Separator for electrochemical device and electrochemical device comprising same

The separator for lithium secondary batteries, composed of a porous polymer substrate with a gas-adsorbing coating layer, addresses gas-related issues in lithium secondary batteries, enhancing performance and safety by mitigating gas accumulation and structural risks.

WO2024215040A1PCT designated stage expired Publication Date: 2024-10-17LG ENERGY SOLUTION LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/004688
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-04-09
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Lithium secondary batteries face performance degradation and potential explosion due to gas generation from electrolyte decomposition, which can cause internal resistance increase and structural deformation.

Method used

A separator for electrochemical devices featuring a porous polymer substrate with a porous coating layer containing modified metal-organic framework particles and a polymer binder, which adsorbs gases like carbon dioxide, preventing performance degradation and structural issues.

Benefits of technology

The separator effectively reduces gas accumulation, maintaining battery performance and safety by adsorbing generated gases, thereby extending battery life and preventing explosions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

The present invention provides a separator for an electrochemical device, the separator including: a porous polymer substrate; and a porous coating layer formed on at least one surface of the porous polymer substrate and including first metal-organic framework (MOF) particles modified with polyimide, second MOF particles, and a polymer binder, wherein at least one type of the first and second MOF particles includes zirconium and has amine groups introduced thereinto.
Need to check novelty before this filing date? Find Prior Art

Description

Separator for electrochemical devices and electrochemical devices containing the same

[0001] This application claims priority based on Korean Patent Application No. 10-2023-0048993, filed with the Korean Intellectual Property Office on April 13, 2023, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a separator for an electrochemical device and an electrochemical device including the same.

[0003] Electrochemical devices convert chemical energy into electrical energy using electrochemical reactions. Recently, lithium secondary batteries, which boast high energy density and voltage, long cycle life, and wide applicability, have become widely used. Lithium secondary batteries may include an electrode assembly comprising a positive electrode, a negative electrode, and a separator positioned between the positive and negative electrodes. The electrode assembly may be manufactured by being housed in a case together with an electrolyte.

[0004] If a lithium secondary battery experiences abnormal operation during storage or operation, such as an internal short circuit, overcharging, or exposure to temperatures higher than its operating temperature, the electrolyte contained within the lithium secondary battery may decompose, generating gas. This gas generated within the battery can increase the battery's internal resistance and shorten its lifespan. Excessive gas generation can cause deformation of the battery case or internal structure, potentially leading to battery fire or explosion. Therefore, research is being conducted on methods to reduce gas generation or battery volume expansion caused by gas.

[0005] The purpose of the present invention is to provide a separator for an electrochemical device capable of adsorbing a gas generated within the electrochemical device and an electrochemical device including the same.

[0006] One aspect of the present invention provides a separator for an electrochemical device, comprising a porous polymer substrate, and first metal-organic framework (MOF) particles modified with polyimide, second metal-organic framework particles, and a polymer binder, and a porous coating layer formed on at least one surface of the porous polymer substrate, wherein at least one of the first metal-organic framework particles and the second metal-organic framework particles comprises zirconium (Zr) and has an amine group introduced therein.

[0007] The first metal-organic framework particles and the second metal-organic framework particles each have an average particle diameter (D) according to particle size distribution analysis (PSD). 50 ) may be 300 nm or more and 10 μm or less.

[0008] The first metal-organic framework particles and the second metal-organic framework particles may each have an average pore diameter of more than 5 nm and less than 200 nm.

[0009] The first metal-organic framework particles and the second metal-organic framework particles each have a pore volume per unit mass of 0.2 cm 3 / g or more than 1.0 cm 3 / g can be less.

[0010] The first metal-organic framework particle and the second metal-organic framework particle may be independently selected from the group consisting of UiO-66-NH2, UiO-67-NH2, NU-1002-NH2, and MOF-808-NH2.

[0011] The first metal-organic framework particles and the second metal-organic framework particles may be included in a weight ratio of 35:65 to 45:55.

[0012] The above metal-organic framework particles and the polymer binder may be included in a weight ratio of 80:20 to 95:5.

[0013] Another aspect of the present invention provides an electrochemical device comprising an anode, a cathode, and a separator disposed between the anode and the cathode, wherein the separator is a separator for another electrochemical device on the one side.

[0014] The above electrochemical device may be a lithium secondary battery.

[0015] The separator for an electrochemical device according to the present invention can prevent performance degradation of an electrochemical device due to gas by adsorbing gases such as carbon dioxide generated by electrolyte decomposition in a coating layer.

[0016] Hereinafter, each component of the present invention will be described in more detail so that a person having ordinary skill in the art to which the present invention pertains can easily practice it; however, this is only an example, and the scope of the rights of the present invention is not limited by the following contents.

[0017] The term "comprises" as used herein is used to list materials, compositions, devices, and methods useful in the present invention, but is not limited to the listed examples.

[0018] As used herein, the terms "about" and "substantially" are used to mean a range or approximation of a numerical value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent infringers from unfairly exploiting the disclosure, which includes precise or absolute numerical values ​​provided to aid understanding of the present invention.

[0019] As used herein, “electrochemical device” may refer to a primary battery, a secondary battery, a super capacitor, etc.

[0020]

[0021] One specific example of the present invention provides a separator for an electrochemical device, comprising a porous polymer substrate, and first metal-organic framework (MOF) particles modified with polyimide, second metal-organic framework particles, and a polymer binder, and a porous coating layer formed on at least one surface of the porous polymer substrate, wherein at least one of the first and second metal-organic framework particles comprises zirconium (Zr) and has an amine group introduced therein.

[0022] The porous polymer substrate may be a porous membrane having a plurality of pores formed therein, which electrically insulates the positive and negative electrodes to prevent short circuits. For example, when the electrochemical device is a lithium secondary battery, the porous polymer substrate may be an ion-conductive barrier that blocks electrical contact between the positive and negative electrodes while allowing lithium ions to pass through. At least a portion of the pores may form a three-dimensional network that connects the surface and the interior of the porous polymer substrate, and a fluid may pass through the porous polymer substrate through the pores.

[0023] The porous polymer substrate may use a material that is physically and chemically stable with respect to the organic solvent electrolyte. For example, the porous polymer substrate may include, but is not limited to, a resin such as a polyolefin-based resin such as polyethylene, polypropylene, and polybutylene, polyvinyl chloride, polyethylene terephthalate, polycycloolefin, polyethersulfone, polyamide, polyimide, polyimideamide, nylon, polytetrafluoroethylene, and copolymers or mixtures thereof. A polyolefin-based resin may be preferably used. A polyolefin-based resin can be processed into a relatively thin thickness and is easy to apply a coating slurry, making it suitable for the manufacture of an electrochemical device with a higher energy density.

[0024] The porous polymer substrate may have a single-layer or multi-layer structure. The porous polymer substrate may include two or more polymer resin layers having different melting points (Tm), thereby providing a shutdown function in the event of a high-temperature runaway of the battery. For example, the porous polymer substrate may include a polypropylene layer having a relatively high melting point and a polyethylene layer having a relatively low melting point. Preferably, the porous polymer substrate may have a three-layer structure in which polypropylene, polyethylene, and polypropylene are laminated in that order. The polyethylene layer melts when the temperature of the battery rises above a predetermined temperature, thereby shutting down the pores, thereby preventing thermal runaway of the battery.

[0025] The thickness of the porous polymer substrate may be 1 ㎛ or more and 100 ㎛ or less. Specifically, the thickness of the porous polymer substrate may be 10 ㎛ or more and 90 ㎛ or less, 20 ㎛ or more and 80 ㎛ or less, 30 ㎛ or more and 70 ㎛ or less, or 40 ㎛ or more and 60 ㎛ or less. Preferably, the thickness of the polymer substrate may be 1 ㎛ or more and 30 ㎛ or less. More preferably, the thickness of the polymer substrate may be 5 ㎛ or more and 15 ㎛ or less, or 8 ㎛ or more and 13 ㎛ or less. By controlling the thickness of the porous polymer substrate within the above-described range, the volume of the electrochemical device can be minimized while electrically insulating the positive and negative electrodes, thereby increasing the amount of active material included in the electrochemical device.

[0026] The above porous polymer substrate may include pores having an average diameter of 0.01 μm or more and 1 μm or less. Specifically, the size of the pores included in the porous polymer substrate may be 0.01 μm or more and 0.09 μm or less, 0.02 μm or more and 0.08 μm or less, 0.03 μm or more and 0.07 μm or less, or 0.04 μm or more and 0.06 μm or less. Preferably, the size of the pores may be 0.02 μm or more and 0.06 μm or less. By controlling the pore size of the porous polymer substrate within the above-described range, the air permeability and ionic conductivity of the entire manufactured membrane can be controlled.

[0027] The porous polymer substrate may have a permeability of 10 s / 100cc or more and 100 s / 100cc or less. Specifically, the permeability of the porous polymer substrate may be 10 s / 100cc or more and 90 s / 100cc or less, 20 s / 100cc or more and 80 s / 100cc or less, 30 s / 100cc or more and 70 s / 100cc or less, or 40 s / 100cc or more and 60 s / 100cc or less. Preferably, the permeability of the porous polymer substrate may be 50 s / 100cc or more and 70 s / 100cc or less. When the permeability of the porous polymer substrate is within the above-described range, the permeability of the manufactured separator may be provided within a range suitable for securing the output and cycle characteristics of the electrochemical device.

[0028] The above air permeability (s / 100cc) means the time (in seconds) it takes for 100cc of air to pass through a porous polymer substrate or membrane of a predetermined area under a constant pressure. The above air permeability can be measured using an air permeability tester (Gurley densometer) according to ASTM D 726-58, ASTM D726-94 or JIS-P8117. For example, using a 4110N device from Gurley, air at a pressure of 0.304 kPa or air at a pressure of 1.215 kN / m 2100 cc of air under the pressure of water occupies 1 square inch (or 6.54 cm 2 ) can be used to measure the time it takes for 100 cc of air to pass through a 1-square-inch sample under a constant pressure of 4.8 inches of water at room temperature. For example, using the Asahi Seico EG01-55-1MR equipment, the time it takes for 100 cc of air to pass through a 1-square-inch sample can be measured.

[0029] The porous polymer substrate may have a porosity of 10 vol% or more and 60 vol% or less. Specifically, the porosity of the porous polymer substrate may be 15 vol% or more and 55 vol% or less, 20 vol% or more and 50 vol% or less, 25 vol% or more and 45 vol% or less, or 30 vol% or more and 40 vol% or less. Preferably, the porosity of the porous polymer substrate may be 30 vol% or more and 50 vol% or less. When the porosity of the porous polymer substrate is in the above-described range, the ionic conductivity of the manufactured separator can be provided in a range suitable for securing the output and cycle characteristics of the electrochemical device.

[0030] The above porosity refers to the volume ratio of pores to the total volume of the porous polymer substrate. The porosity can be measured by methods known in the art. For example, it can be measured by the BET (Brunauer Emmett Teller) measurement method using nitrogen gas adsorption, the capillary flow porosimetry method, or the water or mercury intrusion method.

[0031] The above porous coating layer is formed on at least one surface of the porous polymer substrate and may include metal-organic framework particles and a polymer binder. The metal-organic framework particles may mean one or more of a single type of metal-organic framework particles aggregated to form a structured or amorphous particle.

[0032] The metal-organic framework particles may be identical to each other, but may include a first metal-organic framework particle having at least a portion of the surface modified with polyimide, and a second metal-organic framework particle having no surface modification. Alternatively, the metal-organic framework particles may include two or more different types of metal-organic framework particles, wherein the surface of any one of the particles may be modified with polyimide, and the particle may be referred to as a first metal-organic framework particle.

[0033] The metal-organic framework particles may include one or more metal ions or metals including zirconium, and one or more organic ligands including ligands having an amine group. At least one of the organic ligands may include one or more amine groups and may be coordinated to the metal ion or metal to expose one or more amine groups on the surface of the metal-organic framework particles. For example, at least one of the first metal-organic framework particles and the second metal-organic framework particles may include zirconium and have an amine group introduced thereto. Preferably, both the first metal-organic framework particles and the second metal-organic framework particles may include zirconium, and an organic ligand including an amine group may be coordinated to the zirconium.

[0034] The properties of metal-organic frameworks can vary depending on the type of functional group introduced, and properties related to gas adsorption can be the best in metal-organic frameworks introduced with amine groups. For example, metal-organic frameworks introduced with amine groups can have a higher specific surface area and larger pore diameter than metal-organic frameworks introduced with carboxyl groups, sulfonic acid groups, or hydroxyl groups, and thus can have superior carbon dioxide adsorption capabilities. In addition, metal-organic framework particles having amine groups have superior carbon dioxide adsorption capabilities compared to metal-organic framework particles without amine groups because the amine groups act as Lewis base centers. Metal-organic frameworks having amine groups can provide stable carbon dioxide adsorption capabilities both in the presence and absence of water compared to metal-organic frameworks having polar or hydrophobic functional groups. For example, a metal-organic framework into which an amine group is introduced can form hydrogen bonds with water or carbon dioxide through the amine group, compared to a metal-organic framework into which a naphthyl group, nitro group, or methoxy group is introduced, thereby providing a stable adsorption capacity for carbon dioxide.

[0035] The first metal-organic framework particles are surface-modified with polyimide. The first metal-organic framework particles may be metal-organic framework particles having amine groups, and preferably, at least one amine group may be exposed on the surface of the particles. The polyimide-modified first metal-organic framework particles may include a polyimide formed by using at least some of the amine groups in an imidization reaction, or a polyimide introduced through a portion other than the amine group in the metal-organic framework. The polyimide-modified first metal-organic framework may have at least one amine group exposed on the surface. The polyimide-modified first metal-organic framework particles have superior dispersibility and stability in a coating slurry for forming a porous coating layer compared to unmodified particles. A coating slurry including the polyimide-modified first metal-organic framework particles may have slow sedimentation and sedimentation rates. A porous coating layer manufactured using the above coating slurry has a higher packing density per unit thickness, which can provide improved adsorption capacity for gases generated within an electrochemical device.

[0036] The first metal-organic framework particles and the second metal-organic framework particles may each have an average particle diameter (D50) of 300 nm to 10 μm, as measured by particle size distribution (PSD). Specifically, the average particle diameter of each particle may be 300 nm to 5000 nm, 400 nm to 2000 nm, or 500 nm to 1000 nm. By controlling the average particle diameter of the metal-organic framework particles within the above-described range, the specific surface area of ​​the porous coating layer may be maximized, thereby manufacturing a separation membrane having excellent gas adsorption capacity. The average particle diameter of the first metal-organic framework particles modified with polyimide may be larger than the average particle diameter of the second metal-organic framework particles. Specifically, the average particle diameter of the second metal-organic framework particles may be 300 nm or more and 1000 nm or less, and the average particle diameter of the first metal-organic framework particles may be larger than the average particle diameter of the second metal-organic framework particles within a range of 300 nm or more and 10 ㎛ or less.

[0037] The above particle size distribution analysis can be performed by dispersing metal-organic framework particles in a dispersion medium, and then obtaining the average particle diameter of the particles from the separation velocity distribution. For example, after dispersing one or more particles in the dispersion medium, the light transmittance of the particles being dispersed is measured at regular intervals, and the particle movement velocity obtained from the transmittance profile and the absorbance of the corresponding particles for the maximum absorbance that can be obtained by converting the transmittance into absorbance can be used to obtain the analysis.

[0038] The first metal-organic framework particles and the second metal-organic framework particles may each have an average pore diameter of more than 5 nm and less than 200 nm. Specifically, the average diameter of the pores formed in each particle may be more than 5 nm and less than 190 nm, more than 30 nm and less than 180 nm, more than 50 nm and less than 170 nm, more than 60 nm and less than 160 nm, more than 70 nm and less than 150 nm, more than 80 nm and less than 140 nm, more than 90 nm and less than 130 nm, or more than 100 nm and less than 120 nm. By controlling the pore diameters of the metal-organic framework particles within the above-described range, the specific surface area of ​​the porous coating layer can be maximized, thereby manufacturing a separation membrane having excellent gas adsorption capacity. The average pore diameter of the first metal-organic framework particles modified with polyimide may be smaller than the average pore diameter of the second metal-organic framework. Specifically, the average pore diameter of the second metal-organic framework particles may be 35 nm or more and less than 200 nm, and the average pore diameter of the first metal-organic framework particles may be smaller than the average pore diameter of the second metal-organic framework particles within a range of 5 nm or more and less than 200 nm. The average pore diameter of the first metal-organic framework particles may be 5 nm or more and less than 50 nm, and preferably 7 nm or more and less than 30 nm.

[0039] The average pore diameter of the above metal-organic framework particles may be a value measured in the process of calculating a BET model using a BET-specific surface area analyzer. The first metal-organic framework particles and the second metal-organic framework particles each have a pore volume per unit mass of 0.2 cm 3 / g or more than 1.0 cm 3 / g or less. Specifically, each particle is 0.3 cm 3 / g or more than 0.9 cm 3 / g or less, or 0.5 cm 3 / g or more than 0.8 cm 3 / g or less of pores. By controlling the pore volume of the metal-organic framework particles within the above-described range, the specific surface area of ​​the porous coating layer can be maximized, thereby manufacturing a separation membrane with excellent gas adsorption capacity. The first metal-organic framework particles modified with polyimide can have a pore volume per unit mass smaller than that of the second metal-organic framework particles. Specifically, the pore volume in the second metal-organic framework particles is 0.8 cm 3 / g or more than 1.0 cm 3 / g or less, and the pore volume of the first metal-organic framework particle is 0.2 cm 3 / g or more than 1.0 cm 3 / g or less than the pore volume of the second metal-organic framework particles. The average pore diameter of the first metal-organic framework particles is 0.2 cm. 3 / g or more than 0.5 cm 3 / g can be less.

[0040] The volume of pores per unit mass of the metal-organic framework particles can be measured by a method known in the art, such as the porosity measurement described above.

[0041] The first metal-organic framework particle and the second metal-organic framework particle may be each independently selected from the group consisting of UiO-66, UiO-67, NU-1002, and MOF-808. Specifically, the first metal-organic framework particle and the second metal-organic framework particle may be each independently selected from the group consisting of UiO-66-NH2, UiO-67-NH2, NU-1002-NH2, and MOF-808-NH2. For example, the first metal-organic framework particle may be UiO-66-NH2 modified with polyimide, and may have one or more amine groups exposed on the surface even after modification, and the second metal-organic framework particle may be UiO-66-NH2.

[0042] The porous coating layer may include first metal-organic framework particles modified with polyimide and second metal-organic framework particles not modified with polyimide in a weight ratio of 35:65 to 45:55. Preferably, the porous coating layer may include the first metal-organic framework particles and the second metal-organic framework particles in a weight ratio of 35:65 to 40:60. The first metal-organic framework improves the dispersibility of the coating slurry, thereby improving the packing density of the porous coating layer, and the second metal-organic framework can improve the specific surface area of ​​the porous coating layer. When both the first metal-organic framework particles and the second metal-organic framework particles are included in the above-described weight ratio, a separator having a porous coating layer formed therein having both a high packing density and a high specific surface area can be obtained. When the first metal-organic framework particles are included in an amount greater than the above-described ratio, the specific surface area of ​​the porous coating layer actually decreases, thereby reducing the gas adsorption capacity of the separation membrane.

[0043] The polymer binder can bind the first metal-organic framework particles, the second metal-organic framework particles, or the first metal-organic framework particles and the second metal-organic framework particles included in the porous coating layer, and provide adhesiveness to the porous coating layer.

[0044] The above polymer binder may include an acrylic polymer binder, a fluorine polymer binder, or a combination thereof.

[0045] The above acrylic polymer binder is (meth)acrylic acid, (meth)acrylate, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-amyl acrylate, isoamyl acrylate, n-ethylhexyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-amyl methacrylate, isoamyl methacrylate, n-hexyl methacrylate, n-ethylhexyl methacrylate, 2-ethylhexyl methacrylate, hydroxyethyl methacrylate, (meth)acrylonitrile It may contain, as a repeating unit, one or more monomers selected from the group consisting of butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, ethyl (meth)acrylate, methyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, n-oxyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, lauryl (meth)acrylate, and tetradecyl (meth)acrylate.

[0046] For example, the acrylic polymer binder may include at least one selected from the group consisting of polyacrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butylacrylate, isobutylacrylate, ethylhexylacrylate, methyl methacrylate, styrene-butadiene rubber, nitrile-butadiene rubber, acrylonitrile-butadiene rubber, and acrylonitrile-butadiene-styrene rubber.

[0047] The above fluorinated polymer binder may be polyvinylidene fluoride. For example, the fluorinated polymer binder may be at least one selected from the group consisting of polyvinylidene fluoride, polyhexafluoropropylene, polytetrafluoroethylene, polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyvinylidene fluoride-trichloroethylene (PVDF-TCE), and polyvinylidene fluoride-chlorotrifluoroethylene (PVDF-CTFE), and more specifically, may be a copolymer including polyvinylidene fluoride.

[0048] The polymer binder may be in a particle shape. For example, the polymer binder may be spherical or elliptical, but is not limited thereto. The polymer binder may have an average particle diameter (D50) of 100 nm to 500 nm. Specifically, the polymer binder may have an average particle diameter (D50) of 150 nm to 450 nm, 200 nm to 400 nm, or 250 nm to 350 nm. Preferably, the polymer binder may be a spherical particle having an average particle diameter (D50) of 200 nm to 400 nm. By controlling the particle diameter of the polymer binder particles within the above-described range, the movement path of lithium ions and the adhesion of the porous coating layer to the porous substrate can be secured at the same time.

[0049] The metal-organic framework particles and the polymer binder may be included in a weight ratio of 80:20 to 95:5. The metal-organic framework particles include both the first and second metal-organic framework particles, and the weight ratio of the metal-organic framework particles to the polymer binder may be 85:15, 90:10, or 95:5. By controlling the content of the metal-organic framework particles and the polymer binder within the above-described range, adhesion of the porous coating layer to the porous polymer substrate and thermal shrinkage of the porous polymer substrate can be reduced.

[0050] The packing density of the above porous coating layer is 1 g / cm 3 Above 1.04 g / cm 3 It may be as follows. By controlling the packing density of the porous coating layer within the above-described range, a separator exhibiting stable cycle characteristics in terms of air permeability and resistance can be obtained.

[0051] The porous coating layer may be formed by coating one surface of the porous polymer substrate with a coating slurry including the first metal-organic framework particles, the second metal-organic framework particles, a polymer binder, and a dispersion medium. For example, the separator may be manufactured by applying the coating slurry to at least one surface of the porous polymer substrate and then drying to remove the dispersion medium. The porous coating layer may have a porous structure including an interstitial volume in which the first metal-organic framework particles, the second metal-organic framework particles, or the first metal-organic framework particles and the second metal-organic framework particles are connected by the polymer binder. The porous coating layer may allow lithium ions to pass therethrough and may be adhered to the porous polymer substrate to prevent thermal shrinkage of the porous polymer substrate.

[0052] The coating slurry may include a dispersion medium to dissolve or disperse at least a portion of the polymer binder, and may disperse the first metal-organic framework particles and the second metal-organic framework particles. The coating slurry may be used in which the metal-organic framework particles are uniformly dispersed by controlling the type or content of the dispersion medium. The first metal-organic framework particles may exhibit excellent dispersibility in the coating slurry through polyimide modification. For example, the dispersion medium may be one selected from the group consisting of water, ethanol, acetone, isopropyl alcohol (IPA), dimethylacetamide (DMAc), dimethylformamide (DMF), N-methyl-2-pyrrolidone (NMP), acetonitrile, and combinations thereof. Using the above-described type of dispersion medium, a porous coating layer in which the first metal-organic framework particles and the second metal-organic framework particles are uniformly dispersed may be formed.

[0053] The coating slurry may have a viscosity of 20 cps or more and less than 100 cps. Specifically, the viscosity of the coating slurry may be 30 cps or more and 90 cps or less, or 40 cps or more and 80 cps or less. Preferably, the viscosity of the coating slurry may be 25 cps or more and 40 cps or less. If the viscosity of the coating slurry is 100 cps or more, it becomes difficult to manufacture a separation membrane through continuous application to a porous polymer substrate, making it impossible to secure productivity.

[0054] The above coating slurry may further include additives such as a dispersant, a surfactant, an antifoaming agent, a flame retardant, and a wetting agent to improve dispersibility and flame retardancy and to improve the uniformity of the porous coating layer formed. For example, the dispersant may include at least one selected from the group consisting of a soluble polyamine, a soluble amine compound, fatty acids, fatty alcohols, sorbitan fatty acid esters, tannic acid, and pyrogallic acid. By using the above-described type of dispersant, the stability of the coating slurry can be improved and the uniformity of the porous coating layer formed with the coating slurry can be secured.

[0055] The additive may be included in an amount of 0 wt% or more and 5 wt% or less based on the total weight of the coating slurry. Specifically, the content of the additive may be included in an amount of 0.01 wt% or more and 4 wt% or less, 0.1 wt% or more and 3 wt% or less, or 1 wt% or more and 2 wt% or less. Preferably, the content of the additive may be 3 wt% or more and 5 wt% or less. By controlling the content of the additive within the above-described range, uniform dispersion and stability of the first metal-organic framework particles and the second metal-organic framework particles included in the coating slurry can be achieved.

[0056] The dispersion medium included in the coating slurry may be removed by drying or heating after the formation of the porous coating layer. For example, the porous coating layer may include the dispersion medium at 5 ppm or less. Preferably, the porous coating layer may be composed of first metal-organic framework particles, second metal-organic framework particles, and a polymer binder. In the process of removing the dispersion medium, a plurality of pores may be formed on the surface and inside of the porous coating layer. The pores may include interstitial volumes formed between the first metal-organic framework particles, the second metal-organic framework particles, or the first and second metal-organic framework particles, and may have a structure that forms a three-dimensional network through which a fluid may pass.

[0057] The thickness of the porous coating layer may be 1 ㎛ or more and 15 ㎛ or less. Specifically, the thickness of the porous coating layer may be 2 ㎛ or more and 14 ㎛ or less, 3 ㎛ or more and 13 ㎛ or less, 4 ㎛ or more and 12 ㎛ or less, 5 ㎛ or more and 11 ㎛ or less, 6 ㎛ or more and 10 ㎛ or less, or 7 ㎛ or more and 9 ㎛ or less. Preferably, the thickness of the porous coating layer may be 1 ㎛ or more and 5 ㎛ or less. By controlling the thickness of the porous coating layer within the above-described range, shrinkage of the porous polymer substrate can be minimized and stable adhesion to the porous polymer substrate can be achieved.

[0058] The separator for the electrochemical device may have a permeability of 50 s / 100cc or more and 150 s / 100cc or less. Specifically, the permeability of the separator may be 60 s / 100cc or more and 140 s / 100cc or less, 70 s / 100cc or more and 130 s / 100cc or less, 80 s / 100cc or more and 120 s / 100cc or less, or 90 s / 100cc or more and 110 s / 100cc or less. Preferably, the permeability of the separator may be 50 s / 100cc or more and 80 s / 100cc or less. When the permeability of the separator is within the above-described range, the output, stability, and cycle characteristics of the electrochemical device can be secured.

[0059]

[0060] Another specific example of the present invention provides an electrochemical device comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the separator is a separator for the electrochemical device of the above-described specific example. The electrochemical device can be manufactured by inserting and sealing an electrode assembly comprising the positive electrode, the negative electrode, and the separator interposed between the positive electrode and the negative electrode into a case or pouch. An electrolyte may be injected into the case or pouch before sealing to impregnate the electrode assembly with the electrolyte. The shape of the case or pouch is not limited. For example, the electrochemical device can be a cylindrical, square, coin-shaped, or pouch-shaped lithium secondary battery.

[0061] The positive electrode and the negative electrode may be coated by applying and drying an electrode active material on at least one surface of each current collector. The current collector may be a material that is conductive and does not cause a chemical change in the electrochemical device. For example, the current collector for the positive electrode may be, but is not limited to, aluminum, nickel, titanium, sintered carbon, stainless steel; aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc.; and the like. For example, the current collector for the negative electrode may be, but is not limited to, copper, nickel, titanium, sintered carbon, stainless steel; copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc.; and the like. The current collector may be in various forms, such as a metal plate, film, foil, net, porous body, or foam body.

[0062] The positive electrode has a positive electrode current collector and a positive electrode active material layer including a positive electrode active material, a conductive material, and a binder resin on at least one surface of the positive electrode current collector. The positive electrode active material is a layered compound such as lithium manganese oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; chemical formula LiNi 1-x M x Ni-site type lithium nickel oxide represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga and x = 0.01 to 0.3); chemical formula LiMn 1-x M xA lithium manganese composite oxide represented by O2 (wherein, M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (wherein, M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which a portion of Li in the chemical formula is replaced by an alkaline earth metal ion; a disulfide compound; or a mixture of two or more of Fe2(MoO4)3.

[0063] The above negative electrode has a negative electrode current collector and a negative electrode active material layer including a negative electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The negative electrode includes carbon such as lithium metal oxide, non-graphitizable carbon, and graphite carbon as the negative electrode active material; LixFe2O3(0≤x≤1), Li x WO2(0≤x≤1), Si, SiO x (0 <x<2), SiC, Si 합금 등의 실리콘계 재료; Sn x Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of group 1, 2, and 3 of the periodic table, halogens; 0 <x≤1; 1≤y≤3; 1≤z≤8) 등의 금속 복합 산화물; 리튬 금속; 리튬 합금; 주석계 합금; SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, 및 Bi2O5등의 금속 산화물; 폴리아세틸렌 등의 도전성 고분자; Li-Co-Ni 계 재료; 티타늄 산화물 중 선택된 1종 또는 2종 이상의 혼합물을 포함할 수 있다.

[0064] The conductive material may be one or a mixture of two or more conductive materials selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powders, conductive whiskers, conductive metal oxides, carbon nanotubes, activated carbon, and polyphenylene derivatives. The carbon nanotubes have a graphite sheet in the shape of a cylinder with a nano-sized diameter, and sp 2 It has a bonding structure, and exhibits the characteristics of a conductor or a semiconductor depending on the angle and structure at which the graphite plane is rolled. Carbon nanotubes can be classified into single-walled carbon nanotubes (SWCNTs), double-walled carbon nanotubes (DWCNTs), and multi-walled carbon nanotubes (MWCNTs) depending on the number of bonds forming the wall, and these carbon nanotubes can be appropriately selected depending on the use of the dispersion. More specifically, it can be one selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide, or a mixture of two or more conductive materials among these.

[0065] As the above binder resin, a binder resin commonly used in electrodes of electrochemical devices can be used. Non-limiting examples of such binder resins include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-cotrichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. Examples thereof include, but are not limited to, cellulose acetatepropionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, and carboxyl methyl cellulose.

[0066] The above electrolyte is A + B - As a salt with the same structure, A + is Li + , Na +, K + Contains ions composed of alkali metal cations or combinations thereof, such as B - is PF6 - , BF4 - , Cl - , Br - , I - , ClO4 - , AsF6 - , CH3CO2 - , CF3SO3 - , N(CF3SO2)2 - , C(CF2SO2)3 - A salt comprising an anion such as or a combination thereof may be dissolved or dissociated in an organic solvent comprising propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma butyrolactone or a mixture thereof.

[0067] The electrochemical device including the electrode assembly may be a lithium secondary battery. The battery may be used as a unit cell, and may be used as a battery module including the unit cell, a battery pack including the battery module, or a device including the battery pack as a power source. The devices may include, but are not limited to, small devices such as computers, mobile phones, and power tools; electric vehicles including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs) that are powered by an electric motor; electric two-wheeled vehicles including electric bicycles (E-bikes) and electric scooters; electric golf carts; and power storage systems.

[0068]

[0069] Another specific embodiment of the present invention provides a method for manufacturing a separator for an electrochemical device, comprising the step of forming a porous coating layer comprising first metal-organic framework particles modified with polyimide, second metal-organic framework particles, and a polymer binder on at least one surface of a porous polymer substrate. Any content overlapping with that described in the above-described separator for an electrochemical device is replaced by the description of the preceding specific embodiment.

[0070] The step of forming the porous coating layer may include preparing a coating slurry including first metal-organic framework particles, second metal-organic framework particles, a polymer binder, and a dispersion medium, and applying the coating slurry to the porous polymer substrate and drying it.

[0071] The step of forming the porous coating layer may further include a step of corona discharge treating at least one surface of the porous polymer substrate before applying the coating slurry to the porous polymer substrate. The step of corona discharge treating at least one surface of the porous polymer substrate can prevent a decrease in the bonding strength between the surface of the porous polymer substrate and the surface of the coating layer at high temperatures, and can prevent a decrease in the bonding strength between the surface of the polymer substrate and the surface of the coating layer due to an electrolyte.

[0072] The corona discharge treatment may be a treatment of at least one surface of the porous polymer substrate with a voltage of 0.1 kV or more and 10 kV or less in air. Specifically, the corona discharge treatment may be a treatment with a voltage of 0.2 kV or more and 9 kV or less, 0.3 kV or more and 8 kV or less, 0.4 kV or more and 7 kV or less, 0.5 kV or more and 6 kV or less, 0.6 kV or more and 5 kV or less, 0.7 kV or more and 4 kV or less, 0.8 kV or more and 3 kV or less, 0.9 kV or more and 2 kV or less, or 1.0 kV or more and 2 kV or less in air. Preferably, the corona discharge treatment may be a treatment with a voltage of 1.8 kV in air. By controlling the applied voltage of the corona discharge treatment within the above-described range, an appropriate number of functional groups can be formed on the surface of the polymer substrate, and damage to the surface of the polymer substrate can be prevented.

[0073] The step of forming the porous coating layer may include coating the porous polymer substrate by applying the coating slurry. For example, the coating may be formed by a method such as a bar coater, a wire bar coater, a roll coater, a spray coater, a spin coater, an inkjet coater, a screen coater, a reverse coater, a gravure coater, a knife coater, a slot die coater, a hot melt coater, a comma coater, a direct metering coater, etc., but is not limited thereto. Preferably, the step of forming the porous coating layer may be to simultaneously coat the coating slurry on both sides of the porous polymer substrate using a bar coater or a slot die coater.

[0074] The step of forming the porous coating layer may include applying the coating slurry to a porous polymer substrate and then drying or heating the coating layer to evaporate the dispersion medium included in the coating layer. The removal of the dispersion medium may be performed at a temperature that can evaporate only the dispersion medium included in the coating layer without deforming the polymer binder included in the coating layer. For example, the removal of the dispersion medium may be performed by heating the coating layer to a predetermined temperature, but ensuring that the temperature of the surface of the coating layer does not exceed 60°C. When heating the coating layer under the above conditions, thermal energy may be first used to heat and phase-change the dispersion medium, and may not be used to deform the polymer binder.

[0075]

[0076] Hereinafter, the present invention will be described in more detail through specific examples and experimental examples. The following examples and experimental examples are intended to illustrate the present invention, and the present invention is not limited by the following examples and experimental examples.

[0077] Example 1

[0078] Preparation of coating slurry

[0079] The metal-organic framework particles were UiO-66-NH2 (average particle size (D50): 1 μm, average pore diameter: 7 nm, pore volume: 0.8 cm 3 / g) was used. The first metal-organic framework particle modified with polyimide was prepared by reacting the amine group on the surface of the metal-organic framework with the anhydride of polyimide.

[0080] At room temperature (25°C), 100 mL of distilled water was added with an acrylic polymer binder (Toyo ink, CSB130, solid content 40%, average particle diameter (D50) 177 nm): carboxylmethylcellulose (GL Chem, SG-L02): and a wetting agent in a weight ratio of 8:5:1, and 12 g of the first metal-organic framework particles modified with polyimide and 18 g of the second metal-organic framework particles not modified with polyimide were added (weight ratio of (first metal-organic framework + second metal-organic framework): polymer binder 95:5). The mixture was stirred with a shaker for 60 minutes to prepare a coating slurry.

[0081] Preparation of porous polymer substrate

[0082] As a porous polymer substrate (MI: 0.2 g / 10 min, T m : 135℃, porosity: 45%, average pore size: 45 nm) and a polyethylene film with a size of 20 cm × 30 cm and a thickness of 9 ㎛ was used.

[0083] Manufacturing of membranes

[0084] The coating slurry was coated on both sides of a polyethylene film using a bar coater to form a coating layer with a thickness of 3 μm for each coating.

[0085] A process of applying a low-temperature airflow to a polyethylene film on which a coating layer was formed and removing the dispersion medium was repeated five times to manufacture a separation membrane with a total thickness of 15 μm.

[0086] Example 2

[0087] A separation membrane was manufactured in the same manner as in Example 1, except that 10.5 g of the first metal-organic framework particles and 19.5 g of the second metal-organic framework particles were added when manufacturing the coating slurry.

[0088] Comparative Example 1

[0089] A separation membrane was manufactured in the same manner as in Example 1, except that 18 g of the first metal-organic framework particles and 12 g of the second metal-organic framework particles were added when manufacturing the coating slurry.

[0090] Comparative Example 2

[0091] A separation membrane was manufactured in the same manner as in Example 1, except that 9 g of the first metal-organic framework particles and 21 g of the second metal-organic framework particles were added when manufacturing the coating slurry.

[0092] Comparative Example 3

[0093] A separation membrane was manufactured in the same manner as in Example 1, except that 6 g of the first metal-organic framework particles and 24 g of the second metal-organic framework particles were added when manufacturing the coating slurry.

[0094] Comparative Example 4

[0095] A separation membrane was manufactured in the same manner as in Example 1, except that when manufacturing the coating slurry, only 30 g of the second metal-organic framework particles were added without using the first metal-organic framework particles.

[0096] Comparative Example 5

[0097] When manufacturing a coating slurry, alumina (Sumitomo, AES11, average particle diameter (D50) 500 nm, density 4 g / cm) was used without using the first metal-organic framework particles and the second metal-organic framework particles. 3 ) A membrane was manufactured in the same manner as in Example 1, except that 30 g of particles were added.

[0098]

[0099] Experimental example. Confirmation of the physical properties of the membrane.

[0100] The properties of the membranes manufactured in the examples and comparative examples were confirmed and are shown in Table 1 below.

[0101] Measurement of sedimentation rate of sediment in coating slurry

[0102] The sedimentation rate of the precipitate in the coating slurry prepared during the membrane manufacturing process of the examples and comparative examples was determined. The better the dispersibility of the metal-organic framework particles included in the coating slurry, the slower the sedimentation rate of the precipitate.

[0103] The sedimentation rate of the sediment in the coating slurry was determined using a LUMiSizer Dispersion & Particle Size Analyzer (LUM GmbH). The coating slurry was dispensed into the tube of the device, and a centrifugal force of up to 2,300 G was applied to accelerate the sedimentation or creaming phenomenon of the material in the tube. Near-infrared light was continuously transmitted through the entire tube to obtain a transmission profile, and the sedimentation rate of the sediment was calculated from the profile, which is shown in Table 1 below.

[0104] BET surface area measurement

[0105] When the adsorption isotherm was measured at -196℃ condition up to 1 bar using a BET surface area analyzer (BEL, Microtrac Co.) on the coating layer of each membrane, the BET surface area was calculated using the Brunauer-Ennett-Teller model (BET) from the measured N2 adsorption isotherm.

[0106] Measurement of CO2 adsorption capacity of inorganic particles

[0107] At 25°C, using the BET-specific surface area analyzer, carbon dioxide with a purity of 99.99% was passed through the inorganic particles before preparing the coating slurry for each membrane, and the adsorption isotherm curve was measured to measure the amount of carbon dioxide adsorbed relative to the weight of the inorganic particles.

[0108] Method for obtaining CO2 gas volume data

[0109] Lithium manganese composite oxide: Conductive agent (Denka black): Binder (PVdF) were weighed in a weight ratio of 95:2.5:2.5, then added to N-methylpyrrolidone (NMP) and mixed to prepare a positive electrode active material slurry. The positive electrode active material slurry was coated on a 20 ㎛ thick aluminum foil to a thickness of 200 ㎛, and then rolled and dried to prepare a positive electrode.

[0110] A Li metal plate with a thickness of 200 ㎛ was used as the cathode, and the cathode and anode were laminated with the separator of the example or comparative example interposed between them, and then inserted into an aluminum pouch.

[0111] A cell was manufactured by injecting 1 g of an electrolyte solution containing 3 mol of vinylene carbonate (VC), 1.5 mol of propane sultone (PS), 1 mol of ethylene sulfate (ESa), and 1 mol of lithium salt LiPF6 into a solvent in which ethylene carbonate (EC) / ethyl methyl carbonate (EMC) was mixed in a weight ratio of 3 / 7 into the aluminum pouch, and sealing the pouch.

[0112] The manufactured cell was charged and discharged once at 0.1 C in the voltage range of 3.0 V to 4.4 V in a 25°C chamber, and 1.0 C charging and 1.0 C discharging were repeated 300 times.

[0113] The cell that had undergone the above 300 cycles was pierced to capture the gas inside the cell, and the amount of carbon dioxide contained in the gas was quantified using a flame ionization detector (FID) and a thermal conductivity detector (TCD).

[0114] Sedimentation velocity of sediment in the separation coating slurry (㎛ / s) Thickness of separation membrane (㎛) Weight of separation membrane (g / m) 2 ) Packing density of coating layer (g / cm) 3 ) BET (m) of the membrane coating layer 2 / g)CO2 adsorption amount of inorganic particles (mmol / g)CO2 gas amount in cell (㎕)Comparative example 11.61414.96.21.051823.9115Example 12.05614.85.91.023354.693Example 24.26414.75.71.043824.396Comparative example 210.3514.75.50.964213.0103Comparative example 315.3214.84.30.744603.1118Comparative example 423.6214.94.10.6910723.2124Comparative example 53.214.75.30.926.20.2239

Claims

1. Porous polymer substrate; and A porous polymer substrate comprising first metal-organic framework (MOF) particles modified with polyimide, second metal-organic framework particles, and a polymer binder, and a porous coating layer formed on at least one surface of the porous polymer substrate, A separator for an electrochemical device, wherein at least one of the first metal-organic framework particles and the second metal-organic framework particles contains zirconium and has an amine group introduced therein.

2. In paragraph 1, The first metal-organic framework particle and the second metal-organic framework particle are, The average particle diameter (D) according to the particle size distribution analysis (PSD) 50 ) A separator for an electrochemical device having a thickness of 300 nm or more and 10 μm or less.

3. In paragraph 1, The first metal-organic framework particle and the second metal-organic framework particle are, A separator for an electrochemical device, each having an average pore diameter of more than 5 nm and less than 200 nm.

4. In paragraph 1, The first metal-organic framework particle and the second metal-organic framework particle are, Each pore volume per unit mass is 0.2 cm 3 / g or more than 1.0 cm 3 A separator for electrochemical devices having a mass of / g or less.

5. In paragraph 1, A separator for an electrochemical device, wherein the first metal-organic framework particle and the second metal-organic framework particle are independently selected from the group consisting of UiO-66-NH2, UiO-67-NH2, NU-1002-NH2, and MOF-808-NH2.

6. In paragraph 1, A separator for an electrochemical device, wherein the first metal-organic framework particles and the second metal-organic framework particles are included in a weight ratio of 35:65 to 45:

55.

7. In paragraph 1, A separator for an electrochemical device, wherein the metal-organic framework particles and the polymer binder are included in a weight ratio of 80:20 to 95:

5.

8. An electrochemical device comprising a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, An electrochemical device, wherein the above separator is a separator for an electrochemical device according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Separator for electrochemical device and electrochemical device comprising the same

    KR102951501B1

  • MOF composite material and preparation method and application thereof

    CN113871598A

  • Roller Pin Decoupling type CDA system

    KR1020240046987A

  • Communication device of vehicle and control method thereof