Gel polymer electrolyte and preparation method therefor, battery, charging and discharging method of battery, and electric device

By using temperature to adjust the change in cross-linking degree in the gel polymer electrolyte, the problem of reduced capacity and rate performance after battery cycling is solved, and battery performance recovery and safety improvement are achieved.

WO2024216981A1PCT designated stage expired Publication Date: 2024-10-24CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/134691
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-19
Filing Date
2023-11-28
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The capacity retention and rate performance of existing gel polymer electrolytes are significantly reduced after multiple cycles of the battery, resulting in reduced battery safety and performance.

Method used

A gel polymer electrolyte is used, which has different cross-linking degrees at different temperatures. Through temperature adjustment, it undergoes a depolymerization reaction at high temperatures, increases fluidity to restore battery performance, and improves cross-linking at low temperatures. degree to reduce the risk of short circuit.

Benefits of technology

Through temperature regulation, the capacity retention rate and rate performance of the battery are significantly improved, the probability of internal short circuit and electrolyte leakage of the battery is reduced, and the service life of the battery is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023134691_24102024_PF_FP_ABST
    Figure CN2023134691_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application discloses a gel polymer electrolyte and a preparation method therefor, a battery, a charging and discharging method of a battery, and an electric device. The gel polymer electrolyte has a first state at a first temperature and a second state at a second temperature, mutual switching between the first state and the second state is allowed, the first temperature is higher than the second temperature, and the crosslinking degree of the gel polymer electrolyte in the second state is higher than that of the gel polymer electrolyte in the first state. Thus, even after multiple cycles, the battery comprising the gel polymer electrolyte of the present application still has a high capacity retention rate and high rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Gel polymer electrolyte and preparation method thereof, battery, battery charging and discharging method and electrical device

[0001] Priority information

[0002] This application claims priority and benefits of patent application 202310424149.1 filed with the State Intellectual Property Office of China on April 19, 2023, and the entire text of which is incorporated herein by reference. Technical Field

[0003] The present application relates to the technical field of secondary batteries, and in particular to a gel polymer electrolyte and a preparation method thereof, a battery, a battery charging and discharging method, and an electrical device. Background Art

[0004] Currently, batteries on the market mainly use liquid electrolytes as ion conduction media. Accidents are prone to occur when the batteries are overcharged, overheated, short-circuited, or impacted.

[0005] Therefore, using gel polymer electrolytes instead of liquid electrolytes as ion-conducting media is an effective solution to reduce the probability of battery accidents. However, the capacity retention and rate performance of existing batteries using gel polymer electrolytes will significantly decrease after multiple cycles.

[0006] Public content

[0007] In view of the technical problems existing in the background technology, the present application provides a gel polymer electrolyte, which aims to solve the problem that the capacity retention rate and rate performance of the battery containing the gel polymer electrolyte are significantly reduced after multiple cycles.

[0008] In order to achieve the above-mentioned objectives, the first aspect of the present application provides a gel polymer electrolyte, wherein the gel polymer electrolyte has a first state at a first temperature and a second state at a second temperature, the first state and the second state are mutually transformable, the first temperature is higher than the second temperature, and the cross-linking degree of the gel polymer electrolyte in the second state is higher than the cross-linking degree of the gel polymer electrolyte in the first state.

[0009] Compared to the prior art, the present application provides at least the following beneficial effects: After the battery undergoes multiple cycles at the second temperature, gaps appear between the battery electrode and the gel polymer electrolyte interface, causing the battery capacity to deteriorate. Raising the battery to the first temperature causes the gel polymer electrolyte to depolymerize, increasing the amount of mobile phase in the gel polymer electrolyte, thereby tightening the bond between the battery electrode and the gel polymer electrolyte and restoring the battery's capacity. Furthermore, the increased amount of mobile phase in the gel polymer electrolyte improves the ionic conductivity of the gel polymer electrolyte, thereby enhancing the battery's rate performance.

[0010] In some embodiments of the present application, the ratio of the crosslinking degree of the gel polymer electrolyte in the first state to the crosslinking degree in the second state is 0.2-0.95: 1. Thus, within the above range, the capacity retention rate and rate performance of the battery at the first temperature can be further improved.

[0011] In some embodiments of the present application, the first temperature is greater than or equal to 40° C., and may be 40° C.-120° C. Therefore, within this temperature range, the gel polymer is in the first state, which can further improve the capacity retention and rate performance of the battery at the first temperature.

[0012] In some embodiments of the present application, the crosslinking degree of the gel polymer electrolyte in the first state is 20%-48.5%. Therefore, within the above crosslinking degree range, the crosslinking degree of the gel polymer is relatively low, which can improve the capacity retention and rate performance of the battery in the first state.

[0013] In some embodiments of the present application, the second temperature is -25°C-35°C.

[0014] In some embodiments of the present application, the cross-linking degree of the gel polymer electrolyte in the second state is 50%-99%.

[0015] In some embodiments of the present application, the gel polymer electrolyte further comprises an electrolyte, and the electrolyte accounts for 60% to 98% by weight of the gel polymer electrolyte. Thus, the gel polymer electrolyte obtained within the above ratio range, when used in a battery, can improve the battery's capacity retention and rate performance.

[0016] In some embodiments of the present application, the gel polymer electrolyte includes a first cross-linking agent and a second cross-linking agent, and the decrosslinking temperature of the second cross-linking agent is greater than or equal to 40°C, and can be selected from 40°C to 120°C. Therefore, when the battery is raised to the first temperature, i.e., the decrosslinking temperature of the second cross-linking agent is reached, at least a portion of the second cross-linking agent is decrosslinked, which can improve the capacity retention and rate performance of the battery at the first temperature.

[0017] In some embodiments of the present application, the first cross-linking agent includes at least one of an acrylate cross-linking agent and a conjugated diene.

[0018] In some embodiments of the present application, the acrylate crosslinking agent includes at least one of ethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, trimethylolpropane ethoxylated triacrylate, trimethylolpropane propoxylated triacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol tetraacrylate, pentaerythritol ethoxylated tetraacrylate, dipentaerythritol pentaacrylate, and dipentaerythritol hexaacrylate. Thus, when the battery reaches the first temperature, the gel polymer electrolyte is prevented from completely de-crosslinking, thereby ensuring that the gel polymer electrolyte functions effectively and improving the capacity retention and rate performance of the battery at the first temperature.

[0019] In some embodiments of the present application, the conjugated diene comprises at least one of divinylbenzene and 1,3-butadiene.

[0020] In some embodiments of the present application, the second crosslinker includes at least one of maleimide and an N-substituted derivative of maleimide. Thus, when the battery reaches the first temperature, at least a portion of the second crosslinker decouples, thereby improving the capacity retention and rate performance of the battery at the first temperature.

[0021] In some embodiments of the present application, the molar ratio of the first crosslinking agent to the second crosslinking agent is 0.5-5: 1. Thus, the ratio of the first crosslinking agent to the second crosslinking agent within the above range can improve the capacity retention and rate performance of the battery at the first temperature.

[0022] In some embodiments of the present application, the gel polymer electrolyte further comprises a host material, wherein monomers of the host material include at least one of vinyl, epoxy, allyl, acryloyl, and methacryloyl groups. Thus, during polymerization to form the host material, the monomers of the host material can undergo cross-linking reactions with the first and second cross-linking agents, respectively, thereby improving the battery's capacity retention and rate performance.

[0023] In some embodiments of the present application, the monomers of the host material include at least one of furfuryl methacrylate, ethylene glycol diglycidyl ether, 1,5-hexadiene diepoxide, glycerol propoxylated triglycidyl ether, vinylcyclohexene dioxide, 1,2,7,8-diepoxyoctane, 4-vinylcyclohexene dioxide, butyl glycidyl ether, 1,2-cyclohexanedicarboxylic acid diglycidyl ester, ethylene glycol diglycidyl ether, glycerol triglycidyl ether, and glycidyl methacrylate. Thus, the monomers of the host material can undergo cross-linking reactions with the first cross-linking agent and the second cross-linking agent, respectively, during polymerization to form the host material, thereby improving the capacity retention and rate performance of the battery.

[0024] A second aspect of the present application provides a method for preparing a gel polymer electrolyte, comprising:

[0025] The monomer of the main substance, initiator, cross-linking agent and electrolyte are mixed and polymerized to obtain a gel polymer electrolyte.

[0026] The gel polymer electrolyte has a first state at a first temperature and a second state at a second temperature, the first state and the second state are mutually transformable, the first temperature is higher than the second temperature, and the crosslinking degree of the gel polymer electrolyte in the second state is higher than the crosslinking degree of the gel polymer electrolyte in the first state.

[0027] Therefore, when the gel polymer electrolyte prepared in the present application is used in a battery, after the battery has experienced capacity attenuation after multiple cycles, the capacity retention rate and rate performance of the battery can be improved by raising the battery to a second temperature.

[0028] In some embodiments of the present application, the cross-linking agent includes a first cross-linking agent and a second cross-linking agent, and the de-crosslinking temperature of the second cross-linking agent is greater than or equal to 40° C., and can be selected from 40° C. to 120° C. Thus, when the battery is raised to the first temperature, that is, the de-crosslinking temperature of the second cross-linking agent is reached, at least a portion of the second cross-linking agent is de-crosslinked, which can improve the capacity retention and rate performance of the battery at the first temperature.

[0029] In some embodiments of the present application, the molar ratio of the monomer of the host substance to the cross-linking agent is 1:2-10. Thus, the gel polymer electrolyte obtained within the above ratio range, when used in a battery, can improve the capacity retention rate and rate performance of the battery at the first temperature.

[0030] The third aspect of the present application provides a battery comprising the gel polymer electrolyte described in the first aspect of the present application or the gel polymer electrolyte prepared by the method described in the second aspect, thereby having good capacity retention and rate performance.

[0031] A fourth aspect of the present application provides a battery charging and discharging method,

[0032] The battery includes a gel polymer electrolyte, wherein the gel polymer electrolyte has a first state at a first temperature and a second state at a second temperature, the first state and the second state being mutually transitionable, the first temperature being higher than the second temperature, and the crosslinking degree of the gel polymer electrolyte in the second state being higher than the crosslinking degree of the gel polymer electrolyte in the first state;

[0033] When the battery meets a first preset condition, charging and discharging the battery at a first temperature;

[0034] When the battery meets the second preset condition, the battery is charged and discharged at a second temperature.

[0035] Therefore, under different conditions, by adjusting the battery temperature, the battery capacity retention and rate performance can be improved.

[0036] In some embodiments of the present application, the first preset condition is that a ratio of a current internal resistance of the battery to an initial internal resistance of the battery is greater than 1.5.

[0037] In some embodiments of the present application, the second preset condition is that the ratio of the current internal resistance of the battery to the initial internal resistance of the battery is less than or equal to 1.5.

[0038] In some embodiments of the present application, the first preset condition is that the battery discharge rate is greater than 2C. In some embodiments of the present application, the second preset condition is that the battery discharge rate is less than or equal to 2C.

[0039] A fifth aspect of the present application provides an electrical device, which includes the battery described in the third aspect, and the battery is used to provide electrical energy.

[0040] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become obvious from the description below, or will be learned through practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiment below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the drawings to represent the same components. In the drawings:

[0042] FIG1 is a schematic structural diagram of a battery according to an embodiment of the present application;

[0043] FIG2 is a schematic structural diagram of a battery module according to an embodiment of the present application;

[0044] FIG3 is a schematic structural diagram of a battery pack according to an embodiment of the present application;

[0045] FIG4 is an exploded view of FIG3 ;

[0046] FIG5 is a schematic diagram of an embodiment of an electric device using a battery as a power source.

[0047] Explanation of reference numerals: 1: secondary battery; 2: battery module; 3: battery pack; 4: upper case; 5: lower case. DETAILED DESCRIPTION

[0048] The following embodiments of the technical solution of the present application are described in detail. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only used as examples and are not intended to limit the scope of protection of the present application.

[0049] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0050] For the sake of clarity, only some numerical ranges are specifically disclosed herein. However, any lower limit may be combined with any upper limit to form an unspecified range; and any lower limit may be combined with other lower limits to form an unspecified range, and similarly, any upper limit may be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value may itself serve as a lower limit or upper limit and be combined with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.

[0051] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.

[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.

[0053] With the technological development and increasing demand for electric vehicles and rechargeable mobile devices, secondary batteries, as a representative of the new energy field, and related research work are also developing rapidly.

[0054] Typically, electrolytes are dissolved in a solvent to form an electrolyte solution. Electrolytes are the ionic conductive medium between the positive and negative electrodes in a battery. Currently, batteries used in the market primarily use liquid electrolytes. However, liquid ion batteries are prone to internal short circuits, electrolyte leakage, and combustion during use. To address these risks in liquid ion batteries, researchers have proposed gel polymer electrolytes.

[0055] Gel polymer electrolytes have the advantages of solid electrolytes such as being less prone to short circuits and electrolyte leakage. At the same time, their room temperature ionic conductivity can meet the needs of practical applications. In addition, gel polymer electrolytes have good processability, and the battery design can be flexible and diverse, which greatly promotes the development and large-scale application of the battery industry.

[0056] Existing gel polymer electrolytes have rubber-like elasticity and good processing properties. The most studied gel electrolytes include polyethylene oxide (PEO) system gel electrolytes, polyacrylonitrile system (PAN) gel electrolytes, polymethyl methacrylate system (PMMA) gel electrolytes, polyvinylidene fluoride (PVDF) and its copolymer system gel electrolytes.

[0057] However, after multiple cycles, the interfacial contact between the battery electrodes and the gel polymer electrolyte deteriorates, and the ionic conductivity of the electrolyte decreases, resulting in a significant decrease in the battery's capacity retention and rate performance.

[0058] In the present application, the gel polymer electrolyte used has a first state at a first temperature and a second state at a second temperature. The first state and the second state can be transformed into each other. The first temperature is higher than the second temperature. The battery operates normally in the second temperature range and is discharged at normal power. At this time, the battery electrolyte is semi-solid, and the probability of problems such as internal short circuit, electrolyte leakage, and combustion is low. After the battery capacity deteriorates, the battery is heated to the first temperature for charge and discharge. At this time, part of the gel polymer electrolyte depolymerizes, and the flow state in the gel polymer electrolyte increases, with lower internal resistance and higher ionic conductivity. Under different conditions, by adjusting the operating temperature of the battery, the corresponding charge and discharge temperature can be selected in a targeted manner according to the specific situation of the battery to provide high capacity retention and rate performance.

[0059] The gel polymer electrolyte disclosed in the embodiments of the present application is suitable for gel-state batteries, i.e., semi-solid batteries, and the batteries disclosed in the embodiments of the present application can be used in electrical devices that use batteries as power sources or various energy storage systems that use batteries as energy storage elements. Electrical devices may include, but are not limited to, mobile phones, tablets, laptops, electric toys, electric tools, battery cars, electric cars, ships, spacecraft, and the like. Among them, electric toys may include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, and the like, and spacecraft may include airplanes, rockets, space shuttles, and spacecraft, and the like.

[0060] In a first aspect, the present application provides a gel polymer electrolyte, which has a first state at a first temperature and a second state at a second temperature, the first state and the second state being mutually transformable, the first temperature being higher than the second temperature, and the crosslinking degree of the gel polymer electrolyte in the second state being higher than the crosslinking degree of the gel polymer electrolyte in the first state.

[0061] The degree of crosslinking is a physical quantity used to indicate the degree of crosslinking in a polymer, i.e., the fraction of crosslinked structural units Nc in the crosslinked chain to the total structural units N. The degree of crosslinking can be measured using a nuclear magnetic crosslink density analyzer. Specifically, in the embodiments of the present application, an IIC XLDS-15 crosslink density spectrometer can be used for measurement.

[0062] After the polymer is cross-linked, its fluidity becomes worse. Therefore, in the present application, since the degree of cross-linking at the second temperature is higher than that at the first temperature, the fluidity of the gel polymer electrolyte at the second temperature is worse than that at the first temperature. That is, the fluidity of the gel polymer electrolyte at the second temperature, which is low, is higher than that at the first temperature, which is high in cross-linking and poor in fluidity.

[0063] Compared to the prior art, the present application provides at least the following beneficial effects: After the battery undergoes multiple cycles at the second temperature, gaps appear between the battery electrode and the gel polymer electrolyte interface, causing the battery capacity to deteriorate. Raising the battery to the first temperature causes the gel polymer electrolyte to depolymerize, reducing the degree of crosslinking. This increases the amount of mobile phase in the gel polymer electrolyte, tightening the bond between the battery electrode and the gel polymer electrolyte, thereby restoring the battery's capacity. Furthermore, the increased amount of mobile phase in the gel polymer electrolyte improves the ionic conductivity of the gel polymer electrolyte, thereby enhancing the battery's rate performance.

[0064] In some embodiments of the present application, the ratio of the crosslinking degree of the gel polymer electrolyte in the first state to the crosslinking degree in the second state is 0.2-0.95:1, for example, 0.3-0.9:1, 0.4-0.8:1, 0.5-0.7:1, etc. Thus, within the above range, the crosslinking degree of the gel polymer electrolyte in the first state is low, and the crosslinking degree in the second state is high, which can further improve the capacity retention and rate performance of the battery at the first temperature.

[0065] In some embodiments of the present application, the first temperature is greater than or equal to 40°C. For example, it can be 40°C-120°C, 45°C-120°C, 45°C-110°C, 45°C-100°C, 45°C-90°C, 50°C-80°C, 55°C-75°C, 60°C-70°C, etc. Therefore, within this temperature range, the cross-linking degree of the gel polymer is relatively low, the mobile phase increases, and the capacity retention rate and rate performance of the battery at the first temperature can be further improved.

[0066] In some embodiments of the present application, the crosslinking degree of the gel polymer electrolyte in the first state is 20%-48.5%, for example, 22%-48.5%, 25%-45%, 28%-44%, 30%-40%, 35%-39%, etc. Thus, within the above crosslinking degree range, the crosslinking degree of the gel polymer is relatively low, the mobile phase is increased, and the electrode and the gel polymer electrolyte are tightly bonded, which can improve the capacity retention and rate performance of the battery at the first temperature.

[0067] In some embodiments of the present application, the second temperature is -25°C-35°C. For example, it can be -22°C-35°C, -20°C-30°C, -15°C-25°C, -10°C-20°C, -5°C-15°C, 0°C-10°C, 3°C-8°C, etc. Therefore, within the above temperature range, the cross-linking degree of the gel polymer is relatively high, which can reduce the probability of internal short circuits, electrolyte leakage, combustion, etc. in the battery.

[0068] In some embodiments of the present application, the crosslinking degree of the gel polymer electrolyte in the second state is 50%-99%, for example, 52%-99%, 55%-95%, 60%-90%, 65%-85%, 70%-80%, etc. Thus, within the above crosslinking degree range, the probability of internal short circuits, electrolyte leakage, combustion, etc. in the battery can be reduced.

[0069] In some embodiments of the present application, the gel polymer electrolyte further includes an electrolyte. The mass proportion of the electrolyte in the gel polymer electrolyte is 60%-98%, for example, 60%-95%, 65%-90%, 70%-85%, 75%-80%, etc. Thus, the gel polymer electrolyte obtained within the above ratio range, when used in a battery, can improve the battery's capacity retention and rate performance.

[0070] In some embodiments of the present application, the gel polymer electrolyte includes a first cross-linking agent and a second cross-linking agent, and the decrosslinking temperature of the second cross-linking agent is greater than or equal to 40°C, for example, it can be 40°C-120°C, 45°C-120°C, 45°C-110°C, 40°C-100°C, 45°C-90°C, 50°C-80°C, 55°C-75°C, 60°C-70°C, etc.

[0071] Decrosslinking is the reverse reaction of crosslinking. Crosslinking refers to the reaction in which two or more molecules (usually linear molecules) bond with each other to form a network structure (bulk molecules), while decrosslinking is the reaction in which the molecules of the network structure are decomposed into two or more molecules. For example, if crosslinking is carried out through the Diels-Alder reaction, then decrosslinking is the reverse Diels-Alder reaction.

[0072] The temperature at which the polymer in the gel polymer electrolyte and the second crosslinking agent begin to decrosslink is the decrosslinking temperature, that is, the temperature at which the polymer in the gel polymer electrolyte and the second crosslinking agent begin to decrosslink from a crosslinked state.

[0073] In the embodiment of the present application, in the gel polymer electrolyte, the crosslinking and decrosslinking of the polymer are reversible reactions. At a high first temperature, at least a portion of the second crosslinker undergoes a decrosslinking reaction with the polymer main body, and at a low second temperature, the second crosslinker undergoes a crosslinking reaction with the polymer main body.

[0074] In the embodiment of the present application, the presence of the first cross-linking agent is to prevent the gel polymer electrolyte from being completely de-cross-linked into a mobile phase at a high first temperature. Therefore, when the de-cross-linking temperature of the second cross-linking agent is reached, the first cross-linking agent still remains in a cross-linked state, and at least a portion of the second cross-linking agent is de-cross-linked with the polymer in the gel polymer electrolyte, thereby ensuring that the gel polymer electrolyte functions, and can improve the capacity retention rate and rate performance of the battery at the first temperature.

[0075] In some embodiments of the present application, the first crosslinking agent may include at least one of an acrylate crosslinking agent and a conjugated diene. For example, the acrylate crosslinking agent includes at least one of ethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, trimethylolpropane ethoxylated triacrylate, trimethylolpropane propoxylated triacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol tetraacrylate, pentaerythritol ethoxylated tetraacrylate, dipentaerythritol pentaacrylate, and dipentaerythritol hexaacrylate. The conjugated diene includes at least one of divinylbenzene and 1,3-butadiene. Thus, when the first crosslinking agent is used, all polymers in the gel polymer electrolyte are prevented from de-crosslinking with the second crosslinking agent at the first temperature, thereby ensuring that the gel polymer electrolyte functions effectively and improving the capacity retention and rate performance of the battery.

[0076] In some embodiments of the present application, the second cross-linking agent includes at least one of maleimide and an N-substituted derivative of maleimide.

[0077] N-substituted derivatives of maleimide refer to organic compounds obtained by replacing the hydrogen atoms on the imine group in maleimide with other groups, for example, N-phenylmaleimide (NPMI), N-butylmaleimide (BMI), etc. As long as they are N-substituted derivatives of maleimide, they are within the scope of protection of this application.

[0078] Therefore, by using the above-mentioned second cross-linking agent, when the de-crosslinking temperature of the second cross-linking agent is reached, at least part of the second cross-linking agent and the polymer in the gel polymer electrolyte are de-crosslinked, which can improve the capacity retention rate and rate performance of the battery at the first temperature.

[0079] It is understandable that the first cross-linking agent and the second cross-linking agent mentioned above in the present application can be purchased on the market or prepared by synthetic methods in the art.

[0080] In some embodiments of the present application, the molar ratio of the first crosslinker to the second crosslinker is 0.5-5:1, for example, 0.7-5:1, 1-4.5:1, 1.5-4:1, 2-3.5:1, 2.5-2:1, etc. Thus, when the ratio of the first crosslinker to the second crosslinker is within the above range, the polymer in the gel polymer electrolyte can be partially de-crosslinked at a high first temperature and crosslinked at a low second temperature, thereby improving the capacity retention and rate performance of the battery at the first temperature.

[0081] In some embodiments of the present application, the gel polymer electrolyte further comprises a host material, wherein monomers of the host material comprise at least one of vinyl, epoxy, allyl, acryloyl, and methacryloyl groups. Thus, during polymerization to form the host material, the monomers of the host material can undergo cross-linking reactions with the first and second cross-linking agents, respectively, to achieve partial decrosslinking of the polymers in the gel polymer electrolyte at a first, high temperature and cross-linking at a second, low temperature, thereby improving the battery's capacity retention and rate performance.

[0082] In some embodiments of the present application, the monomers of the host material include at least one of furfuryl methacrylate, ethylene glycol diglycidyl ether, 1,5-hexadiene diepoxide, glycerol propoxylated triglycidyl ether, vinylcyclohexene dioxide, 1,2,7,8-diepoxyoctane, 4-vinylcyclohexene dioxide, butyl glycidyl ether, 1,2-cyclohexanedicarboxylic acid diglycidyl ester, ethylene glycol diglycidyl ether, glycerol triglycidyl ether, and glycidyl methacrylate. Thus, during the polymerization process to form the host material, the monomers of the host material can undergo cross-linking reactions with the first cross-linking agent and the second cross-linking agent, respectively, and achieve partial decrosslinking of the polymer in the gel polymer electrolyte at a high first temperature and cross-linking at a low second temperature, thereby improving the capacity retention and rate performance of the battery at the first temperature.

[0083] It is understandable that the monomers of the above-mentioned main substances can be purchased on the market or prepared by synthetic methods in the art.

[0084] In some embodiments of the present application, the gel polymer electrolyte includes a polymer matrix and an electrolyte solution, and the electrolyte solution may include an electrolyte salt and a solvent.

[0085] When the battery is a lithium-ion battery, as an example, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).

[0086] When the battery is a sodium ion battery, as an example, the electrolyte sodium salt may include at least one of sodium hexafluorophosphate, sodium difluorooxalatoborate, sodium tetrafluoroborate, sodium bisoxalatoborate, sodium perchlorate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide, sodium trifluoromethanesulfonate and sodium bis(trifluoromethylsulfonyl)imide.

[0087] As an example, the solvent may include one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0088] In some embodiments, the electrolyte further includes additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives capable of improving certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature performance.

[0089] A second aspect of the present application provides a method for preparing a gel polymer electrolyte, comprising:

[0090] The monomer of the main substance, initiator, cross-linking agent and electrolyte are mixed and polymerized to obtain a gel polymer electrolyte.

[0091] The gel polymer electrolyte has a first state at a first temperature and a second state at a second temperature, the first state and the second state are mutually transformable, the first temperature is higher than the second temperature, and the crosslinking degree of the gel polymer electrolyte in the second state is higher than the crosslinking degree of the gel polymer electrolyte in the first state.

[0092] Therefore, when the gel polymer electrolyte prepared in this application is used in a battery, after the battery has been cycled multiple times at the second temperature, gaps appear between the battery electrode and the gel polymer electrolyte interface, causing the battery capacity to deteriorate continuously. At this time, raising the battery to the first temperature causes the gel polymer electrolyte to depolymerize, increasing the amount of mobile phase in the gel polymer electrolyte, and making the battery electrode and the gel polymer electrolyte more tightly bonded, thereby restoring the battery's capacity. At the same time, the increase in mobile phase in the gel polymer electrolyte can improve the ionic conductivity of the gel polymer electrolyte, thereby improving the battery's rate performance.

[0093] In some embodiments of the present application, the cross-linking agent includes a first cross-linking agent and a second cross-linking agent, and the decrosslinking temperature of the second cross-linking agent is greater than or equal to 40°C, for example, it can be 40°C-120°C, 45°C-110°C, 40°C-100°C, 45°C-90°C, 50°C-80°C, 55°C-75°C, 60°C-70°C, etc. Thus, when the battery is heated to the first temperature and reaches the decrosslinking temperature of the second cross-linking agent, at least part of the second cross-linking agent is decross-linked with the polymer in the gel polymer electrolyte, and the mobile phase in the gel polymer electrolyte increases, which can improve the capacity retention rate and rate performance of the battery at the first temperature.

[0094] In some embodiments of the present application, the molar ratio of the monomer of the host substance to the cross-linking agent is 1:2-10, for example, 1:3-10, 1:4-9, 1:5-8, 1:6-7, etc. Thus, when the gel polymer electrolyte obtained within the above ratio range is used in a battery, the gel polymer electrolyte and at least a portion of the second cross-linking agent are decrosslinked at a high first temperature and cross-linked at a low second temperature, which can further improve the capacity retention and rate performance of the battery at the first temperature.

[0095] It is understood that when the cross-linking agent includes a first cross-linking agent and a second cross-linking agent, the molar ratio of the monomer of the host substance to the cross-linking agent refers to the ratio of the molar amount of the monomer to the sum of the molar amounts of the first cross-linking agent and the second cross-linking agent. In addition, the temperature at which the monomer of the host substance, the initiator, the cross-linking agent, and the electrolyte are mixed and polymerized is not limited in this application. In some embodiments of this application, the polymerization temperature is 60°C-80°C, for example, 65°C-80°C, 65°C-75°C, 65°C-70°C, etc., to achieve a rapid reaction with minimal side reactions.

[0096] It should be noted that the features and advantages described above for the gel polymer electrolyte are also applicable to the method for preparing the gel polymer electrolyte, and will not be described in detail here.

[0097] The third aspect of the present application provides a battery comprising the gel polymer electrolyte described in the first aspect of the present application or the gel polymer electrolyte prepared by the method described in the second aspect, thereby having good capacity retention and rate performance.

[0098] A battery is a battery that can be recharged to activate the active materials after discharge and continue to be used.

[0099] The positive electrode sheet, separator, and negative electrode sheet can be wound sequentially and placed into a shell. An electrolyte containing polymer monomers is then injected into the shell. The interior of the battery cell is soaked with the electrolyte containing polymer monomers. External conditions, such as heat treatment, trigger a curing reaction of the polymer monomers to form a polymer matrix, thereby ensuring that the battery cell is filled with a gel polymer electrolyte composed of a polymer matrix and electrolyte. Alternatively, the separator can be omitted, and the positive and negative electrode sheets can be wound and placed into the shell. The electrolyte containing polymer monomers is then injected into the shell.

[0100] In some embodiments of the present application, the battery may be a lithium-ion battery or a sodium-ion battery.

[0101] [Positive electrode]

[0102] In a battery, the positive electrode sheet generally includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material.

[0103] The positive electrode current collector may be a conventional metal foil or a composite current collector (a metal material may be disposed on a polymer substrate to form a composite current collector). As an example, the positive electrode current collector may be an aluminum foil.

[0104] There is no limitation on the specific type of the positive electrode active material. Any active material known in the art that can be used for a positive electrode of a battery can be used. Those skilled in the art can select the material based on actual needs.

[0105] For example, when the battery is a lithium-ion battery, as an example, the positive electrode active material may include, but is not limited to, one or more of lithium transition metal oxides, olivine-structured lithium-containing phosphates, and their respective modified compounds. Examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their modified compounds. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, a composite material of lithium manganese iron phosphate and carbon, and their modified compounds. These materials can all be obtained through commercial channels.

[0106] For example, when the battery is a sodium ion battery, as an example, the positive electrode active material may include, but is not limited to, at least one of a layered transition metal oxide, a polyanion compound, and a Prussian blue analog.

[0107] Examples of the layered transition metal oxides include:

[0108] Na 1-x Cu h Fe k Mn l M 1 m O 2-y , where M 1 One or more of Li, Be, B, Mg, Al, K, Ca, Ti, Co, Ni, Zn, Ga, Sr, Y, Nb, Mo, In, Sn and Ba, 0 <x≤0.33,0<h≤0.24,0≤k≤0.32,0<l≤0.68,0≤m<0.1,h+k+l+m=1,0≤y<0.2;

[0109] Na 0.67 Mn 0.7 Ni z M 2 0.3-z O2, where M 2 is one or more of Li, Mg, Al, Ca, Ti, Fe, Cu, Zn and Ba, 0 <z≤0.1;

[0110] Na a Li b Ni c Mn d Fe e O2, of which 0.67 <a≤1,0<b<0.2,0<c<0.3,0.67<d+e<0.8,b+c+d+e=1。

[0111] Examples of the polyanionic compound include:

[0112] A 1 f M 3 g (PO4) i O j X 1 3-j , where A 1 is one or more of H, Li, Na, K and NH4, M 3 is one or more of Ti, Cr, Mn, Fe, Co, Ni, V, Cu and Zn, X 1is one or more of F, Cl, and Br, 0 < f ≤ 4, 0 < g ≤ 2, 1 ≤ i ≤ 3, 0 ≤ j ≤ 2;

[0113] Na n M 4 PO4X 2 , where M 4 is one or more of Mn, Fe, Co, Ni, Cu, and Zn, X 2 is one or more of F, Cl, and Br, 0 < n ≤ 2;

[0114] Na p M 5 q (SO4)3, where M 5 is one or more of Mn, Fe, Co, Ni, Cu, and Zn, where 0 < p ≤ 2, 0 < q ≤ 2;

[0115] Na s Mn t Fe 3-t (PO4)2(P2O7), where 0 < s ≤ 4, 0 ≤ t ≤ 3, for example, t is 0, 1, 1.5, 2, or 3.

[0116] As an example of the above Prussian blue analogs, for example, the following can be listed:

[0117] A u M 6 v [M 7 (CN)6] w ·xH2O, where A is H + 、NH4 + 、an alkali metal cation, and an alkaline earth metal cation, M 6 and M 7 are each independently one or more of transition metal cations, 0 < u ≤ 2, 0 < v ≤ 1, 0 < w ≤ 1, 0 < x < 6. For example, A is H + 、Li + 、Na + 、K + 、NH4 + 、Rb + 、Cs + 、Fr + 、Be 2+ 、Mg 2+ 、Ca<\ 2+ 、Sr 2+ 、Ba 2+ and Ra 2+ is one or more of them, M 6 and M 7Each is independently a cation of one or more transition metal elements selected from Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Sn and W.

[0118] The modified compounds of the above materials may be doping-modified and / or surface-coated modified materials.

[0119] The positive electrode active material layer may also optionally include a binder, a conductive agent, and other optional auxiliary agents.

[0120] As an example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, Super P (SP), graphene, and carbon nanofibers.

[0121] As an example, the binder may include one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB).

[0122] [Negative electrode]

[0123] In a battery, the negative electrode sheet generally includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode active material.

[0124] The negative electrode current collector may be a conventional metal foil or a composite current collector (for example, a metal material may be disposed on a polymer substrate to form a composite current collector). As an example, the negative electrode current collector may be a copper foil.

[0125] The specific type of the negative electrode active material is not limited, and active materials that can be used for the negative electrode of the battery known in the art can be used, and those skilled in the art can choose according to actual needs. As an example, the negative electrode active material may include but is not limited to one or more of artificial graphite, natural graphite, hard carbon, soft carbon, silicon-based materials and tin-based materials. The silicon-based material may include one or more of elemental silicon, silicon oxide compounds (such as silicon monoxide), silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may include one or more of elemental tin, tin oxide compounds, and tin alloys. These materials can all be obtained through commercial channels.

[0126] In some embodiments, to further improve the energy density of the battery, the negative electrode active material may include a silicon-based material.

[0127] The negative electrode active material layer may further include a binder, a conductive agent, and other optional auxiliary agents.

[0128] As an example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0129] As an example, the binder may include one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB).

[0130] As examples, other optional additives may include thickening and dispersing agents (eg, sodium carboxymethyl cellulose CMC-Na), and PTC thermistor materials.

[0131] As the above-mentioned isolation membrane, the present application has no special restrictions and any known porous structure isolation membrane with electrochemical stability and mechanical stability can be selected according to actual needs. For example, it can include a single-layer or multi-layer film containing one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride.

[0132] The embodiment of the present application has no particular limitation on the shape of the battery, which can be cylindrical, square or any other shape. FIG1 shows a square battery 1 as an example.

[0133] In some embodiments, the battery may include an outer packaging for encapsulating the positive electrode sheet, the negative electrode sheet, and the electrolyte.

[0134] In some embodiments, the outer packaging may include a housing and a cover. The housing may include a bottom plate and side plates connected to the bottom plate, with the bottom plate and side plates enclosing a receiving cavity. The housing may have an opening communicating with the receiving cavity, and the cover may be positioned over the opening to seal the receiving cavity.

[0135] The positive electrode sheet, negative electrode sheet, and separator can be wound or laminated to form an electrode assembly. The electrode assembly is encapsulated in the housing. The number of electrode assemblies in a battery can be one or more, adjustable based on demand.

[0136] In some embodiments, the outer packaging of the battery may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell.

[0137] The outer packaging of the battery may also be a soft bag, such as a bag-type soft bag. The material of the soft bag may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0138] In some embodiments, batteries may be assembled into a battery module. The battery module may contain multiple batteries, and the specific number may be adjusted according to the application and capacity of the battery module.

[0139] Figure 2 shows an example battery module 2. Referring to Figure 2 , within the battery module 2, multiple batteries 1 may be arranged sequentially along the length of the battery module 2. Of course, any other arrangement is also possible. Furthermore, the multiple batteries 1 may be secured together using fasteners.

[0140] The battery module 2 may further include a housing having a housing space, wherein the housing space accommodates a plurality of secondary batteries 1. In some embodiments, the battery modules may be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0141] Figures 3 and 4 illustrate an example battery pack 3. Referring to Figures 3 and 4 , the battery pack 3 may include a battery box and multiple battery modules 2 disposed within the battery box. The battery box comprises an upper case 4 and a lower case 5. The upper case 4 can be placed over the lower case 5 to form an enclosed space for accommodating the battery modules 2. The multiple battery modules 2 can be arranged in any manner within the battery box.

[0142] The fourth aspect of the present application provides a battery charging and discharging method,

[0143] The battery includes a gel polymer electrolyte, wherein the gel polymer electrolyte has a first state at a first temperature and a second state at a second temperature, the first state and the second state being mutually transitionable, the first temperature being higher than the second temperature, and the crosslinking degree of the gel polymer electrolyte in the second state being higher than the crosslinking degree of the gel polymer electrolyte in the first state;

[0144] When the battery meets a first preset condition, charging and discharging the battery at a first temperature;

[0145] When the battery meets the second preset condition, the battery is charged and discharged at a second temperature.

[0146] In some embodiments of the present application, the battery normally operates in the second temperature range and is charged and discharged at normal power. At this time, the battery electrolyte is in a gel state and the battery has good safety performance. As the battery cycles multiple times, when the battery capacity decays, the temperature is raised to the first temperature for charging and discharging. At this time, part of the gel polymer electrolyte dissociates and the mobile phase increases. The gel polymer electrolyte has a lower internal resistance and a higher ionic conductivity, so as to improve the capacity retention rate and rate performance of the battery.

[0147] In some embodiments of the present application, the first preset condition is that the ratio of the current internal resistance of the battery to the initial internal resistance of the battery is greater than 1.5. Specifically, when the ratio of the current internal resistance of the battery to the initial internal resistance of the battery is greater than 1.5, the increase in internal resistance leads to increased polarization, affecting the battery's rate performance, indicating that the battery capacity has decayed to a certain extent. At this time, the battery is charged and discharged at the first temperature, at least a portion of the second cross-linking agent in the gel polymer electrolyte de-crosslinks with the main substance, the fluidity of the gel polymer electrolyte increases, the internal resistance of the battery is reduced, the battery's rate performance is improved, and the battery's electrode and the gel polymer electrolyte are in close contact, thereby improving the battery's capacity retention rate.

[0148] A battery's internal resistance refers to the resistance to current flowing through the battery during operation. It consists of two components: ohmic resistance and polarization resistance. Ohmic resistance is determined by factors such as the battery's materials, structure, and contact resistance, while polarization resistance is caused by electrochemical reactions and concentration differences and is related to the battery's active materials and solid-phase diffusion coefficient.

[0149] The initial internal resistance of a battery refers to the internal resistance when the battery is completed.

[0150] In some embodiments of the present application, the second preset condition is that the ratio of the current internal resistance of the battery to the initial internal resistance of the battery is less than or equal to 1.5.

[0151] As one embodiment of the present application, if the ratio of the current internal resistance of the battery to the initial internal resistance of the battery is less than or equal to 1.5, the battery is not heated and is charged and discharged at the second temperature. If the ratio of the current internal resistance of the battery to the initial internal resistance of the battery is greater than 1.5, the battery is heated to the first temperature to partially de-crosslink the gel polymer electrolyte, increase the mobile phase in the gel polymer electrolyte, repair the interface problems between the electrode and the gel polymer electrolyte caused during the charge and discharge process, and reduce the internal resistance of the battery. When the ratio of the current internal resistance of the battery to the initial internal resistance of the battery is less than or equal to 1.5, the battery is switched to the second temperature for charging and discharging.

[0152] In some embodiments of the present application, the first preset condition is that the battery discharge rate is greater than 2C. That is, the battery needs to be charged and discharged at a high rate. In this case, the battery is adjusted to operate at the first temperature, and at least a portion of the second cross-linking agent in the gel polymer electrolyte is de-crosslinked from the host material, increasing the fluidity of the gel polymer electrolyte, thereby improving the rate performance of the battery.

[0153] In some embodiments of the present application, the second preset condition is that the battery discharge rate is less than or equal to 2C. That is, the battery needs to be charged and discharged at a low rate. In this case, the battery is adjusted to operate at the second temperature, and at least a portion of the second cross-linking agent in the polymer gel electrolyte is cross-linked with the host material, reducing the fluidity of the gel polymer electrolyte, thereby reducing the rate performance of the battery.

[0154] In a fifth aspect, the present application provides an electrical device comprising the battery described in the third aspect, wherein the battery is used to provide electrical energy. Thus, the electrical device has a long lifespan. Specifically, the battery can serve as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (such as mobile phones, laptops), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks), electric trains, ships and satellites, and energy storage systems.

[0155] FIG5 shows an example of an electric device, which includes a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle.

[0156] As another example, electric devices may include mobile phones, tablet computers, and laptop computers. These electric devices are generally required to be lightweight and thin, and may use batteries as power sources.

[0157] In order to make the technical problems, technical solutions and beneficial effects solved by the embodiments of the present application clearer, the following will be further described in detail with reference to the embodiments and drawings. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is in no way intended to limit the present application and its applications. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0158] Example 1

[0159] Preparation of secondary batteries containing gel polymer electrolytes

[0160] 1. Preparation of precursor solution of gel polymer electrolyte

[0161] The monomer of the main substance, an initiator (azobisisobutyl cyanide), a first cross-linking agent, a second cross-linking agent and an electrolyte are mixed to obtain a precursor liquid, wherein the preparation method of the electrolyte includes: mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a mass ratio of 30:70 to obtain an organic solvent, dissolving fully dried electrolyte salt LiPF6 in the above mixed solvent, wherein the concentration of the electrolyte salt is 1.0 mol / L, and obtaining an electrolyte after uniform mixing.

[0162] 2. Preparation of secondary batteries

[0163] Preparation of positive electrode

[0164] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), conductive agent carbon black (Super P), and binder polyvinylidene fluoride (PVDF) are mixed evenly in an appropriate amount of solvent N-methylpyrrolidone (NMP) in a mass ratio of 96.2:2.7:1.1 to obtain a positive electrode slurry. The positive electrode slurry is coated on the positive electrode current collector aluminum foil, and the positive electrode sheet is obtained through drying, cold pressing, slitting, and cutting processes.

[0165] Preparation of negative electrode sheet

[0166] The negative electrode active material artificial graphite, conductive agent carbon black (Super P), binder styrene-butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC-Na) are mixed evenly in a proper amount of solvent deionized water at a mass ratio of 96.4:0.7:1.8:1.1 to obtain a negative electrode slurry. The negative electrode slurry is coated on the negative electrode current collector copper foil, and the negative electrode sheet is obtained through the processes of drying, cold pressing, slitting and cutting.

[0167] The isolation film is made of polyethylene film.

[0168] The positive electrode sheet, the separator and the negative electrode sheet are stacked in order and then wound to obtain an electrode assembly; the electrode assembly is placed in an outer package, the prepared precursor liquid is injected into the dried secondary battery, and the battery is heated to 60-80°C to allow the first cross-linking agent to cross-link and cure, and then the temperature is lowered to allow the second cross-linking agent to cross-link and cure to obtain a secondary battery.

[0169] The secondary batteries containing gel polymer electrolytes in Examples 2-20 and the comparative example are the same as those in Example 1 except for the different parameters (see Table 1).

[0170] The compositions of the gel polymer electrolytes in the batteries of Examples 1-20 and the comparative example of the present application are shown in Table 1.

[0171] Table 1

[0172] Secondary battery performance test:

[0173] 1. Capacity retention rate

[0174] Taking Example 1 as an example, at the second temperature, the secondary battery was charged at a constant current rate of 0.5C to a charge cutoff voltage of 4.2V. It was then charged at a constant voltage to a current of ≤0.05C and allowed to rest for 5 minutes. The battery was then discharged at a constant current rate of 0.33C to a discharge cutoff voltage of 2.8V and allowed to rest for 5 minutes. The discharge capacity (C0) at this point was recorded. This charge and discharge method was repeated for 500 cycles, and the discharge capacity after 500 cycles was recorded as C1.

[0175] At the second temperature, the cycle capacity retention rate of the secondary battery = C1 / C0×100%

[0176] The method for measuring the cycle capacity retention rate of a secondary battery at the first temperature is the same as the method for measuring the cycle capacity retention rate at the second temperature, except that the temperature is adjusted to the first temperature. Other conditions and steps are the same as those of the method for measuring the cycle capacity retention rate at the second temperature.

[0177] The testing process of the capacity retention rate of the secondary batteries of Examples 2-20 and the comparative example is the same as above.

[0178] 2. Rate performance

[0179] At the second temperature, discharge at 0.2C to 3.0V, let it stand for 5 minutes, charge at 0.5C to 4.4V, charge at constant voltage to 0.05C and let it stand for 5 minutes, adjust the discharge rate, and perform a discharge test at 2C to obtain the discharge capacity. Compare the capacity obtained at 2C with the capacity obtained at 0.2C to obtain the ratio, which is the rate performance of the battery.

[0180] The method for measuring the rate performance of a secondary battery at the first temperature is the same as the method for measuring the rate performance at the second temperature, except that the temperature is adjusted to the first temperature. Other conditions and steps are the same as those of the method for measuring the rate performance at the second temperature.

[0181] The testing process of the rate performance of the secondary batteries of Examples 2-20 and the comparative example is the same as above.

[0182] The performance test results of the secondary batteries of various embodiments and comparative examples are shown in Table 2.

[0183] Table 2

[0184] As can be seen from Table 2, in Examples 1 to 20 of the present application, after the secondary batteries underwent 500 cycles at the second temperature, the battery's capacity retention and rate performance decreased to a certain extent. However, after the operating temperature of the secondary batteries was raised to the first temperature, the capacity retention and rate performance of the secondary batteries were restored. This indicates that when the operating temperature was raised to the first temperature, the gel polymer electrolyte underwent a depolymerization reaction, i.e., the crosslinking degree of the gel polymer electrolyte decreased. At this time, the mobile phase in the gel polymer electrolyte increased, resulting in a tighter bond between the battery electrode and the gel polymer electrolyte, thereby restoring the battery's capacity. Furthermore, the increased mobile phase in the gel polymer electrolyte can improve the ionic conductivity of the gel polymer electrolyte, thereby improving the battery's rate performance.

[0185] Compared with Examples 1 to 20, the comparative example does not have a first state at the first temperature and a second state at the second temperature. The capacity retention rate and rate performance of the secondary battery at the corresponding first temperature and second temperature are both low, and the capacity retention rate and rate performance cannot be restored to the initial capacity retention rate and rate performance at the first temperature. It can be seen that the gel polymer electrolyte of the present application and the battery containing it still have a high capacity retention rate and rate performance after multiple cycles.

[0186] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A gel polymer electrolyte, wherein: The gel polymer electrolyte has a first state at a first temperature and a second state at a second temperature, the first state and the second state are mutually transformable, the first temperature is higher than the second temperature, and a cross-linking degree of the gel polymer electrolyte in the second state is higher than a cross-linking degree of the gel polymer electrolyte in the first state.

2. The gel polymer electrolyte according to claim 1, wherein The ratio of the crosslinking degree of the gel polymer electrolyte in the first state to the crosslinking degree in the second state is 0.2-0.95:

1.

3. The gel polymer electrolyte according to claim 1 or 2, wherein: The first temperature is greater than or equal to 40°C, and can be 40°C-120°C; and / or, The crosslinking degree of the gel polymer electrolyte in the first state is 20%-48.5%.

4. The gel polymer electrolyte according to any one of claims 1 to 3, wherein: The second temperature is -25°C to 35°C; and / or, The crosslinking degree of the gel polymer electrolyte in the second state is 50%-99%; and / or, The gel polymer electrolyte also includes an electrolyte. In the gel polymer electrolyte, the electrolyte accounts for 60%-98% by mass.

5. The gel polymer electrolyte according to any one of claims 1 to 4, wherein: The gel polymer electrolyte comprises a first crosslinking agent and a second crosslinking agent, wherein the de-crosslinking temperature of the second crosslinking agent is greater than or equal to 40° C., and can be selected from 40° C. to 120° C.

6. The gel polymer electrolyte according to claim 5, wherein the first crosslinking agent comprises at least one of an acrylate crosslinking agent and a conjugated diene; and / or The acrylate crosslinking agent includes at least one of ethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, trimethylolpropane ethoxylated triacrylate, trimethylolpropane propoxylated triacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol tetraacrylate, pentaerythritol ethoxylated tetraacrylate, dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate; and / or, The conjugated diene comprises at least one of divinylbenzene and 1,3-butadiene; and / or, The second cross-linking agent includes at least one of maleimide and an N-substituted derivative of maleimide.

7. The gel polymer electrolyte according to claim 5 or 6, wherein The molar ratio of the first cross-linking agent to the second cross-linking agent is 0.5-5:

1.

8. The gel polymer electrolyte according to any one of claims 1 to 7, wherein: The gel polymer electrolyte further includes a host substance, wherein a monomer of the host substance includes at least one of a vinyl group, an epoxy group, an allyl group, an acryloyl group, and a methacryloyl group.

9. The gel polymer electrolyte according to claim 8, wherein The monomers of the main substance include at least one of furfuryl methacrylate, vinyl cyclohexene dioxide, 1,5-hexadiene diepoxide, glycerol propoxylated triglycidyl ether, vinyl cyclohexene dioxide, 1,2,7,8-diepoxyoctane, 4-vinyl cyclohexene dioxide, butyl glycidyl ether, 1,2-cyclohexanedicarboxylic acid diglycidyl ester, ethylene glycol diglycidyl ether, glycerol triglycidyl ether and methacrylic acid glycidyl ester.

10. A method for preparing a gel polymer electrolyte, wherein: include: The monomer of the main substance, the initiator, the cross-linking agent and the electrolyte are mixed and polymerized to obtain a gel polymer electrolyte. The gel polymer electrolyte has a first state at a first temperature and a second state at a second temperature, the first state and the second state are mutually transformable, the first temperature is higher than the second temperature, and the cross-linking degree of the gel polymer electrolyte in the second state is higher than the cross-linking degree of the gel polymer electrolyte in the first state.

11. The method according to claim 10, wherein: The cross-linking agent comprises a first cross-linking agent and a second cross-linking agent, and the de-cross-linking temperature of the second cross-linking agent is greater than or equal to 40° C., and can be selected from 40° C. to 120° C.

12. The method according to claim 10 or 11, wherein: The molar ratio of the monomer of the main substance to the cross-linking agent is 1:2-10.

13. A battery, wherein: The invention comprises a gel polymer electrolyte as claimed in any one of claims 1 to 9 or a gel polymer electrolyte prepared by the method as claimed in any one of claims 10 to 12.

14. A method for charging and discharging a battery, wherein: The battery includes a gel polymer electrolyte, the gel polymer electrolyte has a first state at a first temperature and a second state at a second temperature, the first state and the second state are mutually transformable, the first temperature is higher than the second temperature, and the crosslinking degree of the gel polymer electrolyte in the second state is higher than the crosslinking degree of the gel polymer electrolyte in the first state; When the battery meets a first preset condition, charging and discharging the battery at a first temperature; When the battery meets the second preset condition, the battery is charged and discharged at a second temperature.

15. The method according to claim 14, wherein: The first preset condition is that the ratio of the current internal resistance of the battery to the initial internal resistance of the battery is greater than 1.5; and / or, The second preset condition is that a ratio of a current internal resistance of the battery to an initial internal resistance of the battery is less than or equal to 1.

5.

16. The method according to claim 14, wherein: The first preset condition is that the discharge rate of the battery is greater than 2C; and / or, The second preset condition is that the battery discharge rate is less than or equal to 2C.

17. An electrical device, wherein: Comprising the battery of claim 13.

Citation Information

Patent Citations

  • Method for preparing lithium battery membrane micropores capable of opening and closing reversibly

    CN106129306A

  • Lithium secondary battery

    JP1999219726A

  • Electrolytes for Lithium Secondary Battery Containing Thermo-reversible Material and Lithium Secondary Battery Comprising the Same

    KR1020160043651A

  • Gas venting device and battery pack comprising the same

    KR1020220120489A

  • Copolymer for bipolar battery

    US20160293998A1