Battery, battery preparation method, and electric device
By using a combination of gel electrolyte and liquid electrolyte in the active layer of the negative electrode sheet of the battery, the problem of reduced dynamic performance caused by the expansion of the active material is solved, and the cycle performance of the battery is significantly improved.
Patent Information
- Application Number
- PCT/CN2024/070854
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-01-05
- Publication Date
- 2024-10-24
AI Technical Summary
During the cycle of the battery, the active material of the negative electrode plate expands, resulting in a decrease in dynamic performance, which in turn affects the cycle performance of the battery.
The active layer of the negative electrode sheet is designed to contain active material, gel electrolyte and liquid electrolyte, and through appropriate mass ratio and stacking settings, the gel electrolyte fixes the liquid electrolyte and reduces the risk of the liquid electrolyte being extruded due to expansion. This maintains the stable dynamic performance of the negative electrode piece.
It effectively improves the cycle performance of the battery, especially when using high specific capacity negative electrode materials. Through the combination of gel electrolyte and liquid electrolyte, the negative impact of active material expansion on kinetic performance is reduced, and the stability of the battery is improved.
Smart Images

Figure CN2024070854_24102024_PF_FP_ABST
Abstract
Description
Battery, battery preparation method and power-using device
[0001] Related applications
[0002] This application claims priority to Chinese patent application number 202310414763X, entitled “BATTERY, BATTERY PREPARATION METHOD AND ELECTRICAL DEVICE,” filed on April 18, 2023, the entire text of which is incorporated herein by reference. Technical Field
[0003] The present application relates to the technical field of secondary batteries, and in particular to a battery, battery preparation, and an electrical device. Background Art
[0004] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.
[0005] During the battery cycle, the active material on the negative electrode plate will expand in volume, which may cause the kinetic performance of the negative electrode plate to decline, resulting in a decline in the battery's cycle performance.
[0006] Summary of the Invention
[0007] The present application provides a battery, wherein the negative electrode plate includes a negative electrode current collector and an active layer, wherein the active layer is located on at least one surface of the negative electrode current collector, and the active layer contains an active material, a gel electrolyte and a liquid electrolyte, and the expansion rate of the negative electrode plate is ≥10%.
[0008] In the above-mentioned battery, the negative electrode plate is designed so that its active layer includes an active material, a gel electrolyte, and a liquid electrolyte, and the mass ratio of the gel electrolyte to the liquid electrolyte is within an appropriate range. In this case, when the active material expands during cycling, the gel electrolyte can more stably fix the liquid electrolyte within the negative electrode plate, reducing the risk of liquid electrolyte being squeezed out due to active material expansion. This allows the negative electrode plate to maintain relatively stable dynamic performance, thereby improving the battery's cycling performance.
[0009] In some embodiments, the expansion rate of the active material is 10% to 100%. The expansion rate = (charge thickness - discharge thickness) / discharge thickness, where the charge thickness represents the thickness of the negative electrode sheet after charge, and the discharge thickness represents the thickness of the negative electrode sheet after discharge. The charge is performed at 0.33C to 4.25V, and the discharge is performed at 0.33C to 2.5V.
[0010] In some embodiments, the active material includes at least one of a carbon-based material, a silicon-based material, a tin-based material, and an iron-based material.
[0011] In some embodiments, the active material includes graphite and a silicon-based material.
[0012] In some embodiments, the active material includes artificial graphite and silicon-oxygen material.
[0013] In some embodiments, the mass ratio of the gel electrolyte to the liquid electrolyte is 7:3 to 9.5:0.5.
[0014] In some embodiments, the active layer includes a first active sublayer and a second active sublayer arranged in a stacked manner, the first active sublayer being closer to the negative electrode current collector than the second active sublayer; the first active sublayer and the second active sublayer both contain the active material, the gel electrolyte and the liquid electrolyte; the mass percentage of the gel electrolyte in the first active sublayer is greater than the mass percentage of the gel electrolyte in the second active sublayer.
[0015] In some embodiments, the mass percentage of the gel electrolyte in the first active sublayer is 90% to 95%.
[0016] In some embodiments, the mass percentage of the gel electrolyte in the second active sub-layer is 70% to 90%.
[0017] In some embodiments, the mass percentage of active material in the first active sub-layer is greater than the mass percentage of active material in the second active sub-layer.
[0018] In some embodiments, the mass percentage of the active material in the first active sub-layer is 20% to 70%.
[0019] In some embodiments, the mass percentage of the active material in the second active sub-layer is 5% to 50%.
[0020] In some embodiments, the total volume of the gel electrolyte and the liquid electrolyte in the first active sublayer is greater than the total volume of the gel electrolyte and the liquid electrolyte in the second active sublayer.
[0021] In some embodiments, the volume of the liquid electrolyte in the first active sub-layer is greater than the volume of the liquid electrolyte in the second active sub-layer.
[0022] In some embodiments, the Dv50 of the active material of the first active sub-layer is greater than the Dv50 of the active material of the second active sub-layer.
[0023] In some embodiments, the Dv50 of the active material of the first active sub-layer is 5 μm to 8 μm.
[0024] In some embodiments, the Dv50 of the active material of the second active sub-layer is 3 μm to 7 μm.
[0025] In some embodiments, the thickness of the first active sub-layer is 40 μm to 120 μm.
[0026] In some embodiments, the second active sub-layer has a thickness of 40 μm to 120 μm.
[0027] The present application also provides a method for preparing a battery, comprising the following steps:
[0028] Assembling a battery assembly including a negative electrode sheet into a battery cell; the negative electrode sheet includes a negative electrode current collector and an active layer located on at least one surface of the negative electrode current collector;
[0029] Injecting a first gel electrolyte solution into the battery cell so that the first gel electrolyte solution enters the active layer of the negative electrode plate to prepare a pre-finished battery, wherein the first gel electrolyte solution includes a first polymerizable monomer, a first initiator, a first electrolyte salt, and a first solvent;
[0030] performing formation treatment on the battery pre-finished product;
[0031] The product after the chemical conversion treatment is subjected to a first curing treatment.
[0032] In some embodiments, the expansion rate of the negative electrode plate is ≥10%.
[0033] In some embodiments, the expansion rate of the negative electrode plate is 10% to 100%.
[0034] In some embodiments, the first curing process is controlled to partially solidify the first gel electrolyte solution entering the active layer of the negative electrode sheet.
[0035] In some embodiments, after partial curing, the mass ratio of the gel electrolyte to the liquid electrolyte in the active layer of the negative electrode plate is 7:3 to 9.5:0.5.
[0036] In some embodiments, the mass percentage of the first polymerized monomer in the first gel electrolyte solution is 5% to 10%.
[0037] In some embodiments, after subjecting the product after the chemical conversion treatment to a first curing treatment, the method further includes: injecting a second gel electrolyte solution into the product after the first curing treatment and subjecting the product to a second curing treatment, wherein the second gel electrolyte solution includes a second polymerizable monomer, a second initiator, a second electrolyte salt, and a second solvent.
[0038] In some embodiments, the mass percentage of the first polymerized monomer in the first gel electrolyte solution is less than the mass percentage of the second polymerized monomer in the second gel electrolyte solution.
[0039] In some embodiments, the mass percentage of the first polymerized monomer in the first gel electrolyte solution is 2% to 6%, and the mass percentage of the second polymerized monomer in the second gel electrolyte solution is 5% to 10%.
[0040] In some embodiments, a mass ratio of the first gel electrolyte solution to the second gel electrolyte solution is 5:5 to 9:1.
[0041] In some embodiments, the active layer of the negative electrode plate includes a first active sublayer and a second active sublayer stacked together, the first active sublayer is closer to the negative electrode current collector than the second active sublayer; and the compaction density of the first active sublayer is less than the compaction density of the second active sublayer.
[0042] In some embodiments, the compacted density of the first active sublayer is 1.4 g / cm 3 ~1.65g / cm 3 .
[0043] In some embodiments, the compacted density of the second active sub-layer is 1.5 g / cm 3 ~1.75g / cm 3 .
[0044] The present application also provides an electrical device, comprising the battery or the battery prepared by the preparation method. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] To more clearly illustrate the technical solution of this application, the following briefly describes the drawings used in this application. Obviously, the drawings described below are merely some embodiments of this application, and those skilled in the art can derive other drawings based on the drawings without inventive effort.
[0046] FIG1 is a schematic diagram of a secondary battery according to one embodiment of the present application.
[0047] FIG. 2 is an exploded view of the secondary battery according to one embodiment of the present application shown in FIG. 1 .
[0048] FIG3 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.
[0049] Explanation of the accompanying drawings: 1. Secondary battery; 11. Housing; 12. Electrode assembly; 13. Top cover assembly; 2. Electric device.
[0050] In order to better describe and illustrate the embodiments and / or examples of the inventions disclosed herein, reference may be made to one or more of the accompanying drawings. The additional details or examples used to describe the accompanying drawings should not be considered to limit the scope of the disclosed inventions, the presently described embodiments and / or examples, and any of the best modes currently understood for these inventions. DETAILED DESCRIPTION
[0051] To facilitate understanding of the present application, a more comprehensive description of the present application will be provided below with reference to the accompanying drawings. The accompanying drawings illustrate preferred embodiments of the present application. However, the present application may be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and comprehensive understanding of the disclosure of the present application.
[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0053] The "ranges" disclosed herein are defined in terms of lower and upper limits, where a given range is defined by selecting a lower limit and an upper limit, and the selected lower and upper limits define the boundaries of the particular range. Ranges defined in this manner can be inclusive or exclusive of the end values and can be combined arbitrarily, i.e., any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60 to 120 and 80 to 110 are listed for a particular parameter, it is understood that ranges of 60 to 110 and 80 to 120 are also contemplated. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, the following ranges are all contemplated: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4, and 2 to 5. In this application, unless otherwise indicated, the numerical range "a to b" is a shorthand representation of any combination of real numbers between a and b, where a and b are both real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0054] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0055] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0056] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, and in some embodiments are performed sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0057] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0058] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true or present, and B is false or absent; A is false or absent, and B is true or present; or both A and B are true, or both A and B are present.
[0059] Unless otherwise indicated, the terms used in this application have the commonly understood meanings generally understood by those skilled in the art. Unless otherwise indicated, the numerical values of the various parameters mentioned in this application can be measured using various measurement methods commonly used in the art. For example, the tests can be performed using the methods described in the examples of this application.
[0060] One embodiment of the present application provides a battery having a negative electrode sheet including a negative electrode current collector and an active layer, the active layer being located on at least one surface of the negative electrode current collector and comprising an active material, a gel electrolyte, and a liquid electrolyte, wherein the expansion rate of the negative electrode sheet is ≥10%.
[0061] In this embodiment, the negative electrode plate is designed so that the active layer of the negative electrode plate includes an active material, a gel electrolyte, and a liquid electrolyte, and the mass ratio of the gel electrolyte to the liquid electrolyte is within an appropriate range. At this time, when the active material expands during the cycle, the gel electrolyte can more stably fix the liquid electrolyte in the negative electrode plate, reducing the risk of the liquid electrolyte being squeezed out due to the expansion of the active material. This can maintain relatively stable dynamic performance of the negative electrode plate, thereby improving the cycle performance of the battery. It is understandable that the gel electrolyte can be obtained by adding a polymer monomer and an initiator to a conventional electrolyte and then performing a curing treatment. The liquid electrolyte can be a conventional electrolyte.
[0062] As consumers' requirements for battery energy density continue to increase, more and more high-specific-capacity negative electrode materials are being applied to batteries. However, high-specific-capacity materials are often accompanied by a higher expansion rate. For example, compared to graphite materials, silicon-based materials have a higher specific capacity, but their expansion rate is also significantly higher than that of graphite materials. When these high-specific-capacity negative electrode materials are used in batteries, the expansion of the material will be more obvious during the cycle, and at this time, the kinetic performance of the negative electrode plate will correspondingly decline more significantly. When the negative electrode active material of the battery in this application adopts these high-specific-capacity materials, the combination of gel electrolyte and liquid electrolyte can better compensate for the kinetic decline caused by the expansion of the active material, so that the negative electrode plate can maintain stable kinetic performance, which is beneficial to improving the cycle performance of the battery and provides a new idea for improving the cycle performance of high-energy-density batteries.
[0063] In some embodiments, the mass ratio of the gel electrolyte to the liquid electrolyte is 7:3 to 9.5:0.5. Alternatively, the mass ratio of the gel electrolyte to the liquid electrolyte is 7:3, 7.5:2.5, 8:2, 8.5:1.5, 9:1, or 9.5:0.5.
[0064] In some embodiments, the expansion rate of the negative electrode plate is 10% to 100%. Optionally, the expansion rate of the negative electrode plate is 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 100%, etc.
[0065] It is understood that the expansion rate indicates the rebound range of the negative electrode sheet after charging and discharging of the battery. It is also understood that the expansion rate of the negative electrode sheet can be tested by performing a thickness test on the negative electrode sheet after charging and discharging. For example, expansion rate = (charge thickness - discharge thickness) / discharge thickness. Among them, the charge thickness indicates the thickness of the negative electrode sheet after charging, and the discharge thickness indicates the thickness of the negative electrode sheet after discharging. Optionally, charging is performed at 0.33C to 4.25 volts (V), and discharging is performed at 0.33C to 2.5V.
[0066] Optionally, the active material comprises at least one of a carbon-based material, a silicon-based material, a tin-based material, and an iron-based material. Optionally, the silicon-based material may be selected from at least one of elemental silicon, a silicon oxide compound, a silicon-carbon complex, a silicon-nitrogen complex, and a silicon alloy. The tin-based material may be selected from at least one of elemental tin, a tin oxide compound, and a tin alloy. The iron-based material may be selected from at least one of elemental iron, an iron oxide compound, and an iron alloy. Further optionally, the tin oxide comprises tin oxide. The iron oxide comprises iron oxide.
[0067] In some embodiments, the active material comprises graphite and a silicon-based material. Further, the active material comprises artificial graphite and a silicon-oxygen material.
[0068] It is understandable that the expansion rate of the negative electrode sheet can be adjusted by adjusting the ratio of the materials in the active substance.
[0069] In some embodiments, the active layer includes a first active sublayer and a second active sublayer arranged in a stacked manner, with the first active sublayer being closer to the negative electrode current collector than the second active sublayer; both the first and second active sublayers contain active materials, a gel electrolyte, and a liquid electrolyte; and the mass percentage of the gel electrolyte in the first active sublayer exceeds the mass percentage of the gel electrolyte in the second active sublayer. In this case, the first active sublayer contains a greater mass percentage of gel electrolyte than the second active sublayer, which allows more liquid electrolyte to be retained in the first active sublayer. In other words, more liquid electrolyte can be retained in the inner layer of the negative electrode plate. This creates a more stable electrolyte environment in the inner layer of the negative electrode plate, enabling the negative electrode plate to maintain stable dynamic performance during cycling, thereby promoting good cycling stability of the battery during cycling. Optionally, the gel electrolyte is evenly distributed in the first active sublayer. The gel electrolyte is evenly distributed in the second active sublayer.
[0070] In some embodiments, the mass percentage of the gel electrolyte in the first active sublayer is 90% to 95%. For example, the mass percentage of the gel electrolyte in the first active sublayer is 90%, 90.5%, 91%, 91.5%, 92%, 92.5%, 93%, 93.5%, 94%, 94.5%, 95%, etc.
[0071] In some embodiments, the mass percentage of the gel electrolyte in the second active sublayer is 70% to 90%. For example, the mass percentage of the gel electrolyte in the second active sublayer is 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, etc.
[0072] In some embodiments, the mass percentage of active material in the first active sublayer is greater than the mass percentage of active material in the second active sublayer. When the mass percentage of active material in the first active sublayer is greater than the mass percentage of active material in the second active sublayer, during the charge and discharge process, due to the expansion of the active material, a larger porosity can be formed in the first active sublayer, which can be filled with more gel electrolyte and liquid electrolyte, thereby maintaining more stable dynamic performance inside the electrode and further improving the cycle performance of the battery. Optionally, the mass percentage of active material in the first active sublayer is 20% to 70%; optionally, the mass percentage of active material in the second active sublayer is 5% to 50%. Further optionally, the mass percentage of active material in the first active layer is 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, etc. The mass percentage of the active material in the second active sublayer is 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc.
[0073] In some embodiments, the total volume of the gel electrolyte and liquid electrolyte in the first active sublayer is greater than the total volume of the gel electrolyte and liquid electrolyte in the second active sublayer. Filling the first active sublayer with more gel electrolyte and liquid electrolyte can maintain more stable dynamic performance within the electrode, further improving the battery's cycling performance. Alternatively, the volume of the liquid electrolyte in the first active sublayer is greater than the volume of the liquid electrolyte in the second active sublayer.
[0074] In some embodiments, the Dv50 of the active material of the first active sublayer is greater than the Dv50 of the active material of the second active sublayer. At this time, during the charge and discharge process, due to the expansion of the active material, a larger porosity can be formed in the first active sublayer, and more gel electrolyte and liquid electrolyte can be filled, so that the internal dynamic performance of the electrode is maintained more stable, further improving the cycle performance of the battery. Optionally, the Dv50 of the active material of the first active sublayer is 5 microns (μm) to 8μm; optionally, the Dv50 of the active material of the second active sublayer is 3μm to 7μm. Further optionally, the Dv50 of the active material of the first active sublayer is 5μm, 6μm, 7μm, 8μm, etc. The Dv50 of the active material of the second active sublayer is 3μm, 4μm, 5μm, 6μm, 7μm, etc.
[0075] It is understood that in this application, Dv50 refers to the particle size corresponding to the 50% cumulative particle size distribution in the volume cumulative distribution curve. Its physical meaning is that particles with a smaller (or larger) size account for 50%. As an example, Dv50 can be conveniently measured using a laser particle size analyzer, such as the Mastersizer 2000E laser particle size analyzer from Malvern Instruments Ltd. in the UK, with reference to GB / T 19077-2016 Particle Size Distribution Laser Diffraction Method.
[0076] In some embodiments, the thickness of the first active sublayer is 40μm to 120μm. The thickness of the second active sublayer is 40μm to 120μm. When the thickness of the first active sublayer and the second active sublayer is within this range, the first active sublayer and the second active sublayer can be better adapted to each other, which is beneficial to improving the overall stability of the electrode and thus improving the cycle stability of the battery. Optionally, the thickness of the first active sublayer is 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, etc. Optionally, the thickness of the second active sublayer is 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, etc.
[0077] It is understood that the battery in the present application includes a secondary battery.
[0078] Another embodiment of the present application provides a method for preparing a battery. The method comprises the following steps: assembling a battery assembly including a negative electrode plate into a battery cell; the negative electrode plate includes a negative electrode current collector and an active layer located on at least one surface of the negative electrode current collector; injecting a first gel electrolyte solution into the battery cell so that the first gel electrolyte solution enters the active layer of the negative electrode plate to prepare a battery pre-finished product, wherein the first gel electrolyte solution includes a first polymerizable monomer, a first initiator, a first electrolyte salt, and a first solvent; performing a formation treatment on the battery pre-finished product; and performing a first curing treatment on the product after the formation treatment.
[0079] In this embodiment of the preparation method, a first gel electrolyte solution is injected into the housing. Due to the first gel electrolyte solution's wetting of the electrode plates, the first gel electrolyte enters the active layer of the negative electrode plate, thereby producing a pre-finished battery. The pre-finished battery is then subjected to a formation treatment, and the post-formation product undergoes a first curing treatment. This results in a uniform and stable gel electrolyte formed within the active layer of the negative electrode plate.
[0080] In some embodiments, the expansion rate of the negative electrode plate is ≥10%. Alternatively, the expansion rate of the negative electrode plate is 10% to 100%. Alternatively, the expansion rate of the negative electrode plate is 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 100%, etc.
[0081] Optionally, when the product undergoes a first curing treatment after the formation treatment, the first curing treatment is controlled to partially cure the first gel electrolyte solution that has entered the active layer of the negative electrode. Specifically, the product undergoes a partial curing treatment after the formation treatment, creating an environment in which the gel electrolyte and the liquid gel electrolyte solution coexist in the active layer of the negative electrode. This can improve the dynamic performance of the electrode, and thereby improve the cycling performance of the battery.
[0082] It is understandable that the addition ratio of the first polymerizable monomer, the first initiator and the first electrolyte salt in the first gel electrolyte solution can be controlled so that a certain amount of liquid electrolyte still exists in the active layer of the electrode after the curing process.
[0083] In some embodiments, after partial curing, the mass ratio of the gel electrolyte to the liquid electrolyte in the active layer of the negative electrode plate is 7:3 to 9.5:0.5. Alternatively, after partial curing, the mass ratio of the gel electrolyte to the liquid electrolyte in the active layer of the negative electrode plate is 7:3, 7.5:2.5, 8:2, 8.5:1.5, 9:1, or 9.5:0.5.
[0084] In some embodiments, the mass percentage of the first polymerized monomer in the first gel electrolyte solution is 5% to 10%. When the mass percentage of the first polymerized monomer in the first gel electrolyte solution is within this range, a gel electrolyte with an appropriate proportion and a suitable degree of cross-linking can be formed, which is beneficial for improving the dispersion uniformity and stability of the gel electrolyte in the active layer.
[0085] In some embodiments, after performing the first curing treatment on the product after the chemical formation treatment, the process further includes: injecting a second gel electrolyte solution into the product after the first curing treatment, and performing a second curing treatment, wherein the second gel electrolyte solution includes a second polymerizable monomer, a second initiator, a second electrolyte salt, and a second solvent. By combining two injections and two curing treatments, the uniformity of the dispersion of the gel electrolyte in the active layer can be improved. For example, after injecting the first gel electrolyte solution, the chemical formation treatment, and the first curing treatment, a gel electrolyte with a network structure can be preliminarily formed in the active layer. Then, when the second gel electrolyte solution is injected, the second gel electrolyte solution can further penetrate into the active layer along the network structure formed by the first curing treatment, which is conducive to improving the sufficiency of the gel electrolyte solution infiltrating the active layer, thereby improving the uniformity and stability of the gel electrolyte in the active layer.
[0086] It is understood that the first gel electrolyte solution and the second gel electrolyte solution may be the same or different. It is also understood that the first polymer monomer and the second polymer monomer may be the same or different. The first initiator and the second initiator may be the same or different. The first electrolyte salt and the second electrolyte salt may be the same or different. The first solvent and the second solvent may be the same or different. It is also understood that the conditions of the first curing treatment and the conditions of the second curing treatment may be the same or different. It is also understood that, in some embodiments, the second curing treatment partially cures the second gel electrolyte solution.
[0087] Optionally, the first polymerizable monomer includes at least one of an ester monomer, an ether monomer, a carbonate monomer, a sulfone monomer, an isocyanate monomer, an amide monomer, a nitrile monomer, a fluorinated monomer, an ether-segmented oligomer, and a siloxane monomer. Further optionally, the first polymerizable monomer includes at least one of methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, n-butyl methacrylate, butyl acrylate, n-octyl methacrylate, n-octyl acrylate, vinyl acetate, vinylene carbonate, vinyl ethylene carbonate, triethylene glycol dimethacrylate, diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, allyl methacrylate, divinylbenzene, polyvinyl alcohol, and styrene.
[0088] Optionally, the first initiator includes at least one of persulfate, azo initiator, and organic peroxide initiator, etc. Further optionally, the first initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl, dicumyl peroxide, dibenzoyl peroxide, and ammonium persulfide.
[0089] Optionally, the second polymerizable monomer includes at least one of an ester monomer, an ether monomer, a carbonate monomer, a sulfone monomer, an isocyanate monomer, an amide monomer, a nitrile monomer, a fluorinated monomer, an ether-segmented oligomer, and a siloxane monomer. Further optionally, the second polymerizable monomer includes at least one of methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, n-butyl methacrylate, butyl acrylate, n-octyl methacrylate, n-octyl acrylate, vinyl acetate, vinylene carbonate, vinylethylene carbonate, triethylene glycol dimethacrylate, diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, allyl methacrylate, divinylbenzene, polyvinyl alcohol, and styrene.
[0090] Optionally, the second initiator includes at least one of persulfate, azo initiator, and organic peroxide initiator, etc. Further optionally, the second initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl, dicumyl peroxide, dibenzoyl peroxide, and ammonium persulfide.
[0091] In some embodiments, the mass percentage of the first polymerized monomer in the first gel electrolyte solution is less than the mass percentage of the second polymerized monomer in the second gel electrolyte solution. In this case, a gel electrolyte with a lower degree of crosslinking can be formed through the first curing treatment, and then a gel electrolyte with a higher degree of crosslinking can be formed through the second curing treatment, thereby further improving the stability of the gel electrolyte in the battery.
[0092] Optionally, the mass percentage of the first polymerized monomer in the first gel electrolyte solution is 2% to 6%, and the mass percentage of the second polymerized monomer in the second gel electrolyte solution is 5% to 10%. Further, optionally, the mass percentage of the first polymerized monomer in the first gel electrolyte solution is 2%, 3%, 4%, 5%, 6%, etc. The mass percentage of the second polymerized monomer in the second gel electrolyte solution is 5%, 6%, 7%, 8%, 9%, 10%, etc.
[0093] In some embodiments, the mass ratio of the first gel electrolyte solution to the second gel electrolyte solution is 5:5 to 9:1. Alternatively, the mass ratio of the first gel electrolyte solution to the second gel electrolyte solution is 5:5, 6:4, 7:3, 8:2, 9:1, etc.
[0094] In some embodiments, the curing temperature of the first curing treatment is 60 degrees Celsius (° C.) to 80° C. The time of the first curing treatment is 8 hours (h) to 15 hours. Alternatively, the curing temperature of the first curing treatment is 60° C., 62° C., 65° C., 68° C., 70° C., 72° C., 75° C., 78° C., 80° C., etc. Alternatively, the time of the first curing treatment is 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, etc.
[0095] In some embodiments, the curing temperature of the second curing treatment is 60° C. to 80° C. The curing time of the second curing treatment is 8 hours to 15 hours. Alternatively, the curing temperature of the second curing treatment is 60° C., 62° C., 65° C., 68° C., 70° C., 72° C., 75° C., 78° C., 80° C., etc. Alternatively, the curing time of the second curing treatment is 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, etc.
[0096] In some embodiments, the active layer of the negative electrode plate includes a first active sublayer and a second active sublayer stacked together, the first active sublayer being closer to the negative electrode current collector than the second active sublayer; the compaction density of the first active sublayer is less than the compaction density of the second active sublayer. At this time, during the charge and discharge process, due to the expansion of the active material, a larger porosity can be formed in the first active sublayer, which can be filled with more gel electrolyte and liquid electrolyte, so that the internal dynamic performance of the plate is maintained more stable, further improving the cycle performance of the battery. Optionally, the compaction density of the first active sublayer is 1.4 g / cm3 (g / cm 3 )~1.65g / cm 3 Optionally, the compacted density of the second active sublayer is 1.5 g / cm 3 ~1.75g / cm 3 As some optional examples, the compacted density of the first active sublayer is 1.4 g / cm 3 , 1.45g / cm 3 , 1.5g / cm 3 , 1.55g / cm 3 , 1.6g / cm 3 , 1.65g / cm 3 The compacted density of the second active sublayer is 1.5 g / cm 3 , 1.55g / cm 3 , 1.65g / cm 3 , 1.7g / cm 3 , 1.75g / cm 3 wait.
[0097] Another embodiment of the present application provides an electrical device, which includes the above-mentioned battery or a battery prepared by the above-mentioned battery preparation method.
[0098] The secondary battery and the electric device of the present application will be described below with reference to the accompanying drawings as appropriate.
[0099] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During the battery's charge and discharge processes, active ions are inserted and removed between the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. The separator, located between the positive and negative electrodes, primarily prevents short circuits between the positive and negative electrodes while allowing ions to pass through.
[0100] Positive electrode
[0101] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.
[0102] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer is provided on either or both of the two facing surfaces of the positive electrode current collector.
[0103] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material on a polymer material substrate. Alternatively, the metal material may include but is not limited to one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. Alternatively, the polymer material substrate may include but is not limited to one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0104] As an example, the positive electrode active material may include positive electrode active materials for batteries that are well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include but are not limited to at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their modified compounds. Optionally, lithium cobalt oxide includes LiCoO2. Lithium nickel oxide includes LiNiO2. Lithium manganese oxide includes at least one of LiMnO2 and LiMn2O4. Lithium nickel cobalt manganese oxide includes LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2(NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM 622 ) and LiNi 0.8 Co 0.1 Mn 0.1O2(NCM 811 ) at least one of. Lithium nickel cobalt aluminum oxide includes LiNi 0.8 Co 0.15 Al 0.05 O2. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon. Optionally, the lithium iron phosphate includes LiFePO4 (LFP). The lithium manganese phosphate includes LiMnPO4. The weight ratio of the positive electrode active material in the positive electrode film layer is 80 weight percent (wt%) to 100 wt%, based on the total weight of the positive electrode film layer.
[0105] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin. The weight ratio of the binder in the positive electrode film layer is 0 to 20 wt%, based on the total weight of the positive electrode film layer.
[0106] In some embodiments, the positive electrode film layer may also optionally include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The weight ratio of the conductive agent in the positive electrode film layer is 0 to 20 wt%, based on the total weight of the positive electrode film layer.
[0107] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent to form a positive electrode slurry. Optionally, the solvent includes N-methylpyrrolidone. The positive electrode slurry has a solid content of 40 wt% to 80 wt%, and the viscosity at room temperature is adjusted to 5000 mPa·s (mPa·s) to 25000 mPa·s. The positive electrode slurry is coated on the surface of the positive electrode collector, dried, and then cold-pressed by a cold rolling mill to form a positive electrode sheet; the positive electrode powder coating unit area density is 150 mg / cm2 (mg / m 2 )~350mg / m 2 The compaction density of the positive electrode is 3.0g / cm 3 ~3.6g / cm 3 , optional 3.4g / cm 3 ~3.6g / cm 3 The calculation formula of the compaction density is: compaction density = coating surface density / (thickness of the electrode after extrusion - thickness of the current collector).
[0108] Negative electrode
[0109] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0110] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0111] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material on a polymer base material. Optionally, the metal material includes at least one of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. The polymer material includes at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0112] In some embodiments, the negative electrode active material may adopt the negative electrode active material for batteries that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more. The weight ratio of the negative electrode active material in the negative electrode film layer is 70wt% to 100wt%, based on the total weight of the negative electrode film layer.
[0113] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS). The weight ratio of the binder in the negative electrode film layer is 0 to 30% by weight, based on the total weight of the negative electrode film layer.
[0114] In some embodiments, the negative electrode film layer may further include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The weight ratio of the conductive agent in the negative electrode film layer is 0 to 20 wt%, based on the total weight of the negative electrode film layer.
[0115] In some embodiments, the negative electrode film layer may further include other additives, such as a thickener. The weight ratio of the other additives in the negative electrode film layer is 0-15 wt%, based on the total weight of the negative electrode film layer. Optionally, the thickener includes sodium carboxymethylcellulose (CMC-Na).
[0116] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent to form a negative electrode slurry. Optionally, the solvent includes deionized water. The solid content of the negative electrode slurry is 30wt% to 70wt%, and the viscosity at room temperature is adjusted to 2000mPa·s to 10000mPa·s; the obtained negative electrode slurry is coated on the negative electrode current collector, and after a drying process, cold pressing, such as rolling, is performed to obtain a negative electrode sheet. The negative electrode powder coating unit area density is 75 grams per square meter (g / m 2 )~220g / m 2 , the compaction density of the negative electrode is 1.2g / cm 3 ~2.0g / cm 3 .
[0117] electrolytes
[0118] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.
[0119] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0120] In some embodiments, the electrolyte salt may be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium bis(oxalatoborate) (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP), and lithium tetrafluorooxalatophosphate (LiTFOP). The concentration of the electrolyte salt is typically 0.5 mol / L to 5 mol / L.
[0121] In some embodiments, the solvent can be selected from one or more of fluoroethylene carbonate (FEC), ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE).
[0122] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0123] Isolation film
[0124] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0125] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0126] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0127] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0128] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic. Examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate. This application does not particularly limit the shape of the secondary battery, which can be cylindrical, square, or any other shape. For example, Figure 1 shows a secondary battery 1 with a square structure as an example.
[0129] In some embodiments, referring to Figure 2, the outer packaging may include a shell 11 and a top cover assembly 13. The shell 11 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 11 has an opening connected to the receiving cavity, and the top cover assembly 13 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 12 through a winding process or a lamination process. The electrode assembly 12 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 12. The number of electrode assemblies 12 contained in the secondary battery 1 can be one or more, and those skilled in the art can select according to specific actual needs.
[0130] In addition, the present application also provides an electrical device, which includes the secondary battery provided in the present application. The secondary battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.
[0131] As the electrical device, a secondary battery can be selected according to its usage requirements.
[0132] Figure 3 shows an example of an electric device 2. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the electric device's requirements for high power and high energy density of secondary batteries, a battery pack or battery module can be used.
[0133] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.
[0134] In order to make the technical problems, technical solutions and beneficial effects solved by this application clearer, the application will be further described in detail below with reference to the embodiments and drawings. Obviously, the described embodiments are only a part of the embodiments of this application, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is in no way intended to limit the present application and its applications. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0135] If no specific techniques or conditions are specified in the examples, the experiments were carried out according to the techniques or conditions described in the literature in the field or according to the product instructions. All reagents or instruments used without specifying the manufacturer are commercially available conventional products.
[0136] Example 1
[0137] (1) Preparation of positive electrode sheets.
[0138] Nickel-cobalt-manganese (NCM) ternary material, conductive carbon black, and binder polyvinylidene fluoride (PVDF) were added to N-methylpyrrolidone in a mass ratio of 97:1:2 and stirred evenly to produce a positive electrode slurry. The slurry was evenly coated onto the positive electrode current collector aluminum foil, dried, cold pressed, and slit to produce the positive electrode sheets.
[0139] (2) Preparation of negative electrode sheets.
[0140] Silicone material, artificial graphite, conductive agent carbon black, binder styrene-butadiene rubber (SBR), and thickener sodium hydroxymethyl cellulose (CMC-Na) are added to deionized water in a weight ratio of 38.8:58.2:0.5:1.25:1.25, mixed and stirred evenly to obtain a negative electrode slurry. The negative electrode slurry is evenly coated on the negative electrode current collector copper foil, dried, cold pressed, and cut to obtain a negative electrode sheet. Among them, the Dv50 of the silicon material is 7μm, the Dv50 of the artificial graphite is 6μm, and the compaction density of the negative electrode active layer is 1.6mg / cm 3 .
[0141] (3) The isolation film is a polypropylene isolation film.
[0142] (4) Preparation of gel electrolyte solution.
[0143] DMC, EMC, EC, methyl acrylate, and azobisisobutyronitrile are mixed in a weight ratio of 58:30:4.5:7:0.5, wherein the electrolyte salt in the gel electrolyte solution is LiPF6, and the concentration of LiPF6 is 1.1 mol / L.
[0144] (5) Preparation of batteries.
[0145] The positive electrode sheet, negative electrode sheet and separator are assembled into a battery cell, the battery cell is placed in a shell, and a gel electrolyte solution is injected into the shell. After soaking at 25°C for 24 hours, the battery cell is formed and then cured at 60°C for 15 hours.
[0146] Example 2 to Example 3
[0147] Compared with Example 1, Examples 2 to 3 differ in that the weight ratio of the silicon oxide material and the artificial graphite is adjusted to obtain negative electrode sheets with different expansion rates, as shown in Table 1.
[0148] Example 4 to Example 7
[0149] Compared with Example 1, Examples 4 to 7 differ in that the ratio of materials in the gel electrolyte solution is adjusted so that the mass percentages of the gel electrolyte and liquid electrolyte in the resulting batteries are different, as shown in Table 1.
[0150] Example 8 to Example 9
[0151] Compared with Example 1, Examples 8 and 9 differ in that the silicon-based material is replaced with tin oxide and iron oxide, respectively, and the expansion rate of the negative electrode plate is set to 40%, as shown in Table 1.
[0152] Example 10
[0153] Compared with Example 1, this embodiment differs in that the gel electrolyte solution is divided into a first gel electrolyte solution and a second gel electrolyte solution. The mass percentage of polymerized monomers in the first gel electrolyte solution is less than the mass percentage of polymerized monomers in the second gel electrolyte solution. The mass ratio of the first gel electrolyte solution to the second gel electrolyte solution is 5:5.
[0154] Preparation of the battery:
[0155] Assemble the positive electrode sheet, negative electrode sheet and isolation membrane into a battery cell, install the battery cell into a shell, inject the first gel electrolyte solution into the shell, soak at 25°C for 24 hours, and then form it, and first cure it at 60°C for 15 hours. Then inject the second gel electrolyte solution, soak at 25°C for 24 hours, and then second cure it at 60°C for 15 hours.
[0156] Example 11
[0157] Different from Example 8, when preparing the battery in this embodiment, the positive electrode sheet, the negative electrode sheet, and the isolation membrane are assembled into a battery cell, the battery cell is placed in a shell, and the second gel electrolyte solution is injected into the shell. After soaking at 25°C for 24 hours, it is formed, and the first curing is carried out at 60°C for 15 hours. Then, the first gel electrolyte solution is injected, soaked at 25°C for 24 hours, and the second curing is carried out at 60°C for 15 hours.
[0158] Example 12
[0159] Compared with Example 1, this embodiment is different in that the preparation method of the battery is different.
[0160] Preparation of the battery:
[0161] Assemble the positive electrode sheet, negative electrode sheet and isolation membrane into a battery cell, install the battery cell into a shell, inject gel electrolyte solution into the shell, soak at 25°C for 24 hours, cure at 60°C for 15 hours, and then form.
[0162] Example 13
[0163] Compared with Example 1, the difference of this embodiment is that the preparation method of the negative electrode plate is different. Preparation of the negative electrode plate of this embodiment:
[0164] (1) First active sublayer slurry: Silicone material, artificial graphite, conductive agent carbon black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) were added to deionized water in a weight ratio of 29.1:67.9:0.5:1.25:1.25 and mixed to obtain a negative electrode slurry. The Dv50 of the silicon material was 7 μm.
[0165] (2) Second active sublayer slurry: Silicone material, artificial graphite, conductive agent carbon black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) were added to deionized water in a weight ratio of 38.8:58.2:0.5:1.25:1.25 and mixed to obtain a negative electrode slurry. The Dv50 of the silicon material was 6 μm.
[0166] (3) The first active sublayer slurry and the second active sublayer slurry are sequentially coated on the negative electrode current collector, dried, cold pressed, and cut to obtain a negative electrode sheet. The mass percentage of the gel electrolyte in the first active sublayer is greater than the mass percentage of the gel electrolyte in the second active sublayer, and the compaction density of the first active sublayer is less than the compaction density of the second active sublayer. The details are shown in Table 2.
[0167] Example 14
[0168] Compared with Example 1, the difference of this embodiment is that the preparation method of the negative electrode plate is different. Preparation of the negative electrode plate of this embodiment:
[0169] (1) First active sublayer slurry: Silicone material, artificial graphite, conductive agent carbon black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) were added to deionized water in a weight ratio of 38.8:58.2:0.5:1.25:1.25 and mixed to obtain a negative electrode slurry. The Dv50 of the silicon material was 6 μm.
[0170] (2) Second active sublayer slurry: Silicone material, artificial graphite, conductive agent carbon black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) were added to deionized water in a weight ratio of 29.1:67.9:0.5:1.25:1.25 and mixed to obtain a negative electrode slurry. The Dv50 of the silicon material was 7 μm.
[0171] (3) The first active sublayer slurry and the second active sublayer slurry are sequentially coated on the negative electrode current collector, dried, cold pressed, and cut to obtain a negative electrode sheet. The mass percentage of the gel electrolyte in the first active sublayer is less than the mass percentage of the gel electrolyte in the second active sublayer, and the compaction density of the first active sublayer is greater than the compaction density of the second active sublayer. The details are shown in Table 2.
[0172] Comparative Example 1
[0173] Compared with Example 1, the difference of this comparative example is that the electrolyte does not contain polymerizable monomers and initiators, and no curing is performed after the electrolyte is injected.
[0174] Test Case
[0175] The batteries in the examples and comparative examples were subjected to cycling performance testing. The test method was as follows: the battery was charged at 0.33C to 4.25V, then charged at 4.25V constant voltage to 0.05C to complete the charge, and then discharged at 0.33C to 2.5V to complete one cycle. The battery was cycled multiple times until the discharge capacity reached 80% of the first cycle discharge capacity. The number of cycles was recorded.
[0176] Table 1
[0177] Table 2
[0178] As can be seen from Table 1, when the negative electrode active layer contains a gel electrolyte and a liquid electrolyte, the battery cycle performance can be improved. When the expansion rate of the negative electrode active material is large, the combination of gel electrolyte and liquid electrolyte in the negative electrode active layer can further improve the battery cycle performance.
[0179] It can be seen from Example 1 and Example 12 in Table 1 that performing a formation treatment and then a curing treatment on the battery pre-finished product is beneficial to improving the cycle performance of the battery.
[0180] As can be seen from Table 2, a ratio of Dv50 of the active material in the first active sublayer to that in the second active sublayer in the negative electrode active layer is beneficial for improving the battery's cycling performance. A ratio of the mass percentage of the active material in the first active sublayer to that in the second active sublayer is beneficial for improving the battery's cycling performance. A ratio of the mass percentage of the gel electrolyte in the first active sublayer to that in the second active sublayer is beneficial for improving the battery's cycling performance. A ratio of the compacted density of the first active sublayer to that of the second active sublayer is beneficial for improving the battery's cycling performance.
[0181] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0182] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that a person skilled in the art could make various modifications and improvements without departing from the spirit of the present application, all of which fall within the scope of protection of the present application. Therefore, the scope of protection of the present patent application shall be determined by the appended claims.
Claims
1. A battery, wherein the negative electrode sheet comprises a negative electrode current collector and an active layer, wherein the active layer is located on at least one surface of the negative electrode current collector, the active layer comprises an active material, a gel electrolyte and a liquid electrolyte, and the expansion rate of the negative electrode sheet is ≥10%.
2. The battery according to claim 1, wherein The expansion rate of the negative electrode plate is 10% to 100%; the expansion rate = (charge thickness - discharge thickness) / discharge thickness, wherein the charge thickness represents the thickness of the negative electrode plate after charge, and the discharge thickness represents the thickness of the negative electrode plate after discharge. The charge is charged to 4.25V at 0.33C, and the discharge is discharged to 2.5V at 0.33C.
3. The battery according to claim 1 or 2, wherein: The mass ratio of the gel electrolyte to the liquid electrolyte is 7:3 to 9.5:0.
5.
4. The battery according to any one of claims 1 to 3, wherein The active material includes at least one of a carbon-based material, a silicon-based material, a tin-based material, and an iron-based material.
5. The battery according to any one of claims 1 to 4, wherein The active materials include graphite and silicon-based materials.
6. The battery according to any one of claims 1 to 5, wherein The active material includes artificial graphite and silicon-oxygen material.
7. The battery according to any one of claims 1 to 6, wherein The active layer includes a first active sublayer and a second active sublayer which are stacked, the first active sublayer being closer to the negative electrode current collector than the second active sublayer; the first active sublayer and the second active sublayer both contain the active material, the gel electrolyte and the liquid electrolyte; the mass percentage of the gel electrolyte in the first active sublayer is greater than the mass percentage of the gel electrolyte in the second active sublayer.
8. The battery according to claim 7, wherein The mass percentage of the gel electrolyte in the first active sublayer is 90% to 95%.
9. The battery according to claim 7 or 8, wherein The mass percentage of the gel electrolyte in the second active sublayer is 70% to 90%.
10. The battery according to any one of claims 7 to 9, wherein The mass percentage of active material in the first active sublayer is greater than the mass percentage of active material in the second active sublayer.
11. The battery according to claim 10, wherein The mass percentage of active material in the first active sub-layer is 20% to 70%.
12. The battery according to claim 10 or 11, wherein The mass percentage of active material in the second active sub-layer is 5% to 50%.
13. The battery according to any one of claims 7 to 12, wherein The total volume of the gel electrolyte and the liquid electrolyte in the first active sublayer is greater than the total volume of the gel electrolyte and the liquid electrolyte in the second active sublayer.
14. The battery according to claim 13, wherein The volume of the liquid electrolyte in the first active sublayer is greater than the volume of the liquid electrolyte in the second active sublayer.
15. The battery according to any one of claims 7 to 14, wherein The Dv50 of the active material of the first active sub-layer is greater than the Dv50 of the active material of the second active sub-layer.
16. The battery according to claim 15, wherein The Dv50 of the active material of the first active sub-layer is 5 μm to 8 μm.
17. The battery according to claim 15 or 16, wherein: The Dv50 of the active material of the second active sub-layer is 3 μm to 7 μm.
18. The battery according to any one of claims 7 to 17, wherein The thickness of the first active sublayer is 40 μm to 120 μm; and / or the thickness of the second active sublayer is 40 μm to 120 μm.
19. A method for preparing a battery, comprising the following steps: Assembling a battery assembly including a negative electrode sheet into a battery cell; the negative electrode sheet includes a negative electrode current collector and an active layer located on at least one surface of the negative electrode current collector; Injecting a first gel electrolyte solution into the battery cell so that the first gel electrolyte solution enters the active layer of the negative electrode plate to prepare a battery pre-product, wherein the first gel electrolyte solution includes a first polymerizable monomer, a first initiator, a first electrolyte salt and a first solvent; Performing formation treatment on the battery pre-finished product; The product after the chemical formation treatment is subjected to a first curing treatment.
20. The preparation method according to claim 19, wherein: The expansion rate of the negative electrode plate is ≥10%.
21. The preparation method according to claim 20, wherein: The expansion rate of the negative electrode plate is 10% to 100%.
22. The preparation method according to any one of claims 19 to 21, wherein The first curing process is controlled to partially cure the first gel electrolyte solution entering the active layer of the negative electrode sheet.
23. The preparation method according to claim 22, wherein: After partial solidification, the mass ratio of the gel electrolyte to the liquid electrolyte in the active layer of the negative electrode plate is 7:3 to 9.5:0.
5.
24. The preparation method according to any one of claims 19 to 23, wherein The mass percentage of the first polymerized monomer in the first gel electrolyte solution is 5% to 10%.
25. The preparation method according to any one of claims 19 to 24, wherein: After subjecting the product after the chemical formation treatment to a first curing treatment, the following steps are further included: A second gel electrolyte solution is injected into the product after the first curing treatment, and a second curing treatment is performed, wherein the second gel electrolyte solution includes a second polymerizable monomer, a second initiator, a second electrolyte salt and a second solvent.
26. The preparation method according to claim 25, wherein: The mass percentage of the first polymerized monomer in the first gel electrolyte solution is less than the mass percentage of the second polymerized monomer in the second gel electrolyte solution.
27. The preparation method according to claim 25 or 26, wherein: The mass percentage of the first polymerized monomer in the first gel electrolyte solution is 2% to 6%, and the mass percentage of the second polymerized monomer in the second gel electrolyte solution is 5% to 10%.
28. The preparation method according to any one of claims 25 to 27, wherein The mass ratio of the first gel electrolyte solution to the second gel electrolyte solution is 5:5 to 9:
1.
29. The preparation method according to any one of claims 19 to 28, wherein The active layer of the negative electrode plate includes a first active sublayer and a second active sublayer which are stacked, the first active sublayer being closer to the negative electrode current collector than the second active sublayer; and the compaction density of the first active sublayer being less than the compaction density of the second active sublayer.
30. The preparation method according to claim 29, wherein: The compacted density of the first active sublayer is 1.4 g / cm 3 ~1.65g / cm 3 .
31. The preparation method according to claim 29 or 30, wherein: The compacted density of the second active sublayer is 1.5 g / cm 3 ~1.75g / cm 3 .
32. An electrical device comprising the battery according to any one of claims 1 to 18 or a battery prepared by the preparation method according to any one of claims 19 to 31.
Citation Information
Patent Citations
Lithium ion secondary battery and preparation method thereof
CN102522560A
Preparation method of gel-phase polymer lithium battery and gel-phase polymer lithium battery
CN104868165A
Polymer lithium ion battery and preparation method thereof
CN111916835A
Gel polymer battery and preparation method thereof
CN114388869A
Manufacturing process of gel electrolyte battery
CN115117439A