Fluorine gas production method

By electrolyzing an electrolytic solution with hydrogen fluoride, metal fluoride, and hexafluoronicel(IV) acid metal salt, the method effectively suppresses mist generation during fluorine gas production, addressing clogging issues and enhancing operational continuity and cost-effectiveness.

WO2024224829A1PCT designated stage expired Publication Date: 2024-10-31RESONAC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008865
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-03-07
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The production of fluorine gas by electrolysis often results in the generation of mist, which can clog pipes and valves, disrupting continuous operation and increasing production costs due to the need for frequent interruptions.

Method used

The method involves electrolyzing an electrolytic solution containing hydrogen fluoride, metal fluoride, and hexafluoronicel(IV) acid metal salt using a nickel or carbonaceous anode and a metal cathode, with specific concentrations and ratios of electrolyte components to minimize mist generation, allowing for reduced clogging without the need for additional mist removal devices.

Benefits of technology

This approach significantly reduces mist generation, minimizing pipe and valve clogging, thereby reducing the frequency of operation interruptions and lowering production costs by maintaining continuous fluorine gas production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008865_31102024_PF_FP_ABST
    Figure JP2024008865_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a fluorine gas production method wherein mist is less likely to occur. According to the present invention, a fluorine gas is produced by a method which comprises an electrolysis step for generating a fluorine gas by electrolyzing an electrolyte solution using a positive electrode and a negative electrode in an electrolytic cell. The electrolyte solution contains hydrogen fluoride, a metal fluoride, and a metal salt of hexafluoronickelate(IV). The positive electrode is a nickel electrode or a carbonaceous electrode, and the negative electrode is a metal electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Fluorine gas production method

[0001] The present invention relates to a method for producing fluorine gas.

[0002] Fluorine gas can be synthesized by electrolyzing an electrolyte containing hydrogen fluoride and a metal fluoride. Since mist (e.g., electrolyte mist) is generated along with fluorine gas during the electrolysis of the electrolyte, the mist is entrained in the fluorine gas discharged from the electrolytic cell. The mist entrained in the fluorine gas turns into powder and may clog the piping and valves used to deliver the fluorine gas. This may force the operation of producing fluorine gas to be interrupted or stopped, hindering continuous operation in the production of fluorine gas by electrolysis. To prevent the clogging of piping and valves due to the mist, Patent Document 1 discloses a technique of heating the fluorine gas entrained with the mist or the piping through which the fluorine gas passes to a temperature above the melting point of the electrolyte. Patent Document 2 also discloses a gas generator having a gas diffusion section, which is a space for roughly collecting the mist, and a filler housing section for housing a filler for adsorbing the mist.

[0003] Japanese Patent Publication No. 5584904 Japanese Patent Publication No. 5919824

[0004] However, in order to more effectively prevent pipes and valves from being clogged with mist, a technology for producing fluorine gas that suppresses the generation of mist itself has been desired. An object of the present invention is to provide a method for producing fluorine gas that is less likely to generate mist.

[0005] In order to solve the above problems, one aspect of the present invention is as follows [1] to [8]: [1] A method for producing fluorine gas, comprising an electrolysis step of electrolyzing an electrolyte solution using an anode and a cathode in an electrolytic cell to generate fluorine gas, wherein the electrolyte solution contains hydrogen fluoride, a metal fluoride, and a metal salt of hexafluoronickel(IV), the anode being a nickel electrode or a carbonaceous electrode, and the cathode being a metal electrode.

[0006] [2] The method for producing fluorine gas according to [1], wherein the metal hexafluoronickelate (IV) is at least one of potassium hexafluoronickelate (IV), cesium hexafluoronickelate (IV), and rubidium hexafluoronickelate (IV). [3] The method for producing fluorine gas according to [1] or [2], wherein the concentration of nickel (IV) ions in the electrolytic solution is 100 ppm by mass or more and 1000 ppm by mass or less.

[0007] [4] The method for producing fluorine gas according to any one of [1] to [3], wherein the metal fluoride is at least one of potassium fluoride and cesium fluoride. [5] The method for producing fluorine gas according to any one of [1] to [4], wherein the ratio of the molar amount of the hydrogen fluoride to the molar amount of the metal fluoride contained in the electrolytic solution is 1.6 or more and 3.2 or less. [6] The method for producing fluorine gas according to any one of [1] to [5], wherein the cathode is an electrode formed of at least one of iron, nickel, copper, and a copper-nickel alloy.

[0008] [7] The method for producing fluorine gas according to any one of [1] to [6], wherein the electrolytic solution is a mixture of the hydrogen fluoride, the metal fluoride, and the metal hexafluoronickelate (IV) having a water content of 0.5 mass% or less. [8] The method for producing fluorine gas according to any one of [1] to [7], wherein the electrolytic solution has an iron ion concentration of 500 mass ppm or less and a copper ion concentration of 200 mass ppm or less.

[0009] According to the present invention, mist is less likely to be generated when fluorine gas is produced by electrolyzing an electrolyte solution.

[0010] 1 is a graph showing the correlation between the current density in electrolysis and the number of mists contained in fluorine gas. 2 is a graph showing the correlation between the current density in electrolysis and the total volume of mists contained in fluorine gas. 3 is a graph showing the particle size distribution of mists contained in fluorine gas.

[0011] An embodiment of the present invention will be described below. Note that this embodiment is merely an example of the present invention, and the present invention is not limited to this embodiment. Furthermore, various modifications and improvements can be made to this embodiment, and such modifications and improvements can also be included in the present invention.

[0012] The present inventors have conducted extensive research into mist, which causes clogging of pipes and valves in the electrolytic synthesis of fluorine gas (F2). In this invention, "mist" refers to liquid or solid particles that are generated together with fluorine gas in an electrolytic cell by electrolysis of an electrolyte. Specifically, it refers to particles of the electrolyte, solid particles resulting from a phase change of the electrolyte particles, and solid particles generated by the reaction of fluorine gas with components that constitute the electrolytic cell (such as metals that form the electrolytic cell, packing for the electrolytic cell, and carbonaceous electrodes).

[0013] The present inventors have investigated the mist contained in the fluid generated inside an electrolytic cell during electrolysis of an electrolyte, and have found that the generation of mist can be suppressed by adding an additive to the electrolyte, which has led to the completion of the present invention. One embodiment of the present invention will be described below.

[0014] The method for producing fluorine gas according to this embodiment includes an electrolysis step in which an electrolytic solution containing hydrogen fluoride (HF), a metal fluoride, and a metal salt of hexafluoronickel(IV) is electrolyzed in an electrolytic cell using an anode and a cathode to produce fluorine gas. The anode is a nickel electrode or a carbonaceous electrode, and the cathode is a metal electrode.

[0015] Since metal hexafluoronickel(IV) salt is added as an additive to the electrolyte, mist is less likely to be generated when fluorine gas is produced by electrolyzing the electrolyte. Mist entrained in fluorine gas turns into powder and may clog pipes and valves used to deliver fluorine gas, but since the amount of mist generated during fluorine gas production is small, clogging of pipes and valves used to deliver fluorine gas can be suppressed without installing a mist removal device in the fluorine gas production equipment. As a result, the frequency of interruptions and shutdowns of fluorine gas production operations can be reduced, thereby lowering the cost of fluorine gas production.

[0016] The method for producing fluorine gas according to this embodiment will be described in further detail below. There are no particular limitations on the form of the electrolytic cell, and any electrolytic cell can be used as long as it is capable of generating fluorine gas by electrolyzing an electrolyte solution containing hydrogen fluoride and a metal fluoride. Usually, the interior of the electrolytic cell is partitioned by a partition member such as a partition wall into an anode chamber in which an anode is disposed and a cathode chamber in which a cathode is disposed, so that the fluorine gas generated at the anode and the hydrogen gas generated at the cathode do not mix.

[0017] The anode may be a carbonaceous electrode made of a carbon material such as diamond, diamond-like carbon, amorphous carbon, graphite, or glassy carbon. In addition to the carbonaceous electrodes, other metal electrodes may be used. The cathode may be a metal electrode made of iron (Fe), nickel, copper (Cu), or a copper-nickel alloy (e.g., Monel™).

[0018] The electrolytic solution contains hydrogen fluoride and a metal fluoride. The type of metal fluoride is not particularly limited, but an alkali metal fluoride is preferred, and at least one of potassium fluoride (KF) and cesium fluoride (CsF) is more preferred. The metal fluorides may be used alone or in combination of two or more. That is, potassium fluoride and cesium fluoride may be used in combination as the metal fluoride. The ratio of the molar amount of hydrogen fluoride to the molar amount of metal fluoride contained in the electrolytic solution ([molar amount of hydrogen fluoride] / [molar amount of metal fluoride]) is preferably 1.6 or more and 3.2 or less, more preferably 1.9 or more and 3.0 or less.

[0019] The electrolyte may be, for example, a mixed molten salt of hydrogen fluoride and potassium fluoride. The molar ratio of hydrogen fluoride to potassium fluoride in the mixed molten salt of hydrogen fluoride and potassium fluoride may be, for example, hydrogen fluoride:potassium fluoride = 1.5 to 2.5: 1. A typical electrolyte is KF·2HF, where the ratio of hydrogen fluoride to potassium fluoride is 2:1, and the melting point of this mixed molten salt is approximately 72°C.

[0020] Furthermore, as an example of the electrolyte, a mixed molten salt of hydrogen fluoride and cesium fluoride can also be used. The molar ratio of hydrogen fluoride to cesium fluoride in the mixed molten salt of hydrogen fluoride and cesium fluoride can be, for example, hydrogen fluoride:cesium fluoride = 1.8 to 3.1:1. A typical electrolyte is CsF·2.4HF when the ratio of hydrogen fluoride to cesium fluoride is 2.4:1, and the melting point of this mixed molten salt is approximately 16°C. Because this electrolyte is corrosive, it is preferable that the parts that come into contact with the electrolyte, such as the inner surface of the electrolytic cell, be made of a metal such as iron, nickel, or Monel (trademark).

[0021] Because hydrogen fluoride in the electrolyte is consumed by electrolysis, it is preferable to continuously or intermittently supply hydrogen fluoride to the electrolyte during electrolysis. Hydrogen fluoride may be supplied to the electrolyte on the cathode chamber side of the electrolytic cell, or to the electrolyte on the anode chamber side. Taking the hydrogen fluoride concentration in a KF·2HF electrolyte (hydrogen fluoride concentration: 40.4 mass%) or CsF·2.4HF electrolyte (hydrogen fluoride concentration: 24.0 mass%) as a reference concentration, the hydrogen fluoride concentration in the electrolyte is preferably controlled to vary within a range of −5 mass% to +5 mass% of the reference concentration, more preferably within a range of −2.5 mass% to +2.5 mass% of the reference concentration, and even more preferably within a range of −1.5 mass% to +1.5 mass% of the reference concentration.

[0022] During electrolysis of the electrolyte, a direct current is applied to the anode and the cathode, and a gas containing fluorine gas is generated at the anode, and a gas containing hydrogen gas is generated at the cathode. Furthermore, because hydrogen fluoride in the electrolyte has a vapor pressure, the gases generated at the anode and the cathode are each accompanied by hydrogen fluoride. Furthermore, in the production of fluorine gas by electrolysis of the electrolyte, the gas generated by electrolysis contains a mist of the electrolyte. Therefore, the gas phase of the electrolytic cell consists of the gas generated by electrolysis, hydrogen fluoride, and a mist of the electrolyte. Therefore, what is sent from the inside of the electrolytic cell to the outside consists of the gas generated by electrolysis, hydrogen fluoride, and a mist of the electrolyte, and in the present invention, this is referred to as a "fluid."

[0023] The main reason why mist is generated during electrolysis of the electrolyte is as follows: The temperature of the electrolyte during electrolysis is adjusted to, for example, 80 to 100°C. Since the melting point of KF-2HF is 71.7°C, the electrolyte is in a liquid state when adjusted to this temperature. Gas bubbles generated at both electrodes of the electrolytic cell rise in the electrolyte and burst at the liquid surface of the electrolyte. At this time, part of the electrolyte is released into the gas phase.

[0024] Because the temperature of the gas phase is lower than the melting point of the electrolyte, the released electrolyte changes phase to a very fine powder-like state. This powder is thought to be a mixture of potassium fluoride and hydrogen fluoride, KF·nHF. This powder becomes mist along with the flow of other gases generated, forming the fluid generated in the electrolytic cell. This mist is difficult to effectively remove using ordinary measures such as installing filters due to its adhesiveness.

[0025] Furthermore, although the amount generated is small, a fine powder of an organic compound may be generated as a mist due to a reaction between the carbonaceous electrode serving as the anode and fluorine gas generated by electrolysis. More specifically, contact resistance often occurs in the portion supplying current to the carbonaceous electrode, and the portion may become hotter than the temperature of the electrolyte due to Joule heat. Therefore, a reaction between the carbon forming the carbonaceous electrode and fluorine gas may generate a soot-like organic compound CFx as a mist.

[0026] The average particle size of the mist contained in the fluid is not particularly limited, but may be 3 μm or less. The average particle size of the mist contained in the fluid can be measured by a measuring device that measures the average particle size by a light scattering method. A measuring device that measures the average particle size by a light scattering method is preferred because it can measure the average particle size of the mist in the fluid flowing through a flow path such as a pipe while the fluorine gas production apparatus is continuously operating.

[0027] The type of measuring device for measuring average particle diameter using the light scattering method is not particularly limited. Laser light emitted from a light source is irradiated onto the fluid inside the pipe. At this time, if a light-reflecting substance such as mist is present in the fluid, the laser light is reflected and scattered. A portion of the scattered light generated when the laser light is scattered by the mist is detected by a photodetector. At this time, the average particle diameter of the mist can be determined from the information obtained from the scattered light. Note that the average particle diameter obtained here is the number-average particle diameter. An example of a measuring device for measuring average particle diameter using the light scattering method is the aerosol spectrometer Welas (registered trademark) Digital 2000 manufactured by PALAS.

[0028] The amount of mist generated during electrolysis of an electrolyte is thought to be affected by the size of gas bubbles generated at the electrodes by electrolysis when they burst on the surface of the electrolyte, the viscosity of the electrolyte, etc. The inventors investigated whether the amount of mist generated could be reduced by adding an additive to the electrolyte, and found that the amount of mist generated could be reduced by adding metal hexafluoronickel(IV) acid, leading to the completion of the present invention.

[0029] That is, the electrolyte contains hydrogen fluoride, a metal fluoride, and a metal hexafluoronickel(IV) salt, and can be obtained by mixing hydrogen fluoride, a metal fluoride, and a metal hexafluoronickel(IV) salt. The type of metal hexafluoronickel(IV) salt is not particularly limited, but examples include potassium hexafluoronickel(IV) (KNiF), cesium hexafluoronickel(IV) (CsNiF), and rubidium hexafluoronickel(IV) (RbNiF). One type of metal hexafluoronickel(IV) salt may be used alone, or two or more types may be used in combination.

[0030] The metal hexafluoronickelate (IV) may be commercially available or prepared by mixing potassium fluoride, cesium fluoride, or rubidium fluoride (RbF) with nickel fluoride (NiF) in a molar ratio of 2:1 and treating the mixture in a fluorine gas atmosphere at a temperature of 250° C. to 450° C.

[0031] The following description will be given taking as an example a case where potassium hexafluoronickelate (IV) is used as an additive to the electrolyte, but it goes without saying that the same applies to a case where cesium hexafluoronickelate (IV) or rubidium hexafluoronickelate (IV) is used as an additive to the electrolyte.

[0032] Because potassium hexafluoronickelate (IV) is an oxidizing solid, it reacts with water to convert to potassium fluoride salt of trivalent nickel (KNiF) or potassium fluoride salt of divalent nickel (KNiF). Potassium pentafluoronickelate (III) (KNiF) and potassium tetrafluoronickelate (II) (KNiF) have lower solubility in the electrolyte than potassium hexafluoronickelate (IV). Therefore, to prevent a decrease in the effect of reducing the amount of mist generated, it is preferable to use potassium hexafluoronickelate (IV) with a low water content as an additive. The water content of potassium hexafluoronickelate (IV) is preferably 0.5% by mass or less, and more preferably 0.3% by mass or less.

[0033] If the water content of potassium hexafluoronickelate (IV) is high, the effect of reducing the amount of mist generated will be reduced. In addition, the water content in the electrolyte will increase, which may increase the amount of electrolysis by-products such as oxygen gas (O), carbon dioxide (CO), and carbon tetrafluoride (CF).

[0034] The method for adding potassium hexafluoronickelate (IV) to the electrolyte is not particularly limited, but the electrolyte may be prepared by mixing a metal fluoride with liquid hydrogen fluoride in which potassium hexafluoronickelate (IV) has been dissolved, or by mixing solid potassium hexafluoronickelate (IV) with a mixture of hydrogen fluoride and a metal fluoride. Furthermore, a predetermined amount of potassium hexafluoronickelate (IV) may be added all at once, or may be added in portions.

[0035] The addition of potassium hexafluoronickelate (IV) causes nickel (IV) ions to be present in the electrolyte, and the concentration of nickel (IV) ions in the electrolyte is preferably 100 mass ppm or more and 1000 mass ppm or less, and more preferably 200 mass ppm or more and 800 mass ppm or less. If the concentration of nickel (IV) ions in the electrolyte is within the above numerical range, the effect of reducing the amount of mist generated is excellent.

[0036] The concentration of nickel (IV) ions in the electrolyte can be measured by inductively coupled plasma (ICP) atomic emission spectroscopy. During electrolysis, nickel (IV) ions in the electrolyte are oxidized and reduced at the anode and cathode, or adsorbed to the anode formed of a carbon material, which can decrease the concentration of nickel (IV) ions in the electrolyte. Therefore, it is preferable to periodically measure the concentration of nickel (IV) ions in the electrolyte to control the concentration of nickel (IV) ions in the electrolyte within a predetermined range.

[0037] The interior of an electrolytic cell is partitioned into an anode chamber in which an anode is placed and a cathode chamber in which a cathode is placed. In some electrolytic cells, the electrolyte solution contained in the anode chamber and the electrolyte solution contained in the cathode chamber are not separated, allowing the electrolyte solutions contained in both chambers to mix freely, and in other cases, the electrolyte solutions contained in both chambers are separated by a diaphragm, making it difficult for them to mix.

[0038] When the interior of the electrolytic cell is designed to allow the electrolyte solutions contained in both the electrode chambers to mix freely, potassium hexafluoronickelate (IV) may be contained in either the electrolyte solution contained in the anode chamber or the electrolyte solution contained in the cathode chamber. On the other hand, when the electrolyte solutions contained in both the electrode chambers are separated by a diaphragm and are designed to make mixing difficult, it is preferable that potassium hexafluoronickelate (IV) be contained only in the electrolyte solution contained in the anode chamber.

[0039] If the concentration of nickel (IV) ions in the electrolyte becomes too low, the effect of reducing the amount of mist generated may be reduced. In order to suppress the decrease in the concentration of nickel (IV) ions in the electrolyte, it is preferable that the concentrations of iron ions and copper ions present in the electrolyte be as low as possible. For example, the concentration of iron ions in the electrolyte is preferably 500 mass ppm or less, more preferably 300 mass ppm or less. Furthermore, the concentration of copper ions in the electrolyte is preferably 200 mass ppm or less, more preferably 100 mass ppm or less. Note that, examples of types of iron ions include divalent iron ions and trivalent iron ions, and examples of types of copper ions include monovalent copper ions and divalent copper ions.

[0040] If the components constituting the electrolytic cell and immersed in the electrolytic solution contain iron, which is a source of iron ions, or copper, which is a source of copper ions, they will dissolve in the electrolytic solution unless they are cathodic protected. Therefore, it is preferable not to use materials containing iron or copper for the components constituting the electrolytic cell and immersed in the electrolytic solution. If cathodic protection is provided, there is no particular problem.

[0041] The present invention will be described in more detail below with reference to examples and comparative examples. [Comparative Example A] The interior of the electrolytic cell is partitioned by a partition wall into an anode chamber containing an anode and a cathode chamber containing a cathode. Sixteen amorphous carbon electrodes (30 cm wide, 45 cm long, and 5 cm thick) manufactured by SGL Carbon Co., Ltd. are installed as anodes, and nickel punched plates are installed as cathodes. The electrolytic cell is electrically connected to the cathode for cathodic protection, and is therefore made of mild steel. The partition wall separating the anode chamber and cathode chamber is also made of nickel.

[0042] 560 L of electrolyte (molten salt) prepared by mixing 434 kg of hydrogen fluoride and 630 kg of potassium fluoride was placed inside the electrolytic cell. Then, the anode and cathode were immersed in the electrolyte. The electrolysis temperature was controlled to 85 to 95°C. First, the temperature of the electrolyte was set to 85°C, and the current density was set to 0.036 A / cm. 2Electrolysis was initiated by applying a direct current of 1000 A to the anode and cathode at 100 kA, and a break-in operation was carried out until the cumulative current flow reached 100 kAh. The break-in operation refers to an operation in which electrolysis is carried out at a relatively low current density in order to remove moisture from the electrolyte and to allow the surfaces of the carbonaceous electrodes to become familiar with the electrolyte.

[0043] After the break-in period is over, the current density is reduced to 0.006 A / cm 2 to 0.079 A / cm 2 Electrolysis was carried out while changing the temperature from 0 to 100°C, and fluorine gas generated from the anode and hydrogen gas generated from the cathode were separated to obtain fluorine gas. The amount (number and volume) and particle size of mist in the fluorine gas were then measured using an aerosol spectrometer, Welas (registered trademark) Digital 2000, manufactured by PALAS.

[0044] The results are shown in Table 1. Table 1 lists the number of mist particles contained in the fluorine gas (number per unit volume) and the total volume of the mist contained in the fluorine gas (volume per unit volume). Graphs of the results shown in Table 1 are shown in Figures 1 and 2. The total volume of the mist was calculated using the particle size distribution of the mist obtained by this measurement. The total volume of the mist was also calculated assuming that the mist was spherical. When the current density was 0.06 to 0.07 A / cm 2 The particle size distribution of the mist generated when the above condition is met is shown in the graph of FIG.

[0045] After the mist measurement was completed, 100 g of the dissolved electrolyte was sampled from the electrolytic cell. The dissolved electrolyte was transparent and solidified into a white solid. The concentration of nickel (IV) ions in this electrolyte was measured by inductively coupled plasma atomic emission spectroscopy and found to be 30 ppm by mass. It was assumed that the dissolved nickel (IV) ions were dissolved in the electrolyte due to corrosion of the nickel forming the partition wall.

[0046]

[0047] [Example A] 3.0 kg of potassium hexafluoronickelate (IV) was added to the electrolyte, and after the same break-in operation as in Comparative Example A, the current density was set to 0.027 A / cm 2 to 0.119 A / cm 2 Electrolysis was carried out in the same manner as in Comparative Example A, except that electrolysis was carried out while changing the current density from 0.06 to 0.07 A / cm, and fluorine gas was obtained. Then, the amount (number and volume) of mist in the fluorine gas and the particle size were measured in the same manner as in Comparative Example A. The results are shown in Table 2. The results shown in Table 2 are graphed in Figures 1 and 2, and are shown in the graphs for the current density of 0.06 to 0.07 A / cm. 2 The particle size distribution of the mist generated when the above condition is met is shown in the graph of FIG.

[0048]

[0049] Potassium hexafluoronickelate (IV) was dissolved by adding 3.0 kg of powder to a dissolved electrolyte maintained at 85°C and leaving it for half a day. After leaving it for half a day to dissolve potassium hexafluoronickelate (IV), 100 g of the dissolved electrolyte was sampled from the electrolytic cell. The dissolved electrolyte was transparent with a slight yellowish tinge and turned pale red when solidified. The concentration of nickel (IV) ions in this electrolyte was measured by inductively coupled plasma atomic emission spectroscopy and was found to be 650 ppm by mass.

[0050] After the break-in was completed, 100 g of the dissolved electrolyte was sampled from the electrolytic cell, and the concentration of nickel (IV) ions in the electrolyte was measured by inductively coupled plasma atomic emission spectroscopy, which was found to be 400 ppm by mass. Although the concentration of nickel (IV) ions had decreased, electrolysis was continued without further addition of potassium hexafluoronickelate (IV).

[0051] As shown in the graph of Figure 1, the number of mist particles increases depending on the current density, indicating that the amount of mist generated increases as the amount of fluorine gas generated increases. It is also clear that when metal hexafluoronickelate (IV) is present, the number of mist particles is less than half of that when it is not present. Furthermore, when comparing the difference in the total volume of mist between the presence and absence of metal hexafluoronickelate (IV), as shown in the graph of Figure 2, when metal hexafluoronickelate (IV) is present, it is less than one-tenth of that when it is not present. This is because the particle size of the generated mist is reduced by the presence of metal hexafluoronickelate (IV).

[0052] Furthermore, from the particle size distribution shown in FIG. 3, it can be seen that the particle size of the maximum number is about 0.25 μm regardless of the presence or absence of metal hexafluoronickel(IV), but the number of mist particles is greater when metal hexafluoronickel(IV) is not present than when it is present.

[0053] Furthermore, from the particle size distribution shown in FIG. 3, it can be seen that when metal hexafluoronickel(IV) is present, mists with particle sizes larger than 1.3 μm are almost not detected, but when metal hexafluoronickel(IV) is not present, mists with particle sizes larger than 1.3 μm are detected.

[0054] Although Fig. 3 shows particle sizes up to 2 µm, when metal hexafluoronickel (IV) acid salt is not present, the maximum particle size of the mist detected was 10 µm. Even if the number of mist particles is small, the amount of mist with a large particle size is large in terms of volume. Therefore, a small total volume of the mist generated has a greater effect on the effect of suppressing clogging of the piping and valves used for supplying fluorine gas than a small number of mist particles. When electrolysis is performed with the addition of metal hexafluoronickel (IV) acid salt, as can be seen from the graph in Fig. 2, the total volume of the generated mist (volume calculated assuming the mist is spherical) reaches 1000 µm. 3 / cm 3 The following fluorine gas can be produced:

[0055] Although the mechanism by which the presence of metal hexafluoronickel(IV) reduces the amount of mist generated is not fully understood, it is thought that the generated fluorine gas bubbles become smaller, and when the bubbles burst on the surface of the electrolyte, they do not burst in a way that generates droplets in the space. Therefore, the additive needs to act on the electrode reaction that generates bubbles at the anode, and also needs to act on the properties of the electrolyte that relate to the bursting of the bubbles, and it is thought that metal hexafluoronickel(IV) satisfies both of these requirements.

[0056] Comparative Example 1: Electrolysis was performed while intermittently supplying hydrogen fluoride to the electrolyte so that the hydrogen fluoride concentration in the electrolyte was 39 to 42% by mass. After the same break-in as in Comparative Example A, the electrolysis was performed at a current density of 0.064 A / cm 2 Electrolysis was carried out in the same manner as in Comparative Example A, except that a direct current of 1780 A was applied to the anode and cathode at 1000 kJ / s, and this was continued until the cumulative amount of current flow reached 20 kAh, to obtain fluorine gas. Then, the amount (number and volume) and particle diameter of the mist in the fluorine gas were measured in the same manner as in Comparative Example A. The measured particle diameters were in the range of 0.18 to 10 μm.

[0057] As a result of the measurement, the number of mists contained in the fluorine gas (number per unit volume) was 43,400 particles / cm 3 The total volume of the mist contained in the fluorine gas (volume per unit volume) was 5000 μm 3 / cm 3 After the mist measurement was completed, 100 g of the dissolved electrolyte was sampled from the electrolytic cell. The dissolved electrolyte was transparent and solidified into a white solid. The concentration of nickel (IV) ions in this electrolyte was measured by inductively coupled plasma atomic emission spectroscopy and was found to be 30 ppm by mass. It was presumed that the dissolved nickel (IV) ions were formed by corrosion of the nickel forming the partition wall and dissolved in the electrolyte.

[0058] Comparative Example 2 Electrolysis was carried out in the same manner as in Comparative Example 1, except that 5 kg of lithium fluoride (LiF) was added to the electrolyte, to obtain fluorine gas. Then, in the same manner as in Comparative Example 1, the amount (number and volume) and particle size of mist in the fluorine gas were measured. The measured particle sizes were in the range of 0.18 to 10 μm. The amount of lithium fluoride added was equivalent to 0.5 mass % of the electrolyte. Lithium fluoride is a substance used as an additive to stabilize the electrolysis voltage when fluorine gas is produced by electrolysis of the electrolyte.

[0059] As a result of the measurement, the number of mists contained in the fluorine gas (number per unit volume) was 38,300 particles / cm 3 The total volume of the mist contained in the fluorine gas (volume per unit volume) was 5190 μm 3 / cm 3 The results of Comparative Examples 1 and 2 show that the addition of lithium fluoride does not reduce the total volume of the mist contained in the fluorine gas.

[0060] Comparative Example 3 Electrolysis was carried out in the same manner as in Comparative Example 2, except that 175 g of nickel fluoride was added instead of lithium fluoride, to obtain fluorine gas. The amount of nickel fluoride added was such that the nickel concentration in the electrolytic solution would be 100 ppm by mass when all of the added nickel fluoride had dissolved to form nickel (II) ions.

[0061] As a result of the measurement, the number of mists contained in the fluorine gas (number per unit volume) was 41,100 / cm 3 The total volume of the mist contained in the fluorine gas (volume per unit volume) was 4870 μm 3 / cm 3 The results of Comparative Examples 1 and 3 show that the addition of nickel fluoride does not reduce the total volume of mist contained in fluorine gas.

[0062] After the mist measurement was completed, 100 g of the dissolved electrolyte was sampled from the electrolytic cell. The dissolved electrolyte was transparent and solidified into a white solid, so it is believed that no tetravalent nickel ions were present. The concentration of nickel (IV) ions in this electrolyte was measured by inductively coupled plasma atomic emission spectroscopy and found to be 95 ppm by mass.

[0063] [Example 1] After the same break-in as in Comparative Example A, electrolysis was performed at a current density of 0.069 A / cm 2 3.0 kg of potassium hexafluoronickel(IV) was added to the electrolyte and electrolysis was carried out to obtain fluorine gas in the same manner as in Example A, except that a direct current was applied to the anode and cathode at 100 kJ / s. Electrolysis was then carried out until the cumulative amount of current flow reached 20 kAh in the same manner as in Comparative Example 1, and the amount (number and volume) and particle diameter of the mist in the fluorine gas were measured. The measured particle diameters were in the range of 0.18 to 10 μm.

[0064] Thereafter, electrolysis was continued for four consecutive days, and the mist was measured once a day. As a result of the measurement, the number of mist particles contained in the fluorine gas (number per unit volume) was 12,800 to 13,700 particles / cm 3 (Average value is 13,300 pieces / cm 3 The total volume of the mist contained in the fluorine gas (volume per unit volume) was 380 to 540 μm 3 / cm 3 (Average value is 460 μm 3 / cm 3 ) Compared with Comparative Example 1, the number of mists was reduced to 1 / 3 or less, and the total volume of the mists was reduced to 1 / 10 or less.

[0065] Example 2 Electrolysis was carried out in the same manner as in Example 1, except that 6.0 kg of potassium hexafluoronickelate (IV) was added to the electrolytic solution (this amount was equal to or greater than the solubility in the electrolytic solution), to obtain fluorine gas. Then, as in Comparative Example 1, electrolysis was carried out until the cumulative amount of current flow reached 20 kAh, and the amount (number and volume) and particle diameter of the mist in the fluorine gas were measured. The measured particle diameters were in the range of 0.18 to 10 μm.

[0066] As a result of the measurement, the number of mists contained in the fluorine gas (number per unit volume) was 13,000 / cm 3 The total volume of the mist contained in the fluorine gas (volume per unit volume) was 480 μm 3 / cm 3 Compared with Comparative Example 1, both the number of mists and the total volume of the mists were significantly reduced.

[0067] The concentration of nickel(IV) ions in the electrolyte at each of the following stages was measured by inductively coupled plasma atomic emission spectroscopy. First, potassium hexafluoronickelate(IV) was dissolved in the electrolyte and left at 85°C for half a day, after which 100 g of the dissolved electrolyte was sampled from the electrolytic cell. The dissolved electrolyte was transparent with a slight yellowish tinge and turned pale red when solidified. The concentration of nickel(IV) ions in this electrolyte was measured by inductively coupled plasma atomic emission spectroscopy and was found to be 670 ppm by mass. The concentration of nickel(IV) ions in the electrolyte saturated with potassium hexafluoronickelate(IV) was expected to be 650 to 700 ppm by mass.

[0068] After the break-in period, 100 g of the dissolved electrolyte was sampled from the electrolytic cell, and the concentration of nickel (IV) ions was measured by inductively coupled plasma atomic emission spectroscopy, which was 650 ppm by mass. This result indicates that there was no decrease in the concentration of nickel (IV) ions due to the break-in period.

Claims

1. A method for producing fluorine gas, comprising an electrolysis step of electrolyzing an electrolyte solution using an anode and a cathode in an electrolytic cell to generate fluorine gas, the electrolyte solution containing hydrogen fluoride, a metal fluoride, and a metal salt of hexafluoronickel(IV), the anode being a nickel electrode or a carbonaceous electrode, and the cathode being a metal electrode.

2. The method for producing fluorine gas according to claim 1, wherein the metal salt of hexafluoronickel(IV) is at least one of potassium hexafluoronickel(IV), cesium hexafluoronickel(IV), and rubidium hexafluoronickel(IV).

3. A method for producing fluorine gas according to claim 1 or 2, wherein the concentration of nickel (IV) ions in the electrolyte is 100 ppm by mass or more and 1000 ppm by mass or less.

4. A method for producing fluorine gas according to claim 1 or 2, wherein the metal fluoride is at least one of potassium fluoride and cesium fluoride.

5. A method for producing fluorine gas according to claim 1 or 2, wherein the ratio of the molar amount of said hydrogen fluoride to the molar amount of said metal fluoride contained in said electrolyte is 1.6 or more and 3.2 or less.

6. A method for producing fluorine gas according to claim 1 or 2, wherein the cathode is an electrode formed from at least one of iron, nickel, copper, and a copper-nickel alloy.

7. A method for producing fluorine gas as described in claim 1 or 2, wherein the electrolyte is a mixture of the hydrogen fluoride, the metal fluoride, and the metal salt of hexafluoronickel (IV) acid having a water content of 0.5 mass% or less.

8. A method for producing fluorine gas according to claim 1 or 2, wherein the concentration of iron ions in the electrolyte is 500 ppm by mass or less and the concentration of copper ions is 200 ppm by mass or less.

Citation Information

Patent Citations

  • Dewatering process of fluorine hydride

    CN101423194A

  • Anode for electrolytic synthesis and method for manufacturing fluorine gas or fluorine-containing compound

    WO2020026854A1

  • Fluorine gas production method and fluorine gas production apparatus

    WO2021131579A1