Secondary battery and electric apparatus

By using a combination of organic lithium salts and inorganic lithium salts in secondary batteries, as well as multi-particle size positive active materials and optimized electrode structures, the problem of insufficient kinetic performance of secondary batteries is solved and high energy density and excellent power are achieved Simultaneous improvement of learning performance.

WO2024217601A1PCT designated stage expired Publication Date: 2024-10-24CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2024/099858
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-06-18
Publication Date
2024-10-24

Smart Images

  • Figure CN2024099858_24102024_PF_FP_ABST
    Figure CN2024099858_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a secondary battery. The secondary battery comprises an electrolyte and a positive electrode, wherein the electrolyte contains an organic lithium salt; and the positive electrode includes a positive-electrode film layer, and the energy density per unit area of a single side of the positive electrode film layer ranges from 18 to 37 mWh / cm2, and optionally ranges 18 from 35.7 mWh / cm2. By means of the mutual cooperation between an electrolyte and a positive electrode, both the energy density and dynamic performance of a battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Secondary batteries and electrical devices

[0001] Cross-references

[0002] This application refers to the PCT patent application entitled “Secondary Batteries and Electrical Devices” filed on April 18, 2023 with patent application number PCT / CN2023 / 089061, which is incorporated herein by reference in its entirety. Technical Field

[0003] The present application relates to the technical field of secondary batteries, and in particular to a high-energy-density secondary battery and an electrical device. Background Art

[0004] Secondary batteries are widely used in electric vehicles, energy storage systems, and mobile electronic devices due to their high energy density, long life, and low self-discharge rate. As secondary batteries have made great progress, higher requirements are placed on their performance.

[0005] High-energy-density secondary batteries often suffer from poor kinetic and rate performance. Producing secondary batteries with excellent overall performance, including energy levels and kinetics, is a technical problem that urgently needs to be solved in this field.

[0006] Summary of the Invention

[0007] The present application has been made in view of the above-mentioned problems, and an object of the present application is to provide a secondary battery having both high energy density and dynamic performance.

[0008] In a first aspect of the present application, a secondary battery is provided, wherein the secondary battery comprises an electrolyte and a positive electrode, wherein the electrolyte comprises an organic lithium salt; the positive electrode comprises a positive electrode film layer, and the energy density per unit area of ​​the positive electrode film layer on a single side is 18 to 37 mWh / cm 2 , can be selected from 18 to 35.7 mWh / cm 2 .

[0009] Organic lithium salts in the electrolyte can effectively improve the electrolyte's ion conductivity, reduce the impedance of the electrolyte / electrode interface, and form a stable and highly ion-conductive passivation film on the electrode surface, thereby improving interfacial stability. Organic lithium salts in the electrolyte can increase the lithium ion transfer rate in the positive electrode film, optimizing the battery's kinetic and rate performance, thereby simultaneously improving the energy density and kinetic performance of secondary batteries.

[0010] In any embodiment, the positive electrode film layer and the organic lithium salt satisfy the following relationship: 0.005≤M-0.0005×w≤0.2, wherein M is the mass content of the organic lithium salt based on the total mass of the electrolyte; w is the surface density of the positive electrode film layer on one side, in mg / cm2 .

[0011] In order to increase the energy density of the battery, it is usually necessary to increase the surface density of the positive electrode film layer. However, a pole piece with a large surface density is not conducive to the transmission of ions in the positive electrode film layer, resulting in reduced battery kinetic performance and rate performance. The present application achieves simultaneous optimization of battery energy density and rate performance by matching the positive electrode film layer with the organic lithium salt. When the positive electrode film layer and the organic lithium salt meet the above relationship, the high energy density positive electrode piece and the organic lithium salt form an effective combination to achieve a simultaneous improvement in battery energy density and kinetic performance.

[0012] In any embodiment, the surface density w of the positive electrode film layer on one side is not less than 20 mg / cm 2 , optionally 25 to 45 mg / cm 2 .

[0013] Controlling the surface density of the single-sided positive electrode film layer within an appropriate range can ensure that the battery has both high energy density and rate performance.

[0014] In any embodiment, the organic lithium salt comprises at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide.

[0015] The above-mentioned organic lithium salt has high ionic conductivity and stable electrochemical properties, which can increase the transmission rate of lithium salt in the positive electrode film layer, reduce electrode polarization, and improve the kinetic performance of the battery.

[0016] In any embodiment, the electrolyte further includes an inorganic lithium salt, and the molar ratio of the organic lithium salt to the inorganic lithium salt is 1:5 to 5:1.

[0017] Compared to organic lithium salts, inorganic lithium salts offer lower costs and higher withstand voltages. Examples include, but are not limited to, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, and lithium perchlorate. When the ratio of inorganic to organic lithium salts is within an appropriate range, the battery's rate performance can be effectively improved while reducing cost.

[0018] In any embodiment, the positive electrode film layer contains positive electrode active material, and the positive electrode active material includes particles A and particles B. The particles A are polycrystalline particles, and the volume average particle size of the particles A is larger than the volume average particle size of the particles B.

[0019] The positive electrode active material of the present application includes two particles of different particle sizes. By grading the large-sized particles A with the small-sized particles B, the pores between the particles can be effectively filled, the compaction density of the pole piece can be increased, and thus the energy density per unit volume of the battery can be increased. During the battery cycle, cracks are easily formed between the grains of the polycrystalline particles A, which is conducive to the diffusion of lithium ions and helps to improve the battery rate performance. At the same time, the grading of the large-sized particles A and the small-sized particles B can also reduce the electrolyte consumption and the increase in pore resistance caused by the excessive pores between the particles of the pole piece, thereby improving the battery rate performance.

[0020] In any embodiment, the positive electrode film layer further satisfies at least one of the following characteristics:

[0021] (1) The particles B are polycrystalline, single crystal or quasi-single crystal particles;

[0022] (2) The primary particle size of the particle A is 50 nm to 400 nm, and may be 80 to 200 nm; the primary particle size of the particle B is 150 nm to 2 μm, and may be 200 nm to 1.2 μm;

[0023] (3) The volume average particle size of the particles A is 2 to 25 μm, and may be 2.5 to 23 μm; the volume average particle size of the particles B is 0.65 to 10 μm, and may be 1.2 to 8.5 μm;

[0024] (4) The mass ratio of the particles A to the particles B is 5:5 to 9:1;

[0025] (5) The laser particle size distribution curve of the positive electrode active material is bimodal, and the peak position difference between the two peaks is 3 to 7 μm;

[0026] (6) The positive electrode includes a positive electrode current collector, and the ratio of the thickness of the positive electrode film layer on a single side to the thickness of the positive electrode current collector is 5.5 to 15, and optionally 5.6 to 8.8.

[0027] When the positive electrode film layer meets at least one of the above conditions, the battery has high energy density and excellent kinetic performance.

[0028] In any embodiment, based on the total molar number of transition metal elements in the positive electrode active material, the molar content of nickel element is not less than 80%; alternatively, not less than 85%; further alternatively, not less than 90%.

[0029] Due to the high relative content of nickel, the gram capacity of the positive electrode active material is correspondingly high, which can effectively improve the energy density of the battery.

[0030] In any embodiment, the compositions of the particles A and B independently satisfy the formula I, Li a1 Nix1 Co y1 Mn z1 M1 b1 O2M1' c1 , Formula I

[0031] Among them, a1 is 0.8-1.2, x1 is 0.85-1, y1 is 0-0.15, z1 is 0-0.15, b1 is 0-0.02, c1=1-x1-y1-z1-b1, M1 includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Sb, Nb, Na, K, B, Mg, Zn, Ca or Ce, and M1' includes at least one of N, F, S or Cl.

[0032] The high nickel content in particles A and B can improve the battery's energy density. Furthermore, the inclusion of M1 in particles A and B can reduce lithium-nickel mixing in the active material during cycling, improving the material's structural stability. This ensures that even after lithium ions are deintercalated from the positive electrode during charging, the positive electrode active material maintains a relatively intact structure, thereby improving the battery's discharge performance.

[0033] In any embodiment, the positive electrode film layer contains a positive electrode active material, and the positive electrode active material is a single crystal or a quasi-single crystal particle and meets at least one of the following characteristics:

[0034] (1) The laser particle size distribution curve of the positive electrode active material is single-peaked;

[0035] (2) The volume average particle size D of the single crystal or quasi-single crystal particles v 50 is 1 to 3.5 μm, optionally 1.2 to 3.0 μm;

[0036] (3) The laser particle size distribution of the single crystal or quasi-single crystal particles satisfies: 0.3≤(D v 99-D v 90) / (2×D v 50)≤0.55;

[0037] (4) The composition of the single crystal or single crystal-like particles is shown in Formula II: Li a2 Ni x2 Co y2 Mn z2 M2 b2 O2M2' c2 , Formula II

[0038] wherein a2 is 0.8 to 1.2, x2 is 0.85 to 1, y2 is 0 to 0.15, z2 is 0 to 0.15, b2 is 0 to 0.02, c2 = 1-x2-y2-z2-b2, M2 includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Sb, Nb, Na, K, B, Mg, Zn, Ca, or Ce, and M2' includes at least one of N, F, S, or Cl; optionally, x2 is 0.90 to 1;

[0039] (5) The positive electrode includes a positive electrode current collector, and the ratio of the thickness of the positive electrode film layer on one side to the thickness of the positive electrode current collector is 4.5 to 9, and optionally 4.5 to 8.5.

[0040] Cathode materials formed from single-crystal particles have a large surface area and a dense structure. This allows the positive electrode active material to maintain good structural stability while having a high compaction density. This reduces side reactions during charge and discharge, slows electrolyte consumption, and improves battery life. Cathode active materials that meet these conditions exhibit good structural stability, enabling batteries containing them to have high energy density and excellent rate performance.

[0041] In any embodiment, the pore volume of the positive electrode film layer accounts for 18% to 35% of the total volume of the positive electrode film layer.

[0042] When the pore volume of the positive electrode film layer is within an appropriate range, the organic lithium salt in the electrolyte can easily enter the pores of the positive electrode film layer and fully contact the positive electrode active material, thereby increasing the migration rate of ions at the electrode / electrolyte interface, reducing the internal resistance of the battery, and improving the cycle performance and rate performance of the battery.

[0043] In any embodiment, the secondary battery further includes a negative electrode, the negative electrode including a negative electrode membrane, the negative electrode membrane including a negative electrode active material, the negative electrode active material including a silicon-based material, the silicon-based material being selected from one or more of elemental silicon, silicon-oxygen materials, and silicon-carbon materials. Silicon-based materials can significantly increase the energy density of the battery.

[0044] In any embodiment, the negative electrode active material further comprises a carbon-based material, and the mass ratio of the carbon-based material to the silicon-based material is no more than 4:6, and can optionally be no more than 2:8.

[0045] When the mass ratio of carbon-based materials to silicon-based materials is within the above range, the battery can have a high energy density while reducing the expansion of the negative electrode and improving the cycle performance and rate performance.

[0046] In any embodiment, the surface density of the negative electrode membrane is 6 to 13 mg / cm 2 .

[0047] When the surface density of the negative electrode film is within the above range, the negative electrode adopts a thick coating design, which helps to improve the energy density of the battery. The second aspect of the present application provides an electrical device including the secondary battery of the first aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] FIG1 is a schematic diagram of a secondary battery cell according to an embodiment of the present application;

[0049] FIG2 is an exploded view of a secondary battery cell according to an embodiment of the present application shown in FIG1 ;

[0050] FIG3 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.

[0051] Description of reference numerals: 5 secondary battery; 51 housing; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION

[0052] Below, the embodiments of the current collector, secondary battery, battery module, battery pack and power device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0053] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0054] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0055] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0056] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0057] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0058] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0059] With the widespread use of secondary batteries, demands for their performance, such as energy density, are gradually increasing. To improve battery energy density, thick coatings of active materials are often employed. However, this thick coating of active material lengthens the migration path of lithium ions within the membrane, increasing the resistance to migration. This increases the polarization resistance of the electrode and reduces the battery's dynamic performance. Therefore, there is an urgent need to develop a secondary battery that combines improved energy density with excellent dynamic performance.

[0060] Based on this, the present application proposes a secondary battery that achieves a simultaneous improvement in battery energy density and dynamic performance through the interaction between the electrolyte and the positive electrode.

[0061] In some embodiments, the secondary battery includes an electrolyte and a positive electrode, wherein the electrolyte includes an organic lithium salt; the positive electrode includes a positive electrode film layer, and the energy density per unit area of ​​the single-side positive electrode film layer is 18 to 37 mWh / cm2 , can be selected from 18 to 35.7 mWh / cm 2 .

[0062] Organic lithium salts can generally be viewed as inorganic lithium salts, formed by introducing one or more electron-withdrawing groups into the salt, and regulating and controlling the structure of the anion. The anions of organic lithium salts generally have a large radius, a dispersed charge distribution, and a strong ionization passivation effect. This reduces the lattice energy of the lithium salt, weakens the interaction between positive and negative ions, and increases the solubility of the lithium salt. Organic lithium salts include, but are not limited to, lithium bis(fluorosulfonyl imide) and lithium bis(trifluoromethylsulfonyl imide).

[0063] In some embodiments, the positive electrode film is located on both sides of the current collector. In some embodiments, the positive electrode film is located on either side of the current collector. It is understood that the term "single-sided positive electrode film" refers to a positive electrode film located on either side of the positive electrode sheet.

[0064] The unit area energy density of the single-sided positive electrode film layer can be measured using methods and equipment commonly used in the field. As an example, the unit area energy density of the positive electrode film layer can be operated according to the following steps: let the battery cell stand at a certain temperature (for example, 25°C) for a certain time (for example, 2h), and ensure that the temperature of the battery cell is room temperature (for example, 25°C). After charging the battery cell to the charge cut-off voltage at a certain rate (for example, 0.33C) at a certain temperature (for example, 25°C), continue to charge at a constant voltage at the charge cut-off voltage until the current is 0.05C and the charge is cut off (C represents the rated capacity of the battery cell). After the battery cell is allowed to stand at a certain temperature (for example, 25°C) for a certain time (for example, 1h), discharge the battery cell to the discharge cut-off voltage at a certain rate (0.33C) at a certain temperature (for example, 25°C), and record the total discharge energy as E0. Disassemble the battery, remove the positive electrode sheet, and use a ruler to measure the length and width of the positive electrode film layer to obtain the area value S0 of the positive electrode film layer. If the positive electrode film layer is coated on both sides, the energy per unit area of ​​the positive electrode film layer = E0 / (2×SS0). If the positive electrode film layer is coated on one side, the energy per unit area of ​​the positive electrode film layer = E0 / S0.

[0065] In the above test method, the charge cut-off voltage of the battery cell is 4.25V, the discharge cut-off voltage is 2.0V, and the charge rate and discharge rate are both 0.33C.

[0066] In some embodiments, the energy density per unit area of ​​the positive electrode film layer on one side is 18mWh / cm 2 、19.3mWh / cm 2 、20mWh / cm 2 、21mWh / cm 2 、22mWh / cm 2 、23mWh / cm2 、24mWh / cm 2 , 25mWh / cm 2 、26mWh / cm 2 、27mWh / cm 2 、28mWh / cm 2 、29mWh / cm 2 、30mWh / cm 2 、31mWh / cm 2 、32mWh / cm 2 、33mWh / cm、34mWh / cm 2 、35mWh / cm 2 、35.7mWh / cm 2 、36mWh / cm 2 、37mWh / cm 2 Or a value in the range formed by any two of the above points.

[0067] Organic lithium salts in the electrolyte can effectively improve the electrolyte's ion conductivity, reduce the impedance of the electrolyte / electrode interface, and form a stable and highly ion-conductive passivation film on the electrode surface, thereby improving interfacial stability. Organic lithium salts in the electrolyte can increase the lithium ion transfer rate in the positive electrode film, optimizing the battery's kinetic and rate performance, thereby simultaneously improving the energy density and kinetic performance of secondary batteries.

[0068] In some embodiments, the positive electrode film layer and the organic lithium salt satisfy the following relationship: 0.005≤M-0.0005×w≤0.2, where M is the mass content of the organic lithium salt based on the total mass of the electrolyte; w is the surface density of the single-sided positive electrode film layer, in mg / cm 2 .

[0069] In order to increase the energy density of the battery, it is usually necessary to increase the surface density of the positive electrode film layer. However, a pole piece with a large surface density is not conducive to the transmission of ions in the positive electrode film layer, resulting in reduced battery kinetic performance and rate performance. The present application achieves simultaneous optimization of battery energy density and rate performance by matching the positive electrode film layer with the organic lithium salt. When the positive electrode film layer and the organic lithium salt meet the above relationship, the high energy density positive electrode piece and the organic lithium salt form an effective combination to achieve a simultaneous improvement in battery energy density and kinetic performance.

[0070] In some embodiments, the thickness of the positive electrode film layer on one side is 70 μm to 160 μm, optionally 80 μm to 140 μm, 90 μm to 130 μm, or 100 μm to 120 μm. Controlling the thickness of the positive electrode film layer on one side within an appropriate range can ensure that the battery has both high energy density and good rate performance.

[0071] In some embodiments, the surface density w of the single-sided positive electrode film layer is not less than 20 mg / cm 2 , optionally 25 to 45 mg / cm 2 .

[0072] In some embodiments, the surface density w of the single-sided positive electrode film layer can be selected to be 20 mg / cm 2 , 25mg / cm 2 、30mg / cm 2 、35mg / cm 2 , 40mg / cm 2 or 45 mg / cm 2 Controlling the surface density of the single-sided positive electrode film layer within an appropriate range can ensure that the battery has both high energy density and rate performance.

[0073] In some embodiments, the organic lithium salt includes at least one of lithium bis(fluorosulfonyl)imide (LiFSI) and lithium bis(trifluoromethylsulfonyl)imide (LiTFSI).

[0074] The above-mentioned organic lithium salt has high ionic conductivity and stable electrochemical properties, which can increase the transmission rate of lithium salt in the positive electrode film layer, reduce electrode polarization, and improve the kinetic performance of the battery.

[0075] In some embodiments, the electrolyte further includes an inorganic lithium salt, and the molar ratio of the organic lithium salt to the inorganic lithium salt is 1:5 to 5:1.

[0076] Compared to organic lithium salts, inorganic lithium salts offer lower costs and higher withstand voltages. Examples include, but are not limited to, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, and lithium perchlorate. When the ratio of inorganic to organic lithium salts is within an appropriate range, the battery's rate performance can be effectively improved while reducing cost.

[0077] In some embodiments, the positive electrode film layer contains a positive electrode active material, the positive electrode active material includes particles A and particles B, particles A are polycrystalline particles, and the volume average particle size of particles A is larger than the volume average particle size of particles B.

[0078] Herein, the “volume average particle size” is also referred to as Dv50, and refers to the particle size corresponding to when the cumulative volume of particles reaches 50% in particle size distribution measurement performed by a laser scattering method.

[0079] The volume average particle size can be measured using equipment and methods known in the art. For example, a Microtrac MRB S3500 series laser particle size analyzer is used for particle size distribution testing. The specific testing process is as follows: 0.05-2g of the positive electrode active material is added to 10-20ml of deionized water. Ultrasound is then applied at a frequency of 53kHz and a power of 120W for 5 minutes to ensure complete dispersion of the sample. The sample is then measured according to GB / T19077-2016 or ISO 13320:2009. The particle size distribution curve is used to measure the Dv50 value of the particles.

[0080] In this article, "polycrystalline" refers to a crystal composed of many single crystal grains with different orientations. The entire structure is not permeated by a uniform lattice. The structure of each small crystal is identical and anisotropic.

[0081] The positive electrode active material of the present application includes two particles of different particle sizes. By grading the large-sized particles A with the small-sized particles B, the pores between the particles can be effectively filled, the compaction density of the pole piece can be increased, and thus the energy density per unit volume of the battery can be increased. During the battery cycle, cracks are easily formed between the grains of the polycrystalline particles A, which is conducive to the diffusion of lithium ions and helps to improve the battery rate performance. At the same time, the grading of the large-sized particles A and the small-sized particles B can also reduce the electrolyte consumption and the increase in pore resistance caused by the excessive pores between the particles of the pole piece, thereby improving the battery rate performance.

[0082] In some embodiments, the particles B are polycrystalline, single crystal, or quasi-single crystal particles.

[0083] In this article, the term "single crystal" refers to a perfectly grown crystal with an internal structure that conforms perfectly to a lattice structure. A single crystal has no grain boundaries on a macroscopic scale, and the crystal orientation remains consistent throughout its structure.

[0084] In this article, "quasi-single crystal" refers to a crystal with a small number of grains and a large grain size.

[0085] Particle B is polycrystalline, which can further improve the rate performance of the battery. Particle B is single crystal or quasi-single crystal, which helps to improve the structural stability of the positive electrode active material during the cycle.

[0086] In some embodiments, the primary particle size of particle A is 50 nm to 400 nm, optionally 80 to 200 nm; the primary particle size of particle B is 150 nm to 2 μm, optionally 200 nm to 1.2 μm.

[0087] In some embodiments, the primary particle size of particle A is any one of 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 250nm, 300nm, 350nm, 400nm or any value therebetween.

[0088] In some embodiments, the primary particle size of particle B is any one of 150 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2 μm, or any value therebetween. As used herein, "primary particle size" refers to the particle size of a primary particle.

[0089] In this article, "primary particles" refer to solid basic particles obtained by dispersion or refinement without changing the essential structure of the substance. Primary particles are particles that have not formed an agglomerate state.

[0090] In some embodiments, the volume average particle size of particles A is 2 to 25 μm, and may be 2.5 to 23 μm; the volume average particle size of particles B is 0.65 to 10 μm, and may be 1.2 to 8.5 μm.

[0091] In some embodiments, the volume average particle size of particles A is any one of 2 μm, 2.5 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm, 25 μm or any value therebetween.

[0092] In some embodiments, the volume average particle size of particles B is any one of 0.65 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 8.5 μm, 9 μm, 10 μm, or any value therebetween. It will be understood that the volume average particle size can be either a primary particle size or a secondary particle size. In some embodiments, for single crystal materials, the volume average particle size is the primary particle size. In some embodiments, for polycrystalline materials, the volume average particle size is the particle size of the secondary particles after agglomeration of the primary particles.

[0093] The volume average particle size of polycrystalline particles A is larger than that of polycrystalline particles B. The migration path of lithium ions in particles A is long, while its primary particle size is small, which can promote the rapid migration of lithium ions and balance the kinetic performance.

[0094] In some embodiments, the mass ratio of particles A to particles B is 5:5 to 9:1. In some embodiments, the laser particle size distribution curve of the positive electrode active material is bimodal, and the peak position difference between the two peaks is 3 to 7 μm.

[0095] In some embodiments, the mass ratio of particles A to particles B is any one of 1, 2, 3, 4, 5, 6, 7, 8, 9 or any value therebetween.

[0096] In some embodiments, the laser particle size distribution curve of the positive electrode active material is bimodal, and the peak position difference between the two peaks is any one of 3μm, 4μm, 5μm, 6μm, 7μm, or any value therebetween. By matching the mass and / or particle size of the large and small particles, the compaction density of the electrode sheet can be further increased, thereby improving the volumetric energy density of the battery.

[0097] In some embodiments, the positive electrode includes a positive electrode current collector, the positive electrode film layer contains a positive electrode active material, the positive electrode active material includes particles A and particles B, and the ratio of the thickness of the single-sided positive electrode film layer to the thickness of the positive electrode current collector is 5.5 to 15, optionally 5.6 to 8.8.

[0098] When the ratio of the thickness of the single-sided positive electrode film layer to the thickness of the positive electrode current collector is within this range, the energy density per unit area of ​​the positive electrode film layer can be improved.

[0099] When the positive electrode film layer meets the above conditions, the positive electrode sheet can achieve an increase in the sheet compaction density through mutual matching between the positive electrode active materials, so that the battery including the positive electrode active material can have both high energy density and excellent rate performance.

[0100] In some embodiments, based on the total molar number of transition metal elements in the positive electrode active material, the molar content of nickel element is not less than 80%; alternatively, not less than 85%; further alternatively, not less than 90%.

[0101] In some embodiments, the molar content of nickel element may be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% or 100% based on the total molar number of transition metal elements in the positive electrode active material.

[0102] Due to the high relative content of nickel, the gram capacity of the positive electrode active material is correspondingly high, which can effectively improve the energy density of the battery.

[0103] In some embodiments, the compositions of particles A and B independently satisfy Formula I, Li a1 Ni x1 Co y1 Mn z1 M1 b1 O2M1' c1 , Formula I

[0104] Among them, a1 is 0.8-1.2, x1 is 0.85-1, y1 is 0-0.15, z1 is 0-0.15, b1 is 0-0.02, c1=1-x1-y1-z1-b1, M1 includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Sb, Nb, Na, K, B, Mg, Zn, Ca or Ce, and M1' includes at least one of N, F, S or Cl.

[0105] In some embodiments, a1 can be selected as 0.8, 0.9, 1.0, 1.1, 1.2 or any value therein.

[0106] In some embodiments, b1 can be selected as 0, 0.01, 0.02, or any value therein.

[0107] In some embodiments, x1 can be selected as 0.85, 0.9, 0.95, 1, or any value therein. In some embodiments, y1 can be selected as 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, or any value therein.

[0108] In some embodiments, z1 can be selected as 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15 or any value therein.

[0109] In some embodiments, Particle A and Particle B have the same composition.

[0110] In some embodiments, Particle A and Particle B have different compositions.

[0111] The high nickel content in particles A and B can improve the battery's energy density. Furthermore, the inclusion of M1 in particles A and B can reduce lithium-nickel mixing in the active material during cycling, improving the material's structural stability. This ensures that even after lithium ions are deintercalated from the positive electrode during charging, the positive electrode active material maintains a relatively intact structure, thereby improving the battery's discharge performance.

[0112] In some embodiments, the positive electrode film layer contains a positive electrode active material, the positive electrode active material is a single crystal or quasi-single crystal particle, and the laser particle size distribution curve of the positive electrode active material is a single peak.

[0113] In some embodiments, the positive electrode film layer contains a positive electrode active material, the positive electrode active material is a single crystal or a quasi-single crystal particle, and the volume average particle size D of the single crystal or the quasi-single crystal particle is v 50 is 1 to 3.5 μm, optionally 1.2 to 3.0 μm.

[0114] In some embodiments, the positive electrode film layer contains a positive electrode active material, the positive electrode active material is a single crystal or a quasi-single crystal particle, and the volume average particle size D of the single crystal or the quasi-single crystal particle is v 50 is 1 μm, 1.2 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, or any value therein.

[0115] In some embodiments, the positive electrode film layer contains a positive electrode active material, the positive electrode active material is a single crystal or a quasi-single crystal particle, and the laser particle size distribution of the single crystal or the quasi-single crystal particle satisfies: 0.3≤(D v 99-D v 90) / (2×D v 50)≤0.55.

[0116] In some embodiments, the positive electrode film layer contains a positive electrode active material, the positive electrode active material is a single crystal or a quasi-single crystal particle, and the laser particle size distribution (D v 99-D v 90) / (2×D v 50) is 0.3, 0.35, 0.4, 0.45, 0.5, 0.55 or any value therein.

[0117] In some embodiments, the positive electrode film layer contains a positive electrode active material, and the positive electrode active material is a single crystal or a quasi-single crystal particle, and the composition of the single crystal or the quasi-single crystal particle is as shown in Formula II: Li a2 Ni x2 Co y2 Mn z2 M2 b2 O2M2' c2 , Formula II

[0118] Among them, a2 is 0.8~1.2, x2 is 0.85~1, y2 is 0~0.15, z2 is 0~0.15, b2 is 0~0.02, c2=1-x2-y2-z2-b2, M2 includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Sb, Nb, Na, K, B, Mg, Zn, Ca or Ce, and M2' includes at least one of N, F, S or Cl; optionally, x2 is 0.90~1.

[0119] In some embodiments, a2 can be selected as 0.8, 0.9, 1.0, 1.1, 1.2 or any value therein.

[0120] In some embodiments, b2 can be selected as 0, 0.01, 0.02, or any value therein.

[0121] In some embodiments, x2 can be selected as 0.85, 0.9, 0.95, 1 or any value therein. In some embodiments, y2 can be selected as 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15 or any value therein.

[0122] In some embodiments, z2 can be selected from 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, or any value thereof. In some embodiments, the positive electrode includes a positive electrode current collector, the positive electrode film layer includes a positive electrode active material, the positive electrode active material is a single crystal or quasi-single crystal particle, and the ratio of the thickness of the single-sided positive electrode film layer to the thickness of the positive electrode current collector is 4.5 to 9, optionally 4.5 to 8.5.

[0123] Cathode materials formed from single-crystal particles have a large surface area and a dense structure. This allows the positive electrode active material to maintain good structural stability while having a high compaction density. This reduces side reactions during charge and discharge, slows electrolyte consumption, and improves battery life. Cathode active materials that meet these conditions exhibit good structural stability, enabling batteries containing them to have high energy density, excellent rate capability, and long cycle life.

[0124] In some embodiments, the pore volume of the positive electrode film layer accounts for 18% to 35% of the total volume of the positive electrode film layer.

[0125] When the pore volume of the positive electrode film layer is within an appropriate range, the organic lithium salt in the electrolyte can easily enter the pores of the positive electrode film layer and fully contact the positive electrode active material, thereby increasing the migration rate of ions at the electrode / electrolyte interface, reducing the internal resistance of the battery, and improving the battery's rate performance.

[0126] In some embodiments, the secondary battery further includes a negative electrode, the negative electrode including a negative electrode membrane, the negative electrode membrane including a negative electrode active material, the negative electrode active material including a silicon-based material, and the silicon-based material is selected from one or more of elemental silicon, silicon-oxygen materials, and silicon-carbon materials. The negative electrode active material preferably includes at least a silicon-carbon material.

[0127] Silicon-based materials can significantly increase the energy density of batteries.

[0128] In some embodiments, the negative electrode active material further comprises a carbon-based material, and the mass ratio of the carbon-based material to the silicon-based material is no more than 4:6, and can optionally be no more than 2:8.

[0129] In some embodiments, the mass ratio of the carbon-based material to the silicon-based material is no more than 4:6, 4:7, 4:8, 4:9, 4:10, 4:11, 4:12, 4:13, 4:14, 4:15, 2:8, or any value therein. When the mass ratio of the carbon-based material to the silicon-based material is within the above range, the battery can have a high energy density while reducing the expansion of the negative electrode, thereby improving the cycle performance and rate performance.

[0130] In some embodiments, the surface density of the negative electrode film is 6 to 13 mg / cm 2 .

[0131] In some embodiments, the surface density of the negative electrode film is 6 mg / cm 2 , 7mg / cm 2 , 8mg / cm 2 , 9mg / cm 2 、10mg / cm 2 , 11mg / cm 2 , 12mg / cm 2 、13mg / cm 2 or any value therein.

[0132] When the surface density of the negative electrode membrane is within the above range, the negative electrode adopts a thick coating design, which helps to improve the energy density of the battery.

[0133] In some embodiments, the negative electrode sheet includes a negative electrode current collector, and the negative electrode film layer of any embodiment is disposed on at least one side of the negative electrode current collector.

[0134] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0135] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0136] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0137] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0138] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0139] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0140] In some embodiments, the positive electrode sheet includes a positive electrode current collector, and the positive electrode film layer of any embodiment is disposed on at least one side of the positive electrode current collector.

[0141] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0142] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0143] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0144] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0145] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0146] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0147] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0148] In one embodiment of the present application, an electric device is provided, comprising the secondary battery of any embodiment.

[0149] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG1 shows a secondary battery 5 with a square structure as an example.

[0150] In some embodiments, referring to Figure 2, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0151] An electrical device includes the secondary battery provided in this application. The secondary battery can be used as a power source for the electrical device or as an energy storage unit for the electrical device. Electrical devices may include, but are not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships, satellites, energy storage systems, etc.

[0152] Figure 3 shows an example of an electric device. This device can be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.

[0153] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.

[0154] Example

[0155] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0156] 1. Preparation method

[0157] 1. Preparation of positive electrode sheet

[0158] Preparation of positive electrode active material: Lithium hydroxide and dried high-nickel ternary precursor are weighed according to the stoichiometric ratio of the chemical formula, the mixture is mixed evenly in a high-speed mixer and then sintered in a kiln. The sintering temperature is S760℃, the sintering time is S20Sh, and the sintering atmosphere is oxygen. After cooling, the matrix material can be obtained. The material is washed with water at a mass ratio of S1:1S for 30 minutes, centrifuged, filtered, and then vibrated and dried at a vibration frequency of S30SHz and a drying time of S5Sh to obtain the positive electrode active material. During this sintering process, the primary particle size is adjusted by adjusting the sintering temperature, and the secondary particle size is adjusted by adjusting the precursor particle size.

[0159] The composition of the positive electrode active material is LiNi 0.93 Co 0.05 Mn 0.01 Al 0.005 N 0.005 O2, wherein the primary particle size of particle A is 200 nm and the volume average particle size is 10 μm; the primary particle size of particle B is 1 μm and the volume average particle size is 5 μm; the mass ratio of particle A to particle B is 4:1.

[0160] The positive electrode active material, conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) were mixed uniformly in N-methylpyrrolidone (NMP) solution at a mass ratio of 97%:1%:2% to prepare the positive electrode slurry. The slurry was then evenly coated on the positive electrode current collector. The slurry was then coated on the surface of aluminum foil using an extrusion coater and dried. The coated electrode was then cold-pressed using a cold press. The compacted density of the positive electrode film was 3.3 mg / cm 3 The final positive electrode sheet was prepared, wherein the thickness of the positive electrode current collector was 13 μm.

[0161] 2. Preparation of negative electrode sheet

[0162] The negative electrode active materials, artificial graphite and carbon silicon material, conductive agent carbon black, carbon nanotubes, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na), are mixed in an appropriate amount of deionized water at a weight ratio of 60.48%: 34.02%: 1%: 0.375%: 2.8%: 1.325% to form a uniform negative electrode slurry. The negative electrode slurry is then coated on the negative electrode current collector and dried to obtain a negative electrode film. The surface density of the negative electrode film is 9.4Smg / cm 2 .

[0163] 3. Isolation film

[0164] Polyethylene film (PE film) is used as the separator.

[0165] 4. Electrolyte

[0166] Ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and fully dried lithium salt LiPF6 is dissolved in the mixed organic solvent to prepare an electrolyte with a LiPF6 concentration of 1 mol / L; then 10 wt% of LiFSI is added and mixed evenly.

[0167] 5. Preparation of batteries

[0168] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets to play an isolating role, and the electrolyte is injected to assemble a secondary battery.

[0169] Specific parameters are shown in Table 1

[0170] Example 2

[0171] The preparation method of Example 2 is basically the same as that of Example 1, except that the type of organic lithium salt is adjusted. Specific parameters are shown in Table 1.

[0172] Examples 3 to 6

[0173] The preparation methods of Examples 3 to 6 are basically the same as those of Example 1, except that the mass content of the organic lithium salt is adjusted. Specific parameters are shown in Table 1.

[0174] Example 7

[0175] The preparation method of Example 7 is basically the same as that of Example 1, except that the B particles of the positive electrode active material are single crystals. Specific parameters are shown in Table 1.

[0176] Examples 8 to 12

[0177] The preparation methods of Examples 8 to 12 are basically the same as those of Example 1, except that the mass content of the organic lithium salt and the surface density of the positive electrode film layer are adjusted. The specific parameters are shown in Table 1. Among them, the compacted density of the positive electrode film layer of Example 8 is 3.3 mg / cm 3 The compacted density of the positive electrode film of Example 12 is 3.2 mg / cm 3 , and the rest are the same as the compaction density of the positive electrode film layer in Example 1.

[0178] Examples 13 to 16

[0179] The preparation methods of Examples 13 to 16 are essentially the same as those of Example 1, except that the composition of the positive electrode active material particles was adjusted. Specific parameters are shown in Table 1. In Examples 13 to 15, the primary and secondary particle sizes of Particles A and B were adjusted by adjusting the sintering temperature. These Particles A and B were obtained by preparing precursors of varying particle sizes. In Example 16, the positive electrode active material comprised only a single crystal particle.

[0180] Comparative Example 1

[0181] The preparation methods of Comparative Example 1 are basically the same as those of Example 1, except that the electrolyte in Comparative Example 1 only includes inorganic lithium salt but not organic lithium salt. Specific parameters are shown in Table 1.

[0182] Comparative Example 2

[0183] The preparation method of Comparative Example 2 is basically the same as that of Example 1, except that the surface density of the positive electrode film layer is adjusted. The specific parameters are shown in Table 1. Among them, the compacted density of the positive electrode film layer is 3.6 mg / cm 3 .

[0184] 2. Performance Testing

[0185] 1. Mass energy density and unit area energy density test

[0186] 1) The discharge energy measurement method of a battery cell is as follows:

[0187] Let the battery cell stand at 25℃ for 2 hours to ensure the temperature of the battery cell is 25℃;

[0188] After charging the battery cell to the charge cut-off voltage at 0.1C at 25°C, continue constant voltage charging at the charge cut-off voltage until the current reaches 0.05C, and then charge is cut off (where C represents the rated capacity of the battery cell);

[0189] Let the battery cells stand at 25°C for 1 hour;

[0190] At 25°C, discharge the battery cells at 0.1C to the discharge cutoff voltage, and record the total discharge capacity (C0) and total discharge energy (E0) of the battery cells. The charge cutoff voltage is 4.25V, and the discharge cutoff voltage is 2.0V.

[0191] 2) The formula for calculating the energy density per unit area of ​​the positive electrode film is as follows:

[0192] If the battery is coated on both sides with positive electrode active material, the energy density per unit area of ​​the positive electrode film layer = battery cell discharge energy E0 / (2×area of ​​the positive electrode film layer);

[0193] If the battery is coated with positive electrode active material on one side, the energy density per unit area of ​​the positive electrode film layer = battery cell discharge energy E0 / area of ​​the positive electrode film layer.

[0194] 2. Dynamic performance

[0195] Charging rate test

[0196] At 25°C, fully charge the battery at xSC and fully discharge it at 1C 10 times. Then, fully charge the battery at xSC. Remove the negative electrode and observe lithium deposition on the surface. If no lithium deposition occurs, increase the charge rate xSC by 0.1C until lithium deposition occurs. Stop testing. Subtract 0.1C from the charge rate at this point to obtain the maximum charge rate. The charge cutoff voltage is 4.25V, and the discharge cutoff voltage is 2.0V.

[0197] Discharge rate performance

[0198] At 25°C, the battery was fully charged at 0.33C and constant-voltage charging with a cutoff current of 0.05C, then fully discharged at 0.33C. The initial capacity (C0) was recorded. The battery was then fully charged at 0.33SC and constant-voltage charging with a cutoff current of 0.05C, then fully discharged at 2C. The capacity (C1S) was recorded. The 2C discharge retention ratio was C1 / C0. The charge cutoff voltage was 4.25V, and the discharge cutoff voltage was 2.0V.

[0199] 3. Measurement method of unit area density of positive electrode film layer and negative electrode film layer

[0200] The unit area density of the positive and negative electrode films is m / S, where m represents the weight of the film and S represents the area of ​​the film. m is calculated by subtracting the weight of the current collector from the weight of the electrode. The length and width of the film can be measured using a ruler. If the electrode is coated on both sides, the area density of the film is calculated as (electrode weight - current collector weight) / (2 × film area).

[0201] 4. Particle size test

[0202] Particle size distribution was measured using a Microtrac MRB S3500 series laser particle size analyzer. The specific testing process was as follows: 0.05-2g of the positive electrode active material was added to 10-20ml of deionized water. Ultrasonication was performed at 53kHz and 120W for 5 minutes to ensure complete dispersion. The sample was then measured according to GB / T19077-2016 or ISO 13320:2009 standards. The volume average particle size and peak position difference were measured using a particle size-volume distribution curve. A scanning electron microscope was used to observe the cross-section of the particles and determine the primary particle size.

[0203] The test results of the embodiments and comparative examples are shown in Table 1.

[0204] According to the above results, the secondary batteries of Examples 1-16 include an electrolyte and a positive electrode, the positive electrode includes a positive electrode film layer, and the energy density per unit area of ​​the single-side positive electrode film layer meets 18-37 mWh / cm 2 .

[0205] Compared to Comparative Example 1, in which the electrolyte of the secondary battery includes only an inorganic lithium salt and no organic lithium salt, the batteries of Examples 1-16 exhibit excellent kinetic performance while maintaining high energy density, with improved maximum charge rate and discharge capacity retention at high rates.

[0206] It can be seen from Examples 1-12 that when the relationship between the positive electrode film layer and the organic lithium salt satisfies 0.005≤M-0.0005×w≤0.2, the organic lithium salt can form an effective combination with the positive electrode film layer, so that the battery has a high charge rate or a capacity retention rate at a high charge rate, that is, the battery's kinetic performance is improved.

[0207] From the comparison between Examples 1-16 and Comparative Example 2, it can be seen that the surface density w of the single-sided positive electrode film layer is not less than 20 mg / cm 2 , can be selected from 25 to 45 mg / cm 2 When the battery has a high energy density.

[0208] It can be seen from Examples 1 and 13-15 that the battery kinetic performance can be improved by grading the two sizes of particles, AB.

[0209] From the comparison among Example 1, Example 7 and Example 16, it can be seen that compared with the positive electrode active material including single crystal, the small particles of the positive electrode active material are all polycrystalline, which is beneficial to improving the dynamic performance of the battery.

[0210] From the comparison between Example 1 and Examples 13-16, it can be seen that when the positive electrode active material includes particles A and particles B, and particles A and particles B have two different particle sizes, it is beneficial to further improve the energy density and kinetic performance of the battery.

[0211] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A secondary battery, wherein: The secondary battery comprises: an electrolyte, wherein the electrolyte comprises an organic lithium salt; and The positive electrode comprises a positive electrode film layer, and the energy density per unit area of ​​the positive electrode film layer on one side is 18 to 37 mWh / cm 2 , can be selected as 18~35.7mWh / cm 2 .

2. The secondary battery according to claim 1, wherein the positive electrode film layer and the organic lithium salt satisfy the following relationship: 0.005≤M-0.0005×w≤0.2 in, M is the mass content of the organic lithium salt based on the total mass of the electrolyte; w is the surface density of the positive electrode film layer on one side, in mg / cm 2 .

3. The secondary battery according to claim 1 or 2, wherein: The surface density w of the positive electrode film layer on one side is not less than 20 mg / cm 2 , optionally 25 to 45 mg / cm 2 .

4. The secondary battery according to any one of claims 1 to 3, wherein The organic lithium salt includes at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide.

5. The secondary battery according to any one of claims 1 to 4, wherein The electrolyte also includes an inorganic lithium salt, and the molar ratio of the organic lithium salt to the inorganic lithium salt is 1:5 to 5:

1.

6. The secondary battery according to any one of claims 1 to 5, wherein The positive electrode film layer contains positive electrode active materials, and the positive electrode active materials include particles A and particles B. The particles A are polycrystalline particles, and the volume average particle size of the particles A is larger than the volume average particle size of the particles B.

7. The secondary battery according to claim 6, wherein The positive electrode film layer also satisfies at least one of the following characteristics: (1) The particle B is a polycrystalline, single crystal or quasi-single crystal particle; (2) The primary particle size of the particle A is 50 nm to 400 nm, and may be 80 to 200 nm; the primary particle size of the particle B is 150 nm to 2 μm, and may be 200 nm to 1.2 μm; (3) The volume average particle size of the particles A is 2 to 25 μm, and may be 2.5 to 23 μm; the volume average particle size of the particles B is 0.65 to 10 μm, and may be 1.2 to 8.5 μm; (4) The mass ratio of the particles A to the particles B is 5:5 to 9:1; (5) The laser particle size distribution curve of the positive electrode active material is bimodal, and the peak position difference between the two peaks is 3 to 7 μm; (6) The positive electrode includes a positive electrode current collector, and the ratio of the thickness of the positive electrode film layer on one side to the thickness of the positive electrode current collector is 5.5 to 15, and optionally 5.6 to 8.

8.

8. The secondary battery according to claim 6 or 7, wherein: Based on the total molar number of transition metal elements in the positive electrode active material, the molar content of nickel element is not less than 80%; optionally, not less than 85%; further optionally, not less than 90%.

9. The secondary battery according to any one of claims 6 to 8, wherein The compositions of the particles A and B independently satisfy Formula I, Li a1 Ni x1 Co y1 Mn z1 M1 b1 O2M1' c1 , Formula I Among them, a1 is 0.8-1.2, x1 is 0.85-1, y1 is 0-0.15, z1 is 0-0.15, b1 is 0-0.02, c1=1-x1-y1-z1-b1, M1 includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Sb, Nb, Na, K, B, Mg, Zn, Ca or Ce, and M1' includes at least one of N, F, S or Cl.

10. The secondary battery according to any one of claims 1 to 5, wherein The positive electrode film layer contains a positive electrode active material, and the positive electrode active material is a single crystal or a quasi-single crystal particle, and meets at least one of the following characteristics: (1) The laser particle size distribution curve of the positive electrode active material is single-peaked; (2) The volume average particle size D of the single crystal or quasi-single crystal particles v 50 is 1~3.5μm, Optionally 1.2 to 3.0 μm; (3) The laser particle size distribution of the single crystal or quasi-single crystal particles satisfies: 0.3≤(D v 99-D v 90) / (2×D v 50)≤0.55; (4) The composition of the single crystal or quasi-single crystal particles is as shown in Formula II: Li a2 Ni x2 Co y2 Mn z2 M2 b2 O2M2' c2 , formula II Wherein, a2 is 0.8-1.2, x2 is 0.85-1, y2 is 0-0.15, z2 is 0-0.15, b2 is 0-0.02, c2=1-x2-y2-z2-b2, M2 includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Sb, Nb, Na, K, B, Mg, Zn, Ca or Ce, and M2' includes at least one of N, F, S or Cl; optionally, x2 is 0.90-1; (5) The positive electrode includes a positive electrode current collector, and the ratio of the thickness of the positive electrode film layer on one side to the thickness of the positive electrode current collector is 4.5 to 9, and optionally 4.5 to 8.

5.

11. The secondary battery according to any one of claims 1 to 10, wherein The secondary battery further comprises a negative electrode, which comprises a negative electrode membrane, which comprises a negative electrode active material, which comprises a silicon-based material, and which comprises one or more of elemental silicon, silicon-oxygen material, and silicon-carbon material.

12. The secondary battery according to claim 11, wherein The negative electrode active material further comprises a carbon-based material, and a mass ratio of the carbon-based material to the silicon-based material is no more than 4:6, and can be optionally no more than 2:

8.

13. The secondary battery according to claim 11 or 12, wherein: The surface density of the negative electrode membrane is 6 to 13 mg / cm 2 .

14. An electrical device comprising the secondary battery according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • Non-aqueous secondary battery

    CN103891028A

  • High energy density, high power density, high capacity, and room temperature capable "anode-free" rechargeable batteries

    CN109526240A

  • High-compaction-density positive electrode material and electrochemical energy storage device

    CN111384372A

  • Electrolyte suitable for lithium metal negative electrode secondary battery

    CN115117443A

  • Non-aqueous electrolyte secondary battery

    JP2019207757A

Cited By

  • Battery monomer, battery device and electric device

    CN119993980A

  • Battery cell, battery device and electric device

    CN120109157A

  • Battery cell, battery device, and electric device

    CN120127103A

  • Battery cell, battery apparatus and electric device

    WO2026174446A1