Thermogel drug delivery system
The thermogel drug delivery system, using glycol chitosan derivatives and bioreactive linkers, addresses biodegradability and biocompatibility issues, enabling controlled and sustained drug release and targeted delivery, overcoming limitations of existing systems.
Patent Information
- Application Number
- PCT/KR2024/095243
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-02-15
- Publication Date
- 2024-10-24
AI Technical Summary
Current thermogel drug delivery systems face challenges with biodegradability, biocompatibility, and controlled drug release, particularly requiring high concentrations of poloxamers that are not fully biodegradable and can cause side effects, while also lacking effective targeting and sustained release capabilities.
A thermogel drug delivery system utilizing a polymer such as glycol chitosan derivative, combined with a bioreactive linker, which undergoes sol-gel transition at body temperature, allowing for controlled drug release and improved biocompatibility, using a reaction product of a drug active substance and a bioreactive linker to enhance drug delivery and stability.
The system achieves controlled and sustained drug release over a period of 1 day to 45 days, exhibits excellent physical stability and elastic recovery, and ensures effective delivery of anti-inflammatory and anti-cancer drugs to target locations with improved biocompatibility and reduced side effects.
Smart Images

Figure KR2024095243_24102024_PF_FP_ABST
Abstract
Description
Thermogel drug delivery system
[0001] This invention claims the benefit of Korean Patent Application No. 10-2023-0052739, filed with the Korean Intellectual Property Office on April 21, 2023, the entire contents of which are incorporated herein by reference. The present invention relates to a thermogel drug delivery system, and more particularly, to a thermogel drug delivery system comprising a polymer for preparing a thermogel; and a precursor containing a reaction product of a drug-active substance and a bioreactive linker.
[0002] Thermogel, also known as temperature-sensitive hydrogel, is an important biomaterial widely used in the field of drug delivery. It is a polymer that maintains a solution state at room temperature and exhibits a reversible sol-gel phase transition as the temperature increases.
[0003] As described above, thermogels exhibiting thermo-reversible sol-gel transition properties are suitable for in vivo drug delivery because they can be injected in a sol state and gel in the body. Thermogels can be mixed with drugs in a sol state to encapsulate the drugs. When injected, the drug-mixed thermogel solidifies into a gel at body temperature. Poloxamer, a representative thermogel, has been used for drug delivery to the inner ear. However, poloxamer requires high concentrations (greater than 20 wt%) for effective thermogelation, has insufficient biodegradability and physical stability, and has been reported to have side effects.
[0004] Meanwhile, a prodrug is a drug that has no medicinal effect on its own, but whose structure changes through metabolic processes in the body and produces an effect. Thermo-sensitive hydrogels conventionally used as prodrugs include, for example, poly(N-isopropylacrylamide), polyethylene oxide-polypropylene oxide-polyethylene oxide copolymer (PEO-PPO-PEO), cellulose derivatives, and chitosan-glycerophosphate.
[0005] There is a need to develop a drug delivery system that includes the properties of the thermogel and the properties of the prodrug as described above, but has sufficient biodegradability, biocompatibility, and physical safety when administered into the body, and can effectively control the initial drug release amount.
[0006] The technical problem to be achieved by the present invention is to provide a thermogel drug delivery system that exhibits sol-gel transition characteristics, has improved drug loading capacity, and allows controlled drug release.
[0007] The technical problem to be achieved by the present invention is to provide a thermogel drug delivery system exhibiting excellent physical stability and elastic recovery properties.
[0008] The technical problem to be achieved by the present invention is to provide a thermogel drug delivery system with excellent biocompatibility.
[0009] The technical task to be achieved by the present invention is to provide a thermogel drug delivery system capable of effectively delivering various drug substances to a target location in the body.
[0010] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be clearly understood by those skilled in the art from the description below.
[0011] One embodiment of the present invention provides a thermogel drug delivery system comprising a polymer for producing a thermogel; and a precursor containing a reaction product of a drug-active substance and a bioreactive linker.
[0012] According to one embodiment of the present invention, the polymer for producing the thermogel may be any one selected from the group consisting of glycol chitosan derivatives, cellulose, carboxymethyl cellulose, hydroxypropyl methylcellulose, chitin, dextran, dextrin, gelatin, hyaluronic acid, pectin, rhamnogalacturonan, xylan, and copolymers thereof.
[0013] According to one embodiment of the present invention, the glycol chitosan derivative may include a straight-chain or branched acyl group having 2 to 20 carbon atoms.
[0014] According to one embodiment of the present invention, the drug-active substance may be one selected from the group consisting of anti-inflammatory substances, anticancer substances, and combinations thereof.
[0015] According to one embodiment of the present invention, the bioreactive linker may include an acid anhydride.
[0016] According to one embodiment of the present invention, the degree of substitution (DS) of the reaction product in the precursor may be 1% or more and 30% or less.
[0017] According to one embodiment of the present invention, the precursor may be in powder form.
[0018] According to one embodiment of the present invention, the content of the precursor may be 1 wt% or more and 10 wt% or less.
[0019] According to one embodiment of the present invention, a solvent may be further included.
[0020] According to one embodiment of the present invention, the thermogel drug delivery system may be in a sol phase at room temperature and in a gel phase at a temperature of 30°C or higher and 40°C or lower.
[0021] According to one embodiment of the present invention, the thermogel drug delivery system may release a drug over a period of 1 day or more and 45 days or less in phosphate buffered saline (PBS) at 37°C and pH 7.4.
[0022] A thermogel drug delivery system according to one embodiment of the present invention not only has sol-gel transition characteristics according to temperature changes, but also can increase drug loading amount and effectively control initial drug release amount.
[0023] A thermogel drug delivery system according to one embodiment of the present invention exhibits excellent physical stability and elastic recovery properties and has excellent biocompatibility.
[0024] By widely using the thermogel drug delivery system according to one embodiment of the present invention for various inflammatory and anticancer treatments, various injectable controlled-release drug preparations can be provided.
[0025] FIG. 1 is a schematic diagram of a method for manufacturing a precursor of a thermogel drug delivery system (HGC-AA-DEX) according to one embodiment of the present invention.
[0026] Figure 2A shows the 1H-NMR spectra of DEX and DEX-SA according to one embodiment of the present invention.
[0027] Figure 2B shows the 1H-NMR spectra of DEX and DEX-AA according to one embodiment of the present invention.
[0028] Figure 3A shows the 1H-NMR spectrum of HGC, a polymer synthesized with GC, and a thermogel drug delivery system (HGC-SA-DEX) according to one embodiment of the present invention.
[0029] Figure 3B shows the 1H-NMR spectrum of HGC, a polymer synthesized with GC according to one embodiment of the present invention, and a thermogel drug delivery system (HGC-AA-DEX).
[0030] FIG. 4 shows the ATR-FTIR spectrum of HGC, a polymer synthesized with DEX-SA and GC, and a thermogel drug delivery system (HGC-SA-DEX) according to one embodiment of the present invention.
[0031] Figure 5A shows the ATR-FTIR spectra of DEX and DEX-AA according to one embodiment of the present invention.
[0032] FIG. 5B shows the ATR-FTIR spectrum of HGC, a polymer synthesized with GC according to one embodiment of the present invention, and a thermogel drug delivery system (HGC-AA-DEX).
[0033] Figure 6A shows a sol-gel transition diagram of a thermogel drug delivery system (HGC-SA-DEX) according to one embodiment of the present invention, as analyzed by a tube tilting method.
[0034] Figure 6B shows a sol-gel transition diagram of a thermogel drug delivery system (HGC-AA-DEX) according to one embodiment of the present invention, as analyzed by a tube tilting method.
[0035] FIG. 7A is an image showing the sol-gel transition at 20°C and 37°C of HGC and a 4 wt% thermogel drug delivery system (HGC-SA-DEX) according to one embodiment of the present invention.
[0036] FIG. 7B is an image showing the sol-gel transition at 20°C and 37°C of a 3 wt% to 5 wt% thermogel drug delivery system (HGC-AA-DEX) according to one embodiment of the present invention.
[0037] Figure 8 shows the rheological behavior of HGC and 4 wt% thermogel drug delivery system (HGC-SA-DEX) samples according to one embodiment of the present invention according to temperature change.
[0038] Figure 9 shows the rheological behavior of HGC and thermogel drug delivery system (HGC-AA-DEX) samples according to temperature change at various concentrations of 2, 3, 4, and 5 wt% according to one embodiment of the present invention.
[0039] Figure 10 shows the shear thinning characteristics and thixotropic recovery characteristics of thermogel drug delivery system (HGC-SA-DEX) samples according to one embodiment of the present invention.
[0040] Figure 11 shows the behavior of the complex viscosity according to the temperature change of HGC and thermogel drug delivery system (HGC-AA-DEX) samples at various concentrations of 2, 3, 4, and 5 wt% according to one embodiment of the present invention.
[0041] Figure 12A is an FE-SEM image of the surface and cross-section of thermogel drug delivery system (HGC-SA-DEX) samples according to one embodiment of the present invention.
[0042] Figure 12B is an FE-SEM image of the surface and cross-section of thermogel drug delivery system (HGC-AA-DEX) samples according to one embodiment of the present invention.
[0043] Figure 13A shows the hydrolysis ability of a thermogel drug delivery system (HGC-SA-DEX) in PBS (pH 7.4, 37°C) according to one embodiment of the present invention as a 1H-NMR spectrum over time.
[0044] Figure 13B shows the hydrolysis ability of a thermogel drug delivery system (HGC-AA-DEX) in PBS (pH 7.4, 37°C) according to one embodiment of the present invention as a 1H-NMR spectrum over time.
[0045] Figure 14A shows the residual amount of a thermogel drug delivery system (HGC-SA-DEX) over time in PBS (pH 7.4, 37°C) according to one embodiment of the present invention.
[0046] Figure 14B shows the residual amount of a thermogel drug delivery system (HGC-AA-DEX) over time in PBS (pH 7.4, 37°C) according to one embodiment of the present invention.
[0047] Figure 15A shows the residual amount of a thermogel drug delivery system (HGC-SA-DEX) over time in PBS (pH 7.4, 37°C) containing lysozyme according to one embodiment of the present invention.
[0048] Figure 15B shows the residual amount of a thermogel drug delivery system (HGC-AA-DEX) over time in PBS (pH 7.4, 37°C) containing lysozyme according to one embodiment of the present invention.
[0049] Figure 16A shows an in vitro initial drug release evaluation of DSP and thermogel drug delivery system (HGC-SA-DEX) in PBS (pH 7.4, 37°C) according to one embodiment of the present invention.
[0050] Figure 16B shows an in vitro initial drug release evaluation of DSP and thermogel drug delivery system (HGC-AA-DEX) in PBS (pH 7.4, 37°C) according to one embodiment of the present invention.
[0051] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0052] In this specification, “A and / or B” means “A and B, or A or B.”
[0053] In this specification, MWCO (Molecular Weight of Cut-off) means that substances with a molecular weight lower than that are permeated and substances with a molecular weight higher than that are excluded.
[0054] In this specification, GC means glycol chitosan and HGC means hexanoyl glycol chitosan.
[0055] In this specification, DEX means dexamethasone, DEX-SA means dexamethasone succinate, and DEX-AA means dexamethasone adipate.
[0056] In this specification, HGC-DEX5 means that 5.3% of DEX-SA is combined with HGC, and the supply molar ratio of DEX-SA is 0.11.
[0057] In this specification, HGC-DEX7 means that 7.0% of DEX-SA is combined with HGC, and the supply molar ratio of DEX-SA is 0.14.
[0058] In this specification, HGC-DEX10 means that 9.5% of DEX-SA is combined with HGC, and the supply molar ratio of DEX-SA is 0.18.
[0059] In this specification, HGC-DEX15 means that 2.3% of DEX-AA is combined with HGC, and the supply molar ratio of DEX-AA is 0.15.
[0060] In this specification, HGC-DEX20 means that 2.95% of DEX-AA is combined with HGC, and the supply molar ratio of DEX-AA is 0.20.
[0061] In this specification, room temperature means 20±5℃.
[0062]
[0063] Hereinafter, the present invention will be described in more detail.
[0064]
[0065] One embodiment of the present invention is a thermogel drug delivery system, comprising a polymer for producing a thermogel; and a precursor containing a reaction product of a drug-active substance and a bioreactive linker.
[0066] According to one embodiment of the present invention, a thermogel drug delivery system comprises a polymer for thermogel production, thereby exhibiting sol-gel transition properties at a specific temperature and imparting gelation properties within the body to the drug delivery system. Furthermore, according to one embodiment of the present invention, a thermogel drug delivery system comprises a reaction product of a drug-active substance and a bioreactive linker, thereby effectively delivering a drug to a target location within the body under bioreactive conditions.
[0067] According to one embodiment of the present invention, the thermogel drug delivery system comprises a polymer for thermogel production. Specifically, the polymer for thermogel production can impart sol-gel transition characteristics at a specific temperature and gelation characteristics in the body to the drug delivery system by chemically bonding with a reaction product of a drug-active substance and a bioreactive linker, which will be described later, and can effectively deliver the drug to a target location in the body under bioreactive conditions.
[0068] According to one embodiment of the present invention, the thermogel drug delivery system comprises a drug-active substance and a reaction product of a bioreactive linker. As described above, by including the reaction product of the drug-active substance and the bioreactive linker, the drug can be effectively delivered to a target location in the body under bioreactive conditions, thereby enhancing therapeutic efficacy.
[0069] According to one embodiment of the present invention, the polymer for producing a thermogel may be any one selected from the group consisting of a glycol chitosan derivative, cellulose, carboxymethyl cellulose, hydroxypropyl methylcellulose, chitin, dextran, dextrin, gelatin, hyaluronic acid, pectin, rhamnogalacturonan, xylan, and copolymers thereof. Preferably, the polymer for producing a thermogel may be a glycol chitosan derivative. The glycol chitosan derivative may be soluble even at neutral pH, and may have low toxicity, biocompatibility, and biodegradability.
[0070] According to one embodiment of the present invention, the glycol chitosan derivative may include a straight or branched acyl group having 2 to 20 carbon atoms. Preferably, the acyl group may be at least one selected from the group consisting of an acetyl group, a propionyl group, a butyryl group, a valeryl group, a hexanoyl group, a heptanoyl group, and an octanoyl group. Since the sol-gel transition temperature of the drug delivery system tends to decrease as the hydrophobic portion of the acyl group becomes longer, the drug delivery system can be synthesized by appropriately selecting the acyl group.
[0071] According to one embodiment of the present invention, the glycol chitosan derivative may be hexanoyl glycol chitosan (HGC). As described above, as the hydrophobic portion of the acyl group becomes longer, the sol-gel transition temperature of the drug delivery system tends to decrease, and N-hexanoyl glycol chitosan, which has been shown experimentally to undergo a sol-gel transition within the biological temperature range, may be included as a polymer for producing a thermogel.
[0072] Figure 1 is a schematic diagram of a method for preparing a precursor of a thermogel drug delivery system (HGC-DEX) according to an embodiment of the present invention. As shown in Figure 1A, the synthesis of hexanoyl glycol chitosan (HGC) can be performed through the modification of glycol chitosan (GC). Specifically, GC was dissolved in distilled water to prepare a homogeneous solution, and then methanol was added. For N-hexanoylation, hexanoic anhydride was added and the mixture was reacted at room temperature for 12 to 36 hours. Thereafter, the reacted solution was precipitated in acetone, and the precipitated material was obtained through gravity filtration. The precipitate was dissolved in distilled water and dialyzed against distilled water using a dialysis membrane (MWCO: 12-14 kDa). After removing impurities through a syringe filter, the final dried powder form of hexanoyl glycol chitosan (HGC) product was obtained through freeze-drying.
[0073] According to one embodiment of the present invention, the pharmaceutically effective substance may be one selected from the group consisting of anti-inflammatory substances, anticancer substances, and combinations thereof. The pharmaceutically effective substance may be derived from a hydrophilic drug or a hydrophobic drug. Specifically, the above-mentioned drug active substance may be a steroid compound, and more specifically, may be clobetasol, halometasone, dexamethasone, diflorasone, fluocinonide, halobetasol, amcinonide, halcinonide, hydrocortisone, fluticasone, mometasone, fluocinolone, desonide, prednisone, methylprednisolone, prednisolone, a hydrate or solvate thereof, or a combination thereof.
[0074] The above drugs are not specifically limited to anti-inflammatory substances and anticancer substances, but specific examples include paclitaxel, doxorubicin, docetaxel, gemcitabine, cilolimus, etoposide, vinblastine, vinca alkaloids, cisplatin, Gleevec, adriamycin, cyclophosphamide, teniposide, 5-fluorouracil, camptocecin, tamoxifen, anasterozole, floxuridine, leuprolide, flotamide, zoledronate, vincristine, streptozotocin, carboplatin, topotecan, belotecan, irinotecan, vinorelbine, hydroxyurea, valrubicin, retinoic acid series, methotrexate, mechlorethamine, chlorambucil, busulfan, It may include one or more selected from the group consisting of doxifluridine, prednisone, testosterone, mitoxantrone, aspirin, salicylate, ibuprofen, naproxen, fenoprofen, indomethacin, phenylbutazone, cyclophosphamide, mechlorethamine, dexamethasone, celecoxib, valdecoxib, nimesulide, cortisone, corticosteroids, and mitomycin C. The drug may be chemically bonded to a polymer for producing a thermogel, which is a hydrophilic polymer.
[0075] According to one embodiment of the present invention, the bioreactive linker may include an acid anhydride. According to one embodiment of the present invention, the bioreactive linker may include a cyclic acid anhydride. Specifically, the bioreactive linker may include a cyclic acid anhydride having 4 to 6 carbon atoms. The cyclic acid anhydride may be at least one selected from the group consisting of succinic anhydride, glutaric anhydride, and adipic anhydride.
[0076] According to one embodiment of the present invention, the molar ratio of the drug substance and the bioreactive linker may be 1:1 to 1:5. By controlling the molar ratio of the drug substance and the bioreactive linker within the above-described range, the yield of the reaction product of the drug substance and the bioreactive linker may be improved. Preferably, the molar ratio of the drug substance and the bioreactive linker may be 1:3 to 1:5.
[0077] According to one embodiment of the present invention, the reaction product of the drug substance and the bioreactive linker may be a dexamethasone derivative. Specifically, the dexamethasone derivative may be synthesized by reacting dexamethasone among the drug substances with succinic anhydride or adipic anhydride among the bioreactive linkers.
[0078] FIG. 1 is a schematic diagram of a method for preparing a precursor of a thermogel drug delivery system (HGC-DEX) according to an embodiment of the present invention. As shown in FIG. 1B, the dexamethasone derivative (DEX-AA) was synthesized by introducing adipic anhydride (AA), which is an ester bond-based bioreactive linker, into dexamethasone (DEX), a hydrophobic drug, at a molar ratio of 1:1 to 1:5. Specifically, dexamethasone (DEX) and adipic anhydride (AA) were dissolved in pyridine at a molar ratio of 1:3 and then reacted at room temperature for 12 to 36 hours. The solution after the reaction was distilled under reduced pressure to evaporate the pyridine. The concentrate obtained through this was dissolved in ethanol, and then triple-distilled water was added dropwise and stored at 4℃ to precipitate a dexamethasone derivative (DEX-AA). The precipitated dexamethasone derivative (DEX-AA) was selectively separated through reduced pressure filtration and dried in a vacuum oven at room temperature to obtain a dexamethasone derivative (DEX-AA) product in the form of white needle-like crystals. In addition, a dexamethasone derivative (DEX-SA) product can be obtained by performing the same process as described above, except that dexamethasone (DEX) and succinic anhydride (SA) are added in a molar ratio of 1:4.3.
[0079] FIG. 1 is a schematic diagram of a method for preparing a precursor of a thermogel drug delivery system (HGC-DEX) according to an embodiment of the present invention. As shown in FIG. 1C, the precursor of the thermogel drug delivery system (HGC-DEX) was synthesized through the chemical bonding of hexanoyl glycol chitosan (HGC) and a dexamethasone derivative (DEX-AA). In a round flask, hexanoyl glycol chitosan (HGC) was dissolved in triple-distilled water. In another round flask, dexamethasone derivative (DEX-AA) was dissolved in absolute ethanol at a predetermined molar ratio (HGC: DEX-AA = 1: 0.1 to 0.3), and then catalysts such as EDC and NHS were added and stirred for 30 minutes at room temperature under a nitrogen atmosphere. Thereafter, the two solutions were combined and reacted at room temperature for 36 to 60 hours under nitrogen gas. After the reaction solution was precipitated in acetone, the precipitate was collected, dissolved in triple-distilled water, and dialyzed against distilled water using a dialysis membrane (MWCO: 12-14 kDa). After removing impurities through a syringe filter, the product was finally obtained in the form of a dried powder through lyophilization. In addition, the precursor of the thermogel drug delivery system (HGC-DEX) can be obtained by performing the same process as described above, except that the dexamethasone derivative (DEX-SA) is added instead of the dexamethasone derivative (DEX-AA) at a specified molar ratio (HGC: DEX-SA = 1: 0.05 to 0.25).
[0080] According to one embodiment of the present invention, the degree of substitution of the reaction product in the precursor may be 1% or more and 30% or less. Specifically, the degree of substitution of the reaction product of the drug-active substance and the bioreactive linker in the precursor may be 2% or more and 28% or less, 4% or more and 26% or less, 4% or more and 26% or less, 4% or more and 26% or less, 4% or more and 26% or less, 4% or more and 26% or less, 4% or more and 26% or less, 4% or more and 26% or less, 4% or more and 26% or less, 4% or more and 26% or less, 4% or more and 26% or less, 4% or more and 26% or less, 4% or more and 26% or less, 4% or more and 26% or less, 4% or more and 7% or less, or 5% or more and 6% or less. By controlling the degree of substitution of the reaction product within the above-described range, the temperature-sensitive characteristics and physical properties of the drug delivery system can be controlled. Specifically, as the degree of substitution of the reaction product increases, the critical gelation concentration decreases, and the sol-gel transition temperature may also decrease. Furthermore, as the degree of substitution of the reaction product increases, it is cross-linked at a higher density, requiring a longer time for decomposition, and thus may be stable as a biomaterial.
[0081] According to one embodiment of the present invention, the precursor may be in powder form. A thermogel drug delivery system may be prepared by dissolving the powdered precursor in a solvent. The solvent may be at least one selected from water, methanol, ethanol, propanol, ethylene glycol, acetone, and butanone. Preferably, the solvent may be water. A thermogel drug delivery system further comprising water may exist in a sol form at room temperature.
[0082] According to one embodiment of the present invention, in the thermogel drug delivery system further comprising the solvent, the content of the precursor may be 1 wt% or more and 10 wt% or less. Specifically, the content of the precursor may be 2 wt% or more and 9 wt% or less, 3 wt% or more and 8 wt% or less, 4 wt% or more and 7 wt% or less, or 5 wt% or more and 6 wt% or less. By controlling the content of the precursor within the above-described range, the thermosensitive characteristics and physical properties of the drug delivery system in the sol formulation can be controlled. As the content of the precursor in the powder formulation increases, the hydrophobic interaction becomes stronger, thereby lowering the sol-gel phase transition temperature. In addition, since it is crosslinked at a high density, it takes a longer time for decomposition, so it can have stability as a biomaterial.
[0083] According to one embodiment of the present invention, the drug delivery system may be in a sol phase at room temperature and in a gel phase at a temperature of 30°C or higher and 40°C or lower. Specifically, it may be used as an injectable formulation in a sol phase at room temperature without surgical intervention, and may be transformed into a gel phase within the biological temperature range, whereby the bioreactive linker is hydrolyzed, thereby delivering the drug to a local site. From this, it can be seen that the drug delivery system may be utilized as an injectable drug delivery system as a prodrug thermogel.
[0084] According to one embodiment of the present invention, the thermogel drug delivery system may be biodegradable within 48 hours in phosphate buffered saline (PBS) containing lysozyme at 37°C and pH 7.4. Specifically, the thermogel drug delivery system can be utilized as a biomaterial because it can be biodegraded in the human body. In addition, it can exhibit excellent effects as a biomaterial due to the excellent biocompatibility, low cytotoxicity, and mucosal adhesiveness of hexanoyl glycol chitosan.
[0085] According to one embodiment of the present invention, the thermogel drug delivery system can release a drug over a period of 1 to 45 days in phosphate buffered saline (PBS) at 37°C and pH 7.4. Specifically, while the water-soluble drug DSP was rapidly released in about 4 hours, the thermogel drug delivery system released the drug over several days to several weeks even though it contained the hydrophobic drug dexamethasone (DEX). From this, it can be confirmed that the thermogel drug delivery system can suppress rapid initial release and control drug release.
[0086] Hereinafter, the present invention will be described in detail using examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention is not limited to the examples described below. The examples in this specification are provided to more fully explain the present invention to those of ordinary skill in the art.
[0087] Reagents and Materials
[0088] Glycol chitosan (GC, DP ≥ 200), succinic anhydride (SA), and adipic anhydride (AA) were purchased from Wako Pure Chemical Industries (Japan). Hexanoic anhydride (>95%) and pyridine were purchased from Sigma-Aldrich (India). Deuterium oxide (D2O), methanol-d4, dimethyl sulfoxide-d6 (DMSO-d6), and Dulbecco's phosphate buffered saline (PBS) were purchased from Sigma-Aldrich (USA). Methanol, ethanol, and acetone were purchased from Samjeon Chemical Co., Ltd. (Korea). Dexamethasone (DEX) was purchased from Farmabios (Italy), and dexamethasone phosphate disodium salt (DSP) was purchased from Steraloids (USA). N-hydroxysuccinimide (NHS) was purchased from Sigma-Aldrich (Japan). Lysozyme (from chicken egg white) was purchased from Sigma-Aldrich (Canada). 1-(3-Dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC) was purchased from Tokyo Chemical Industry (Japan). Dialysis membranes (MWCO: 12–14 kDa) were purchased from Spectrum Laboratories, Inc. (USA). Triple-distilled water was used.
[0089]
[0090] <Manufacturing Example 1: Manufacturing of hexanoyl glycol chitosan (HGC)>
[0091] 3 g of glycol chitosan (GC) was dissolved in 375 mL of distilled water to prepare a homogeneous solution, and then 375 mL of methanol was added. For N-hexanoylation, 0.743 mL of hexanoic anhydride was added and reacted at room temperature for 24 h. The reacted solution was then precipitated in acetone, and the precipitated material was obtained through gravity filtration. The precipitate was dissolved in distilled water and dialyzed against distilled water for 2 days using a dialysis membrane (molecular weight cut-off (MWCO) = 12-14 kDa). After removing impurities through a 0.8 μm syringe filter, hexanoyl glycol chitosan (HGC) was finally obtained in the form of a dried powder through lyophilization.
[0092]
[0093] <Manufacturing Example 2: Preparation of dexamethasone derivatives (DEX-SA, DEX-AA)>
[0094] Dexamethasone succinate (DEX-SA) and dexamethasone adipate (DEX-AA) were synthesized by introducing an ester bond-based bioreactive linker to dexamethasone (DEX), a hydrophobic drug.
[0095] <Dexamethasone succinate (DEX-SA)의 제조>
[0096] A solution of dexamethasone (DEX; 0.982 g), succinic anhydride (4.208 g), and 4-dimethylaminopyridine (DMAP; 0.318 g) dissolved in acetone (160 ml) under nitrogen gas was stirred at room temperature overnight. The white crystals obtained by evaporating acetone from the stirred resultant were dissolved in ethanol (50 ml), and then deionized water (300 ml) was slowly added to prepare a dexamethasone succinate solution. The dexamethasone succinate solution was maintained at 4°C for 2 days, resulting in the precipitation of white needle-like crystals. The precipitate was filtered and dried under reduced pressure to synthesize dexamethasone succinate (DEX-SA). This re-sedimentation process was performed twice.
[0097] <Dexamethasone adipate (DEX-AA)의 제조>
[0098]
[0099] 1 g of DEX and 0.98 g of adipic anhydride (AA) were dissolved in 30 mL of pyridine and reacted at room temperature for 24 hours. The solution was distilled under reduced pressure to evaporate the pyridine. The concentrate obtained was dissolved in 100 mL of ethanol, and 500 mL of triple-distilled water was added dropwise. The mixture was stored at 4°C for 24 hours to precipitate dexamethasone adipate (DEX-AA). The precipitated DEX-AA was selectively separated through reduced pressure filtration and dried in a vacuum oven at room temperature to obtain white needle-like crystals of DEX-AA.
[0100]
[0101] <Manufacturing Example 3: Preparation of Precursor (HGC-DEX)>
[0102] DEX-conjugated HGC (precursor) was synthesized through direct chemical bonding of HGC and DEX-SA or DEX-AA. 0.5 g of HGC was dissolved in 50 mL of distilled water in a round flask. In another round flask, DEX-SA or DEX-AA was dissolved in 100 mL of absolute ethanol at a given molar ratio (HGC: DEX-SA or DEX-AA = 1: 0.05 to 0.30). Then, EDC and NHS, which are catalysts, were added in an amount equivalent to 1.5 M of the added DEX-SA or DEX-AA, and the mixture was stirred for 30 minutes at room temperature under a nitrogen atmosphere. Afterwards, the two solutions were combined and reacted at room temperature for 48 hours under a nitrogen gas atmosphere. The reaction solution was precipitated in acetone, the precipitate was collected, dissolved in distilled water, and dialyzed against distilled water for 2 days using a dialysis membrane (MWCO = 12-14 kDa). After removing impurities through a 0.8 μm syringe filter, the product was finally obtained in a dried powder form through lyophilization.
[0103]
[0104] <Manufacturing Example 4: Manufacturing of thermogel drug delivery system (HGC-DEX)>
[0105] A thermogel drug delivery system (HGC-DEX) was manufactured by dissolving the precursor (HGC-DEX) manufactured through Manufacturing Example 3 in distilled water in an amount of 1 wt% to 7 wt%.
[0106]
[0107] <Method of measuring physical properties>
[0108] The structural characteristics and chemical composition of hexanoyl glycol chitosan (HGC), dexamethasone derivatives (DEX-SA, DEX-AA) and precursor (HGC-DEX) manufactured through Manufacturing Examples 1 to 3 were obtained through AVANCE Ⅲ 600 (BRUKER, Germany) operated at 600 MHz. 1H-NMR spectra were used for analysis. The HGC sample for analysis was prepared using D2O as a solvent, DEX-SA and DEX-AA were prepared using methanol-d4, and the HGC-DEX conjugate was prepared using DMSO-d6. Dissolved in D2O co-solvent. Each sample was prepared by dissolving it at a concentration of 0.5 wt%.
[0109] To confirm the structural changes in molecular bonds before and after synthesis, the ATR-FTIR spectrum of the powder sample was analyzed using a Nicolet iS5 (Thermo scientific, USA). 4000-750 cm -1 4 cm in frequency range -1 The resolution was measured through 32 scans.
[0110] The sol-gel transition temperatures of the synthesized HGC and thermogel drug delivery system (HGC-DEX) were measured over a temperature range of 20-50°C using the tube-tilting method. Each sample was prepared by dissolving it in distilled water at a concentration of 1-7 wt%. The sol-gel transition temperature was determined based on the temperature at which no flow occurred after 30 s in a tilted tube, and the temperature was increased at a rate of 1°C / min.
[0111] A rheometer (Model: HR-10, TA Instruments, USA) was used to observe the viscosity value trend, storage modulus, and loss modulus with temperature change of the synthesized HGC solution and the thermogel drug delivery system (HGC-DEX) manufactured according to Manufacturing Example 4. At this time, the difference in rheological behavior according to the concentration of the precursor (HGC-DEX) was examined. The thermogel drug delivery system to be measured (1-7 wt%, distilled water) was loaded between two plates with a radius of 40 mm, and the plate gap was set to 500 μm. Then, the measurement was performed by applying a constant stress of 10 Pa in the temperature range of 10-50 ℃ at a heating rate of 3 ℃ / min, and fixing the vibration frequency to 1 Hz.
[0112] A field emission scanning electron microscope (FE-SEM) (Model: S-4800, Hitachi, Japan) was used to observe the crosslinked morphology and microstructure of the crosslinked thermogel drug delivery system (HGC-DEX). The sol-formed thermogel drug delivery system was placed in a constant temperature water bath maintained at 37°C for 30 min for gelation and then completely dried through freeze-drying. All prepared samples were platinum-coated for 30 s as a pretreatment step for SEM analysis.
[0113] The ability to release the drug dexamethasone (DEX) through hydrolysis of ester bonds in a thermogel drug delivery system (HGC-DEX) was evaluated. The precursor (HGC-DEX) was dissolved in distilled water at a concentration of 1 wt% and placed in a dialysis membrane (MWCO: 12-14 kDa). The dialysis membrane was immersed in 1 L PBS (pH 7.4) and kept at 37°C and 100 rpm. Samples inside the dialysis membrane were collected at designated times (3, 6, 12, 24, and 48 h) and then lyophilized. The residual amount of dexamethasone (DEX) was 1 It was confirmed using H-NMR.
[0114] The physical stability of the thermogel drug delivery system (HGC-DEX) was compared and evaluated according to the concentration of the precursor (HGC-DEX) and the degree of substitution of the dexamethasone derivatives (DEX-SA, DEX-AA). 0.5 mL of the thermogel drug delivery system (HGC-DEX) was prepared in each 5 mL vial and placed in a 37 °C water bath for 30 minutes for gelation. After weighing all samples, 2 mL of 37 °C PBS (pH 7.4) was added to each vial and placed in the water bath, and the PBS was replaced at regular intervals. The mass of the remaining thermogel drug delivery system (HGC-DEX) before replacing the PBS was measured and converted into a percentage by comparing it to the initial gel mass. The experiment was performed three times in total, and the experimental data are expressed as the mean value ± standard deviation. The percentage of residual thermogel drug delivery system (HGC-DEX) weight was calculated using the following equation:
[0115] Residual weight(%)=W t / W i X 100
[0116] In this formula, W i is the weight of the initially measured thermogel drug delivery system (HGC-DEX), and W t is the weight of the thermogel drug delivery system (HGC-DEX) over time.
[0117] The biodegradability of the thermogel drug delivery system (HGC-DEX) was evaluated by monitoring the mass change of the thermogel drug delivery system over time in the presence of lysozyme (5 mg / ml), a degrading enzyme, in a PBS solution (pH 7.4, 37°C). The experiment followed the same process as the physical stability evaluation experiment, except that lysozyme was added to the PBS. The experiment was performed three times, and the experimental data were expressed as the mean ± standard deviation.
[0118] To investigate the drug release behavior of the thermogel drug delivery system (HGC-DEX), 1 mL of the thermogel drug delivery system (HGC-DEX) was placed in a dialysis membrane (MWCO = 12-14 kDa, width: 10 mm) and gelled. The dialysis membrane was placed in a conical tube containing 25 mL of phosphate-buffered saline (PBS) solution (pH 7.4, 37°C) and placed in a constant temperature water bath set at 37°C and 100 rpm, and a release test was performed. At set time intervals, the dialysis membrane in the conical tube was removed and transferred to a new conical tube containing 25 mL of PBS solution. A sample was taken from the previous conical tube and the amount of released drug was analyzed. The drug release over time was measured using a UV-Vis spectrophotometer, and the drug release amount was calculated by measuring the absorbance at 242 nm, the maximum absorbance wavelength of DEX. The experiment was conducted three times in total, and the experimental data were expressed as the mean value ± standard deviation value.
[0119]
[0120] <Experimental Example: Interpretation of Results>
[0121] <Experimental Example 1: Characteristic Analysis of HGC, DEX-SA, DEX-AA, and HGC-DEX>
[0122] The structural characteristics and chemical composition of hexanoyl glycol chitosan (HGC), dexamethasone derivatives (DEX-SA, DEX-AA) and precursor (HGC-DEX) manufactured through Manufacturing Examples 1 to 3 were obtained through AVANCE Ⅲ 600 (BRUKER, Germany) operated at 600 MHz. 1 It was analyzed using H-NMR spectrum.
[0123] Figure 2A is a diagram of DEX and DEX-SA according to one embodiment of the present invention. 1 It shows the H-NMR spectrum, and FIG. 2B shows the DEX and DEX-AA according to one embodiment of the present invention. 1It shows the H-NMR spectrum.
[0124] As shown in Fig. 2A, it can be seen that the peaks at positions indicated by a and b in the dexamethasone derivative (Dexamethasone adipate, DEX-SA) are additionally observed compared to dexamethasone (DEX). In addition, as shown in Fig. 2B, it can be seen that the peaks at positions indicated by d, e, f, and g in the dexamethasone derivative (Dexamethasone adipate, DEX-AA) are additionally observed compared to dexamethasone (DEX).
[0125] Figure 3A is a diagram of HGC and a thermogel drug delivery system (HGC-SA-DEX), which is a polymer synthesized with GC according to one embodiment of the present invention. 1 It shows the H-NMR spectrum. Figure 3B shows the HGC and thermogel drug delivery system (HGC-AA-DEX), which is a polymer synthesized with GC according to one embodiment of the present invention. 1 This shows the H-NMR spectrum. Referring to Figures 3A and 3B, the D2O peak at 4.85 ppm was set as the reference peak for analysis. The peaks appearing at 3.2 to 4.2 ppm correspond to the hydrogen atoms (H2 to H8) of the glucopyranosyl ring, and the peak appearing at 2.7 ppm is due to the hydrogen atoms of the primary amine residue, which are common peaks of GC and HGC. Among the characteristic hydrogen atom peaks of HGC, 0.8 ppm (-CH3) corresponds to the hydrogen atoms of the methyl group, and 1.3 ppm (- CH2-CH2-CH3), 1.6 ppm (-CO-CH2-CH2-), and 2.3 ppm (-CO-CH2-) correspond to the hydrogen atoms of the methylene group of the hexanoyl group, respectively. The degree of hexanoylation in HGC was measured by comparing the integral values of the hydrogen atom peaks of the glucopyranosyl ring and the hexanoyl group, and was calculated to be approximately 26%.
[0126] Referring to Fig. 3A, the peak of HGC-DEX was identified by the characteristic peak of DEX appearing between 6 and 8 ppm, and the peak of GC was confirmed to be distributed between 3.05 and 3.98 ppm. The peak of HGC was identified by the characteristic peak of HGC appearing between 0.75 and 2.5 ppm. The degree of substitution (DS) of DEX was measured by comparing the integral values of the hydrogen atom peaks of the glucopyranosyl ring and the DEX-SA group, and was calculated to be 5% or more and 10% or less. As a result, the thermogel drug delivery systems (HGC-DEX) having substitution degrees of 5.3%, 7.0%, and 9.5% were named HGC-DEX5, HGC-DEX7, and HGC-DEX10, respectively.
[0127] Referring to Fig. 3B, the peak of HGC-DEX was identified by the characteristic peak of DEX appearing between 6 and 8 ppm, and the peak of GC was confirmed to be distributed between 3.05 and 3.98 ppm. The peak of HGC was identified by the characteristic peak of HGC appearing between 0.75 and 2.5 ppm. The degree of substitution (DS) of DEX was measured by comparing the integral values of the hydrogen atom peaks of the glucopyranosyl ring and the DEX-AA group, and was calculated to be 1% or more and 5% or less. As a result, the drug delivery systems (HGC-DEX) with substitution degrees of 2.3% and 2.95% were named HGC-DEX15 and HGC-DEX20, respectively.
[0128]
[0129] In order to confirm the structural changes in the molecular bonds of hexanoyl glycol chitosan (HGC), dexamethasone derivatives (DEX-SA, DEX-AA) and precursor (HGC-DEX) manufactured through Manufacturing Examples 1 to 3, ATR-FTIR spectral analysis was performed.
[0130] Figure 4 shows the ATR-FTIR spectrum of DEX-SA, HGC, a polymer synthesized with GC, and a thermogel drug delivery system (HGC-DEX) according to one embodiment of the present invention. Referring to Figure 4, the 3484 cm of DEX-SA -1 and 3579 cm -1 The absorption bands are attributed to the stretching vibration of the -OH bond and are at 1617, 1660, 1712 and 1733 cm -1 It can be confirmed that the stretching vibration in is due to the C=O bond. GC 1649 cm -1 The stretching vibration corresponds to the C=O bond and is at 1587 cm -1 It can be confirmed that the absorption peak is due to the bending vibration of the amino group. For HGC and HGC-DEX, it is 1587 cm -1 The characteristic amino group band disappears at 1552 cm -1 The amide II band was observed, suggesting that HGC and HGC-DEX were synthesized.
[0131] Figure 5A shows the ATR-FTIR spectra of DEX and DEX-AA according to one embodiment of the present invention. Referring to Figure 5A, the 3500 cm of DEX-AA -1 The absorption band near 1725 cm is due to the stretching vibration of the -OH bond. -1 It can be confirmed that the elastic vibration in originates from the C=O bond.
[0132] Figure 5B shows the ATR-FTIR spectrum of HGC and thermogel drug delivery system (HGC-DEX), which are polymers synthesized with GC according to one embodiment of the present invention. Referring to Figure 5B, 1655 cm of GC -1 The stretching vibration corresponds to the C=O bond and is at 1589 cm -1 It can be confirmed that the absorption peak is due to the bending vibration of the amino group. For HGC and HGC-DEX, it is 1589 cm -1The characteristic amino group band disappears at 1556 cm -1 Amide II band was observed at 1725 cm for HGC-DEX. -1 It was found that the synthesis of HGC and HGC-DEX was successful, as a characteristic peak corresponding to the C=O group of DEX appeared.
[0133]
[0134] In the process of manufacturing glycol chitosan (hexanoyl glycol chitosan, HGC), dexamethasone derivatives (DEX-SA, DEX-AA) and precursors (HGC-DEX) through Manufacturing Examples 1 to 3, the molar ratio of dexamethasone derivatives (DEX-SA, DEX-AA) was adjusted to synthesize drug delivery systems (HGC-DEX) having different degrees of substitution. Table 1 below summarizes the analysis results of HGC and drug delivery systems (HGC-DEX).
[0135] Sample hexanoic acid anhydride molar ratio a DEX-SA molar ratio b DEX-AA molar ratio c Hexanoyl group substitution degree (%) d DEX-SA substitution rate (%) e DEX-AA substitution degree (%) f Drug content (%) g Yield (%) HGC260.25--26.2---81.7HGC-DEX5-0.11--5.3-5.795.7HGC-DEX7-0.14--7.0-7.797.3HGC-DEX10-0.18--9.5-9.692.3HGC-DEX15--0.15--2.302.391.24HGC-DEX20--0.20--2.953.190.92a) Supply molar ratio of hexanoic anhydride to the glucosamine group of GCb) Supply molar ratio of DEX-SA to the glucosamine group of HGCc) Supply molar ratio of DEX-AA to the glucosamine group of HGCd) 1 The degree of hexanoylation determined by peak integration of H NMR e) 1DEX-SA degree determined by peak integration of H NMR f) 1 DEX-AA degree determined by peak integration of H NMRg) Drug content in HGC-DEX determined by UV-visible measurement
[0136] <Experimental Example 2: Temperature-dependent sol-gel transition characteristics of thermogel drug delivery system (HGC-DEX)>
[0137] The sol-gel transition characteristics of thermogel drug delivery systems (HGC-DEX) containing the synthesized samples shown in Table 1 were analyzed. The sol-gel transition temperatures of thermogel drug delivery systems (HGC-DEX) containing HGC, HGC-DEX5, HGC-DEX7, HGC-DEX10, HGC-DEX15, and HGC-DEX20 at various concentrations of 2, 3, 4, and 5 wt% were measured by the tube-tilting method in the temperature range of 20-50°C, and are shown in Table 2 below. Table 2 below summarizes the sol-gel transition temperatures of the drug delivery systems (HGC-DEX) samples at various concentrations.
[0138]
[0139] Sample T gel (℃)2wt%3wt%4wt%5wt%6wt%7wt%HGC26SolSolSolSolSolSolHGC-DEX5SolSol46393223HGC-DEX7Sol4 627GelGelGelHGC-DEX102922GelGelGelGelHGC-DEX15Sol413730GelGelHGC-DEX20413226GelGelGel
[0140] <Experimental Example 3: Analysis of Tube Tilt Method and Rheological Behavior of Thermogel Drug Delivery System (HGC-DEX)>
[0141] Fig. 6 shows a sol-gel transition diagram of a thermogel drug delivery system (HGC-DEX) according to an embodiment of the present invention through tube tilting method analysis. Specifically, Fig. 6A shows an analysis of the gelation behavior of a thermogel drug delivery system (HGC-SA-DEX) containing DEX-SA according to the concentration and degree of substitution of DEX-SA, and Fig. 6B shows an analysis of the gelation behavior of a thermogel drug delivery system (HGC-AA-DEX) containing DEX-AA according to the concentration and degree of substitution of DEX-AA.
[0142] As shown in Table 2 and Fig. 6, HGC did not undergo a sol-gel transition at 2 to 7 wt% and always existed in a sol state. HGC-DEX5, with a DEX-SA substitution degree of 5.3%, exhibited a sol-gel transition at 4 wt% or more, HGC-DEX7, with a DEX-SA substitution degree of 7.0%, exhibited a sol-gel transition at 3 wt% or more, and HGC-DEX10, with a DEX-SA substitution degree of 9.5%, exhibited a sol-gel transition at 2 wt% or more. Therefore, the critical gelation concentrations of HGC-DEX5, HGC-DEX7, and HGC-DEX10 can be said to be 4 wt%, 3 wt%, and 2 wt%, respectively.
[0143] HGC-DEX15, which has a substitution degree of DEX-AA of 2.3%, did not show a sol-gel transition phenomenon at 2 wt%, but at 3, 4, and 5 wt%, the sol-gel transition phenomenon was observed at 41, 37, and 30 ℃, respectively. Therefore, the critical gelation concentration of HGC-DEX15 can be said to be 3 wt%. HGC-DEX20, which has a substitution degree of DEX-AA of 2.95%, has a critical gelation concentration of 2 wt%, and showed a sol-gel transition phenomenon at 41, 32, and 26 ℃ at 2, 3, and 4 wt%, respectively, but at 5 wt%, it always existed in a gel state in the temperature range of 20-50 ℃.
[0144] FIG. 7 is an image showing the gelation behavior of a thermogel drug delivery system (HGC-DEX) according to an embodiment of the present invention at room temperature and at 37°C, which is the body temperature. Specifically, FIG. 7A is an image showing the sol-gel transition of HGC and a 4 wt% thermogel drug delivery system (HGC-SA-DEX) at 20°C and 37°C, and FIG. 7B is an image showing the sol-gel transition of a 3 wt% to 5 wt% thermogel drug delivery system (HGC-AA-DEX) at 20°C and 37°C.
[0145] It can be confirmed that the thermogel drug delivery system containing 4 wt% of HGC-DEX5 exists in a sol state at room temperature (20°C) and body temperature (37°C). It can be confirmed that the thermogel drug delivery system containing 4 wt% of HGC-DEX7 exists in a sol state at room temperature (20°C) and in a gel state at body temperature (37°C). It can be confirmed that the thermogel drug delivery system containing 4 wt% of HGC-DEX10 exists in a gel state at room temperature (20°C) and body temperature (37°C).
[0146] It can be seen that a thermogel drug delivery system containing 4 wt% or more and 5 wt% or less of HGC-DEX15 exists in a sol state at room temperature and in a gel state at 37°C, which is a body temperature. In addition, it can be seen that a thermogel drug delivery system containing 3 wt% or more and 4 wt% or less of HGC-DEX20 exists in a sol state at room temperature and in a gel state at 37°C, which is a body temperature.
[0147]
[0148] These results confirmed that as the concentration of the thermogel drug delivery system (HGC-DEX) increases, the hydrophobic interaction becomes stronger and the sol-gel phase transition temperature decreases, and that as the degree of substitution of DEX-SA and DEX-AA increases, the critical gelation concentration decreases, and when compared at the same concentration of the thermogel drug delivery system, as the degree of substitution of DEX-SA and DEX-AA increases, the sol-gel transition temperature decreases.
[0149] The rheological properties of the hexanoyl glycol chitosan (HGC) and thermogel drug delivery system (HGC-DEX) samples shown in Table 2 above were analyzed by measuring the viscoelasticity and viscosity behavior according to temperature change using a rheometer.
[0150] FIG. 8 shows the rheological behavior of HGC and 4 wt% thermogel drug delivery system (HGC-SA-DEX) samples according to an embodiment of the present invention according to temperature change. The temperature-dependent rheological behavior experiment was performed under the conditions of 10 to 50 ℃, a heating rate of 3 ℃ / min, a frequency of 1 Hz, and a constant stress of 10 Pa. The temperature at which the elastic modulus (G') and the loss modulus (G") intersect is defined as the gelation point when determining the sol-gel transition, and it was confirmed that the elastic modulus (G') values of HGC, HGC-DEX5, and HGC-DEX7 were initially consistently lower than the loss modulus (G"), but the elastic modulus (G') tended to increase rapidly as the temperature increased. As shown in FIGS. 8B and 8C, the temperatures at which the elastic modulus (G') and loss modulus (G") values of HGC-DEX5 and HGC-DEX7 intersect are 46.0°C and 26.9°C, respectively, and it was confirmed that this is consistent with the analysis results of the tube tilting method.
[0151] Figure 9 shows the rheological behavior of HGC and thermogel drug delivery system (HGC-AA-DEX) samples with temperature change at various concentrations of 2, 3, 4, and 5 wt% according to one embodiment of the present invention. Specifically, the gel point is affected by the concentration and degree of substitution of the sample, and the sol-gel transition phenomenon of HGC and thermogel drug delivery system (HGC-DEX) is a result of the increase in hydrophobic interactions with increasing temperature.
[0152] As shown in Fig. 9A, in the case of HGC, the elastic modulus (G') was continuously lower than the loss factor (G") at 2, 3, and 4 wt%, indicating a sol state, and at 5 wt%, the elastic modulus (G') increased rapidly starting from the sol-gel transition temperature and intersected with the loss factor (G"). As shown in Fig. 9B, in the case of HGC-DEX15, no intersection of the elastic modulus (G') and the loss factor (G") was observed at 2 wt%, and as the concentration increased to 3, 4, and 5 wt%, the elastic modulus (G') and the loss factor (G") tended to intersect at lower temperatures. As shown in Fig. 9C, for HGC-DEX20, as the concentration increased to 2, 3, 4, and 5 wt%, the elastic modulus (G') and the loss factor (G") crossed at a lower temperature. In addition, compared to HGC-DEX15 at the same concentration, it was confirmed that the elastic modulus (G') and the loss factor (G") crossed at a lower temperature because the hydrophobic DEX-AA content was higher.
[0153]
[0154] <Experimental Example 4: Analysis of shear thinning properties, thixotropic recovery properties, and complex viscosity behavior for injection applications>
[0155] Figure 10 shows the shear thinning characteristics and thixotropic recovery characteristics of thermogel drug delivery system (HGC-SA-DEX) samples according to one embodiment of the present invention.
[0156] Figure 10A shows the shear rate (s) of a thermogel drug delivery system (HGC-DEX) exhibiting shear-thinning property. -1 ) is a graph showing the viscosity (Pa.s) according to the shear rate. The shear thinning characteristics were performed by a steady shear rate sweep test at 25°C. Referring to Fig. 10A, it can be confirmed that the viscosity of the thermogel drug delivery system (HGC-DEX) decreases as the shear rate increases for all of HGC-DEX5, HGC-DEX7, and HGC-DEX10 at 25°C, and thus it can be inferred that they can be injected. That is, HGC-DEX5, HGC-DEX7, and HGC-DEX10 all show desirable shear thinning behavior with the viscosity decreasing as the shear rate increases, and thus can be applied as an injectable thermogel drug delivery system (HGC-DEX). Fig. 10B shows the thixotropic recovery property of HGC-DEX7. Referring to Figure 10B, a high shear rate (100 s) for 100 s is used to illustrate the force applied to the drug delivery system of the syringe during injection. -1 ) was used, and a shear rate close to zero for 200 seconds was used to describe the state of the drug delivery system before injection. This thixotropic recovery experiment was repeated four times, and the thermogel drug delivery system containing HGC-DEX7 exhibited excellent elastic recovery properties.
[0157] Figure 11 shows the behavior of the complex viscosity according to the temperature change of HGC and thermogel drug delivery system (HGC-AA-DEX) samples at various concentrations of 2, 3, 4, and 5 wt% according to one embodiment of the present invention. As shown in Figures 11A to 11C, it was confirmed that the complex viscosity showed an increasing behavior starting from the gelation point, and it was found that the complex viscosity increased as the concentration of the sample increased and the degree of DEX-AA substitution increased. Through this, it was confirmed that it is possible to appropriately control the sol-gel transition temperature by controlling the concentration and the degree of DEX-AA substitution of the thermogel drug delivery system (HGC-DEX).
[0158]
[0159] <Experimental Example 5: Morphological Characteristics of HGC-DEX, Hydrolysis Ability of Ester Bonds in HGC-DEX, Physical Stability, and Biocompatibility Evaluation>
[0160] To analyze the morphological characteristics of thermogel drug delivery systems (HGC-DEX) with different concentrations and degrees of substitution, the surface and cross-section of completely dried thermogel drug delivery systems (HGC-DEX) were observed using FE-SEM.
[0161] FIG. 12 is an FE-SEM image of the surface and cross-section of a thermogel drug delivery system (HGC-DEX) according to an embodiment of the present invention. Referring to FIG. 12A, it can be confirmed that HGC-DEX5, HGC-DEX7, and HGC-DEX10 all form a sponge-like porous three-dimensional structure. Referring to FIG. 12B, it can be confirmed that HGC-DEX15 and HGC-DEX20 also form a porous three-dimensional structure. Specifically, it was confirmed that a porous three-dimensional structure was formed by cross-linking due to the hydrophobic interaction between the hydrophobic hexanoyl group and the DEX molecular structure, and it was confirmed that the pore size decreased as the concentration of the thermogel drug delivery system (HGC-DEX) and the degree of substitution of DEX-AA increased.
[0162] An experiment was conducted to confirm that the ester bonds in the thermogel drug delivery system (HGC-DEX) are hydrolyzed and DEX is released. The powdered precursor (HGC-DEX) was dissolved in distilled water at a concentration of 1 wt%, placed in a dialysis membrane, and then immersed in PBS (pH 7.4, 37°C). Samples were collected at regular intervals over a period of two days. Afterwards, they were freeze-dried. 1 The residual amount of DEX over time was observed using H-NMR.
[0163] Figure 13A shows the hydrolysis ability of a thermogel drug delivery system (HGC-SA-DEX) over time in PBS (pH 7.4, 37°C) according to one embodiment of the present invention. 1 This is represented by the H-NMR spectrum. Referring to Figure 13A, it can be confirmed that the ester bond of HGC-SA-DEX is hydrolyzed after 24 hours, and the peak related to DEX does not appear. These results can be inferred that HGC-SA-DEX can be converted into a DEX formulation within 24 hours and reach the target site.
[0164] Figure 13B shows the hydrolysis ability of a thermogel drug delivery system (HGC-AA-DEX) over time in PBS (pH 7.4, 37°C) according to one embodiment of the present invention. 1 This is represented by the H-NMR spectrum. Referring to Figure 13B, it can be confirmed that after 48 hours, the ester bond of HGC-AA-DEX is hydrolyzed, and the peak related to DEX does not appear. From this, it was confirmed that the thermogel drug delivery system (HGC-AA-DEX) can slowly release the drug through hydrolysis of the ester bond.
[0165] To confirm the physical stability of the thermogel drug delivery system (HGC-DEX), the residual amount of the thermogel drug delivery system (HGC-DEX) was measured while replacing PBS hourly in a constant temperature water bath maintained at 37°C.
[0166] FIG. 14A shows the residual amount of a thermogel drug delivery system (HGC-SA-DEX) over time in PBS (pH 7.4, 37°C) according to one embodiment of the present invention. Referring to FIG. 14A, the residual weights of HGC-DEX5, HGC-DEX7, and HGC-DEX10 all slightly increased in the beginning, reached peaks around 10 hours, and then rapidly decreased due to mass loss of the hydrogel. It can be inferred that the reason for the rapid decrease in residual weight is that a rapid mass loss occurs due to the loss of the hydrogel structure as the ester bond between DEX and HGC is hydrolyzed. It can be inferred that the hydrogel gradually and simultaneously erodes and releases the drug structurally, thereby performing the function of a drug delivery system for a long time in the patient's body, thereby supplying a safe drug formulation without concerns about side effects to the body.
[0167] FIG. 14B shows the residual amount of the thermogel drug delivery system (HGC-AA-DEX) over time in PBS (pH 7.4, 37°C) according to one embodiment of the present invention. Referring to FIG. 14B, both HGC-DEX15 and HGC-DEX20 showed a behavior in which the residual weight increased until equilibrium swelling was achieved and then eventually dissolved. It was confirmed that the higher the concentration of the thermogel drug delivery system (HGC-DEX) and the degree of substitution of DEX-AA, the higher the crosslinking density, so swelling occurred better. Among the four samples, HGC-DEX15 4 wt%, which had the highest sol-gel transition temperature, was observed to dissolve the fastest. It was confirmed that HGC-DEX15 5 wt% had a higher concentration than HGC-DEX15 4 wt%, so it was crosslinked at a higher density and thus took a longer time to decompose. When comparing HGC-DEX15 4 wt% with HGC-DEX20 4 wt%, it was confirmed that HGC-DEX20 with a high DEX-AA substitution degree had a higher density of crosslinking and thus greater stability. From this, it was confirmed that the thermogel drug delivery system (HGC-DEX) has the potential to supply a safe drug formulation to the body with no concerns about side effects and long-term stability in the patient's body as a biomaterial.
[0168] To evaluate the biocompatibility of the thermogel drug delivery system (HGC-DEX), the degradation behavior of HGC-DEX was observed in PBS in the presence of lysozyme at set time intervals.
[0169] Figure 15A shows the residual amount of a thermogel drug delivery system (HGC-SA-DEX) over time in PBS (pH 7.4, 37°C) containing lysozyme according to one embodiment of the present invention. Referring to Figure 15A, it can be confirmed that all of the thermogel drug delivery systems (HGC-DEX) including HGC-DEX5, HGC-DEX7, and HGC-DEX10 exhibited very rapid dissolution behavior, resulting in a 100% loss of total mass in just 48 hours.
[0170] FIG. 15B shows the residual amount of a thermogel drug delivery system (HGC-AA-DEX) over time in PBS (pH 7.4, 37°C) containing lysozyme according to one embodiment of the present invention. Referring to FIG. 15B, the thermogel drug delivery system (HGC-DEX) containing 4 wt% of HGC-DEX15 and 3 wt% of HGC-DEX20 was completely decomposed after 24 hours of addition to PBS containing 5 mg / ml of lysozyme, and the thermogel drug delivery system (HGC-DEX) containing 5 wt% of HGC-DEX15 and 4 wt% of HGC-DEX20 was completely decomposed after 48 hours. This is thought to be because lysozyme penetrates relatively slowly between the HGC-DEX15 5 wt% and HGC-DEX20 4 wt% thermogel drug delivery systems (HGC-DEX), which form relatively firm gels with higher crosslinking density, resulting in slower degradation behavior. Consequently, it was confirmed that the biodegradable thermogel drug delivery system (HGC-DEX) can be usefully utilized as a biocompatible biomaterial.
[0171]
[0172] <Experimental Example 6: Initial Drug Release Evaluation of Thermogel Drug Delivery System (HGC-DEX)>
[0173] To evaluate the drug release behavior of the thermogel drug delivery system (HGC-DEX), the drug release behavior of the thermogel drug delivery system (HGC-DEX) was confirmed in PBS (pH 7.4, 37 ℃).
[0174] FIG. 16A shows the in vitro initial drug release evaluation of DSP and the thermogel drug delivery system (HGC-SA-DEX) in PBS (pH 7.4, 37°C) according to one embodiment of the present invention. Referring to FIG. 16A, the DSP (dexamethasone sodium phosphate) formulation rapidly released the drug regardless of the drug concentration. In contrast to DSP, a low-molecular-weight drug with high water solubility, which was completely released within 1 hour, the thermogel drug delivery system (HGC-SA-DEX) formulation did not initially show sustained release or explosive release due to the entanglement of large molecules. Since the release rate of DEX in the thermogel drug delivery system (HGC-SA-DEX) depends on the degree of hydrolysis of the ester bond between HGC and DEX, it was confirmed that the thermogel drug delivery system (HGC-SA-DEX) formulation can effectively control the initial release rate of a desired drug.
[0175] FIG. 16B shows the in vitro initial drug release evaluation of DSP and thermogel drug delivery system (HGC-AA-DEX) in PBS (pH 7.4, 37°C) according to one embodiment of the present invention. Referring to FIG. 16B, in the case of DSP, a water-soluble drug, the accumulated drug release amount reached about 80% in 2 hours, and it was released quickly. On the other hand, in the thermogel drug delivery system (HGC-AA-DEX), which releases the drug due to hydrolysis of the ester bond, the rapid initial drug release was suppressed, and it was confirmed that the thermogel drug delivery system (HGC-AA-DEX) formulation can effectively control the initial drug release rate of a desired drug by releasing it slowly at a constant rate.
[0176]
[0177] Therefore, the thermogel drug delivery system (HGC-DEX) according to one embodiment of the present invention includes glycol chitosan (GC), which is a natural polymer with a hydrophilic glycol group introduced into it, and thus can be dissolved even at neutral pH and can have the low toxicity, biocompatibility, and biodegradability of chitosan. In addition, it can enhance the efficiency of treatment by releasing the drug in the body by including the reaction product of the drug-active substance and the bioreactive linker.
[0178] A thermogel drug delivery system (HGC-DEX) according to one embodiment of the present invention is biodegradable, can release a drug over a period of 1 day to 45 days under biological conditions, is in a sol phase at room temperature and in a gel phase at 30°C to 40°C, and can be used as an injectable drug delivery system as a thermogel, which is a temperature-sensitive hydrogel, and as a prodrug.
Claims
1. Polymer for manufacturing thermogel; and A thermogel drug delivery system comprising a precursor containing a reaction product of a drug-active substance and a bioreactive linker.
2. In paragraph 1, The polymer for manufacturing the above thermogel is, A thermogel drug delivery system comprising any one selected from the group consisting of glycol chitosan derivatives, cellulose, carboxymethyl cellulose, hydroxypropyl methylcellulose, chitin, dextran, dextrin, gelatin, hyaluronic acid, pectin, rhamnogalacturonan, xylan, and copolymers thereof.
3. In paragraph 2, A thermogel drug delivery system wherein the glycol chitosan derivative contains a straight or branched acyl group having 2 to 20 carbon atoms.
4. In paragraph 1, The above drug substance is, A thermogel drug delivery system comprising one selected from the group consisting of anti-inflammatory substances, anti-cancer substances and combinations thereof.
5. In paragraph 1, A thermogel drug delivery system wherein the bioreactive linker comprises an acid anhydride.
6. In paragraph 1, A thermogel drug delivery system wherein the degree of substitution (DS) of the reaction product in the precursor is 1% or more and 30% or less.
7. In paragraph 1, A thermogel drug delivery system wherein the precursor is in powder form.
8. In paragraph 7, A thermogel drug delivery system wherein the content of the precursor is 1 wt% or more and 10 wt% or less.
9. In paragraph 1, A thermogel drug delivery system further comprising a solvent.
10. In paragraph 9, At room temperature, it is in a sol phase, A thermogel drug delivery system that is in a gel phase at a temperature of 30°C or higher and 40°C or lower.
11. In paragraph 9, A thermogel drug delivery system that releases a drug over a period of 1 to 45 days in phosphate buffered saline (PBS) at 37°C and pH 7.4.
Citation Information
Patent Citations
Injectable thermosensitive pluronic derivative hydrogels with high biodegradability and biocompatibility for tissue regeneration and preparation method thereof
KR1020100044607A
Bidirectional drain panel structure
KR102654123B1