1 (4.4 g), 2-isocyanatoethyl acrylate (0.4 g), and THF (10 mL) were mixed. Diazabicycloundecene (0.01 g) was added thereto, and the mixture was stirred for 3 hours. After completion of the reaction, the reaction solution was poured into 50 mL of an aqueous ammonium chloride solution, extracted with 200 mL of ethyl acetate, washed with 100 mL of saturated brine, dried over anhydrous magnesium sulfate, filtered, and concentrated. The obtained crude product was purified by column chromatography, yielding 3.4 g of compound M-1.
[0308] The NMR measurement data of compound M-1 was as follows: 1 H NMR (400 MHz, CDCl 3 , δ, ppm) 8.81-8.66 (Ar, 6H), 8.33-8.26 (Ar, 1H), 8.13-8.01 (Ar, 2H), 7.99 -7.85 (Ar, 6H), 7.84-7.78 (Ar, 2H), 7.73-7.57 (Ar, 12H), 5.67-5.54 (C=CH 2 , 1H), 5.34-5.26 (C=CH 2 , 1H), 4.28-3.83 (NH, 1H), 3.29-2.82 (CH 2 , 2H), 2.78-2.13 (CH 2 , 2H), 1.67-1.58 (Me, 3H)
[0309] <Preparation of Compound M-2> Compound M-2 was prepared by the following synthesis method.
[0310]
[0311] Tetrabromobisphenol A (10.0 g), phenanthrene-9-boronic acid (18.1 g), and sodium carbonate (9.9 g) were suspended in 250 mL of toluene, 250 mL of ethanol, and 125 mL of water, and the suspension was degassed by passing nitrogen gas through the suspension. 1.4 mg of dichlorobis[di-t-butyl(p-dimethylaminophenyl)phosphino]palladium(II) was added to the reaction solution, and nitrogen gas was passed through the suspension for an additional 10 minutes. The reaction solution was heated under a nitrogen atmosphere and stirred under reflux for 4 hours. After cooling to room temperature, 100 mL of water was added, and the suspension was extracted with toluene. The organic layer was dried over sodium sulfate, and then concentrated. 19.9 g of crude compound S-2 was obtained by the concentration.
[0312] The NMR measurement data of the compound S-2 was as follows: 1 H-NMR (400MHz, CDCl 3 , δ, ppm) 8.81-8.67 (Ar, 8H), 7.94-7.31 (Ar, 32H), 4.92-4.87 (OH, 2H), 1.91-1.76 (Me, 6H)
[0313] Crude compound S-2 (15.7 g), 2-isocyanatoethyl methacrylate (5.3 g), and dichloromethane (100 mL) were mixed under a nitrogen atmosphere. Diazabicycloundecene (20.0 mg) was added to the mixture, and the mixture was stirred at room temperature. After the reaction was completed, 8 g of neutral silica gel was added to the reaction solution, and the mixture was stirred at room temperature for 30 minutes. The silica gel and solid components were then filtered off, and the solid was washed with dichloromethane / ethyl acetate (10:1). The resulting organic layer was concentrated and then dissolved in dichloromethane (30 mL), and the solution was added dropwise to 300 mL of methanol cooled to 0°C. The resulting solid was filtered, washed with a small amount of cold methanol, and then dried in a vacuum dryer, yielding 14.5 g of compound M-2.
[0314] The NMR measurement data of the compound M-2 was as follows: 1 H-NMR (400MHz, CDCl 3 , δ, ppm) 8.82-8.61 (Ar, 8H), 8.01-7.51 (Ar, 28H), 7.44-7.18 (Ar, 4H), 5.62-5.48 (C=CH 2 , 2H), 5.32-5.19 (C=CH2 , 2H), 4.28-3.78 (NH, 2H), 3.33-2.73 (CH 2 , 4H), 2.73-2.05 (CH 2 , 4H), 1.98-1.79 (Me, 6H), 1.62-1.52 (Me, 6H)
[0315] <Preparation of Holographic Recording Medium> 0.2938 g of a mixture (molar ratio 90:10) of compound M-1 (0.1789 g) and compound M-2 (0.1149 g) as polymerizable monomers, 0.0096 g of photopolymerization initiator HLI02, and 3.30 mg of radical scavenger TEMPOL were dissolved in 2.51 g of Duranate (registered trademark) TSS-100 to prepare solution A. Separately, 1.74 g of Placcel PCL-205U and 0.75 g of Placcel PCL-305 were mixed (Placcel PCL-205U:Placcel PCL-305 = 70:30 (mass ratio)), and 0.2 mg of a solution of tris(2-ethylhexanoate)bismuth in octylic acid was dissolved in the mixture to prepare solution B.
[0316] After degassing each of the solutions A and B under reduced pressure at room temperature or 45°C for 2 hours, 2.38 g of solution A and 2.12 g of solution B were mixed by stirring and further degassed under vacuum for several minutes. The vacuum-degassed mixture was then poured onto a glass slide with 0.5 mm-thick spacer sheets placed on two opposing edges. A glass slide was then placed over the glass slide, the edges secured with clips, and the mixture was heated at 80°C for 24 hours to produce a holographic recording medium as an evaluation sample. This evaluation sample had a 0.5 mm-thick recording layer formed between the glass slides that served as covers.
[0317] <Hologram Recording and Evaluation> Using the hologram recording medium prepared as an evaluation sample, hologram recording and evaluation of the hologram recording performance of the hologram recording medium were carried out according to the procedures described below.
[0318] Hologram recording was performed using a semiconductor laser with a wavelength of 405 nm and an exposure power density of 10.2 mW / cm per beam. 2Using the exposure device shown in Figure 1, two-beam plane wave hologram recording was performed. The medium was rotated from -22.5° to 22.5°, and angle multiplexed recording was performed at the same location. The diffraction efficiency for each multiplexed recording was measured. Δn was calculated from the obtained diffraction efficiencies, and the sum of the entire multiplexed recording was taken as total Δn. This will be explained in detail below.
[0319] (Hologram Recording) Figure 1 is a structural diagram showing an overview of the device used for hologram recording. In Figure 1, S is a sample of a hologram recording medium, and M1 to M3 all represent mirrors. PBS represents a polarizing beam splitter. L1 represents a laser light source for recording light that emits light with a wavelength of 405 nm (a single-mode laser manufactured by TOPTICA Photonics ("L1" in Figure 1) that can obtain light with a wavelength of around 405 nm). L2 represents a laser light source for reproducing light that emits light with a wavelength of 633 nm. PD1, PD2, and PD3 represent photodetectors. 1 represents an LED unit.
[0320] As shown in Figure 1, light with a wavelength of 405 nm was split by a polarizing beam splitter ("PBS" in the figure), and the two beams were made to intersect on the recording surface at an angle of 59.3°. At this time, the bisector of the angle between the two beams was set perpendicular to the recording surface, and further, the vibration plane of the electric field vectors of the two beams obtained by splitting was set perpendicular to the plane containing the two intersecting beams.
[0321] After the hologram was recorded, a He-Ne laser capable of producing light with a wavelength of 633 nm (V05-LHP151 manufactured by Melles Griot: "L2" in the figure) was used. The light was irradiated onto the hologram recording medium at an angle of 50.7°, and the diffracted light was detected using a photodiode and photosensor amplifier (S2281, C9329 manufactured by Hamamatsu Photonics: "PD1" in the figure) to determine whether the hologram was recorded correctly.
[0322] (Measurement of Diffraction Efficiency) The angle at which the sample was moved relative to the optical axis (the angle between the bisector of the interior angle at the point where the two beams, i.e., the incident light from mirrors M1 and M2 in Figure 1, intersect and the normal from the sample) was changed from -22.5° to 22.5° in 0.3° increments to perform 151 multiplexed recordings.
[0323] After multiplex recording, the LED unit (1 in the figure, central wavelength 405 nm) was turned on for a certain period of time to consume the remaining initiator and monomer. This process is called post-exposure. The LED power was 30 mW / cm. 2 The cumulative energy is 3.6 J / cm 2 The irradiation was carried out so that
[0324] The diffraction efficiency of a hologram is given by the ratio of the intensity of diffracted light to the sum of the intensity of transmitted light and the intensity of diffracted light. Light (wavelength 405 nm) from mirror M1 in Figure 1 was irradiated, and the diffraction efficiency was measured from angles of -23° to 23°. From the obtained diffraction efficiency, Δn was calculated using the following formula based on Coupled Wave Theory (H. Kogelnik, The Bell System Technical Journal (1969), 48, 2909-2947), and the sum of the entire multiplexed recording was taken as total Δn.
[0325]
[0326] Here, η is the diffraction efficiency, T is the thickness of the medium, λ is the wavelength of the reference light, and θ is the incident angle of the reference light (29.65°).
[0327] Using multiple samples, evaluations were performed multiple times under different irradiation energy conditions, such as increasing or decreasing the irradiation energy at the beginning of recording and increasing or decreasing the total irradiation energy, to find the conditions under which the polymerizable monomer is almost completely consumed (total Δn reaches almost equilibrium during multiple recording), and the total Δn was maximized.The maximum value obtained was then used as the total Δn of the medium.The evaluation results are shown in Table 2 below.
[0328] Example 2 A holographic recording medium was prepared and evaluated in the same manner as in Example 1, except that a mixture of compound M-1 (0.2264 g) and compound M-2 (0.0379 g) (molar ratio 90:10) was used as the polymerizable monomer.
[0329] Comparative Example 1 A holographic recording medium was prepared in the same manner as in Example 1, except that compound M-1 (0.2515 g) was used alone as the polymerizable monomer, and the holographic recording medium was evaluated.
[0330] Comparative Example 2 A holographic recording medium was prepared in the same manner as in Example 1, except that compound M-2 (0.3821 g) was used alone as the polymerizable monomer, and the holographic recording medium was evaluated.
[0331] [Measurement of Refractive Index] The refractive indexes of the photopolymerizable monomers M-1 and M-2 produced in the examples were measured by the following method. The results are shown in Table 1.
[0332] Test solutions were prepared by dissolving the sample to a predetermined concentration in a mixed solution of 3-phenoxybenzyl acrylate and trimethylolpropane trimethacrylate in a mass ratio of 4:1. Two types of test solutions were prepared, with sample concentrations of 10 mass% and 20 mass%.
[0333] The refractive index of each test solution was measured using a Kalnew precision refractometer (Shimadzu Corporation, product name: KPR-2000). The temperature of the test solution was 23°C, and the measurement wavelength was the d-line of a helium lamp (587.6 nm). Based on the measurement results, a calibration curve showing the correlation between sample concentration and refractive index was created, and from the resulting calibration curve, the refractive index when the sample concentration was 100% by mass was determined and used as the refractive index of the sample.
[0334]
[0335] From Table 1, it can be seen that the refractive indexes of the compounds M-1 and M-2 produced in the examples are all 1.65 or more, making them excellent high refractive index materials.
[0336] [Recording archival stability] The holographic recording media for which the total Δn had been measured were heated and stored in dry air at 75°C for 100 hours, and the total Δn after heating was measured to calculate the Δn retention before and after heating. A retention of 95% or more was evaluated as ◎, a retention of 85% or more but less than 95% was evaluated as ○, a retention of 75% or more but less than 85% was evaluated as △, and a retention of less than 75% was evaluated as ×. The results are shown in Table 2.
[0337] [Fluorescence Intensity] A hologram recording medium other than the one for which total Δn was measured was measured using an LED unit (1 in the figure, central wavelength 405 nm) with a light irradiation power of 80 mW / cm 2 The light irradiation energy is 48 J / cm 2 The hologram recording medium was irradiated so that the fluorescence intensity was 450 nm. The fluorescence intensity was then measured using a fluorescence spectrophotometer (Hitachi High-Tech Science F-7000). The conditions for measuring the fluorescence intensity were an excitation wavelength of 450 nm, a fluorescence measurement wavelength range of 465 nm to 700 nm, and a measurement wavelength interval of 0.2 nm. As reference data for the instrument, the fluorescence intensity of only the same slide glass used in the hologram recording medium was subtracted from the fluorescence intensity of the hologram recording medium. The integrated fluorescence intensity was calculated by integrating the fluorescence intensities over the entire measurement range. An integrated fluorescence intensity of less than 7000 was evaluated as ○, and an integrated fluorescence intensity of 7000 or more was evaluated as ×. The results are shown in Table 2.
[0338]
[0339] As shown in Table 2, in Comparative Example 1, in which M-1, a monofunctional photopolymerizable monomer of Compound (1), was used alone as the photopolymerizable monomer, the total Δn of the holographic recording medium before heating was 0.0223, but after heating it decreased to 0.0120, and the Δn retention rate was 54%. On the other hand, in Examples 1 and 2 of the present invention, in which a monofunctional photopolymerizable monomer containing Compound (1) was used in combination with a polyfunctional photopolymerizable monomer, the holographic recording medium had a total Δn of 0.024 or more before heating and a Δn retention rate of over 85% after heating. Furthermore, with regard to fluorescence intensity, while the integrated fluorescence intensity was 7000 or more in Comparative Examples 1 and 2, it was less than 5500 in Examples 1 and 2, which was significantly lower than the comparative examples in which each monomer was used alone.
[0340] When used as an optical element in an AR glass light guide plate, a holographic recording medium with a higher total Δn can brighten the projected image and widen the viewing angle. For memory applications, improving total Δn can improve recording capacity. Additionally, the higher the archival properties of these holographic recording media with a high total Δn, the longer they can continue to exhibit the above-mentioned performance. Compared to the comparative examples, the examples of this study have significantly higher archival properties, demonstrating the superiority of the photosensitive composition for holographic recording of the present invention.
[0341] Furthermore, holographic recording media require high transparency, and turbidity and noise due to the inclusion or generation of insoluble matter can lead to the formation of unintended interference fringes during holographic recording, leading to a decrease in the performance of the holographic recording media. In particular, in AR glass waveguide applications, this unintended light scattering reduces light utilization efficiency and aesthetics. Furthermore, if insoluble matter precipitates in the waveguide over time, the absorption intensity of the guided light also changes over time, leading to a decrease in the performance stability of the waveguide. Therefore, by using the composition of the present invention, which can suppress the fluorescence phenomenon caused by phosphors that are generally produced as a by-product during the photopolymerization of polymerizable monomers, it is possible to produce AR glass light guide plates with excellent light utilization efficiency, aesthetics, and long-term performance stability. From the above, it can be said that the composition of the present invention used in the examples is superior to the compounds used in the comparative examples.
[0342] Although the present invention has been described in detail using specific embodiments, it will be apparent to those skilled in the art that various modifications are possible within the scope of the effects of the invention. This application is based on Japanese Patent Application No. 2023-053748 filed on March 29, 2023, and is incorporated by reference in its entirety.
[0343] S Hologram recording medium M1, M2, M3 Mirrors L1 Semiconductor laser light source for recording light L2 Laser light source for reproducing light PD1, PD2, PD3 Photodetectors PBS Polarizing beam splitter 1 LED unit
Claims
1. A photosensitive composition for hologram recording comprising a photopolymerization initiator and at least two different photopolymerizable monomers which are a combination of a monofunctional photopolymerizable monomer and a polyfunctional photopolymerizable monomer, wherein at least one of the photopolymerizable monomers is a compound selected from the group consisting of a compound represented by the following formula (1-1) and a compound represented by the following formula (1-2): [In formula (1-1), A 1 represents a photopolymerizable group. 1 represents a single bond or an optionally branched divalent linking group. 1 represents a fused aromatic ring group which may have a substituent. 1 is an integer from 2 to 5, and a plurality of R 1 may be the same or different. 1 The benzene ring having the formula A 1 -L 1 -O, and R 1 In addition, it may further have a substituent. [In formula (1-2), A 2 represents a photopolymerizable group. 2 represents a single bond or an optionally branched divalent linking group. 2 represents a fused aromatic ring group which may have a substituent. 2 is an integer from 2 to 4, and a plurality of R 2 may be the same or different. n represents an integer of 2 to 4. When n is 2, X represents a single bond or a divalent group selected from the group consisting of structures represented by the following formulas (1a) to (1g). When n is 3, X represents a trivalent organic group. When n is 4, X represents a carbon atom or a silicon atom. A, which is present in plurality in formula (1-2), 2 , L 2 , R 2 , m 2 may be the same or different. 2 The benzene ring having the formula A 2 -L 2 -O, R 2 and X may further have a substituent. [In formula (1a), R 3 and R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
2. The photosensitive composition for hologram recording according to claim 1, wherein said n is 2.
3. The above m 1 and m 2 2. The photosensitive composition for hologram recording according to claim 1, wherein is 2 or 3.
4. Section A above 1 and A 2 2. The photosensitive composition for hologram recording according to claim 1, wherein is a (meth)acryloyl group or an allyl group.
5. The above R 1 and R 2 2. The photosensitive composition for hologram recording according to claim 1, wherein the condensed aromatic ring is any one of a naphthalene ring, a phenanthrene ring, a dibenzothiophene ring, and a thianthrene ring.
6. The photosensitive composition for hologram recording according to claim 1, wherein at least one of the monofunctional photopolymerizable monomers contains a compound represented by formula (1-1), and at least one of the polyfunctional photopolymerizable monomers contains a compound represented by formula (1-2).
7. A holographic recording medium comprising the photosensitive composition for holographic recording according to any one of claims 1 to 6.
8. A polymer obtained by polymerizing the photosensitive composition for hologram recording according to any one of claims 1 to 6.
9. An optical material comprising the polymer according to claim 8.
10. An optical component comprising the polymer of claim 8.
11. A large capacity memory including the holographic recording medium according to claim 7.
12. An optical element obtained by holographically recording on the holographic recording medium according to claim 7.
13. An AR light guide plate comprising the optical element according to claim 12.
14. AR glasses comprising the optical element according to claim 12.
Citation Information
Patent Citations
Metallocene, manufacture and photopolymerizable composition containing same
JP1984152396A
Titanocenes and radiation-curable composition containing same
JP1986151197A
Photopolymerizable composition
JP1990000069A
Line controller
JP1990055446A
Curable composition containing sulfonium compound and sensitizer
JP1993230189A