Binder for secondary battery and preparation method therefor, separator, battery cell, battery and electric device

By using acrylate copolymer and water-soluble polymer binder on the battery separator, the gap problem between the pole piece and the separator caused by the opening of the battery cell is solved, the cycle performance and hardness of the battery are improved, and the electrochemical impedance is reduced. .

WO2024212343A1PCT designated stage expired Publication Date: 2024-10-17CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/099993
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2023-06-13
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Battery cells have the problem of large openings, which easily form gaps between the pole pieces and the separators, affecting the battery's cycle performance.

Method used

A binder including an acrylate copolymer and a water-soluble polymer is used, and is coated on the separator, and the water-soluble polymer is used as a support to connect the first polymer to form a network structure, thereby improving the connection between the separator and the separator. The bonding force of the pole pieces is enhanced through mechanical interlocking during the cold pressing process.

Benefits of technology

It improves the cold-pressed adhesion between the separator and the pole piece, alleviates the problem of cell opening, enhances the hardness of the cell and the dynamic performance of the secondary battery, reduces the electrochemical impedance, and improves the rate and cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023099993_17102024_PF_FP_ABST
    Figure CN2023099993_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of secondary batteries, in particular to a binder for a secondary battery and a preparation method therefor, a separator comprising the binder, a battery cell, a battery and an electric device. The binder for the secondary battery comprises a first polymer and a second polymer, wherein the first polymer comprises an acrylate copolymer, and the second polymer comprises a water-soluble polymer. During the coating of the separator, the binder is stirred in water until uniform, the separator is then coated with same and is dried, and a bonding layer is formed on the separator; the bonding layer comprises a side facing the separator and a side deviating from the separator; and the bonding layer is bonded to the separator, and the side deviating from the separator does not have cohesiveness, such that the separator can be conveniently wound and unwound. When the separator is subjected to a cold pressing process after being wound with positive and negative electrode sheets, the binder has a relatively good bonding force, making the positive and negative electrode sheets and the separator tightly attached to each other, such that the hardness of a battery core and the cycle performance of a secondary battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Binder for secondary battery and preparation method thereof, as well as separator, battery cell, battery and electrical device

[0001] Related applications

[0002] This application claims priority to Chinese patent application No. 202310402475.2 filed on April 14, 2023, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application relates to the technical field of secondary batteries, and in particular to a binder for secondary batteries and a preparation method thereof, as well as a separator, a battery cell, a battery and an electrical device. Background Art

[0004] With the rapid growth of portable electronic devices and electric vehicles, the demand for power batteries is also growing. Among them, the electrochemical performance of batteries is also attracting more and more attention.

[0005] Currently, battery cells have a problem of large openings, that is, gaps are easily formed between the electrode and the diaphragm, resulting in poor battery cycle performance.

[0006] Summary of the Invention

[0007] The main purpose of this application is to provide a binder for secondary batteries, which aims to improve the bonding force between the separator and the electrode and improve the cycle performance of the battery.

[0008] To achieve the above objectives, the present application provides a binder for a secondary battery, wherein the binder includes a first polymer and a second polymer, wherein the first polymer includes an acrylic acid ester copolymer, and the second polymer includes a water-soluble polymer.

[0009] Acrylate copolymers have good adhesion. The use of acrylic copolymers can improve the adhesion between the diaphragm and the electrode after cold pressing.

[0010] Water-soluble polymers are soluble in water and are non-sticky in the dry state.

[0011] The binder includes a first polymer and a second polymer, the first polymer includes an acrylic copolymer, and the second polymer includes a water-soluble polymer. When the binder is applied to the diaphragm, the water-soluble polymer serves as a support to support the first polymer, connects the first polymer to the water-soluble polymer, and bonds the first polymer to the diaphragm. Specifically, in the process of applying the binder to the diaphragm, the binder and water are mixed to form a slurry, and then the slurry is applied to the diaphragm. The water-soluble polymer has adhesiveness after contacting water, and the water-soluble polymer can bond to the diaphragm. The water-soluble polymer can bond the first polymer (including the acrylic copolymer) to the diaphragm. The acrylic copolymer and / or the water-soluble polymer in the binder can partially penetrate into the pores of the diaphragm to achieve bonding with the diaphragm. When After the slurry is dried, due to the volatilization of water, the water-soluble polymer molecules are entangled with each other, and the molecules interact with each other, thereby forming a network structure, which supports and connects the first polymer (including acrylic copolymers) and bonds the first polymer particles to the diaphragm. The slurry layer becomes an adhesive layer after drying. The adhesive layer has a side facing the diaphragm and a side facing away from the diaphragm. During the slurry coating process, the water-soluble polymer can be bonded to the diaphragm, or the acrylic copolymer and / or water-soluble polymer in the adhesive can partially penetrate into the pores of the diaphragm to achieve bonding with the diaphragm. Therefore, the adhesive layer is bonded to the diaphragm. Since the acrylic copolymer and the water-soluble polymer have no stickiness after drying, the side of the adhesive layer facing away from the diaphragm has no stickiness, which facilitates the winding and unwinding of the diaphragm.

[0012] When the adhesive is cold-pressed after being wound with the positive and negative electrode sheets, the adhesive has better bonding strength, so that the positive and negative electrode sheets and the diaphragm are tightly attached to each other. Specifically, after cold pressing, the bonding strength is mainly provided by the mechanical interlocking effect of the acrylic copolymer and water-soluble polymer in the adhesive penetrating into the pores of the electrode sheets, as well as the intermolecular force of the acrylic copolymer. Therefore, the adhesive of the present application improves the cold-pressing bonding strength between the diaphragm and the positive and negative electrode sheets, reduces problems such as cell opening and soft cells, thereby improving the hardness of the cell. At the same time, the adhesive is coated on the diaphragm and applied to the secondary battery, which improves the dynamic performance of the secondary battery, reduces the electrochemical impedance, and can improve the rate performance and battery cycle performance of the secondary battery.

[0013] Optionally, the mass ratio of the first polymer to the second polymer is 1:(0.1-10); preferably, 1:(0.2-5).

[0014] Setting the mass ratio of the first polymer to the second polymer within the above range can help the bonding layer form a continuous network structure, bond the first polymer to the separator, and improve the bonding performance of the bonding layer at room temperature.

[0015] That is, as the amount of the second polymer increases, the bonding strength of the bonding layer increases first and then decreases. By controlling the quality of the first polymer and the second polymer within the above range, the bonding strength of the adhesive applied to the diaphragm can be effectively improved.

[0016] Optionally, the second polymer includes one or more of polyacrylamide, polyacrylic acid, polyvinyl pyrrolidone, polyvinyl alcohol, polyethylene glycol, and polymaleic anhydride.

[0017] The second polymer includes the above-mentioned water-soluble polymers. These water-soluble polymers contain hydrophilic groups and a certain number of hydrophobic groups, and thus have a certain surface activity, which can reduce the surface tension of water to a certain extent and improve the solubility and dispersion properties of the binder in the aqueous phase. That is, when preparing the diaphragm coating slurry, the water-soluble polymer is used to control the viscosity and rheological properties of the slurry, so that the binder is better dispersed and suspended. In addition, the second polymer also has a chemical reaction function (for example, a carboxyl group, a hydroxyl group, etc. that reacts with other groups). The polar groups on the water-soluble polymer structure can form hydrogen bonds with the first polymer and the diaphragm and the electrode, thereby improving the bonding force between the diaphragm and the electrode.

[0018] Optionally, the binder has a volume particle size distribution Dv50 of 1 μm to 15 μm; preferably, 3 μm to 12 μm.

[0019] Theoretically, the volume average particle size Dv50 of the binder in this application can be lower than 1 μm or higher than 15 μm. However, considering that the binder in this application is used on the diaphragm, the volume average particle size Dv50 of the binder is set within the above range to improve the problem of the binder blocking the pores of the diaphragm, reducing the problem of lithium ions (taking lithium-ion batteries as an example, of course, other types of secondary batteries) passing through the diaphragm, and improving the problem of the binder being coated on the diaphragm to form a thicker coating, which affects the energy density of the battery prepared later. Therefore, the volume particle size distribution Dv50 of the binder is 1 μm to 15 μm; preferably, 3 μm to 12 μm.

[0020] It can be understood that, as shown in Figure 1, the binder particles are secondary particles containing primary particles of a first polymer and primary particles of a second polymer. In this way, the second polymer serves as a skeleton. When the binder slurry is applied to the diaphragm, the second polymer plays a role in supporting and connecting the first polymer, bonding the first polymer to the diaphragm. After the slurry is dried to form a bonding layer, the bonding layer can bond to the diaphragm, but the side of the bonding layer facing away from the diaphragm has no bonding force, which facilitates the winding and unwinding of the diaphragm. Moreover, when the diaphragm and the positive and negative pole pieces are wound and then cold pressed, after being squeezed, the first polymer and the second polymer can be deformed by force and penetrate into the pores of the diaphragm and the pole piece, thereby achieving a bonding effect.

[0021] Optionally, the shape of the binder includes a spherical shape.

[0022] The spherical shape facilitates uniform dispersion during the stirring of the slurry, which is conducive to uniform coating.

[0023] Optionally, the first polymer includes an acrylate monomer, and the structure of the acrylate monomer includes:

[0024] Wherein, R1 includes a hydrogen atom or an alkyl group of 1 to 12 carbon atoms, and R2 includes an alkyl group of 1 to 12 carbon atoms.

[0025] Acrylate monomers include unsaturated ester groups, which can improve the polymer's anti-swelling ability. As a flexible monomer segment in the molecular chain, it can adjust the polymer's glass transition temperature, improve the toughness of the adhesive during application, and help to achieve good bonding.

[0026] Optionally, the acrylic acid ester monomer includes one or more of methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate.

[0027] By using any one or more of the above-mentioned acrylic ester monomers, the glass transition temperature of the polymer can be adjusted and the anti-swelling ability of the polymer can be improved.

[0028] Optionally, the first polymer includes an acrylonitrile monomer, and the structure of the acrylonitrile monomer includes:

[0029] Wherein, R3 includes a hydrogen atom or an alkyl group of 1 to 6 carbon atoms.

[0030] The unsaturated cyano group in the structure of acrylonitrile monomers helps to improve ionic conductivity and enhance adhesion.

[0031] Optionally, the acrylonitrile monomer includes one or more of acrylonitrile and methacrylonitrile.

[0032] The use of any one or more of the above-mentioned acrylonitrile monomers can improve the ionic conductivity of the binder.

[0033] Optionally, the first polymer includes an acrylamide monomer, and the structure of the acrylamide monomer includes:

[0034] wherein R4 comprises a hydrogen atom or an alkyl group of 1 to 6 carbon atoms, and R5 comprises a hydrogen atom, an alkyl group of 1 to 6 carbon atoms substituted with a hydroxyl group, or an alkoxy group of 1 to 6 carbon atoms.

[0035] The third unit includes an unsaturated amide group, which plays a cross-linking role and also has good adhesion.

[0036] Optionally, the acrylamide monomers include one or more of acrylamide, N-hydroxymethyl acrylamide and N-butoxymethyl acrylamide.

[0037] The use of any one or more of the above-mentioned acrylamide monomers can play a role in regulating the molecular weight, so as to adjust the molecular weight of the polymer. The molecular weight of the adhesive is helpful to improve the adhesiveness within a certain range.

[0038] It is understood that the constituent monomers of the first polymer may include one, two or three of the above three monomers, without specific limitation.

[0039] Optionally, the first polymer includes an acrylate monomer, an acrylonitrile monomer and an acrylamide monomer, and the mass ratio of the acrylate monomer, the acrylonitrile monomer and the acrylamide monomer is in the range of 100:(1-80):(1-20), preferably, 100:(20-60):(5-15).

[0040] In order to improve the comprehensive performance of the first polymer, the first polymer includes an acrylate monomer, an acrylonitrile monomer and an acrylamide monomer. The mass ratio of the acrylate monomer, the acrylonitrile monomer and the acrylamide monomer is in the range of 100:(1-80):(1-20). Preferably, when the ratio is 100:(20-60):(5-15), the bonding effect is better.

[0041] The present application also provides a method for preparing a binder for a secondary battery, comprising:

[0042] Mixing water, an emulsifier, an initiator, and monomers constituting the first polymer, stirring, and heating for reaction to obtain a first polymer emulsion;

[0043] The first polymer emulsion and the second polymer are mixed and stirred, and then spray-dried to obtain a binder.

[0044] In the present application, a first polymer emulsion is obtained by emulsion polymerization, and a binder is obtained by spray drying.

[0045] The binder particles are secondary particles containing primary particles of a first polymer and primary particles of a second polymer. In this way, the second polymer serves as a skeleton to support the first polymer. When the binder is prepared into a slurry and coated on the diaphragm, the first polymer is bonded to the diaphragm through the second polymer. After the slurry on the diaphragm is dried, the second polymer forms a network structure, which supports and connects the first polymer and bonds the first polymer particles to the diaphragm.

[0046] An embodiment of the present application provides a separator, which includes the aforementioned binder for a secondary battery or an adhesive prepared by the aforementioned method for preparing the binder for a secondary battery.

[0047] An embodiment of the present application provides a battery cell, which includes the separator as described above.

[0048] An embodiment of the present application provides a battery, which includes the above-mentioned battery cell.

[0049] An embodiment of the present application provides an electrical device, which includes the above-mentioned battery cell or the above-mentioned battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.

[0051] FIG1 is a scanning electron microscope image of the adhesive provided in Example 1 of the present application;

[0052] FIG2 is a partially enlarged schematic diagram of the adhesive in Example 1 of FIG1 ;

[0053] FIG3 is a schematic structural diagram of the improved diaphragm according to an embodiment of the present application;

[0054] FIG4 is a schematic flow chart of a method for preparing a binder for a secondary battery provided in an embodiment of the present application;

[0055] FIG5 is a schematic diagram of an electrode assembly provided in an embodiment of the present application;

[0056] FIG6 is an exploded view of the electrode assembly provided by the embodiment of the present application shown in FIG5 ;

[0057] FIG7 is a schematic diagram of a battery module provided in an embodiment of the present application;

[0058] FIG8 is a schematic diagram of a battery pack provided in an embodiment of the present application;

[0059] FIG9 is an exploded view of the battery pack provided by the embodiment of the present application shown in FIG8 ;

[0060] FIG10 is a schematic diagram of an electrical device provided in an embodiment of the present application.

[0061] Description of Figure Numbers:

[0062] The realization of the objectives, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0063] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0064] Below, the binder and its preparation method of the present application, as well as the embodiments of the diaphragm, electrode assembly, battery cell, battery and electrical device containing the binder are described in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0065] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0066] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0067] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0068] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0069] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0070] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0071] The battery cell has a problem of large openings, that is, a gap is easily formed between the electrode and the diaphragm, resulting in poor battery cycle performance.

[0072] The commonly used adhesive on the diaphragm is polyvinylidene fluoride, but the price of polyvinylidene fluoride has increased sharply at this stage, and the market supply is tight. At the same time, a hot pressing process is required to make the diaphragm and the electrode tightly bonded; but as production speeds up, the hot pressing process will gradually be replaced by the cold pressing process. The cold pressing of the battery electrode refers to the shaping of the core to reduce the elasticity of the battery cell, improve the qualified rate of the core installation and ensure the consistency of the thickness of the finished battery cell.

[0073] The bonding force between the positive and negative pole pieces and the separator is insufficient, which often leads to problems such as cell opening. At the same time, the wettability to the electrolyte is poor, which cannot meet the performance requirements of the secondary battery for the coated separator. The separator fits tightly to the pole piece, which can improve the discharge capacity of the battery, reduce internal resistance, reduce polarization loss, extend the cycle life of the battery, and improve the utilization rate of the secondary battery.

[0074] It is understandable that the battery cell is formed by bonding the positive electrode sheet, the negative electrode sheet and the separator. The battery cell has a certain hardness. That is, because the bonded positive and negative electrode sheets and the separator adhere to each other and support each other, a structure with a certain thickness is formed. A structure with a certain thickness has a certain hardness. The negative electrode will expand during the charge and discharge process. When the bonding force is weak, a gap is easily formed between the positive and negative electrode sheets and the separator, making it difficult for the positive and negative electrode sheets and the separator to adhere to each other and support each other, resulting in the battery cell becoming loose and the hardness becoming lower. At this time, the power performance of the battery cell will deteriorate, for example, the rate performance will be reduced, and at the same time, the cycle performance will deteriorate. For example, in electric vehicles, the battery cell becomes loose, resulting in a slower battery charging speed and a deterioration in the battery cycle performance, which directly shortens the battery life. Electric vehicles require frequent battery replacement, and consumers spend more on electric vehicles.

[0075] Based on this, the present application proposes a binder for a secondary battery, the binder including a first polymer and a second polymer, the first polymer including an acrylic ester copolymer, and the second polymer including a water-soluble polymer.

[0076] Binder refers to a material with adhesive properties that is used to bond different substances together.

[0077] Acrylate copolymers are a general term for polymers produced by copolymerization of acrylate monomers and other comonomers.

[0078] The acrylic ester monomer has an acrylate group in its structure, for example, methyl acrylate, ethyl acrylate, and n-butyl acrylate.

[0079] Acrylate copolymers have good adhesion. The use of acrylic copolymers can improve the adhesion between the diaphragm and the electrode after cold pressing.

[0080] Water-soluble polymer is a hydrophilic high molecular material that can dissolve or swell in water to form a solution or dispersion. In the dry state, it is non-sticky.

[0081] The binder includes a first polymer and a second polymer, the first polymer includes an acrylic copolymer, and the second polymer includes a water-soluble polymer. When the binder is applied to the diaphragm, the water-soluble polymer serves as a support to support the first polymer, connects the first polymer to the water-soluble polymer, and bonds the first polymer to the diaphragm. Specifically, in the process of applying the binder to the diaphragm, the binder and water are mixed to form a slurry, and then the slurry is applied to the diaphragm. The water-soluble polymer has adhesiveness after contacting water, and the water-soluble polymer can bond to the diaphragm. The water-soluble polymer can bond the first polymer (including the acrylic copolymer) to the diaphragm. The acrylic copolymer and / or the water-soluble polymer in the binder can partially penetrate into the pores of the diaphragm to achieve bonding with the diaphragm. When After the slurry is dried, due to the volatilization of water, the water-soluble polymer molecules are entangled with each other, and the molecules interact with each other, thereby forming a network structure, which supports and connects the first polymer (including acrylic copolymers) and bonds the first polymer particles to the diaphragm. The slurry layer becomes an adhesive layer after drying. The adhesive layer has a side facing the diaphragm and a side facing away from the diaphragm. During the slurry coating process, the water-soluble polymer can be bonded to the diaphragm, or the acrylic copolymer and / or water-soluble polymer in the adhesive can partially penetrate into the pores of the diaphragm to achieve bonding with the diaphragm. Therefore, the adhesive layer is bonded to the diaphragm. Since the acrylic copolymer and the water-soluble polymer have no stickiness after drying, the side of the adhesive layer facing away from the diaphragm has no stickiness, which facilitates the winding and unwinding of the diaphragm.

[0082] When the adhesive is cold-pressed after being wound with the positive and negative electrode sheets, the adhesive has better bonding strength, so that the positive and negative electrode sheets and the diaphragm are tightly attached to each other. Specifically, after cold pressing, the bonding strength is mainly provided by the mechanical interlocking effect of the acrylic copolymer and water-soluble polymer in the adhesive penetrating into the pores of the electrode sheets, as well as the intermolecular force of the acrylic copolymer. Therefore, the adhesive of the present application improves the cold-pressing bonding strength between the diaphragm and the positive and negative electrode sheets, reduces problems such as cell opening and soft cells, thereby improving the hardness of the cell. At the same time, the adhesive is coated on the diaphragm and applied to the secondary battery, which improves the dynamic performance of the secondary battery, reduces the electrochemical impedance, and can improve the rate performance and battery cycle performance of the secondary battery.

[0083] That is, the water-soluble polymer has adhesiveness after being dissolved in water, the slurry is coated on the diaphragm, the water-soluble polymer can be bonded to the diaphragm, the acrylic copolymer and / or water-soluble polymer in the adhesive can partially penetrate into the pores of the diaphragm, so that the acrylic copolymer and water-soluble polymer in the adhesive are bonded to the diaphragm, that is, as shown in Figure 3, the side 21 of the adhesive layer 20 facing the diaphragm is bonded to the diaphragm 10.

[0084] After drying, the side 23 of the adhesive layer 20 facing away from the diaphragm has no adhesiveness, which facilitates the winding of the diaphragm. When the electrode is placed on the surface of the adhesive layer and cold pressed, part of the acrylic copolymer and / or water-soluble polymer in the adhesive further penetrates into the pores of the diaphragm and the electrode, and forms intermolecular forces with the molecules on the diaphragm and the electrode, effectively bonding the diaphragm and the electrode through the adhesive.

[0085] In one embodiment, the mass ratio of the first polymer to the second polymer is 1:(0.1-10); preferably, 1:(0.2-5).

[0086] The binder includes a first polymer and a second polymer. The mass of the first polymer is defined as M1, the mass of the second polymer is defined as M2, and the mass ratio of the first polymer to the second polymer is defined as M1:M2.

[0087] The mass ratio is tested by recording the mass M1 of the first polymer and the mass M2 of the second polymer during the preparation of the binder. The mass ratio of the first polymer to the second polymer is M1:M2.

[0088] Setting the mass ratio of the first polymer to the second polymer within the above range can help the bonding layer form a continuous network structure, bond the first polymer to the separator, and improve the bonding property of the bonding layer at room temperature.

[0089] That is, as the amount of the second polymer increases, the bonding strength of the bonding layer increases first and then decreases. By controlling the quality of the first polymer and the second polymer within the above range, the bonding strength of the adhesive applied to the diaphragm can be effectively improved.

[0090] In the above 1:(0.1~10), the values ​​include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1:0.1, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, etc., as well as the range values ​​between any two of the above point values.

[0091] In the above 1:(0.2~5), the values ​​include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1:0.2, 1:1, 1:2, 1:3, 1:4, 1:5, etc., as well as the range values ​​between any two of the above point values.

[0092] In one embodiment, the second polymer includes one or more of polyacrylamide, polyacrylic acid, polyvinyl pyrrolidone, polyvinyl alcohol, polyethylene glycol, polymaleic anhydride, and polyethyleneimine.

[0093] The second polymer includes the above-mentioned water-soluble polymers. These water-soluble polymers contain hydrophilic groups and a certain number of hydrophobic groups, and thus have a certain surface activity, which can reduce the surface tension of water to a certain extent and improve the solubility and dispersion properties of the binder in the aqueous phase. That is, when preparing a slurry for the diaphragm, the water-soluble polymer is used to control the viscosity and rheological properties of the slurry, so that the binder is better dispersed and suspended. In addition, the second polymer also has a chemical reaction function (for example, a carboxyl group, a hydroxyl group, etc. that reacts with other groups). The polar groups on the water-soluble polymer structure can form hydrogen bonds with the first polymer and the diaphragm and the electrode, thereby improving the bonding force between the diaphragm and the electrode.

[0094] In one embodiment, the volume particle size distribution Dv50 of the binder is 1 μm to 15 μm; preferably, 3 μm to 12 μm.

[0095] Dv50: Among the sample particles, 50% of the total volume of the particles have a particle size larger than this value, and another 50% of the total volume of the particles have a particle size smaller than this value; Dv50 can represent the median particle size of the sample.

[0096] The volume average particle size Dv50 of the adhesive can be measured using methods known in the art. For example, GB / T 19077-2016 can be used for characterization testing using a Malvern laser particle size analyzer, such as a Malvern Mastersizer-3000.

[0097] Theoretically, the volume average particle size Dv50 of the binder in this application can be lower than 1 μm or higher than 15 μm. However, considering that the binder in this application is used on the diaphragm, the volume average particle size Dv50 of the binder is set within the above range to improve the problem of the binder blocking the pores of the diaphragm, reducing the problem of lithium ions (taking lithium-ion batteries as an example, of course, other types of secondary batteries) passing through the diaphragm, and improving the problem of the binder being coated on the diaphragm to form a thicker coating, which affects the energy density of the battery prepared later. Therefore, the volume particle size distribution Dv50 of the binder is 1 μm to 15 μm; preferably, 3 μm to 12 μm.

[0098] In the above-mentioned 1μm to 15μm, the values ​​include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0099] In the above-mentioned 3μm to 12μm, the values ​​include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0100] It can be understood that, as shown in Figures 1 and 2, the binder particles are secondary particles containing primary particles of a first polymer and primary particles of a second polymer. In this way, the second polymer serves as a skeleton. When the binder slurry is applied to the diaphragm, the second polymer plays a role in supporting and connecting the first polymer, bonding the first polymer to the diaphragm. After the slurry is dried to form a bonding layer, the bonding layer can bond to the diaphragm, but the side of the bonding layer facing away from the diaphragm has no bonding force, which facilitates the winding and unwinding of the diaphragm. Moreover, when the diaphragm and the positive and negative pole pieces are wound and then cold pressed, after being squeezed, the first polymer and the second polymer can be deformed by force and penetrate into the pores of the diaphragm and the pole piece, thereby achieving a bonding effect.

[0101] In one embodiment, the shape of the binder includes a spherical shape.

[0102] Theoretically, the shape of the binder in this application is not limited, for example, it can be spherical, rod-shaped, etc. Considering that the spherical shape is conducive to uniform dispersion during the stirring process of the slurry and is conducive to uniform coating, the spherical shape is preferably included.

[0103] In one embodiment, the first polymer includes an acrylate monomer, and the structure of the acrylate monomer includes:

[0104] Wherein, R1 includes a hydrogen atom or an alkyl group of 1 to 12 carbon atoms, and R2 includes an alkyl group of 1 to 12 carbon atoms.

[0105] Acrylate monomers include unsaturated ester groups, which can improve the polymer's anti-swelling ability. As a flexible monomer segment in the molecular chain, it can adjust the polymer's glass transition temperature, improve the toughness of the adhesive during application, and help to achieve good bonding.

[0106] In one embodiment, the acrylic acid ester monomer includes one or more of methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate.

[0107] Theoretically, this application does not limit the types of acrylate monomers, as long as the acrylate monomers satisfy the above structure, that is, the acrylate monomers include the above-listed substances and substances not listed in this application.

[0108] By using any one or more of the above-mentioned acrylic ester monomers, the glass transition temperature of the polymer can be adjusted and the anti-swelling ability of the polymer can be improved.

[0109] In one embodiment, the first polymer includes an acrylonitrile monomer, and the structure of the acrylonitrile monomer includes:

[0110] Wherein, R3 includes a hydrogen atom or an alkyl group of 1 to 6 carbon atoms.

[0111] The unsaturated cyano group in the structure of acrylonitrile monomers helps to improve ionic conductivity and enhance adhesion.

[0112] In one embodiment, the acrylonitrile monomer includes one or more of acrylonitrile and methacrylonitrile.

[0113] Theoretically, this application does not limit the types of acrylonitrile monomers, as long as the acrylonitrile monomers satisfy the above structure, that is, the acrylonitrile monomers include the above-listed substances and substances not listed in this application.

[0114] The use of any one or more of the above-mentioned acrylonitrile monomers can improve the ionic conductivity of the binder.

[0115] In one embodiment, the first polymer includes an acrylamide monomer, and the structure of the acrylamide monomer includes:

[0116] wherein R4 comprises a hydrogen atom or an alkyl group of 1 to 6 carbon atoms, and R5 comprises a hydrogen atom, an alkyl group of 1 to 6 carbon atoms substituted with a hydroxyl group, or an alkoxy group of 1 to 6 carbon atoms.

[0117] The third unit includes an unsaturated amide group, which plays a cross-linking role and also has good adhesion.

[0118] In one embodiment, the acrylamide monomer includes one or more of acrylamide, N-methylol acrylamide, and N-butoxymethyl acrylamide.

[0119] Theoretically, this application does not limit the types of acrylamide monomers, as long as the acrylamide monomers meet the above structure, that is, acrylamide monomers include the above-listed substances and substances not listed in this application.

[0120] The use of any one or more of the above-mentioned acrylamide monomers can play a role in regulating the molecular weight, so as to adjust the molecular weight of the polymer. The molecular weight of the adhesive is helpful to improve the adhesiveness within a certain range.

[0121] It is understood that the constituent monomers of the first polymer may include one, two, or three of the above three monomers, without limitation. It is understood that when the three monomers are used simultaneously to prepare the first polymer, the bonding performance of the first polymer is better.

[0122] Commonly used polyvinylidene fluoride adhesives require a hot pressing process to achieve better bonding effects. As production speeds up and capacity is reduced, hot pressing will gradually be replaced by cold pressing. After the battery cell is wound, it undergoes a cold pressing process. Since conventional polyvinylidene fluoride is a homopolymer with a crystallinity of approximately 50%, the adhesion between the separator and the positive and negative electrodes is insufficient. Traditional polyacrylate adhesives also do not meet the required adhesion under cold pressing, often resulting in problems such as cell opening and soft cells. At the same time, their poor wettability with the electrolyte cannot meet the performance requirements of the coated separator for secondary batteries.

[0123] The adhesive comprises an acrylic copolymer and a water-soluble polymer prepared from the above monomers, so that the adhesive has good adhesiveness.

[0124] In one embodiment, the first polymer includes acrylate monomers, acrylonitrile monomers and acrylamide monomers, and the mass ratio of acrylate monomers, acrylonitrile monomers and acrylamide monomers is in the range of 100:(1-80):(1-20), preferably, 100:(20-60):(5-15).

[0125] In order to improve the comprehensive performance of the first polymer, the first polymer includes acrylate monomers, acrylonitrile monomers and acrylamide monomers, and the mass ratio of acrylate monomers, acrylonitrile monomers and acrylamide monomers is in the range of 100: (1 to 80): (1 to 20). Preferably, when the ratio is 100: (20 to 60): (5 to 15), the bonding effect is better.

[0126] In the above 100:(1~80):(1~20), the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 100:1:1, 100:10:1, 100:30:1, 100:50:1, 100:80:1, 100:10:5, 100:10:10, 100:10:20, 100:30:10, 100:30:20, 100:50:20, 100:80:20, etc., as well as the range values ​​between any two of the above point values.

[0127] In the above 100:(20~60):(5~15), the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 100:20:5, 100:30:10, 100:60:15, etc., as well as the range values ​​between any two of the above point values.

[0128] The present application also provides a method for preparing a binder for a secondary battery, comprising: blending and stirring water, an emulsifier, an initiator, and monomers constituting a first polymer, and heating the mixture for reaction to obtain a first polymer emulsion;

[0129] The first polymer emulsion and the second polymer are mixed and stirred, and then spray-dried to obtain a binder.

[0130] In the present application, a first polymer emulsion is obtained by emulsion polymerization, and a binder is obtained by spray drying.

[0131] Emulsion polymerization is a process in which monomers are dispersed in water with the help of emulsifiers and mechanical stirring to form an emulsion, and then an initiator is added to initiate monomer polymerization.

[0132] Emulsifiers are substances that can transform mutually incompatible oil and water into an emulsion that is difficult to separate. Emulsifiers are usually surfactants that have both hydrophilic polar groups and hydrophobic (lipophilic) non-polar groups.

[0133] Initiators are substances that can initiate polymerization reactions of monomers. For example, free radical initiators are compounds that readily decompose into free radicals (i.e., primary free radicals) upon exposure to heat. They can be used to initiate free radical polymerization and copolymerization reactions of olefins and dienes.

[0134] Water, emulsifier, initiator, and monomers constituting the polymer are blended and stirred. The water and emulsifier are stirred and dispersed to form an emulsion, that is, the emulsifier forms micelles in the aqueous phase, and most of the micelles are solubilized with monomers. Under heating conditions, the initiator initiates polymerization of the monomers inside the micelles to obtain an emulsion.

[0135] Spray drying, through mechanical action, disperses the material to be dried (a mixture of the first polymer emulsion and the second polymer) into very fine mist-like particles (increasing the water evaporation area and accelerating the drying process). When in contact with hot air, most of the water is removed instantly, and the solid matter in the material is dried into powder.

[0136] A binder containing the first polymer and the second polymer is obtained through a spray drying process.

[0137] The present application also provides a separator, comprising the aforementioned secondary battery binder or a separator produced by the aforementioned secondary battery binder production method. Because the binder utilizes all of the technical solutions of all of the aforementioned embodiments, it possesses at least all of the beneficial effects of the technical solutions of the aforementioned embodiments, and therefore will not be further detailed here.

[0138] The diaphragm is coated with the above-mentioned adhesive, which can improve the bonding performance between the pole piece and the adhesive and improve the opening problem of the existing battery cell pre-cold pressing process.

[0139] The embodiments of the present application further provide a battery cell including the above-mentioned separator. Since the separator adopts all the technical solutions of all the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be described in detail here.

[0140] Applying the above-mentioned separator to a battery cell can improve the large-clamp cycle performance of the battery cell.

[0141] The embodiment of the present application further provides a battery, which includes the above-mentioned battery cell. Since the battery cell adopts all the technical solutions of all the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be described in detail here.

[0142] Batteries include battery modules and battery packs.

[0143] The embodiments of the present application further provide an electrical device comprising the aforementioned battery cell or battery. Since the battery cell or battery employs all the technical solutions of all the aforementioned embodiments, it at least has all the beneficial effects brought about by the technical solutions of the aforementioned embodiments, which will not be detailed here.

[0144] In addition, the electrode assembly, battery cell, battery, and electric device of the present application will be described below with appropriate reference to the drawings.

[0145] In one embodiment of the present application, an electrode assembly is provided.

[0146] Typically, an electrode assembly includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery's charge and discharge process, active ions are embedded in and released from the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. The separator is located between the positive and negative electrodes, primarily preventing a short circuit between the positive and negative electrodes while allowing ions to pass through. The separator is the separator described above in this application.

[0147] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector.

[0148] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0149] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0150] In some embodiments, when the electrode assembly is a lithium-ion battery, the positive electrode active material may be a positive electrode active material for lithium-ion batteries that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0151] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0152] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0153] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0154] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.

[0155] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0156] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0157] In some embodiments, the negative electrode active material may adopt the negative electrode active material for batteries known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may include at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may include at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0158] In some embodiments, the negative electrode film layer may further optionally include a binder. The binder may include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0159] In some embodiments, the negative electrode film layer may further include a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0160] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0161] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0162] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. This application has no specific restrictions on the type of electrolyte, and it can be selected according to needs.

[0163] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0164] In some embodiments, the electrolyte salt may include at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium bisoxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0165] In some embodiments, the solvent may include at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.

[0166] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0167] In some embodiments, the electrode assembly further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0168] In some embodiments, the material of the separator may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.

[0169] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0170] In some embodiments, the electrode assembly may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0171] In some embodiments, the outer packaging of the electrode assembly may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the electrode assembly may be a soft shell, such as a bag-type soft shell. The soft shell may be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0172] The present application has no particular limitation on the shape of the electrode assembly, which may be cylindrical, square, or any other shape. For example, FIG5 shows a secondary battery 5 having a square structure as an example.

[0173] In some embodiments, referring to Figure 6, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the diaphragm can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0174] In some embodiments, the electrode assemblies may be assembled into a battery module. The number of electrode assemblies contained in the battery module may be one or more. The specific number may be selected by those skilled in the art based on the application and capacity of the battery module.

[0175] Figure 7 shows an example battery module 4. Referring to Figure 7 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured together using fasteners.

[0176] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0177] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0178] Figures 8 and 9 illustrate an example battery pack 1. Referring to Figures 8 and 9 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be positioned over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0179] In addition, the present application also provides an electrical device, which includes at least one of the electrode assembly, battery module, or battery pack provided in the present application. The electrode assembly, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0180] As an electrical device, an electrode assembly, battery module or battery pack can be selected according to its usage requirements.

[0181] Figure 10 shows an example of an electric device. This device can be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the electrode assembly, a battery pack or battery module can be used.

[0182] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use an electrode assembly as a power source.

[0183] Example

[0184] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0185] Preparation of the first polymer emulsion

[0186] Preparation Example 1

[0187] According to the mass ratio of the three monomers of 100:1:10, methyl acrylate, acrylonitrile, and acrylamide were weighed respectively and the monomers were mixed evenly. 200g of the mixed monomers, 5g of sodium lauryl sulfate emulsifier, 1.8g of ammonium persulfate initiator, and 260g of deionized water were added to a 1000mL four-necked flask equipped with a mechanical stirrer, a thermometer, and a condenser, and emulsified at high speed for 30min. Under nitrogen protection, the temperature was raised to 75°C for reaction for 4h, then the temperature was lowered to below 40°C, the pH was adjusted to neutral with aqueous ammonia, and the material was filtered to obtain the first polymer emulsion preparation example 1.

[0188] Preparation Example 2 to Preparation Example 12

[0189] On the basis of Preparation Example 1, the monomer types and mass ratios were adjusted to obtain Preparation Examples 2 to 12.

[0190] Example 1

[0191] Preparation of binder

[0192] The first polymer and the second polymer were weighed and added in a weight ratio of 1:1, and deionized water was added to adjust the solid content of the system to 20%. After stirring and mixing, the membrane adhesive was prepared by spray drying. The spray drying process conditions were an inlet air temperature of 110°C and an outlet air temperature of 50°C.

[0193] Example 2 to Example 24

[0194] On the basis of Example 1, the types and weight ratios of the first polymer and the second polymer were adjusted to obtain Examples 2 to 24.

[0195] Comparative Example 1

[0196] On the basis of Example 1, only the second polymer was used to prepare the adhesive.

[0197] Comparative Example 2

[0198] Based on Example 7, only the first polymer was used to prepare the adhesive.

[0199] Preparation of cells and batteries

[0200] Preparation of diaphragm

[0201] A commercially available PE microporous film with a thickness of 7 μm and an average pore size of 80 nm (from Zhuo Gao Electronic Technology Co., Ltd.) was used as the substrate. The membrane binder prepared above was stirred and mixed uniformly in deionized water to obtain a slurry (solid content of 20%). The slurry was sprayed onto both surfaces of the substrate and dried to remove the solvent. The coating density of the coating composition on the substrate was 1.5 g / m 2 , and obtain a diaphragm.

[0202] Preparation of positive electrode

[0203] Polyvinylidene fluoride (PVDF), lithium iron phosphate (LFP), conductive carbon black, and N-methylpyrrolidone (NMP) were mixed in a mass ratio of 1.2:58.38:0.42:40 and stirred thoroughly to prepare a positive electrode slurry. 2 The loading amount is evenly coated on the positive electrode current collector aluminum foil, and then dried, cold pressed and cut to obtain the positive electrode sheet.

[0204] Preparation of negative electrode sheet

[0205] Artificial graphite, conductive agent acetylene black, binder styrene butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC-Na) were added into deionized water in a mass ratio of 96.2:1.0:1.6:1.2, and stirred thoroughly to prepare a negative electrode slurry (solid content of 63%). 2 The loading amount is coated on the negative electrode current collector copper foil, and then dried, cold pressed and cut to obtain the negative electrode sheet.

[0206] Preparation of electrolyte

[0207] At 25°C, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain a mixed solvent, and then LiPF6 is dissolved in the above mixed solvent to obtain an electrolyte, wherein the concentration of LiPF6 is 1 mol / L.

[0208] Preparation of secondary batteries

[0209] The positive electrode sheets, separators, and negative electrode sheets are stacked in sequence, wound, and cold-pressed (during which the separators and the electrodes are bonded) to obtain a battery cell; the battery cell is placed in an outer package, and the above-prepared electrolyte is added. After packaging, standing, formation, aging, and other processes, a secondary battery is obtained.

[0210] Performance Testing

[0211] Cold press adhesion test:

[0212] The battery negative electrode and separator were stacked together and placed on a hot press. Pressing parameters were set at 25°C, 7t, and 30s to produce a bonded separator / positive electrode sample. The separator / electrode sample was cut into 150mm x 20mm rectangular strips. The electrode side of the strip was affixed to a steel plate using double-sided tape. At one end of the strip, the separator and electrode were separated by 2cm along the length to produce the test specimen.

[0213] The steel plate was held horizontally and secured with the lower clamp of a universal testing machine (Xie Qiang Instrument Manufacturing (Shanghai) Co., Ltd., Model CTM2100). The peeled end of the separator, as described above, was secured with the upper clamp of the universal testing machine and connected to a tensile testing machine. The test conditions were set to a tensile rate of 20 mm / min and a horizontal pull of 10 cm. Once the tensile force stabilized, the tensile force was recorded. The ratio of the tensile force to the sample width was used to determine the adhesion strength between the separator and the electrode.

[0214] EIS data (electrochemical impedance spectroscopy):

[0215] Using a Shanghai Chenhua CHI660D electrochemical workstation, a small-amplitude sinusoidal voltage signal with a frequency of W1 is applied to the battery system. The system generates a sinusoidal current response with a frequency of W2. The change in the ratio of the excitation voltage to the response current is the impedance spectrum of the electrochemical system. In the AC impedance test, the test frequency range is 10mHz to 100kHz, with an amplitude of 5mV. This test can obtain information such as the real and imaginary parts of the impedance at different frequencies.

[0216] Rate performance of lithium-ion batteries:

[0217] Using Wuhan Jinnuo Electronics' CT-2001 A LAND battery testing system, the testing environment is room temperature 25°C, the voltage range is 2.5-3.65V, and the test battery assembled with the prepared electrode material is subjected to 5 constant current charge and discharge cycles at rates of 0.2C, 0.5C, 1C, 2C, 5C, and 0.2C, respectively. The specific process is 0.2C (cycle 5 times, with the capacity of the 5th time being recorded as C1), and then 0.5C (cycle 5 times), 1C (cycle 5 times), 2C (cycle 5 times), 5C (cycle 5 times), 0.2C (cycle 5 times, with the capacity of the 5th time being recorded as C2), that is, the battery capacity after 5 constant current charge and discharge cycles at 0.2C for the first time is recorded as C1, and the battery capacity after 5 constant current charge and discharge cycles at 0.2C for the second time is recorded as C2, and the rate performance P=(C2 / C1)×100%.

[0218] Table 1 Preparation parameters of the first polymer emulsion

[0219] Table 2 Preparation parameters of diaphragm binder

[0220] Table 3 Performance test parameters

[0221] The first polymer is prepared by suitable monomers, the mass ratio of the first polymer to the second polymer is regulated within a suitable range, and a binder is obtained through a spray drying process. The obtained binder has good bonding properties within a suitable range and is applied to the diaphragm, which is beneficial to improving the performance of the battery.

[0222] The above is only a preferred embodiment of the present application and does not limit the patent scope of the present application. All equivalent structural transformations made based on the contents of the present application specification and drawings, or direct / indirect application in other related technical fields, are included in the patent protection scope of the present application.

Claims

1. A binder for a secondary battery, wherein: The binder includes a first polymer and a second polymer, wherein the first polymer includes an acrylic copolymer, and the second polymer includes a water-soluble polymer.

2. The binder for secondary batteries according to claim 1, wherein The mass ratio of the first polymer to the second polymer is 1:(0.1-10); preferably, 1:(0.2-5).

3. The binder for secondary batteries according to claim 1 or 2, wherein The second polymer includes one or more of polyacrylamide, polyacrylic acid, polyvinyl pyrrolidone, polyvinyl alcohol, polyethylene glycol, polymaleic anhydride, and polyethylene imine.

4. The secondary battery binder according to any one of claims 1 to 3, wherein The volume particle size distribution Dv50 of the binder is 1 μm to 15 μm; preferably, 3 μm to 12 μm.

5. The secondary battery binder according to any one of claims 1 to 4, wherein The shape of the binder includes a spherical shape.

6. The binder for secondary batteries according to any one of claims 1 to 5, wherein The first polymer includes an acrylate monomer, and the structure of the acrylate monomer includes: Among them, R1 includes a hydrogen atom or an alkyl group of 1 to 12 carbon atoms, and R2 includes an alkyl group of 1 to 12 carbon atoms.

7. The binder for secondary batteries according to claim 6, wherein The acrylic acid ester monomers include one or more of methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-propyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate.

8. The secondary battery binder according to any one of claims 1 to 7, wherein The first polymer includes an acrylonitrile monomer, and the structure of the acrylonitrile monomer includes: Here, R3 includes a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

9. The binder for secondary batteries according to claim 8, wherein The acrylonitrile monomer includes one or more of acrylonitrile and methacrylonitrile.

10. The secondary battery binder according to any one of claims 1 to 9, wherein The first polymer includes an acrylamide monomer, and the structure of the acrylamide monomer includes: Among them, R4 includes a hydrogen atom or an alkyl group of 1 to 6 carbon atoms, and R5 includes a hydrogen atom, an alkyl group of 1 to 6 carbon atoms substituted with a hydroxyl group, or an alkoxy group of 1 to 6 carbon atoms.

11. The binder for secondary batteries according to claim 10, wherein The acrylamide monomers include one or more of acrylamide, N-hydroxymethyl acrylamide and N-butoxymethyl acrylamide.

12. The secondary battery binder according to any one of claims 1 to 11, wherein The first polymer includes acrylate monomers, acrylonitrile monomers and acrylamide monomers, and the mass ratio of the acrylate monomers, the acrylonitrile monomers and the acrylamide monomers is in the range of 100:(1-80):(1-20), preferably, 100:(20-60):(5-15).

13. A method for preparing a secondary battery binder according to any one of claims 1 to 12, wherein: include: Mixing water, an emulsifier, an initiator, and monomers constituting the first polymer, stirring, and heating for reaction to obtain a first polymer emulsion; The first polymer emulsion and the second polymer are mixed and stirred, and then spray-dried to obtain a binder.

14. A diaphragm, wherein: The separator includes the binder for a secondary battery according to any one of claims 1 to 12 or the binder prepared by the method for preparing the binder for a secondary battery according to claim 13 .

15. A battery cell, wherein: The battery cell includes the separator according to claim 14 .

16. A battery, wherein: The battery comprises the battery cell as claimed in claim 15 .

17. An electrical device, wherein: The electrical device comprises the battery cell according to claim 15 or the battery according to claim 16 .

Citation Information

Patent Citations

  • Porous membrane for secondary battery, slurry for secondary battery porous membrane and secondary battery

    CN103403919A

  • Acrylonitrile copolymer adhesive and application thereof in lithium ion batteries

    CN106220779A

  • Lithium ion battery cathode binder

    CN109378478A

  • Diaphragm slurry, preparation method and application thereof

    CN112259913A

  • Water-based binder, modified diaphragm, battery and preparation method of water-based binder

    CN115260403A