Positive electrode material of sodium-ion battery, and sodium-ion battery

By adopting a composite layered material structure in the sodium-ion battery cathode material, and utilizing the first phase of polycrystalline morphology and the second phase structure of the protective layer, the stability and capacity problems of layered oxide materials in sodium-ion batteries are solved. , achieving electrode material performance of high capacity, multiple rates and long life.

WO2024217295A1PCT designated stage expired Publication Date: 2024-10-24ANHUI XINNA MATERIAL SCIENCE & TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2024/086739
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-04-09
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Layered oxide cathode materials in sodium-ion batteries have problems such as poor stability in the air, poor processability, and poor actual capacity performance, and existing improvement solutions are difficult to fully improve water absorption performance and capacity.

Method used

Composite layered material preparation technology is used to form first-phase and second-phase structural materials through dual design of the composition and structure of the electrode material. The first phase is polycrystalline nanoparticles, and the second phase is used as a protective layer coating. In the first phase, it is formed through in-situ reaction, which simplifies the sintering process and is suitable for large-scale mass production.

Benefits of technology

It achieves high discharge capacity, multiple rate performance and long cycle life, improves the stability and processing performance of the material in humid environments, and ensures the high capacity characteristics and structural stability of the electrode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024086739_24102024_PF_FP_ABST
    Figure CN2024086739_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the field of sodium-ion batteries. Disclosed are a positive electrode material of a sodium-ion battery, and a sodium-ion battery. A first-phase material prepared in the present invention has a polycrystalline structure, and the particle size of primary particles is adjustable, which facilitates reversible deintercalation of sodium ions, thereby improving the capacity and rate capability of an electrode material; and by means of adding a structural stabilizer to a first phase, and an in-situ reaction on the surface of the first phase, a second-phase sodium material having a controllable thickness is generated, wherein the second-phase sodium material has a highly stable structure with respect to water, and by means of coating the surface of the first phase, the stability of a composite material with respect to air and water is fundamentally ensured, thereby completely improving the storage and processing performance of the material; the second-phase sodium material can adapt to an interface problem with an electrolyte under a high charging voltage, the structural stability of the composite material at a high electric potential is improved, and the occurrence of side reactions is reduced; and the second-phase sodium material itself has a relatively high reversible discharge capacity, and therefore compared with other coating layers, the second-phase sodium material protects the first-phase material and does not sacrifice the discharge capacity of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Sodium ion battery positive electrode material and sodium ion battery Technical Field

[0001] The present invention relates to the field of sodium ion batteries, and in particular to a sodium ion battery positive electrode material and a sodium ion battery. Background Art

[0002] my country's new energy lithium battery industry has made significant progress in recent years. However, it's also important to note that factors such as the severe imbalance in lithium resource distribution and the rapid development of the lithium battery industry have led to a surge in lithium carbonate prices, making it a new strategic commodity. Sodium batteries have comparable processes, raw materials, and performance to lithium batteries. Sodium reserves are extremely abundant and evenly distributed throughout the Earth's crust. Vigorously developing sodium batteries aligns with my country's energy security strategy and addresses the enormous future market potential for energy storage and other sectors.

[0003] Among the various technological approaches for sodium-ion batteries, layered oxide cathode materials offer advantages such as high theoretical specific capacity, ample room for component structure optimization, and industrialization processes that can be adapted from lithium-ion materials. These materials are key to the industrialization of sodium-ion batteries. However, these materials also face challenges such as poor stability in air, poor processing performance, and inadequate actual capacity utilization. The composition of layered materials significantly influences their performance. Generally speaking, sodium-rich phase materials have high discharge capacity but poor stability in air and prone to water absorption, resulting in poor processing performance and cycle life. Sodium-poor phase materials have lower capacity, but certain components possess high interfacial stability. In response to the problem of air stability, the Xiamen University research team systematically studied the water absorption mechanism of such materials and found that some materials with high sodium removal potential have very good stability and will decompose in humid air or even in water, but the comprehensive performance of the materials, such as cycle capacity, cannot meet actual needs (Zuo, W., Qiu, J., Liu, X. et al. The stability of P2-1ayered sodium transition metal oxides in ambient atmospheres. Nat Commun 11, 3544 (2020).); For high-capacity materials, interfacial stability can be improved by doping, but there is difficulty in achieving complete avoidance of hydrolysis (Xie Man, Wu Feng, Huang Yongxin. Advanced Technology and Application of Sodium Ion Batteries, National Heavy Equipment Publishing Project, 2020.), or its solution is difficult to mass-produce. Therefore, the rational design of the components and structures of layered materials, balancing key performance parameters such as capacity, processing performance, and life, plays a vital role in their rapid industrialization. At present, there is no effective solution for the comprehensive improvement of performance such as water absorption and capacity.

[0004] Summary of the Invention

[0005] Based on the obvious defects of the prior art, the present invention provides a preparation process for sodium ion layered positive electrode materials and their application in sodium ion batteries. The present invention provides a preparation technology for composite layered materials, which achieves high discharge capacity, high rate performance, long cycle life, excellent processing performance, etc. through the dual design of the components and structure of the electrode materials, and is applied in sodium ion batteries. The raw materials required for the present invention, such as transition metal oxide precursors, can be purchased from mature material companies or made in-house, which has no decisive impact on the technology of the present invention. In addition, the preparation process of the present invention is simple, and only two sintering processes are required to prepare the finished material, without the need for additional water washing and pre-sintering processes, and is basically compatible with the current equipment for lithium battery layered materials, making it very suitable for large-scale mass production.

[0006] The technical solutions of the present invention are as follows:

[0007] The present invention provides a sodium ion battery positive electrode material, wherein the sodium ion battery positive electrode material comprises a first phase structural material and a second phase structural material;

[0008] The molecular formula of the first phase structural material is: Na a M b Ni c Fe d Mn e O2,

[0009] Wherein, M is selected from at least one of Al, Ti, Ca, Cu, K, Sn, Li, Mg, Co, Ag, Ce, and Ba; 1.0≤a≤1.1, 0≤b≤0.05, 0.2≤c≤0.5, 0.2≤d≤0.4, and 0.3≤e≤0.4;

[0010] The molecular formula of the second phase structural material is: Na x N w Ni y Mn z O2,

[0011] Wherein, N is selected from at least one of Mn, Ni, Ca, Al, Mg, and Zn; 0.5≤x≤0.7, 0.0≤y≤0.33, 0.62≤z≤0.8, 0.05≤w≤0.1;

[0012] The second phase structural material is coated on the first phase structural material, and the second phase structural material is in-situ grown on the surface of the first phase structural material.

[0013] Preferably, the first phase structural material accounts for 81%-99% by mass of the sodium ion battery positive electrode material; the second phase structural material accounts for 1%-20% by mass of the sodium ion battery positive electrode material. The optimal molar ratio of the first phase to the second phase is 90:10.

[0014] Specifically, the first phase structure material is a layered structure, and the second phase structure material is a layered structure or a three-dimensional structure.

[0015] Preferably, the M is selected from at least one of Ti, Sn, K and Ca.

[0016] The first phase material of the sodium ion battery positive electrode described in the present invention has a polycrystalline morphology, and the primary nanoparticles have a large specific surface area, which increases the active sites and improves the electrode reaction activity, thereby improving the discharge capacity of the electrode; trace doping in the structure alleviates phenomena such as water absorption and deliquescence of the material, maintaining a certain stability; on this basis, a second material phase is introduced and formed in situ on the surface of the first material phase. This material phase has high stability, can exist stably in water, and contributes to the capacity of the battery. In this two-composite structure, the second phase acts as a protective layer to maintain the structural stability of the internal first phase, avoiding the degradation of processing performance caused by water absorption. The first phase acts as the main phase to exert high capacity characteristics and provide a stable sodium source for the second phase material, keeping the second phase in a shallow injection and shallow discharge process, which can continuously protect the structural stability of the first phase.

[0017] The present invention also provides a method for preparing the sodium ion battery positive electrode material, comprising the following steps:

[0018] (1) mixing and sintering a nickel-iron-manganese hydroxide precursor and a sodium source to prepare a first phase structure material;

[0019] (2) mixing and sintering the first phase structure material prepared in step (1) with the nano precursor, and preparing the second phase structure material by in-situ reaction on the surface of the first phase structure material to obtain the sodium ion battery positive electrode material;

[0020] The nano precursor is at least one of NiO, Al2O3, ZnO, MgCO3, Ni2O3, Mn2O3, MnO2, CaCO3, CaO, MgO, and TiO2.

[0021] The precursor of the sintered first phase material in the present invention is a precursor prepared by a coprecipitation process, which is usually purchased or homemade, and has the molecular formula: Ni c Fe d Mn e (OH)2, where 0.2≤c≤0.5, 0.2≤d≤0.4, 0.3≤e≤0.4;

[0022] The sodium source is at least one of Na2C2O4, Na2CO3, NaHCO3, HCOONa, and NaOH.

[0023] The first phase material is prepared by sintering a precursor with a sodium source, the sintering atmosphere is air or oxygen, the first phase sintering temperature is 850-900 degrees, and the sintering time is 15-18 hours;

[0024] The second phase material is prepared by in-situ reaction on the surface of the first phase material. The sintering atmosphere is air or oxygen. The second phase sintering temperature is 850-950 degrees and the sintering time is 5-15 hours.

[0025] The present invention also provides a positive electrode, which includes a positive electrode collector and the sodium ion battery positive electrode material arranged on both side surfaces of the positive electrode collector.

[0026] The present invention also provides a sodium ion battery comprising a positive electrode, a negative electrode and an organic electrolyte, wherein the positive electrode is the positive electrode described above.

[0027] Beneficial effects of the present invention:

[0028] (1) The first-phase material prepared by the present invention has a polycrystalline structure, and the particle size of the primary particles can be adjusted. The nanostructure provides abundant reaction sites at the electrode / electrolyte interface, which is conducive to the reversible insertion and extraction of sodium ions, thereby improving the capacity and rate performance of the electrode material;

[0029] (2) By adding a structural stabilizer to the first phase, the reaction of sodium ions in the structure with moisture and carbon dioxide in the air is inhibited at the atomic level, thereby improving the stability of the electrode and enhancing the stability of the electrode material in a humid environment;

[0030] (3) Through in-situ reaction on the surface of the first phase, a second phase sodium material with controllable thickness is generated. The second phase material has three main functions: (a) It has a highly stable structure to water. By coating the surface of the first phase, the air and water stability of the composite material is fundamentally stabilized, and the storage and processing performance of the material are completely solved; (b) It can adapt to the interface problem with the electrolyte under high charging voltage, improve the structural stability of the composite material at high potential, and reduce the occurrence of side reactions; (c) It has a higher reversible discharge capacity itself. Compared with other coating layers, it protects the first phase material without sacrificing the discharge capacity of the composite material.

[0031] (4) The present invention fully considers the design and optimization of factors such as the composition, morphology, and structure of the electrode material. Through a simple sintering process, the comprehensive performance of material processing and storage, discharge energy / rate / cycle, etc. can be improved, which has very outstanding advantages in sodium ion batteries for power and energy storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] FIG1 is an XRD diagram of the positive electrode materials prepared in Example 1 and Comparative Example 1.

[0033] Figure 2 is an SEM image of the positive electrode materials prepared in Example 1 and Comparative Example 1; wherein A is an SEM image of the positive electrode material prepared in Example 1, and B is an SEM image of the positive electrode material prepared in Comparative Example 1.

[0034] FIG3 is a graph showing the gram capacity data of the positive electrode materials prepared in Example 1 and Comparative Example 1.

[0035] Figure 4 is a slurry diagram of the positive electrode materials prepared in Example 2 and Comparative Example 2; wherein the left diagram is the slurry of the positive electrode material prepared in Example 2, and the right diagram is the slurry of the positive electrode material prepared in Comparative Example 2.

[0036] FIG5 is a graph showing the discharge capacity of full cells equipped with the positive electrode materials of Example 5 (first phase / second phase) and Comparative Example 3 (first phase).

[0037] FIG6 is a graph showing the cycle performance of a full battery equipped with the positive electrode materials of Example 5 (first phase / second phase) and Comparative Example 3 (first phase).

[0038] FIG7 is a diagram showing the gas production of soft-pack batteries equipped with the positive electrode materials of Example 5 (left) and Comparative Example 3 (right). DETAILED DESCRIPTION

[0039] Example 1

[0040] Nickel-iron-manganese composite hydroxide Ni 0.33 Fe 0.33 Mn 0.33 (OH)2 and anhydrous sodium carbonate Na2CO3 were put into a mixer according to the molar ratio of X(Fe+Mn+Ni):Na of 1:1.05 and mixed. The ball-to-material ratio was 2.5:1. After mixing for 2 hours, the sample was taken out and placed in a box furnace for sintering. The heating rate was maintained at 5℃ / min. After heating to 500℃ and holding for 5 hours, it was continued to rise to 850℃ at 5℃ / min and held for 18 hours to obtain a polycrystalline positive electrode material NaNi 0.33 Fe 0.33 Mn 0.33 O2.

[0041] Comparative Example 1

[0042] Nickel-iron-manganese composite hydroxide Ni 0.33 Fe 0.33 Mn 0.33 (OH)2 and anhydrous sodium carbonate Na2CO3 were mixed in a mixer at a molar ratio of X(Fe+Mn+Ni):Na of 1:1.0, with a ball-to-material ratio of 2.5:1. After mixing for 2 hours, the sample was taken out and placed in a box furnace for sintering. The heating rate was maintained at 5°C / min. After heating to 500°C and holding for 5 hours, it was continued at 5°C / min to 950°C and held for 30 hours to obtain a single crystal morphology positive electrode material NaNi0.33 Fe 0.33 Mn 0.33 O2.

[0043] Example 1 and Comparative Example 1 illustrate the control of polycrystalline and single crystal morphologies and their impact on discharge capacity. XRD and SEM characterization of the positive electrode materials prepared in Example 1 and Comparative Example 1 were performed. As shown in Figures 1 and 2, XRD confirmed that both materials had a pure-phase O3-type crystal structure. However, SEM images revealed significant differences in the morphology of the two materials. The material in Example 1 had a typical polycrystalline morphology, with a primary particle size of approximately 100 nm and a secondary particle size of 4-6 μm, while the material in Comparative Example 1 had a single crystal morphology with a particle size of approximately 5 μm.

[0044] The two types of materials were assembled into button-type batteries for electrical performance evaluation. Both batteries had the same positive electrode formula: active material: Super P: PVDF = 96:2.5:1.5, a sodium metal sheet for the negative electrode, and an electrolyte consisting of 1 mol NaPF6 dissolved in EC + PC (v:v = 1:1). Figure 3 shows that under the same test conditions, the gram capacity of the material in Example 1 was approximately 5 mAh / g higher than that of the material in Comparative Example 1, demonstrating that the polycrystalline material has more reactive sites, enabling it to better utilize its high specific capacity characteristics.

[0045] Example 2

[0046] Nickel-iron-manganese composite hydroxide Ni 0.27 Fe 0.3 Cu 0.03 Ti 0.05 Mn 0.35 (OH)2 and anhydrous sodium oxalate Na2C2O4 were mixed in a mixer at a molar ratio of X(Fe+Mn+Ni+Cu+Ti):Na of 1:1.03, with a ball-to-material ratio of 2.5:1. After mixing for 2 hours, the sample was taken out and placed in a box furnace for sintering. The heating rate was maintained at 5℃ / min. After heating to 500℃ and holding for 5 hours, it was continued to rise at 5℃ / min to 900℃ and held for 18 hours. The positive electrode Cu and Ti-doped positive electrode material Na 0.95 Ni 0.27 Fe 0.3 Cu 0.03 Ti 0.05 Mn 0.35 O2.

[0047] Example 3

[0048] Nickel-iron-manganese composite hydroxide Ni 0.28 Fe 0.3 Ca 0.04 Sn 0.05 Mn 0.35(OH)2 and sodium bicarbonate NaHCO3 are mixed in a mixer at a molar ratio of X(Fe+Mn+Ni+Ca+Sn):Na of 1:1.03, and the ball-to-material ratio is 2.5:1. After mixing for 2 hours, the sample is taken out and placed in a box furnace for sintering. The heating rate is maintained at 5℃ / min. After heating to 500℃ and holding for 5 hours, it is continued to rise at 5℃ / min to 900℃ and holding for 18 hours. The positive electrode material NaNi doped with Ca and Sn 0.28 Fe 0.3 Ca 0.04 Sn 0.05 Mn 0.35 O2.

[0049] Example 4

[0050] Nickel-iron-manganese composite hydroxide Ni 0.3 Fe 0.27 K 0.03 Ti 0.05 Mn 0.35 (OH)2 and sodium acetate HCOONa were mixed in a mixer at a molar ratio of X(Fe+Mn+Ni+K+Ti):Na of 1:1, and the ball-to-material ratio was 2.5:1. After mixing for 2 hours, the sample was taken out and placed in a box furnace for sintering. The heating rate was maintained at 5℃ / min. After heating to 500℃ and holding for 5 hours, it was continued to rise to 900℃ at 5℃ / min and held for 18 hours. The positive electrode material Na doped with K and Ti was 0.95 Ni 0.3 Fe 0.27 K 0.03 Ti 0.05 Mn 0.35 O2.

[0051] Comparative Example 2

[0052] Nickel-iron-manganese composite hydroxide Ni 0.3 Fe 0.3 Mn 0.4 (OH)2 and anhydrous sodium oxalate Na2C2O4 were mixed in a mixer at a molar ratio of X(Fe+Mn+Ni):Na of 1:1.02, with a ball-to-material ratio of 2.5:1. After mixing for 2 hours, the sample was taken out and placed in a box furnace for sintering. The heating rate was maintained at 5°C / min. After heating to 500°C and holding for 5 hours, the temperature was continued to rise at 5°C / min to 900°C and held for 18 hours to obtain the positive electrode material NaNi 0.3 Fe 0.3 Mn 0.4 O2.

[0053] After the two types of materials prepared in Example 2 and Comparative Example 2 were placed in an environment with a relative humidity of 70% for 48 hours, they were mixed with deionized water at a mass ratio of 1:20, and the pH test was performed after the slurry was prepared. The results are shown in Table 1. The results show that doping the materials with Cu and Ti as stabilizers can improve the sensitivity of the materials to moisture. Further studies on the two types of materials showed that the material in Example 2 was able to maintain good slurry fluidity and viscosity when preparing the electrode in an environment with a relative humidity of 70%, while the comparative example clearly showed a jelly gel phenomenon (Figure 4). This comparison shows that a small amount of stabilizer can slow down the adsorption and reaction of the material to water and improve the processing performance of the material.

[0054] Table 1

[0055] Example 5

[0056] Nickel-iron-manganese composite hydroxide Ni 0.33 Fe 0.33 Mn 0.33 (OH)2 and sodium hydroxide NaOH were mixed in a mixer at a molar ratio of X(Fe+Mn+Ni):Na of 1:1.1, with a ball-to-material ratio of 2.5:1. After mixing for 2 hours, the sample was taken out and sintered in a box furnace. The heating rate was maintained at 5°C / min. After heating to 500°C and holding for 5 hours, the temperature was continued to rise at 5°C / min to 850°C and held for 15 hours. The sample was then cooled naturally to room temperature as the first phase material (Na 1.07 Ni 0.33 Fe 0.33 Mn 0.33 O2) was used. The sintered first phase material was remixed with nano Mn2O3, NiO and CaCO3 (molar ratio of Mn2O3: NiO: CaCO3 = 31: 33: 5) with a pellet ratio of 2: 1. After mixing for 1 hour, the sample was taken out and placed in a box furnace for sintering at a temperature of 900 ° C and a sintering time of 12 hours. The first phase and the second phase (chemical formula Na 0.67 Ca 0.05 Mn 0.62 Ni 0.33 The molar ratio of O2) is 90:10.

[0057] Example 6

[0058] Nickel-iron-manganese composite hydroxide Ni 0.2 Fe 0.4 Mn 0.35 Ti 0.05(OH)2 and sodium hydroxide Na2CO3 were mixed in a mixer at a molar ratio of X(Fe+Mn+Ni+Ti):Na of 1:1.1, with a ball-to-material ratio of 2.5:1. After mixing for 2 hours, the sample was taken out and sintered in a box furnace. The heating rate was maintained at 5°C / min. After heating to 500°C and holding for 5 hours, the temperature was continued to rise at 5°C / min to 850°C and held for 15 hours. The sample was then cooled naturally to room temperature as the first phase material (Na 1.08 Ni 0.2 Fe 0.4 Mn 0.35 Ti 0.05 O2) is used. The sintered first phase material is mixed with nano Mn2O3, ZnO and MgCO3 (molar ratio of Mn2O3: ZnO: MgCO3 = 40: 10: 10) again, with a ball-to-material ratio of 2: 1. After mixing for 1 hour, the sample is taken out and placed in a box furnace for sintering at a temperature of 870 ° C and a sintering time of 12 hours. The first phase and the second phase (Na 0.5 Mn 0.8 Zn 0.05 Mg 0.05 The molar ratio of O2) is 90:10.

[0059] Example 7

[0060] Nickel-iron-manganese composite hydroxide Ni 0.5 Fe 0.18 Al 0.02 Mn 0.3 (OH)2 and sodium hydroxide NaOH were mixed in a mixer at a molar ratio of X(Fe+Mn+Ni+Al):Na of 1:1.05, with a ball-to-material ratio of 2.5:1. After mixing for 2 hours, the sample was taken out and sintered in a box furnace. The heating rate was maintained at 5°C / min. After heating to 500°C and holding for 5 hours, the temperature was continued to rise at 5°C / min to 850°C and held for 15 hours. The sample was then cooled naturally to room temperature as the first phase material (Na 1.03 Ni 0.5 Fe 0.18 Mn 0.3 Al 0.02 O2). The sintered first phase material was remixed with nano-Al2O3, NiO, Mn2O3 and CuO (molar ratio Al2O3: NiO: Mn2O3: CuO = 5: 20: 33.5: 10), with a pellet ratio of 2: 1. After mixing for 1 hour, the sample was taken out and sintered in a box furnace at a temperature of 900 ° C for 12 hours. 0.7 Ni 0.2 Al 0.1 Cu 0.1 Mn 0.67 The molar ratio of O2) is 95:5.

[0061] Comparative Example 3

[0062] The first phase material in Example 5 was cooled without further processing.

[0063] (1) Sensitivity to moisture

[0064] The moisture sensitivity of the materials prepared in Example 5 and Comparative Example 3 is shown in Table 2. The results show that the pH value of the composite material in Example 5 is very stable in water, remaining essentially at around 11.5-11.6 over the 3-minute test period. In contrast, the pH value of the composite material in Comparative Example gradually increases over time, clearly indicating hydrolysis. This comparison demonstrates the significant improvement in moisture sensitivity achieved by the second-phase material in Example 5.

[0065] Table 2

[0066] (2) Discharge capacity

[0067] The two materials prepared in Example 5 and Comparative Example 3 were assembled into cylindrical batteries, and the discharge capacity of these batteries was measured. Both batteries had the same positive electrode formulation: active material: Super P: PVDF = 96:2.5:1.5. The negative electrode used sodium metal sheet, and the electrolyte consisted of 1 mol NaPF6 dissolved in EC + PC (v:v = 1:1). The experimental results, shown in Figure 5, show that the capacity of the coated materials remained essentially stable, demonstrating that while the second-phase material improved stability, the overall battery performance did not decrease due to its activity.

[0068] (3) Cycle performance

[0069] FIG6 shows the cycle performance of the two materials of Comparative Example 5 and Comparative Example 3.

[0070] The experimental results show that under the same electrochemical window (1.5-3.95V), the battery cell prepared with the material of Example 5 has a capacity retention rate of 97.7% after 300 cycles, while the battery cell prepared with the material of Comparative Example 3 has a capacity retention rate of only 95.1% under the same conditions, proving that the second-phase coated composite material has higher stability.

[0071] (4) Gas production

[0072] FIG7 shows the gas production of the two materials of Comparative Example 5 and Comparative Example 3 in soft-pack batteries.

[0073] The experimental results show that under the same cycle conditions (rate 0.5C, window 1.5-3.95V), the soft-pack battery cell prepared in Example 5 showed no obvious gas production after 500 cycles, while the material in Comparative Example 3 could not be used normally due to severe gas production after 420 cycles.

Claims

1. A sodium ion battery positive electrode material, characterized in that: The sodium ion battery positive electrode material comprises a first phase structural material and a second phase structural material; The molecular formula of the first phase structural material is: Na a M b Ni c Fe d Mn e O2, Wherein, M is selected from at least one of Ti, Cu, Ca, K, Sn, Li, Al, Mg, Co, Ag, Ce, and Ba; 0.95≤a≤1.1, 0≤b≤0.05, 0.2≤c≤0.5, 0.2≤d≤0.4, and 0.3≤e≤0.4; The molecular formula of the second phase structural material is: Na x N w Ni y Mn z O2, Wherein, N is selected from at least one of Mn, Ni, Ca, Al, Mg, and Zn; 0.5≤x≤0.7, 0.0≤y≤0.33, 0.62≤z≤0.8, 0.05≤w≤0.1; The second phase structural material is coated on the first phase structural material, and the second phase structural material is formed by in-situ growth on the surface of the first phase structural material.

2. The sodium ion battery positive electrode material according to claim 1, characterized in that The first phase structural material accounts for 81%-99% of the mass percentage of the sodium ion battery positive electrode material; the second phase structural material accounts for 1%-20% of the mass percentage of the sodium ion battery positive electrode material.

3. The sodium ion battery positive electrode material according to claim 1, characterized in that The M is selected from at least one of Ti, Cu, Sn, K and Ca.

4. The sodium ion battery positive electrode material according to claim 1, characterized in that The first phase structure material is a layered structure, and the second phase structure material is a layered structure or a three-dimensional structure.

5. The method for preparing the positive electrode material for a sodium ion battery according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) mixing and sintering a nickel-iron-manganese hydroxide precursor and a sodium source to prepare a first phase structure material; (2) mixing and sintering the first phase structure material prepared in step (1) with the nano precursor, preparing the second phase structure material by in-situ reaction on the surface of the first phase structure material, and preparing the sodium ion battery positive electrode material; The nano precursor is at least one of NiO, Al2O3, ZnO, MgCO3, Ni2O3, Mn2O3, MnO2, CaCO3, CaO, MgO, and TiO2.

6. The method for preparing a positive electrode material for a sodium ion battery according to claim 5, characterized in that: The molecular formula of the nickel iron manganese hydroxide precursor in step (1) is: Ni c Fe d Mn e (OH)2, where 0.2≤c≤0.5, 0.2≤d≤0.4, 0.3≤e≤0.4; The sodium source is at least one of Na2C2O4, Na2CO3, NaHCO3, HCOONa, and NaOH.

7. The method for preparing a positive electrode material for a sodium ion battery according to claim 5, characterized in that: In step (1), the sintering atmosphere is air or oxygen, the sintering temperature is 850-900° C., and the sintering time is 15-18 hours.

8. The method for preparing a positive electrode material for a sodium ion battery according to claim 5, characterized in that: In step (2), the sintering atmosphere is air or oxygen, the sintering temperature is 850-950° C., and the sintering time is 5-15 hours.

9. A positive electrode, characterized in that The positive electrode comprises a positive electrode current collector and a positive electrode material for a sodium ion battery according to any one of claims 1 to 4 arranged on both side surfaces of the positive electrode current collector.

10. A sodium ion battery comprising a positive electrode, a negative electrode and an organic electrolyte, characterized in that: The positive electrode is the positive electrode according to claim 9.

Citation Information

Patent Citations

  • Core-shell structure sodium ion battery positive electrode material and preparation method and application thereof

    CN110277540A

  • Doped coated sodium ion battery positive electrode material and preparation method and application thereof

    CN110838576A

  • Coated modified sodium ion battery positive electrode material, preparation method thereof, and battery

    CN113937286A

  • O3-P2 composite phase sodium ion positive electrode material as well as preparation method and application thereof

    CN115148984A

  • Monocrystalline sodium ion battery positive electrode material, preparation method thereof and battery

    CN115275178A

Cited By

  • Positive electrode active material and preparation method thereof, sodium ion battery and electric equipment

    CN119361664A

  • Modified sodium ion battery positive electrode material and preparation method and application thereof

    CN119612553A

  • P '2-phase sodium-electrode layered transition metal oxide positive electrode material as well as preparation method and application thereof

    CN119612595A