Grain-oriented electromagnetic steel sheet and method for forming insulating coating
The grain-oriented electrical steel sheet with a crystalline metal phosphate intermediate layer and tension coating layer on grooved base steel plates addresses the challenge of improving adhesion and magnetic properties, ensuring effective coating tension and corrosion resistance.
Patent Information
- Application Number
- PCT/JP2024/014842
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-17
AI Technical Summary
It is challenging to simultaneously improve film adhesion and magnetic properties in grain-oriented electrical steel sheets without a forsterite-based coating, as existing methods often result in compromised coating tension, corrosion resistance, and elution properties.
A grain-oriented electrical steel sheet with grooves formed on the base steel plate, featuring an insulating coating comprising a crystalline metal phosphate intermediate layer and a tension coating layer, applied under specific processing conditions to enhance adhesion and maintain magnetic properties.
The solution achieves excellent film adhesion, magnetic properties, and sufficient coating tension, corrosion resistance, and elution properties, making it suitable for high-performance applications.
Smart Images

Figure JP2024014842_17102024_PF_FP_ABST
Abstract
Description
Grain-oriented electrical steel sheet and method for forming insulating coating
[0001] The present invention relates to a grain-oriented electrical steel sheet and a method for forming an insulating coating on the grain-oriented electrical steel sheet.This application claims priority based on Japanese Patent Application No. 2023-065385, filed on April 13, 2023, the contents of which are incorporated herein by reference.
[0002] Grain-oriented electrical steel sheets are primarily used in transformers. Transformers are continuously excited over a long period of time, from installation to disposal, and continue to generate energy loss. Therefore, the energy loss during magnetization with AC, i.e., core loss, is a major indicator that determines the performance of a transformer.
[0003] To reduce the iron loss of grain-oriented electrical steel sheets, many technologies have been developed to date, including (a) increasing the concentration in the {110}<001> orientation (Goss orientation), (b) increasing the content of solid solution elements such as Si to increase the electrical resistance of the steel sheet, or (c) reducing the thickness of the electrical steel sheet.
[0004] Furthermore, applying tension to steel sheets is effective in reducing iron loss. Forming a coating made of a material with a smaller thermal expansion coefficient than the steel sheet at high temperatures on the steel sheet surface is an effective means for reducing iron loss. A forsterite-based coating (inorganic coating) with excellent coating adhesion is produced by the reaction of oxides on the steel sheet surface with an annealing separator during the finish annealing process of electrical steel sheets. This coating can apply tension to steel sheets.
[0005] For example, the method disclosed in Patent Document 1, in which a coating solution mainly composed of colloidal silica and phosphate is baked onto the surface of a steel sheet to form an insulating coating, is an effective method for reducing iron loss because it is highly effective in applying tension to the steel sheet. Therefore, a common method for producing grain-oriented electrical steel sheets is to leave the forsterite-based coating formed in the final annealing process and then apply an insulating coating mainly composed of phosphate on top of it.
[0006] However, in recent years, there has been an increasing demand for smaller and higher-performance transformers. To achieve this, grain-oriented electrical steel sheets are required to have excellent high-field iron loss characteristics, i.e., good iron loss even at high magnetic flux densities. At the same time, it has become clear that forsterite-based coatings hinder domain wall movement, adversely affecting iron loss. In grain-oriented electrical steel sheets, magnetic domains change due to domain wall movement under an AC magnetic field. Smooth and rapid domain wall movement is effective in reducing iron loss. However, forsterite-based coatings are themselves nonmagnetic and have an uneven structure at the interface between the steel sheet and the coating. This uneven structure is thought to hinder domain wall movement and adversely affect iron loss. Therefore, as means for improving high magnetic field iron loss, research has been conducted on a variety of techniques, including methods for removing the forsterite-based coating by mechanical means such as polishing or chemical means such as pickling, techniques for producing grain-oriented electrical steel sheets that do not have a forsterite-based coating by preventing the formation of a forsterite-based coating during high-temperature finish annealing, and techniques for making the steel sheet surface mirror-finished (in other words, techniques for magnetically smoothing the steel sheet surface).
[0007] As a technique for preventing the formation of a forsterite-based coating, for example, Patent Document 2 discloses a technique in which, after normal finish annealing, the steel sheet is pickled to remove surface deposits, and then chemically or electrolytically polished to a mirror finish. It has been found that forming a tensioned insulating coating on the surface of a grain-oriented electrical steel sheet that does not have a forsterite-based coating and that has been obtained by such a known method can provide an even more excellent iron loss improvement effect. Furthermore, the tensioned insulating coating can impart various properties, such as corrosion resistance, heat resistance, and slip resistance, in addition to improving iron loss.
[0008] However, in addition to exhibiting insulating properties, forsterite-based coatings also function as intermediate layers that ensure adhesion when forming tension coatings (tension-applying insulating coatings). That is, because forsterite-based coatings are formed in a state where they penetrate deeply into the steel sheet, they have excellent adhesion to the metal steel sheet. Therefore, when a tension-applying coating (tension coating) containing colloidal silica, phosphate, or the like as a main component is formed on the surface of a forsterite-based coating, the coating exhibits excellent adhesion. On the other hand, because bonding between metal and oxide is generally difficult, it has been difficult to ensure sufficient adhesion between the tension coating and the steel sheet surface in the absence of a forsterite-based coating. Therefore, when forming a tension coating on a grain-oriented electrical steel sheet that does not have a forsterite-based coating, the provision of a layer that serves as an intermediate layer for the forsterite-based coating has been considered.
[0009] Patent Document 3 discloses a technique for ensuring the adhesion of a tensioned insulating coating by applying an intermediate coating beforehand when forming the tensioned coating. However, the technique disclosed in Patent Document 3 has a problem in that it is not possible to maintain good adhesion of a tensioned insulating coating that has a large tension.
[0010] Furthermore, for example, Patent Document 4 discloses a grain-oriented electrical steel sheet having a base steel sheet and an insulating coating formed on the surface of the base steel sheet, the insulating coating being formed on the side of the base steel sheet, an intermediate layer containing a crystalline metal phosphate, and a tensile coating layer formed on the surface side of the insulating coating. Patent Document 4 shows that the grain-oriented electrical steel sheet does not have a forsterite-based coating, and has excellent coating adhesion, excellent coating tension, and excellent magnetic properties.
[0011] On the other hand, a so-called magnetic domain refining technique is known to improve the magnetic properties of grain-oriented electrical steel sheets, reducing the width of magnetic domains present within the steel sheet. A known method for magnetic domain control, as disclosed in Patent Document 5, involves irradiating the surface of grain-oriented electrical steel sheets after finish annealing with a laser beam to refine magnetic domains and reduce eddy current loss, thereby reducing iron loss. However, this method utilizes the magnetic domain refining phenomenon, which is primarily caused by thermal strain induced in the steel sheet by laser irradiation. Wound cores, which are often used primarily in small and medium-sized transformers, are often manufactured by core manufacturing methods using mechanical bending. In this manufacturing method, stress relief annealing (e.g., at 800°C for approximately 2 to 4 hours) is typically performed after the core shape is machined to eliminate the increase in iron loss due to processing strain induced in the steel sheet by bending. While such stress relief annealing reduces or eliminates the mechanical processing-induced strain induced in the core, the thermal strain induced for magnetic domain refining disappears in steel sheets that have undergone magnetic domain control by laser irradiation. For this reason, grain-oriented electrical steel sheets, which have been subjected to magnetic domain refinement by the introduction of thermal strain, typically by laser irradiation, are generally considered to be unsuitable for wound cores.
[0012] A known magnetic domain control technology that does not lose its magnetic domain control effect even after stress relief annealing is the "groove-introducing magnetic domain control technology," which forms linear grooves periodically in a direction intersecting the rolling direction. When considering application to wound cores, the application of groove-introducing magnetic domain control technology must be a prerequisite.
[0013] The technology disclosed in Patent Document 4 makes it possible to obtain a grain-oriented electrical steel sheet that does not have an inorganic coating and that has excellent coating adhesion, excellent coating tension, and excellent magnetic properties. However, Patent Document 4 does not fully consider strain relief annealing or the formation of grooves. As a result of investigations by the present inventors, it was found that with the method of Patent Document 4, when grooves are formed, the adhesion of the insulating coating in the groove portions is insufficient, and as a result, sufficient improvements in magnetic properties and corrosion resistance after strain relief annealing are not necessarily obtained.
[0014] Japanese Unexamined Patent Publication No. 48-039338 Japanese Unexamined Patent Application No. 49-96920 Japanese Unexamined Patent Application No. 5-279747 International Publication No. 2022 / 215709 Japanese Unexamined Patent Application No. 56-51522
[0015] As described above, in the past, it has not been easy to simultaneously improve coating adhesion and magnetic properties in grain-oriented electrical steel sheets having grooves formed in the base steel sheet and no forsterite-based coating. Therefore, an object of the present invention is to provide a grain-oriented electrical steel sheet having grooves formed in the base steel sheet, which does not have a forsterite-based coating and has excellent coating adhesion and magnetic properties. Another object of the present invention is to provide a method for forming an insulating coating for such grain-oriented electrical steel sheet. However, even if coating adhesion is improved, a decrease in coating tension, corrosion resistance, and elution is undesirable in practical use, so it is assumed that these properties are not reduced.
[0016] The inventors have discovered that in a grain-oriented electrical steel sheet having grooves formed in the base steel sheet, the adhesion of the base steel sheet to the insulating coating can be improved even in the grooved areas by forming a coating on the surface of the base steel sheet under specific processing conditions after the grooves are formed.
[0017] The present invention has been made in light of the above findings. The gist of the present invention is as follows: [1] A grain-oriented electrical steel sheet according to one aspect of the present invention is a grain-oriented electrical steel sheet comprising a base steel sheet and an insulating coating formed on a surface of the base steel sheet, wherein the base steel sheet has a flat portion and grooves extending in a direction at an angle of 45 to 135° with respect to the rolling direction, the grooves having a depth of 10 to 30 μm and a width of 10 to 200 μm, the insulating coating comprising an intermediate layer having a thickness of 0.1 to 15.0 μm and containing a crystalline metal phosphate formed on the base steel sheet side, and a tensile coating layer formed on the surface side of the insulating coating, wherein the base steel sheet is covered with the insulating coating comprising the tensile coating layer and the intermediate layer having a thickness of 0.1 to 9.0 μm over an area ratio of 50% or more of the grooves. [2] In the grain-oriented electrical steel sheet according to [1], the crystalline metal phosphate contained in the intermediate layer may be one or more of zinc phosphate, manganese phosphate, iron phosphate, and zinc calcium phosphate, and the tensile coating layer may contain a metal phosphate and silica, and the content of silica in the tensile coating layer may be 20 to 60 mass %. [3] A method for forming an insulating coating according to another aspect of the present invention is a method for forming the insulating coating provided in the grain-oriented electrical steel sheet according to [1], comprising the steps of: 2 O 3a finish annealing step of applying an annealing separator containing 10 to 100 mass % of the above-mentioned compound to the steel sheet, drying the steel sheet, and then performing finish annealing; an annealing separator removing step of removing excess annealing separator from the steel sheet after the finish annealing step; a groove forming step of forming grooves extending in a direction of 45 to 135° with respect to the rolling direction by using a tooth profile or a laser on the steel sheet before the finish annealing step or after the annealing separator removing step; and a solution of the above-mentioned compound containing 10 to 100 mass % of the above-mentioned compound at a liquid temperature of 30 to 85° C. and a metal phosphate having a concentration of 1.0 to 15.0 mass % and a total concentration of 0.01 to 10.0 mass %. [4] The method for forming an insulating coating according to [3] includes an intermediate layer forming step of immersing a steel sheet for 5 to 90 seconds in a mixed treatment solution containing one or more acids selected from hydrofluoric acid, nitric acid, and phosphoric acid and a concentration of sodium hydroxide, sodium carbonate, or sodium phosphate in a range from 0.01 to 1.50 mass%, rinsing the mixed treatment solution with water to remove the mixed treatment solution, and then drying the steel sheet, and a tensile coating layer forming step of applying a coating solution containing a metal phosphate and colloidal silica to the steel sheet after the intermediate layer forming step, the coating solution containing 30 to 150 parts by mass of colloidal silica per 100 parts by mass of the metal phosphate, drying, and then holding the steel sheet at a sheet temperature of 700 to 950°C for 10 to 90 seconds.
[0018] According to the above aspects of the present invention, it is possible to provide a grain-oriented electrical steel sheet having excellent coating adhesion and magnetic properties, and a method for forming an insulating coating on this grain-oriented electrical steel sheet.
[0019] 1 is a diagram showing a schematic diagram of a grain-oriented electrical steel sheet according to an embodiment of the present invention, and is a diagram showing a cross section taken along line AA in FIG.
[0020] A grain-oriented electrical steel sheet according to one embodiment of the present invention (grain-oriented electrical steel sheet according to this embodiment) and a method for manufacturing the same will be described. As shown in Figures 1 and 2, the grain-oriented electrical steel sheet 1 according to this embodiment has a base steel sheet 11 and an insulating coating 21 formed on the surface of the base steel sheet 11, and the surface of the base steel sheet 11 is substantially free of a forsterite-based coating (sometimes called a glass coating) (this is not intentionally formed). Even if a forsterite-based coating is unintentionally formed and remains, the coating has a density of 0.5 g / m 2 (The details are described below.) In the grain-oriented electrical steel sheet 1 according to this embodiment, the base steel sheet 11 has flat portions 2 and groove portions 3 extending in a direction at an angle of 45 to 135° with respect to the rolling direction RD. In the groove portions 3, 50% or more of an area is covered with an insulating coating 21. The insulating coating 21 has an intermediate layer 211 formed on the base steel sheet 11 side and a tensile coating layer 212 formed on the surface side. Each of these will be described below.
[0021] <Insulating Coating> The insulating coating 21 has an intermediate layer 211 formed on the base steel sheet side, containing a crystalline metal phosphate, and having a thickness of 0.1 to 15.0 μm, and a tensile coating layer 212 formed on the surface side.
[0022] [Intermediate Layer] The intermediate layer is formed on the base steel sheet side of the insulating coating, contains a crystalline metal phosphate, and is a layer (coating) with a thickness of 0.1 to 15.0 μm. However, as described below, the thickness of the intermediate layer in the grooves is 0.1 to 9.0 μm. As described above, grain-oriented electrical steel sheets generally have an inorganic coating (forsterite-based coating) formed in the final annealing process and an insulating coating (tensile insulating coating) formed thereon. However, in recent years, it has become clear that this forsterite-based coating hinders domain wall movement and adversely affects iron loss. Therefore, grain-oriented electrical steel sheets without a forsterite-based coating have been investigated to further improve magnetic properties. However, without a forsterite-based coating, it is difficult to ensure sufficient adhesion between the tensile coating layer and the surface of the base steel sheet.
[0023] In the grain-oriented electrical steel sheet 1 according to this embodiment, an intermediate layer 211 containing a crystalline metal phosphate is formed between the base steel sheet 11 and the tensile coating layer 212, thereby improving adhesion between the base steel sheet 11 and the tensile coating layer 212 via the intermediate layer 211. When the intermediate layer 211 contains a crystalline metal phosphate, the tensile coating formed thereon (which becomes the tensile coating layer 212 after formation) also contains a metal phosphate, resulting in high affinity and excellent adhesion between the intermediate layer 211 and the tensile coating layer 212. Furthermore, when the intermediate layer 211 is formed by immersion in a treatment solution containing a metal phosphate, as described below, it can be formed on the surface of the base steel sheet 11 using a chemical reaction, thereby ensuring adhesion between the intermediate layer 211 and the base steel sheet 11. If the intermediate layer 211 does not contain a crystalline metal phosphate, the above-described effect cannot be obtained. The proportion of the crystalline metal phosphate in the intermediate layer is preferably 80% by mass or more, and may be 100% by mass. In terms of adhesion, the metal phosphate is preferably one or more of zinc phosphate, manganese phosphate, iron phosphate, and zinc calcium phosphate. The metal phosphate is preferably not a hydrate, since hydrates reduce corrosion resistance. Even in the grain-oriented electrical steel sheet according to this embodiment, hydrates inevitably formed during the formation of the intermediate layer may ultimately remain, but only in small amounts (usually less than 5.0 mass% of the entire insulating coating 21). The intermediate layer 211 may contain oxides and elements such as Fe and Si diffused from the base steel sheet as the remainder of the metal phosphate. Although the intermediate layer 211 is formed at a different time from the tensile coating layer formed thereon, both the intermediate layer 211 and the tensile coating layer 212 function as the insulating coating 21.
[0024] The amount of hydrate in the metal phosphate can be roughly determined by measuring the amount of water by thermobalance.
[0025] If the average thickness of the intermediate layer 211 is less than 0.1 μm, the effect of improving the adhesion between the base steel sheet and the insulating coating via the intermediate layer is insufficient. On the other hand, if the average thickness of the intermediate layer exceeds 15.0 μm, the magnetic properties deteriorate significantly. The thickness here refers to the thickness in the flat portion 2 of the base steel sheet 11. In the groove portion 3, the thickness is 0.1 to 9.0 μm. If the thickness of the intermediate layer 211 in the groove portion 3 exceeds 9.0 μm, the adhesion becomes poor.
[0026] [Tension Coating Layer] In the grain-oriented electrical steel sheet 1 according to this embodiment, a tension coating is formed on the surface of the intermediate layer 211, thereby providing a tension coating layer 212 on the surface of the insulating coating 21. The tension coating layer 212 is not particularly limited as long as it is used as an insulating coating for a grain-oriented electrical steel sheet. However, from the viewpoint of adhesion to the intermediate layer 211 (adhesion to the base steel sheet 11 via the intermediate layer 211), it preferably contains a metal phosphate and silica (derived from colloidal silica in the coating liquid) so that the silica content is 20% by mass or more. On the other hand, a silica content of more than 60% by mass in the tensile coating layer 212 can cause powdering, so it is preferably 60% by mass or less. The tensile coating layer 212 preferably contains a total of 70% by mass or more of metal phosphate and silica. The remainder of the tensile coating layer 212, other than the metal phosphate and silica, may include ceramic fine particles such as alumina or silicon nitride. Although the thickness of the tensile coating layer 212 is not limited, the average thickness of the insulating coating 21 (intermediate layer 211 + tensile coating layer 212) is preferably 1.0 to 20.0 μm in both the flat and grooved portions. If the average thickness of the insulating coating 21 is less than 1.0 μm, sufficient coating tension cannot be obtained. Furthermore, the amount of phosphate elution increases. This can cause stickiness and reduced corrosion resistance, and may even lead to coating peeling. Furthermore, if the thickness of the insulating coating 21 exceeds 20.0 μm, the space factor decreases, deteriorating magnetic properties, and cracks can occur, resulting in reduced adhesion and reduced corrosion resistance.
[0027] The thicknesses of the intermediate layer 211, the tensile coating layer 212, and the insulating coating are determined by the following method. For flat portions, the cross section of the sample is observed with a scanning electron microscope, and the thicknesses are measured at five or more points and averaged to determine the average thickness of each. The intermediate layer 211 and the tensile coating layer 212 in the insulating coating 21 can be distinguished by the detected amount of silicon derived from silica (as mentioned above, the tensile coating layer contains silica, with a silica content of 10% by mass or more). The average thickness of the insulating coating 21 is the sum of the average thickness of the intermediate layer 211 and the average thickness of the tensile coating layer 212. For grooved portions, the average thickness is determined by measuring the bottom position of the groove at five points and averaging the measurements.
[0028] The mass percentage and type of metal phosphate in the intermediate layer 211 and the tensile coating layer 212 can be determined by the following method. Similar to the method for measuring the thickness of the intermediate layer 211 and the tensile coating layer 212, the mass percentage and type of metal phosphate can be determined by using a scanning electron microscope and an energy dispersive elemental analyzer. Whether the metal phosphate in the intermediate layer 211 is crystalline can be determined by X-ray crystal structure analysis. The silica content of the tensile coating layer 212 can be measured by using a scanning electron microscope and an energy dispersive elemental analyzer.
[0029] <Base steel sheet> [Chemical composition] The grain-oriented electrical steel sheet 1 according to this embodiment is significantly characterized by the structure of the insulating coating 21 formed on the surface of the base steel sheet 11, and the base steel sheet 11 included in the grain-oriented electrical steel sheet 1 is not limited in terms of its chemical composition. However, in order to obtain the properties generally required of a grain-oriented electrical steel sheet, it is preferable that the chemical components that make up the chemical composition include the following: In this embodiment, % relating to the chemical components is % by mass unless otherwise specified.
[0030] C: 0.010% or less C (carbon) is an element effective for controlling the structure of steel sheets in the manufacturing process up to the completion of the decarburization annealing process. However, if the C content exceeds 0.010%, the magnetic properties of the finished grain-oriented electrical steel sheet deteriorate. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the C content is preferably 0.010% or less. The C content is more preferably 0.005% or less. Although a lower C content is preferable, reducing the C content to less than 0.0001% saturates the effect of structural control and simply increases manufacturing costs. Therefore, the C content may be 0.0001% or more.
[0031] Si: 2.50 to 4.00% Si (silicon) is an element that increases the electrical resistance of grain-oriented electrical steel sheets and improves their iron loss characteristics. If the Si content is less than 2.50%, a sufficient eddy current loss reduction effect cannot be obtained. Therefore, the Si content is preferably 2.50% or more. The Si content is more preferably 2.70% or more, and even more preferably 3.00% or more. On the other hand, if the Si content exceeds 4.00%, the grain-oriented electrical steel sheets become embrittled and their threading properties deteriorate significantly. Furthermore, the workability of the grain-oriented electrical steel sheets decreases, and the steel sheets may break during rolling. Therefore, the Si content is preferably 4.00% or less. The Si content is more preferably 3.80% or less, and even more preferably 3.70% or less.
[0032] Mn: 0.01 to 0.50% Mn (manganese) is an element that combines with S to form MnS during the manufacturing process. This precipitate functions as an inhibitor (a suppressor of normal grain growth) and induces secondary recrystallization in the steel. Mn also enhances the hot workability of the steel. If the Mn content is less than 0.01%, the above-mentioned effects cannot be fully achieved. Therefore, the Mn content is preferably 0.01% or more. The Mn content is more preferably 0.02% or more. On the other hand, if the Mn content exceeds 0.50%, secondary recrystallization does not occur and the magnetic properties of the steel deteriorate. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the Mn content is preferably 0.50% or less. The Mn content is more preferably 0.20% or less, and even more preferably 0.10% or less.
[0033] N: 0.010% or less N (nitrogen) is an element that bonds with Al during the manufacturing process to form AlN, which functions as an inhibitor. However, if the N content exceeds 0.010%, excessive inhibitors remain in the base steel sheet of the grain-oriented electrical steel sheet, resulting in reduced magnetic properties. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the N content is preferably 0.010% or less. The N content is more preferably 0.008% or less. On the other hand, the lower limit of the N content is not particularly specified, but reducing the N content to less than 0.001% only increases manufacturing costs. Therefore, the N content may be 0.001% or more.
[0034] Sol. Al: 0.020% or less Sol. Al (acid-soluble aluminum) is an element that bonds with N to form AlN, which functions as an inhibitor, during the manufacturing process of grain-oriented electrical steel sheets. However, if the sol. Al content of the base steel sheet exceeds 0.020%, excessive inhibitors remain in the base steel sheet, resulting in reduced magnetic properties. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the sol. Al content is preferably 0.020% or less. The sol. Al content is more preferably 0.010% or less, and even more preferably less than 0.001%. There is no particular restriction on the lower limit of the sol. Al content, but reducing it to less than 0.0001% only increases manufacturing costs. Therefore, the sol. Al content may be 0.0001% or more.
[0035] S: 0.010% or less S (sulfur) is an element that combines with Mn during the manufacturing process to form MnS, which functions as an inhibitor. However, if the S content exceeds 0.010%, the magnetic properties will be reduced due to the remaining inhibitor. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the S content is preferably 0.010% or less. The S content in the grain-oriented electrical steel sheet is preferably as low as possible. For example, less than 0.001%. However, reducing the S content in the base steel sheet of the grain-oriented electrical steel sheet to less than 0.0001% will only increase the manufacturing cost. Therefore, the S content in the base steel sheet of the grain-oriented electrical steel sheet may be 0.0001% or more.
[0036] Balance: Fe and impurities The chemical composition of the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment may contain the above-mentioned elements, with the balance being Fe and impurities. However, for the purpose of improving magnetic properties, etc., Sn, Cu, Se, and Sb may also be contained in the ranges shown below. Furthermore, even if other elements, such as W, Nb, Ti, Ni, Co, V, Cr, and Mo, are contained in a total of 1.0% or less, the effects of the grain-oriented electrical steel sheet according to this embodiment are not impaired. Here, impurities refer to elements that are mixed in from raw materials such as ore, scrap, or the manufacturing environment during industrial production of the base steel sheet, and are allowed to be contained in amounts that do not adversely affect the function of the grain-oriented electrical steel sheet according to this embodiment.
[0037] Sn: 0 to 0.50% Sn (tin) is an element that contributes to improving magnetic properties through controlling the primary recrystallization structure. To obtain the effect of improving magnetic properties, the Sn content is preferably 0.01% or more. The Sn content is more preferably 0.02% or more, and even more preferably 0.03% or more. On the other hand, if the Sn content exceeds 0.50%, secondary recrystallization becomes unstable and magnetic properties deteriorate. Therefore, the Sn content is preferably 0.50% or less. The Sn content is more preferably 0.30% or less, and even more preferably 0.10% or less.
[0038] Cu: 0 to 0.50% Cu (copper) is an element that contributes to increasing the Goss orientation occupancy rate in the secondary recrystallized structure. To achieve the above effect, the Cu content is preferably 0.01% or more. The Cu content is more preferably 0.02% or more, and even more preferably 0.03% or more. On the other hand, if the Cu content exceeds 0.50%, the steel sheet becomes embrittled during hot rolling. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the Cu content is preferably 0.50% or less. The Cu content is more preferably 0.30% or less, and even more preferably 0.10% or less.
[0039] Se: 0 to 0.020% Se (selenium) is an element that has the effect of improving magnetic properties. When Se is contained, the Se content is preferably 0.001% or more to effectively exhibit the effect of improving magnetic properties. The Se content is more preferably 0.003% or more, and even more preferably 0.006% or more. On the other hand, if the Se content exceeds 0.020%, the adhesion of the coating deteriorates. Therefore, the Se content is preferably 0.020% or less. The Se content is more preferably 0.015% or less, and even more preferably 0.010% or less.
[0040] Sb: 0 to 0.50% Sb (antimony) is an element that has the effect of improving magnetic properties. When Sb is contained, the Sb content is preferably 0.005% or more to effectively exhibit the effect of improving magnetic properties. The Sb content is more preferably 0.01% or more, and even more preferably 0.02% or more. On the other hand, if the Sb content exceeds 0.50%, the adhesion of the coating significantly deteriorates. Therefore, the Sb content is preferably 0.50% or less. The Sb content is more preferably 0.30% or less, and even more preferably 0.10% or less.
[0041] As described above, the chemical composition of the base steel sheet of the grain-oriented electrical steel sheet in this embodiment is, for example, one that contains the above-mentioned elements with the balance being Fe and impurities.
[0042] The chemical composition of the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment can be measured using a known ICP atomic emission spectroscopy. However, when an insulating coating is formed on the surface, it is removed before measurement. The removal can be achieved by immersing the sample in a highly concentrated alkaline solution (e.g., a 30% sodium hydroxide solution heated to 85°C) for 20 minutes or more. Peeling can be determined visually. For small samples, removal can also be achieved by surface grinding.
[0043] [Groove] The base steel sheet 11 has flat portions 2 and grooves 3 on its rolled surface. Magnetic domain control can be achieved by periodically forming linear grooves (groove portions) in a direction intersecting the rolling direction. In the base steel sheet 11 of the grain-oriented electrical steel sheet 1 according to this embodiment, the depth D of the grooves 3 is 10 to 30 μm, and the width W of the grooves 3 is 10 to 200 μm. If the depth D of the grooves 3 is less than 10 μm, the magnetic domain control effect is poor. On the other hand, if the depth D exceeds 30 μm, the decrease in the magnetic flux density B8 value is excessively large. If the width W of the grooves 3 is 10 μm, the magnetic domain control effect is poor. On the other hand, if the width W exceeds 200 μm, the decrease in the magnetic flux density B8 value is excessively large. In addition, it is preferable that a plurality of grooves are periodically present in the rolling direction, and the distance between adjacent grooves in the rolling direction is 1.0 to 20.0 mm. The spacing between grooves is the distance from the center of the width of a groove to the center of the width of an adjacent groove. The shape of the grooves is not limited, and for example, the cross section may be substantially rectangular or substantially triangular. The cross section may also be arch-shaped, constituting a part of a circle. In this embodiment, the direction intersecting the rolling direction is a direction at 45 to 135° with respect to the rolling direction (90±45° with respect to the rolling direction). The magnetic domain control effect is greater when the angle is closer to 90° with respect to the rolling direction, so the angle may be 70 to 110° with respect to the rolling direction.
[0044] In the grain-oriented electrical steel sheet according to this embodiment, 50% or more of the surface area (side and bottom surfaces) in the grooves 3 is covered with the insulating coating 21 (coverage rate is 50% or more). In the grooves, the thickness of the intermediate layer of the insulating coating is 0.1 to 9.0 μm. If the coverage rate is less than 50%, the adhesion of the tension coating after stress relief annealing decreases, resulting in partial peeling and poor corrosion resistance. In the grain-oriented electrical steel sheet according to this embodiment, the insulating coating is formed under specific processing conditions, as described below, so that the adhesion of the insulating coating is high and the coverage rate is high, even in the grooves.
[0045] The depth and width of the grooves are determined by the following method. The steel sheet is cut into several mm squares so as to include the vicinity of the area where a groove is visually determined to be formed. After ion milling (CP processing) is performed to remove microscopic shape defects such as sagging and cracks in the cross section, a cross section parallel to the rolling direction and thickness direction of the steel sheet is observed at 1000x magnification using a scanning electron microscope, and one or multiple recesses formed at a predetermined interval are determined to be grooves. The longest (deepest) part of the recess in the observed cross section, measured perpendicularly from an extension of the surface of the flat portion of the base steel sheet (a portion not affected by the groove processing), is determined to be the bottom of the groove, and the linear distance connecting one end of the recess to the other end on the extension of the surface is determined to be the width. Here, the end of the recess refers to the position where the recess begins to sink at a gradient of 30° or more relative to an extension of the surface of the flat portion. Three or more grooves are observed in the above manner, and the average of the respective measured values is taken as the depth and width of the groove.
[0046] The coverage rate of the insulating coating in the grooves is determined as follows. Similar to the method for observing the grooves, after ion milling, a cross section of the steel sheet parallel to the rolling direction and thickness direction is observed with a scanning electron microscope at 1000x magnification, and the proportion of the surface (side and bottom) within the groove that is not covered with the insulating coating is calculated. However, portions with an insulating coating thickness of less than 1.0 μm are considered to be uncovered because the insulating coating does not provide its intended effect. Furthermore, portions with an intermediate layer thickness of less than 0.1 μm or more than 9.0 μm are considered to be uncovered because the insulating coating does not provide sufficient adhesion. The proportion (%) of the portion not covered with the insulating coating is obtained by subtracting from 100 (%) the proportion (%) of the portion covered with the insulating coating (coverage rate). To calculate the coverage rate, three or more grooves are observed, and the average of the measured values is used.
[0047] <Manufacturing Method> The grain-oriented electrical steel sheet according to this embodiment can be suitably manufactured by a manufacturing method that satisfies the manufacturing conditions described below. However, it goes without saying that the grain-oriented electrical steel sheet according to this embodiment is not particularly limited to a manufacturing method. In other words, a grain-oriented electrical steel sheet having the configuration described above is considered to be the grain-oriented electrical steel sheet according to this embodiment, regardless of its manufacturing conditions.
[0048] The grain-oriented electrical steel sheet according to this embodiment includes: (I) a hot rolling step of hot-rolling a steel slab having a predetermined chemical composition to obtain a hot-rolled sheet; (II) a hot-rolled sheet annealing step of annealing the hot-rolled sheet; (III) a cold-rolling step of cold-rolling the hot-rolled sheet after the hot-rolled sheet annealing to obtain a cold-rolled sheet; (IV) a decarburization annealing step of decarburizing the cold-rolled sheet; and (V) a step of adding Al to the cold-rolled sheet after the decarburization annealing step. 2 O 3(VI) an annealing separator removing step of removing excess annealing separator from the steel sheet after the finish annealing step; and (VII) a groove forming step of forming grooves extending in a direction at an angle of 45 to 135° to the rolling direction by using a tooth profile or a laser in the steel sheet before the finish annealing step or after the annealing separator removing step. (VIII) an intermediate layer forming step of immersing the steel sheet that has been through the annealing separator removing step and the groove forming step in a mixed treatment solution containing a metal phosphate and one or more acids selected from hydrofluoric acid, nitric acid, and phosphoric acid having a total concentration of 0.01 to 10.0 mass%, and a sodium hydroxide, sodium carbonate, or sodium phosphate having a concentration of 0.01 to 1.50 mass%, at a liquid temperature of 30 to 85°C for 5 to 90 seconds, removing the mixed treatment solution with water and then drying the steel sheet; (IX) a tensile coating layer forming step of applying a coating solution containing a metal phosphate and colloidal silica, the content of colloidal silica being 30 to 150 parts by mass per 100 parts by mass of the metal phosphate, drying, and then maintaining the steel sheet at a sheet temperature of 700 to 950°C for 10 to 90 seconds; The method for producing a grain-oriented electrical steel sheet according to this embodiment may further include: (X) a nitriding step of nitriding the cold-rolled sheet between the decarburization annealing step and the finish annealing step. Of these, the production of a grain-oriented electrical steel sheet according to this embodiment is characterized by the steps (V) finish annealing step to (IX) tension coating layer forming step (method for forming an insulating coating), which are mainly related to the formation of an insulating coating; other steps or conditions not described can be known conditions. These steps will be described below.
[0049] <Hot Rolling Step> In the hot rolling step, a billet such as a slab having a predetermined chemical composition is heated and then hot rolled to obtain a hot-rolled sheet. The heating temperature of the billet is preferably within the range of 1100 to 1450°C. The heating temperature is more preferably 1300 to 1400°C. The chemical composition of the billet may be changed depending on the chemical composition of the base steel sheet of the grain-oriented electrical steel sheet that is ultimately to be obtained, and may be, for example, in mass %, C: 0.01 to 0.20%, Si: 2.50 to 4.00%, sol. An example of a chemical composition is Al: 0.01 to 0.040%, Mn: 0.01 to 0.50%, N: 0.020% or less, S: 0.005 to 0.040%, Cu: 0 to 0.50%, Sn: 0 to 0.50%, Se: 0 to 0.020%, Sb: 0 to 0.50%, and the balance being Fe and impurities. The hot rolling conditions are not particularly limited and may be set appropriately based on the desired properties. The thickness of the hot-rolled sheet is preferably, for example, in the range of 2.0 mm to 3.0 mm.
[0050] <Hot-rolled sheet annealing process> The hot-rolled sheet annealing process is a process of annealing a hot-rolled sheet manufactured through a hot rolling process. This annealing process is preferable because it causes recrystallization in the steel sheet structure and enables the realization of good magnetic properties. When hot-rolled sheet annealing is performed, the hot-rolled sheet manufactured through the hot rolling process may be annealed according to a known method. The means for heating the hot-rolled sheet during annealing is not particularly limited, and known heating methods can be adopted. Furthermore, the annealing conditions are not particularly limited. For example, the hot-rolled sheet may be annealed in a temperature range of 900 to 1200°C for 10 seconds to 5 minutes.
[0051] <Cold Rolling Step> In the cold rolling step, the hot-rolled sheet after the hot-rolled sheet annealing step is subjected to cold rolling to obtain a cold-rolled sheet. The cold rolling may be a single cold rolling, or multiple cold rolling steps with intermediate annealings may be performed by interrupting the cold rolling and performing at least one or two intermediate annealings before the final pass of the cold rolling step. When intermediate annealing is performed, it is preferable to hold the temperature at 1000 to 1200°C for 5 to 180 seconds. The annealing atmosphere is not particularly limited. Considering production costs, the number of intermediate annealings is preferably three or less. Furthermore, the surface of the hot-rolled sheet may be pickled before the cold rolling step.
[0052] In the cold rolling process according to this embodiment, the hot-rolled sheet is cold-rolled according to a known method to obtain a cold-rolled sheet. For example, the final reduction can be in the range of 80 to 95%. A final reduction of 80% or more is preferable because it is possible to obtain Goss nuclei with a high concentration of {110}<001> orientation in the rolling direction. On the other hand, a final reduction of more than 95% is not preferable because it increases the possibility of secondary recrystallization becoming unstable in the subsequent finish annealing process. The final reduction is the cumulative reduction of cold rolling, and if intermediate annealing is performed, it is the cumulative reduction of cold rolling after final intermediate annealing.
[0053] <Decarburization annealing step> In the decarburization annealing step, the obtained cold-rolled sheet is subjected to decarburization annealing. In the decarburization annealing, the cold-rolled sheet is subjected to primary recrystallization, and the decarburization annealing conditions are not limited as long as C, which adversely affects magnetic properties, can be removed from the steel sheet. For example, the degree of oxidation (PH) in the annealing atmosphere (furnace atmosphere) can be adjusted. 2 O / PH 2 ) is set to 0.3 to 0.6, and the annealing temperature is set to 800 to 900° C., and the holding is performed for 10 to 600 seconds.
[0054] <Nitriding Process> Nitriding may be performed between the decarburization annealing process and the finish annealing process described below. In the nitriding process, for example, the steel sheet after decarburization annealing is maintained at approximately 700 to 850°C in a nitriding atmosphere (an atmosphere containing hydrogen, nitrogen, and a nitriding gas such as ammonia) to perform nitriding. When AlN is used as an inhibitor, it is preferable to set the nitrogen concentration of the steel sheet to 40 ppm or more by the nitriding process. On the other hand, if the nitrogen concentration of the steel sheet exceeds 1000 ppm, excess AlN remains in the steel sheet even after the completion of secondary recrystallization in the finish annealing. Such AlN can cause iron loss degradation. For this reason, it is preferable to set the nitrogen concentration of the steel sheet after the nitriding process to 1000 ppm or less.
[0055] <Finish annealing step> In the finish annealing step, Al is added to the cold-rolled sheet that has been subjected to the decarburization annealing step or further to the nitriding treatment step. 2 O 3 In a conventional method for producing grain-oriented electrical steel sheets, an annealing separator containing 10 to 100 mass % of Al is applied, dried, and then finish annealed. In contrast, in the method for producing grain-oriented electrical steel sheets according to the present embodiment, an annealing separator containing mainly MgO is applied and finish annealed to form a forsterite-based coating on the surface of the steel sheet (cold-rolled sheet). 2 O 3 On the other hand, an annealing separator containing Al is used. 2 O 3 The proportion of Al may be 100 mass %, but 2 O 3 From the viewpoint of preventing seizure of Al, in the method for producing a grain-oriented electrical steel sheet according to this embodiment, the annealing separator preferably contains MgO. Although the content of MgO may be 0%, in order to obtain the above effect, the content of MgO is preferably 5 mass% or more. When MgO is contained, the content of MgO is preferably 10 mass% or more. 2 O 3 The content of Al relative to the annealing separator is 90 mass % or less to ensure this. The content of MgO is preferably 50 mass % or less. 2 O 3The total of MgO and MgO may be more than 50% by mass in terms of solid content. Furthermore, in the method for producing a grain-oriented electrical steel sheet according to this embodiment, the annealing separator may further contain chloride. The inclusion of chloride in the annealing separator provides the effect of making it more difficult for a forsterite-based coating to form. The chloride content is not particularly limited and may be 0%, but to obtain the above effect, 0.5 to 10% by mass is preferred. Examples of effective chlorides include bismuth chloride, calcium chloride, cobalt chloride, iron chloride, and nickel chloride. The finish annealing conditions are not limited, but for example, a temperature of 1150 to 1250°C for 10 to 60 hours can be employed.
[0056] [Annealing Separator Removal Step] In the annealing separator removal step, excess annealing separator is removed from the steel sheet after the finish annealing step. For example, excess annealing separator can be removed by washing with water.
[0057] [Groove Forming Step] In the groove forming step, grooves extending in a direction of 45 to 135° relative to the rolling direction are formed in the steel sheet using a tooth profile or a laser. The groove forming step may be performed after the decarburization annealing step and before the finish annealing step, or may be performed after the annealing separator removal step. When grooves are formed using a tooth profile, this is a method using physical contact, and the conditions are set appropriately so that the grooves have a predetermined extension direction, depth, and width, and the grooves are formed physically. When irradiating with a laser, for example, a fiber laser, YAG laser, semiconductor laser, or CO 2 High-power lasers generally used for industrial purposes, such as lasers, can be used. The output type may be a pulsed laser or a continuous wave laser. To form grooves of a predetermined shape, it is preferable that the laser output is 200 to 3000 W, the focused spot diameter in the rolling direction of the laser beam (the diameter containing 86% of the laser output) is 10 to 1000 μm, the focused spot diameter in the sheet width direction is 10 to 1000 μm, and the laser scanning speed is in the range of 5 to 100 m / s. Methods for removing the molten material from the surface include spraying of an assist gas, such as air or CO 2By simultaneously blowing gas such as argon or the like onto the irradiated area with the laser and providing a suction area nearby, it is possible to reduce the re-adhesion of molten material onto the steel sheet surface. From the viewpoint of reliability, machining using a toothed profile is preferred.
[0058] [Intermediate Layer Formation Process] In the intermediate layer formation process, the steel sheet that has undergone the annealing separator removal process and the groove formation process is immersed for 5 to 90 seconds in a mixed treatment solution at a liquid temperature of 30 to 85°C, containing a metal phosphate at a concentration of 1.0 to 15.0 mass%, one or more acids selected from hydrofluoric acid, nitric acid, and phosphoric acid at a total concentration of 0.01 to 10.0 mass%, and a sodium hydroxide, sodium carbonate, or sodium phosphate at a concentration of 0.01 to 1.50 mass%, and then removed from the mixed treatment solution by rinsing with water. The steel sheet is then dried. This process forms an intermediate layer containing a crystalline metal phosphate and having a thickness of 0.1 to 15.0 μm on the surface of the base steel sheet. The intermediate layer is formed not only in the flat portions but also in the groove portions. The supply of phosphoric acid and metal, which are the components of the intermediate layer, tends to be insufficient inside the grooves compared to the flat portions. Furthermore, hydrogen generated during the formation of the intermediate layer is likely to adhere to the surface in the grooves, creating unfavorable conditions for the formation of the intermediate layer. Therefore, the thickness of the intermediate layer is 0.1 to 9.0 μm under the above conditions.
[0059] If the liquid temperature is below 30°C or the immersion time is less than 5 seconds, an intermediate layer of sufficient thickness cannot be obtained. On the other hand, if the liquid temperature is above 85°C or the immersion time is more than 90 seconds, the intermediate layer will be excessively thick. The mixed treatment liquid contains a metal phosphate salt having a concentration of 1.0 to 15.0 mass%, one or more acids (additional acids) selected from hydrofluoric acid, nitric acid, and phosphoric acid having a total concentration of 0.01 to 10.0 mass%, and a sodium hydroxide, sodium carbonate, or sodium phosphate (pH adjuster) having a concentration of 0.01 to 1.50 mass%. Using such a treatment liquid increases the wettability of the treatment liquid with the surface of the base steel sheet (flat portions and groove portions), thereby improving the adhesion of the intermediate layer. As described above, the formation of an intermediate layer is particularly difficult in grooves compared to flat areas. However, in this embodiment, the formation of an intermediate layer in grooves can be promoted by increasing the concentration of metal phosphate and using a treatment solution containing one or more of hydrofluoric acid, nitric acid, and phosphoric acid as an oxidizing agent for oxidizing hydrogen. If the mixed treatment solution does not contain one or more acids selected from hydrofluoric acid, nitric acid, and phosphoric acid, the above effect cannot be achieved. To achieve the above effect, the treatment solution contains 0.01% by mass or more of the one or more acids selected from hydrofluoric acid, nitric acid, and phosphoric acid. On the other hand, if the proportion of the one or more acids selected from hydrofluoric acid, nitric acid, and phosphoric acid in the treatment solution is too high, the formation of an intermediate layer in flat areas may be suppressed. Therefore, the treatment solution contains 10.0% by mass or less of the one or more acids selected from hydrofluoric acid, nitric acid, and phosphoric acid. Of hydrofluoric acid, nitric acid, and phosphoric acid, hydrofluoric acid is preferred in terms of accelerating the formation of an intermediate layer in grooves. Furthermore, if the metal phosphate content of the treatment solution is less than 1.0 mass %, the formation of the intermediate layer in the groove portion will be slow. On the other hand, if the metal phosphate content exceeds 15.0 mass %, the intermediate layer in the flat portion will become too thick. Therefore, the metal phosphate content of the treatment solution is set to 1.0 to 15.0 mass %. The metal phosphate contained in the treatment solution is preferably one or more of zinc phosphate, manganese phosphate, and zinc calcium phosphate.Furthermore, if the concentration of the metal phosphate is low, the formation of the intermediate layer takes a long time, resulting in a large amount of dissolution of the steel sheet, making the intermediate layer porous. If the concentration is high, the intermediate layer forms quickly, resulting in an uneven intermediate layer made of coarse crystals. Furthermore, if the concentration of the pH adjuster, sodium hydroxide, sodium carbonate, or sodium phosphate, is low, the acidity increases and corrosion resistance decreases, while if it is high, the treatment solution becomes unstable. The use of sodium hydroxide, sodium carbonate, or sodium phosphate as the pH adjuster is not only cost-effective but also provides greater stability to the treatment solution. The treatment solution may further contain a sludge inhibitor, such as a chelating agent, as needed.
[0060] [Tension Coating Layer Formation Process] In the tension coating layer formation process, a coating liquid containing metal phosphate and colloidal silica, with the colloidal silica content being 30 to 150 parts by mass per 100 parts by mass of the metal phosphate, is applied to the steel sheet after the intermediate layer formation process, dried, and then held (baked) at a sheet temperature of 700 to 950°C for 10 to 90 seconds. This forms a tension coating. The layer consisting of this tension coating (tensile coating layer) and the intermediate layer constitute an insulating coating. If the sheet temperature is below 700°C, the tension will be low and the magnetic properties will be inferior. Therefore, it is preferable that the sheet temperature be 700°C or higher. On the other hand, if the sheet temperature is above 950°C, the rigidity of the steel sheet will decrease and it will be prone to deformation. In this case, the steel sheet may be distorted during transportation, etc., resulting in inferior magnetic properties. Therefore, it is preferable that the sheet temperature be 950°C or lower. Furthermore, if the holding time is less than 10 seconds, the leaching will be inferior. Therefore, the holding time is set to 10 seconds or more. On the other hand, if the holding time exceeds 90 seconds, adhesion will decrease, and attempts to avoid this decrease in adhesion will result in poor productivity. Therefore, a holding time of 90 seconds or less is preferable. The coating liquid contains a metal phosphate and colloidal silica in a ratio of 30 to 150 parts by mass of colloidal silica per 100 parts by mass of the metal phosphate. The total amount of the metal phosphate and colloidal silica in the coating liquid, calculated as solid content, should be greater than 50% by mass. Examples of metal phosphates that can be used include one or a mixture of two or more selected from aluminum phosphate, zinc phosphate, magnesium phosphate, nickel phosphate, copper phosphate, lithium phosphate, and cobalt phosphate. The coating liquid may contain additional elements such as vanadium, tungsten, molybdenum, and zirconium. S-type and C-type colloidal silica can be used. S-type colloidal silica refers to an alkaline silica solution, while C-type colloidal silica refers to a silica solution in which the silica particle surface is aluminum-treated and the silica solution is alkaline to neutral. S-type colloidal silica is widely used and relatively inexpensive, but care must be taken when mixing it with an acidic metal phosphate solution as it may aggregate and precipitate.Type C colloidal silica is stable even when mixed with a metal phosphate solution and there is no risk of precipitation, but it is relatively expensive due to the large number of processing steps required. It is preferable to use the type C colloidal silica depending on the stability of the coating solution to be prepared.
[0061] A slab containing, by mass%, C: 0.08%, Si: 3.31%, sol. Al: 0.028%, N: 0.008%, Mn: 0.07%, S: less than 0.0005%, with the balance being Fe and impurities was cast. This slab was heated to 1350 ° C and then hot rolled to obtain a hot-rolled sheet having a thickness of 2.2 mm. This hot-rolled sheet was annealed at 1100 ° C for 10 seconds (hot-rolled sheet annealing), and then cold-rolled to a thickness of 0.22 mm to obtain a cold-rolled sheet. This cold-rolled sheet was subjected to (PH 2 O / PH 2 The cold-rolled sheets were then subjected to decarburization annealing at 830°C for 90 seconds in an atmosphere with a saturation temperature of 0.4. 2 O 3 50% by mass, MgO 46.5% by mass, bismuth chloride BiCl 3 After drying, the cold-rolled sheet was subjected to finish annealing at 1200°C for 20 hours. 2 O 3 An annealing separator consisting of chisel (100% by mass) was applied to the steel sheet, which was then dried and subjected to finish annealing at 1200°C for 20 hours.
[0062] After the final annealing process, the steel sheet was washed with water to remove excess annealing separator, revealing that no forsterite-based coating was formed on the steel sheet surface. A plurality of grooves, each 50 μm wide and 20 μm deep, extending in a direction perpendicular to the rolling direction (at an angle of 82° relative to the rolling direction) were formed in the steel sheet at a pitch of 6.0 mm along the rolling direction using a tooth profile. The steel sheet was immersed in the treatment solution shown in Table 1, then heated and dried to form an intermediate layer. The average thickness of the intermediate layer was as shown in Table 1. X-ray crystal structure analysis revealed that all of the metal phosphates were crystalline metal phosphates, and the proportion of crystalline metal phosphate in the intermediate layer was 80 mass% or more.
[0063]
[0064] Steel plates having any of the intermediate layers Nos. 1 to 16 formed thereon were cut into multiple pieces as necessary, and a coating solution containing a metal phosphate salt and colloidal silica shown in Table 2 was applied to each steel plate, and the steel plate was baked in a drying oven for the time shown in Table 2 so as to reach the plate temperature shown in Table 2, thereby forming a tension coating on the surface. When vanadium, tungsten, molybdenum, or zirconium was contained in the coating solution, an oxyacid (V) was added in the molar ratio shown in Table 2. 2 O 4 , W.O. 3 , MoO 3 , ZrO 2 ) was added. The thickness of the tensile coating layer was varied by changing the amount of coating solution applied. Some of the coating solutions contained alumina or silicon nitride as the remainder. Samples (grain-oriented electrical steel sheets) Nos. 101 to 121 were produced in this manner.
[0065] The average thickness of the insulating coating of these steel sheets was determined using the method described above. The results are shown in Table 2.
[0066]
[0067] The chemical composition of the base steel sheet was determined using the method described above and found to contain 0.002% C, 3.31% Si, less than 0.001% sol. Al, 0.001% N, 0.07% Mn, and less than 0.0005% S, with the balance being Fe and impurities. The adhesion, coating tension, corrosion resistance, elution, and magnetic properties of the insulating coating were also determined for these steel sheets using the methods described below. The results are shown in Table 3.
[0068] [Adhesion] Coating adhesion was evaluated by taking a sample 30 mm wide and 300 mm long from the steel sheet, subjecting this sample to stress relief annealing at 850°C for 2 hours in a nitrogen stream, and then winding it around a 10 mmφ cylinder and unwinding it to a bending adhesion test. The coating adhesion was evaluated based on the degree of peeling (area ratio) of the coating over the entire sample, including grooves and flat areas. The evaluation criteria were as follows, and A or B was determined to be excellent in coating adhesion. A: Peeling area ratio 0 to 0.5% B: Peeling area ratio more than 0.5% and 5.0% or less C: Peeling area ratio more than 5.0% and 20% or less D: Peeling area ratio more than 20% and 50% or less E: Peeling area ratio more than 50%
[0069] [Coating tension] A sample was taken from the steel sheet, and the insulating coating on one side of the sample was peeled off to calculate the coating tension by back-calculating from the state of curvature. When the obtained coating tension was 4.0 MPa or more, it was determined that the coating tension was excellent.
[0070] [Corrosion Resistance] In accordance with the salt spray test of JIS Z2371:2015, a 5% NaCl aqueous solution was allowed to fall naturally onto the sample for 7 hours in an atmosphere at 35°C. The rust area was then evaluated on a 10-point scale. The evaluation criteria were as follows, and a score of 5 or more (5 to 10) was considered to indicate excellent corrosion resistance. 10: No rust occurred 9: Very little rust occurred (area ratio = 0.10% or less) 8: Area ratio of rust occurred = more than 0.10% but not more than 0.25% 7: Area ratio of rust occurred = more than 0.25% but not more than 0.50% 6: Area ratio of rust occurred = more than 0.50% but not more than 1.0% 5: Area ratio of rust occurred = more than 1.0% but not more than 2.5% 4: Area ratio of rust occurred = more than 2.5% but not more than 5.0% 3: Area ratio of rust occurred = more than 5.0% but not more than 10% 2: Area ratio of rust occurred = more than 10% but not more than 25% 1: Area ratio of rust occurred = more than 25% but not more than 50%
[0071] [Leaching] A sample was taken from the obtained steel sheet, and the sample was boiled in boiling pure water for 10 minutes, and the amount of phosphoric acid eluted into the pure water was measured. The amount of eluted phosphoric acid was divided by the area of the insulating coating of the boiled grain-oriented electrical steel sheet to calculate the elution (mg / m 2The amount of phosphoric acid dissolved in the pure water was measured by cooling the pure water (solution) into which the phosphoric acid had dissolved, and then diluting the cooled solution with pure water to obtain a sample, and measuring the phosphoric acid concentration of the resulting sample by ICP-AES. The amount of elution per unit area was 40 mg / m 2 If the dissolution rate was less than this, it was determined that the dissolution rate was excellent.
[0072] [Magnetic Properties] After stress relief annealing in a nitrogen gas flow at 850°C for 2 hours, the magnetic properties were measured, including B8 (magnetic flux density at a magnetizing force of 800 A / m) and W17 / 50 (iron loss per mass at a magnetic flux density amplitude of 1.7 T and 50 Hz). These property values were measured using a single sheet magnetic property measurement method (Single Sheet Tester: SST) in accordance with JIS C2556.
[0073]
[0074] As shown in Tables 1 to 3, in the inventive examples, grooves were formed and then an insulating coating (intermediate layer and tensile coating) was formed on the surface of the base steel sheet under specific processing conditions, resulting in the formation of predetermined grooves in the base steel sheet, with the predetermined insulating coating covering 50% or more by area. As a result, the coating adhesion and magnetic properties were excellent. The coating tension, corrosion resistance, and elution properties were also sufficient. On the other hand, in the comparative examples, the grooves were not sufficiently covered by the insulating coating, resulting in poor coating adhesion and / or magnetic properties.
[0075] The present invention provides a grain-oriented electrical steel sheet that has excellent coating adhesion and magnetic properties, and a method for forming an insulating coating on the grain-oriented electrical steel sheet, which has high industrial applicability.
[0076] REFERENCE SIGNS LIST 1 Grain-oriented electrical steel sheet 2 Flat portion 3 Groove portion 11 Base steel sheet 21 Insulation coating 211 Intermediate layer 212 Tensile coating layer RD Rolling direction TD Width direction ND Sheet thickness direction D Groove depth W Groove width
Claims
1. A grain-oriented electrical steel sheet comprising: a base steel sheet; and an insulating coating formed on a surface of the base steel sheet, wherein the base steel sheet has a flat portion and a groove portion extending in a direction at an angle of 45 to 135° to the rolling direction, the groove portion having a depth of 10 to 30 μm and a width of 10 to 200 μm, the insulating coating comprising: an intermediate layer having a thickness of 0.1 to 15.0 μm and containing a crystalline metal phosphate, formed on the base steel sheet side, and a tensile coating layer formed on the surface side of the insulating coating, wherein 50% or more of the groove portion in terms of area ratio is covered by the insulating coating comprising the tensile coating layer and the intermediate layer having a thickness of 0.1 to 9.0 μm.
2. The grain-oriented electrical steel sheet according to claim 1, wherein the crystalline metal phosphate contained in the intermediate layer is one or more of zinc phosphate, manganese phosphate, iron phosphate, and zinc calcium phosphate; the tensile coating layer contains a metal phosphate and silica, and the silica content in the tensile coating layer is 20 to 60 mass %.
3. A method for forming the insulating coating of the grain-oriented electrical steel sheet according to claim 1, comprising the steps of: 2 O 3 a finish annealing step of applying an annealing separator containing 10 to 100 mass % of the above-mentioned, drying the steel sheet, and then performing finish annealing; an annealing separator removing step of removing excess annealing separator from the steel sheet after the finish annealing step; and a groove forming step of forming grooves extending in a direction of 45 to 135° to the rolling direction by using a tooth profile or a laser in the steel sheet before the finish annealing step or after the annealing separator removing step. an intermediate layer forming step of immersing the steel sheet that has been subjected to the annealing separator removing step and the groove forming step in a mixed treatment solution having a liquid temperature of 30 to 85°C for 5 to 90 seconds, the mixed treatment solution containing a metal phosphate having a concentration of 1.0 to 15.0 mass%, one or more acids selected from hydrofluoric acid, nitric acid, and phosphoric acid having a total concentration of 0.01 to 10.0 mass%, and a sodium hydroxide, sodium carbonate, or sodium phosphate having a concentration of 0.01 to 1.50 mass%, and the mixed treatment solution is washed away with water, and then the steel sheet is dried; and a tensile coating layer forming step of applying a coating solution containing a metal phosphate and colloidal silica to the steel sheet after the intermediate layer forming step, the coating solution having a colloidal silica content of 30 to 150 parts by mass per 100 parts by mass of the metal phosphate, drying, and then maintaining the sheet at a sheet temperature of 700 to 950°C for 10 to 90 seconds.
4. The method for forming an insulating coating according to claim 3, wherein the annealing separator further contains one or both of the following: MgO: 5 to 90 mass %; and chloride: 0.5 to 10.0 mass %.
Citation Information
Patent Citations
JP1973039338A
JP1974096920A
Production of magnetic steel sheet with superior iron loss characteristic for electric machinery
JP1981051522A
Formation of insulating film on grain oriented electrical steel sheet
JP1993279747A
Display device manufacturing method
JP2023065385A