Positive electrode for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery
The positive electrode for non-aqueous electrolyte secondary batteries, featuring a lithium-containing transition metal composite oxide coated with a sulfonic acid compound and specific additives, addresses the issue of increased reaction resistance and cycle deterioration by protecting the electrode from hydrogen fluoride, resulting in improved battery performance.
Patent Information
- Application Number
- PCT/JP2024/013954
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-04
- Publication Date
- 2024-10-31
AI Technical Summary
Lithium-containing transition metal composite oxides with high Ni content used as positive electrode active materials in non-aqueous electrolyte secondary batteries experience increased reaction resistance and deteriorated cycle characteristics due to side reactions with the electrolyte, leading to hydrogen fluoride deposition and elution, which affects battery performance.
A positive electrode comprising a lithium-containing transition metal composite oxide with a layered structure, coated with a sulfonic acid compound and containing additives such as P, Ca, Sr, B, Zr, Er, Ti, or Al, which reduces reaction resistance and protects the electrode from hydrogen fluoride by allowing it to react preferentially with the additives.
The proposed solution effectively reduces reaction resistance and improves cycle characteristics by shielding the lithium-containing transition metal composite oxide from hydrogen fluoride, thereby enhancing the battery's performance and longevity.
Smart Images

Figure JP2024013954_31102024_PF_FP_ABST
Abstract
Description
Positive electrode for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery
[0001] The present disclosure relates to a positive electrode for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery.
[0002] In recent years, the use of non-aqueous electrolyte secondary batteries has expanded to include power sources for electric vehicles and energy storage devices for utilizing natural energy. Because the positive electrode significantly affects battery characteristics, including battery capacity, output characteristics, and cycle characteristics, much research has been conducted on the positive electrode. For example, Patent Document 1 discloses a positive electrode for a non-aqueous electrolyte secondary battery that uses, as a positive electrode active material, a lithium-containing transition metal composite oxide in which a compound containing elements such as zirconium (Zr), titanium (Ti), and aluminum (Al) is present at the particle interface, with the aim of improving cycle characteristics. Furthermore, Patent Document 2 discloses a positive electrode for a non-aqueous electrolyte secondary battery that uses, as a positive electrode active material, a lithium-containing transition metal composite oxide in which a low-solubility Li salt is dotted on the surface, with the aim of reducing reaction resistance during storage at high temperatures.
[0003] JP 2022-113728 A JP 2019-169286 A
[0004] In recent years, lithium-containing transition metal composite oxides with a high Ni content have been attracting attention as a positive electrode active material that can realize high battery capacity. However, when a lithium-containing transition metal composite oxide with a high Ni content is used as a positive electrode active material, highly reactive Ni is formed on the particle surface of the composite oxide at a high state of charge (SOC). 4+ Since a large amount of hydrogen fluoride is present, a side reaction between the lithium-containing transition metal composite oxide and the electrolyte is likely to occur. Then, hydrogen fluoride generated by the side reaction reacts with the lithium-containing transition metal composite oxide, and the product is deposited on the surface of the lithium-containing transition metal composite oxide, or the transition metal is eluted from the lithium-containing transition metal composite oxide. As a result, the reaction resistance of the battery increases, and the charge-discharge cycle characteristics deteriorate.
[0005] A positive electrode for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core. The positive electrode mixture layer includes a positive electrode active material and an additive. The positive electrode active material includes a lithium-containing transition metal composite oxide having a layered structure, and the lithium-containing transition metal composite oxide is represented by the general formula Li x Ni a Co b Mn c M d O 2-y (wherein 0.8<x<1.2, 0.75≦a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr), and the secondary particles are formed by aggregation of primary particles, and the sulfonic acid compound represented by formula (I) is present on the surface of the secondary particles, and the additive contains a compound containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, Ti, and Al. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)
[0006] A non-aqueous electrolyte secondary battery according to one aspect of the present disclosure includes the above positive electrode, a negative electrode, and a non-aqueous electrolyte.
[0007] According to a positive electrode for a non-aqueous electrolyte secondary battery according to one aspect of the present disclosure, it is possible to provide a non-aqueous electrolyte secondary battery having improved cycle characteristics while reducing the reaction resistance of the battery.
[0008] 1 is a longitudinal cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment of the present invention;
[0009] As described above, lithium-containing transition metal composite oxides with a high Ni content are prone to side reactions with electrolytes, particularly at high SOCs. Therefore, when such composite oxides are used as positive electrode active materials, hydrogen fluoride generated by the side reactions reacts with the lithium-containing transition metal composite oxide, resulting in the deposition of products on the surface of the lithium-containing transition metal composite oxide or the elution of transition metals from the lithium-containing transition metal composite oxide. As a result, the reaction resistance of the battery increases.
[0010] As a result of investigations by the present inventors, it has been found that the reaction resistance of a battery can be reduced by adding a sulfonic acid compound represented by the above formula (I) to the surface of secondary particles of a lithium-containing transition metal composite oxide used as a positive electrode active material. This is thought to be because the reaction resistance at the positive electrode is reduced by the function of the sulfonic acid compound. However, the presence of the sulfonic acid compound has created a new problem: reduced cycle performance at high voltages. This is thought to be because the amount of hydrogen fluoride generated by a side reaction between the lithium-containing transition metal composite oxide and the electrolyte increases during repeated charge and discharge due to the increased reactivity at the positive electrode in addition to the increased potential of the positive electrode.
[0011] The present inventors have further conducted extensive research and found that the presence of a compound containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, Ti, and Al as an additive in the positive electrode mixture layer constituting the positive electrode reduces the reaction resistance of the battery and improves the cycle characteristics. This is presumably because the sulfonic acid compound reduces the reaction resistance in the positive electrode, while hydrogen fluoride generated by a side reaction reacts preferentially with the additive, thereby protecting the lithium-containing transition metal composite oxide from hydrogen fluoride.
[0012] Hereinafter, an example of an embodiment of a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail with reference to the drawings. Note that configurations obtained by selectively combining the components of the multiple embodiments and variations described below are included within the scope of the present disclosure. Note that in this specification, "to" refers to a range that includes the upper and lower limits before and after "to."
[0013] In the following, a cylindrical battery in which a wound electrode assembly 14 is housed in a cylindrical, bottomed exterior body 16 is exemplified as a nonaqueous electrolyte secondary battery; however, the exterior body of the battery is not limited to a cylindrical exterior body. The nonaqueous electrolyte secondary battery according to the present disclosure may be, for example, a prismatic battery with a prismatic exterior body, a coin-type battery with a coin-type exterior body, or a pouch-type battery with an exterior body composed of a laminate sheet including a metal layer and a resin layer. Furthermore, the electrode assembly is not limited to a wound type, but may also be a stacked type electrode assembly in which multiple positive electrodes and multiple negative electrodes are alternately stacked with separators interposed therebetween. Furthermore, the design of the nonaqueous electrolyte secondary battery according to the present disclosure is not limited to the design of the exemplified nonaqueous electrolyte secondary battery, and known nonaqueous electrolyte secondary battery designs may also be applied.
[0014] FIG. 1 is an axial cross-sectional view of a cylindrical nonaqueous electrolyte secondary battery 10 according to an embodiment. As shown in FIG. 1 , the nonaqueous electrolyte secondary battery 10 includes a wound electrode assembly 14, a nonaqueous electrolyte, and an exterior body 16 that accommodates the electrode assembly 14 and the nonaqueous electrolyte. The electrode assembly 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a wound structure in which the positive electrode 11 and the negative electrode 12 are spirally wound with the separator 13 interposed therebetween. The exterior body 16 is a cylindrical metal container with a bottom that is open on one axial side, and the opening of the exterior body 16 is closed by a sealing body 17. Hereinafter, for convenience of explanation, the sealing body 17 side of the battery will be referred to as the top, and the bottom side of the exterior body 16 will be referred to as the bottom.
[0015] The positive electrode 11, negative electrode 12, and separator 13 that make up the electrode assembly 14 are all rectangular, elongated bodies that are spirally wound in the longitudinal direction and stacked alternately in the radial direction of the electrode assembly 14. The separator 13 isolates the positive electrode 11 and the negative electrode 12 from each other. Two separators 13 are arranged, for example, to sandwich the positive electrode 11. The electrode assembly 14 includes a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like. In the electrode assembly 14, the longitudinal direction of the positive electrode 11 and the negative electrode 12 is the winding direction, and the lateral direction of the positive electrode 11 and the negative electrode 12 is the axial direction. That is, the lateral end faces of the positive electrode 11 and the negative electrode 12 form the axial end faces of the electrode assembly 14.
[0016] Insulating plates 18 and 19 are disposed above and below the electrode body 14. In the example shown in Fig. 1 , the positive electrode lead 20 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and the negative electrode lead 21 passes outside the insulating plate 19 and extends toward the bottom side of the exterior body 16. The positive electrode lead 20 is connected to the underside of an internal terminal plate 23 of the sealing body 17 by welding or the like, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the internal terminal plate 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom surface of the exterior body 16 by welding or the like, and the exterior body 16 serves as the negative electrode terminal.
[0017] A gasket 28 is provided between the exterior body 16 and the sealing body 17 to ensure airtightness inside the battery. The exterior body 16 has a grooved portion 22 formed on its side surface that protrudes inward and supports the sealing body 17. The grooved portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior body 16, and supports the sealing body 17 on its top surface. The sealing body 17 is fixed to the top of the exterior body 16 by the grooved portion 22 and the open end of the exterior body 16 that is crimped to the sealing body 17.
[0018] The sealing body 17 has a structure in which, in order from the electrode body 14 side, an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked. Each member constituting the sealing body 17 has, for example, a disk or ring shape, and each member except for the insulating member 25 is electrically connected to one another. The lower valve body 24 and the upper valve body 26 are connected at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0019] The positive electrode 11, the negative electrode 12, the separator 13, and the nonaqueous electrolyte that constitute the nonaqueous electrolyte secondary battery 10 will be described in detail below, with the positive electrode 11 being particularly described below.
[0020] [Positive Electrode] The positive electrode 11 has, for example, a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core. The positive electrode mixture layer is preferably formed on both sides of the positive electrode core. The positive electrode core can be made of a foil of a metal, such as aluminum or an aluminum alloy, that is stable within the potential range of the positive electrode 11, or a film with such a metal disposed on the surface. The thickness of the positive electrode core is, for example, 10 μm to 30 μm.
[0021] The positive electrode mixture layer contains a positive electrode active material and an additive made of a compound containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, Ti, and Al. The thickness of the positive electrode mixture layer is, for example, 10 μm to 150 μm on one side of the positive electrode core.
[0022] The positive electrode active material includes a lithium-containing transition metal composite oxide having a layered structure. The lithium-containing transition metal composite oxide includes secondary particles formed by aggregation of primary particles. The particle size of the primary particles constituting the secondary particles of the lithium-containing transition metal composite oxide is, for example, 0.02 μm to 2 μm. The particle size of the primary particles is measured as the diameter of the circumscribed circle in a particle image observed with a scanning electron microscope (SEM). The average particle size of the secondary particles of the lithium-containing transition metal composite oxide is, for example, 2 μm to 30 μm. Here, the average particle size refers to the volume-based median diameter (D50). D50 refers to the particle size at which the cumulative frequency in the volume-based particle size distribution is 50% from the smallest particle size, and is also referred to as the median diameter. The particle size distribution of the secondary particles of the lithium-containing transition metal composite oxide can be measured using a laser diffraction particle size distribution analyzer (e.g., MT3000II, manufactured by Microtrac-Bell Corporation) using water as a dispersion medium.
[0023] Examples of the layered structure of the lithium-containing transition metal composite oxide include a layered structure belonging to the space group R-3m and a layered structure belonging to the space group C2 / m. From the viewpoints of increasing capacity and stabilizing the crystal structure, the lithium-containing transition metal composite oxide preferably has a layered structure belonging to the space group R-3m. The layered structure of the lithium-containing transition metal composite oxide may include a transition metal layer and a Li layer.
[0024] The lithium-containing transition metal composite oxide has the general formula Li xNi a Co b Mn c M d O 2-y (wherein 0.8<x<1.2, 0.75≦a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr.) The content of the elements constituting the lithium-containing transition metal composite oxide can be measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), or the like.
[0025] By setting the Ni content in the lithium-containing transition metal composite oxide to 75 mol % to 95 mol %, a battery with a high capacity can be obtained. The higher the Ni content, the higher the capacity of the battery.
[0026] The content of Co in the lithium-containing transition metal composite oxide is 0 mol % to 15 mol %, and Co is an optional component. In other words, the lithium-containing transition metal composite oxide does not need to contain Co. By containing Co, the lithium-containing transition metal composite oxide can improve the heat resistance of the battery.
[0027] The content of Mn in the lithium-containing transition metal composite oxide is 0 mol % to 25 mol %, and Mn is an optional component. In other words, the lithium-containing transition metal composite oxide does not necessarily contain Mn. By containing Mn, the lithium-containing transition metal composite oxide can stabilize its crystal structure.
[0028] The content of M (M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr) in the lithium-containing transition metal composite oxide is 0 mol % to 10 mol %, and M is an optional component. In other words, the lithium-containing transition metal composite oxide does not necessarily contain M.
[0029] The sulfonic acid compound represented by formula (I) is present on the surface of the secondary particles of the lithium-containing transition metal composite oxide. In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2. A is preferably a Group 1 element. Among them, Li or Na is more preferable, and Li is particularly preferable. The sulfonic acid compound may be present in the form of dots so as to cover at least a portion of the surface of the secondary particles of the lithium-containing transition metal composite oxide, or may be present so as to cover the entire surface of the secondary particles. Furthermore, the sulfonic acid compound may be present on the surface of the primary particles of the lithium-containing transition metal composite oxide.
[0030] In formula (I), R is preferably an alkyl group. The number of carbon atoms in the alkyl group is preferably 5 or less, more preferably 3 or less. From the viewpoint of reducing reaction resistance, a suitable example of R is an alkyl group having 3 or less carbon atoms, and among these, a methyl group is preferred. In R, some of the hydrogen atoms bonded to the carbon may be substituted with fluorine. In formula (I), n is preferably 1.
[0031] Specific examples of the sulfonic acid compound include lithium methanesulfonate, lithium ethanesulfonate, lithium propanesulfonate, sodium methanesulfonate, sodium ethanesulfonate, magnesium methanesulfonate, lithium fluoromethanesulfonate, etc. Among these, at least one selected from the group consisting of lithium methanesulfonate, lithium ethanesulfonate, and sodium methanesulfonate is preferred, with lithium methanesulfonate being particularly preferred.
[0032] The sulfonic acid compound reduces the reaction resistance in the positive electrode 11, thereby reducing the reaction resistance of the battery. Even a very small amount of sulfonic acid compound can achieve this effect, but it is preferably present on the secondary particle surface of the composite oxide in an amount of 0.05% by mass or more, and more preferably 0.1% by mass or more, relative to the mass of the lithium-containing transition metal composite oxide. The upper limit of the sulfonic acid compound content is not particularly limited, but from the viewpoint of cycle characteristics, 1.5% by mass relative to the mass of the lithium-containing transition metal composite oxide is preferred. Therefore, an example of a suitable range for the amount of sulfonic acid compound is 0.05% by mass to 1.5% by mass relative to the mass of the lithium-containing transition metal composite oxide.
[0033] The presence of the sulfonic acid compound on the surface of the secondary particles of the lithium-containing transition metal composite oxide can be confirmed by Fourier transform infrared spectroscopy (FT-IR). In the infrared absorption spectrum obtained by FT-IR, the positive electrode active material containing lithium methanesulfonate exhibits, for example, a peak at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 It has an absorption peak around 1238 cm -1 , 1175 cm -1 , 1065 cm -1 The peak around 785 cm is due to the SO stretching vibration of lithium methanesulfonate. -1 The peak around 1000 nm is a peak due to the C-S stretching vibration derived from lithium methanesulfonate. Note that the presence of a positive electrode active material containing a sulfonic acid compound other than lithium methanesulfonate can also be confirmed from the absorption peak derived from the sulfonic acid compound in the infrared absorption spectrum.
[0034] The presence of the sulfonic acid compound can also be confirmed by X-ray photoelectron spectroscopy (XPS). In the spectrum obtained by XPS, a peak with a binding energy of approximately 165 to 170 eV and an intensity (c / s) of 200 to 1000 is observed for the positive electrode active material containing lithium methanesulfonate. The presence of the sulfonic acid compound on the secondary particle surface of the lithium-containing transition metal composite oxide can also be confirmed by ICP, atomic absorption spectroscopy, synchrotron XRD measurement, TOF-SIMS, etc.
[0035] The positive electrode active material, which is one example of the embodiment, can be produced by the following method: Note that the production method described here is only an example, and the method for producing the positive electrode active material is not limited to this method.
[0036] The manufacturing process of the positive electrode active material includes a synthesis step of obtaining a lithium-containing transition metal composite oxide, a washing step of washing the lithium-containing transition metal composite oxide obtained in the synthesis step with water and dehydrating it to obtain a cake-like composition, an adding step of adding at least one of a sulfonic acid compound and a sulfonic acid solution to the cake-like composition, and a drying step of drying the cake-like composition to obtain a powder-like composition.
[0037] In the synthesis step, for example, a metal oxide containing 75 mol% to 95 mol% of Ni, 0 mol% to 15 mol% of Co, 0 mol% to 25 mol% of Mn, and 0 mol% to 10 mol% of M (M is at least one element selected from W, Mg, Mo, Nb, Ti, Si, Al, and Zr) is mixed with a Li compound to obtain a mixture.
[0038] The metal oxide can be obtained, for example, by adding an alkaline solution such as sodium hydroxide dropwise to a stirred solution of a metal salt containing Ni and an arbitrary metal element (Co, Mn, M, etc.) to adjust the pH to the alkaline side (e.g., 8.5 to 12.5) to precipitate (co-precipitate) a composite hydroxide containing Ni and the arbitrary metal element, and then heat-treating the composite hydroxide. The heat-treatment temperature is not particularly limited, but is, for example, in the range of 250°C to 600°C.
[0039] Examples of Li compounds include Li 2 CO 3, LiOH, Li 2 O 2 , Li 2 O, LiNO 3 , LiNO 2 , Li 2 SO 4 , LiOH·H 2 Examples of the metal oxide include O, LiH, and LiF. In order to easily adjust each of the above parameters to the ranges specified above, the mixing ratio of the metal oxide and the Li compound is preferably such that the molar ratio of the total amount of metal elements in the metal oxide to Li falls within a range of 1:0.8 to 1:1.2, and more preferably falls within a range of 1.0 to 1.1.
[0040] Next, the synthesis step includes a calcination step in which the resulting mixture is calcined. The calcination step is a multi-stage calcination step that includes at least a first calcination step in which the mixture is calcined at 300°C to 680°C under an oxygen stream, and a second calcination step in which the calcined product obtained by the first calcination step is calcined at a temperature exceeding 680°C under an oxygen stream. In the first calcination step, the temperature is increased to a first set temperature of 680°C or less at a first temperature increase rate of 0.2°C / min to 4.5°C / min. In the second calcination step, the temperature is increased to a second set temperature of 900°C or less at a first temperature increase rate of 0.5°C / min to 3.5°C / min. Note that multiple first and second temperature increase rates may be set for each temperature range as long as they are within the above-specified range.
[0041] The holding time of the first set temperature in the first firing step is preferably 5 hours or less, more preferably 3 hours or less. The holding time of the first set temperature is the time during which the first set temperature is maintained after reaching the first set temperature, and the holding time may be zero. The holding time of the second set temperature in the second firing step is preferably 1 hour to 10 hours, more preferably 1 hour to 5 hours. The holding time of the second set temperature is the time during which the second set temperature is maintained after reaching the second set temperature. The firing of the mixture is carried out, for example, in an oxygen stream with an oxygen concentration of 60% or more, and the flow rate of the oxygen stream is set to 10 cm / min. 3 The flow rate shall be 0.2 mL / min to 4 mL / min per kg of the mixture or 0.3 L / min or more per kg of the mixture.
[0042] The synthesis step is not limited to the above steps, and may include, for example, a known synthesis method in which a precursor obtained by co-precipitating or mixing a compound such as a hydroxide, oxide, or carbonate containing at least one element selected from Ni, Co, Mn, and M (M is at least one element selected from W, Mg, Mo, Nb, Ti, Si, Al, and Zr) is mixed with a Li source and fired to obtain a lithium-containing transition metal composite oxide. When the precursor does not contain a compound such as M, these compounds such as M may be mixed and fired when the precursor and Li source are mixed and fired. Furthermore, these compounds may be pulverized to appropriately change the particle shape or particle size, or may be used after adjusting the water content by including a hydrate.
[0043] In the washing step, the lithium-containing transition metal composite oxide is washed with water and dehydrated to obtain a cake-like composition. The particulate lithium-containing transition metal composite oxide obtained in the synthesis step can be used. By washing with water, unreacted lithium compounds added in the synthesis step and impurities other than the lithium compounds can be removed. When washing with water, for example, 300 g to 5000 g of lithium-containing transition metal composite oxide is added to 1 L of water. Note that water washing may be repeated multiple times. Dehydration after water washing can be performed, for example, using a filter press.
[0044] In the addition step, at least one of a sulfonic acid compound and a sulfonic acid solution is added to the cake-like composition obtained in the washing step. This allows the sulfonic acid compound to adhere to the surface of the lithium-containing transition metal composite oxide. The sulfonic acid compound may be in either powder or solution form. The sulfonic acid solution is, for example, a methanesulfonic acid solution obtained by dissolving methanesulfonic acid in water. Li compounds remain in the cake-like composition, and these remaining Li compounds are dissolved in the water contained in the cake-like composition. Therefore, even when the sulfonic acid solution is added, a Li-containing sulfonic acid compound is formed. From the viewpoint of more easily achieving the effects of the present application, a Li compound or a Li compound solution may be added to the cake-like composition together with the sulfonic acid solution, or a mixed solution obtained by premixing the sulfonic acid solution with the Li compound or the Li compound solution may be added to the cake-like composition. The Li compound is, for example, LiOH, and the Li compound solution is, for example, a LiOH solution obtained by dissolving LiOH in water. The amounts of the Li compound and sulfonic acid solution added to the cake-like composition preferably satisfy the relationship of 0≦Li compound / sulfonic acid≦1.3 in molar ratio. The amount of sulfonic acid compound or sulfonic acid added is preferably 0.05% by mass to 1.5% by mass, and more preferably 0.1% by mass to 1.0% by mass, relative to the mass of the lithium-containing transition metal composite oxide. The concentrations of the sulfonic acid solution and the sulfonic acid compound solution are, for example, 0.5% by mass to 40% by mass.
[0045] In the drying step, the cake-like composition obtained in the washing step is dried to obtain a powdery composition. The drying step may be performed in a vacuum atmosphere. The drying conditions are, for example, 150°C to 400°C and 0.5 hours to 15 hours.
[0046] The additive contained in the positive electrode mixture layer includes a compound containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, Ti, and Al. The additive is present, for example, in particulate form in the gaps between the positive electrode active materials. The additive is highly reactive with hydrogen fluoride and therefore reacts preferentially with hydrogen fluoride produced by decomposition of the non-aqueous electrolyte. As a result, the lithium-containing transition metal composite oxide can be protected from hydrogen fluoride.
[0047] The additive is, for example, a compound containing at least one of phosphate, sulfate, oxide, hydroxide, and chloride containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, and Al. 3 P.O. 4 , CaO, CaCl 2 , Ca(OH) 2 , SrO, SrCl 2 , Sr(OH) 2 , B 2 O 3 , B(OH) 3 , ZrSO 4 , ZrO 2 , ZrF 4 , Er 2 (SO 4 ) 3 , TiO 2 , Ti(OH) 4 , Al 2 O 3 , Al(OH) 3 , AlPO 4 , AlF 3 The additives may be used singly or in combination of two or more. These compounds may be pulverized to appropriately change the particle shape or particle size, or may be used as hydrates with the water content adjusted.
[0048] The amounts of P, Ca, Sr, B, Zr, Er, Ti, and Al contained in the additives in the positive electrode mixture layer are preferably 0.001% by mass to 1% by mass, and more preferably 0.01% by mass to 1% by mass, relative to the total mass of the positive electrode active material. In this case, the effects of the present disclosure are more pronounced. When multiple additives are used, it is preferable that the total amount of P, Ca, Sr, B, Zr, Er, Ti, and Al contained in all the additives falls within the above range. Furthermore, the content of the additives may vary in the thickness direction of the positive electrode mixture layer, but is preferably approximately the same throughout the thickness direction of the positive electrode mixture layer.
[0049] The presence of the additive can be confirmed by synchrotron radiation XRD measurement, X-ray photoelectron spectroscopy (XPS), time-of-flight secondary ion mass spectrometry (TOF-SIMS), or the like.
[0050] The positive electrode mixture layer contains, in addition to the positive electrode active material and the additive, for example, a conductive agent and a binder. Examples of the conductive agent contained in the positive electrode mixture layer include carbon black (CB) such as acetylene black (AB) and ketjen black, carbon nanotubes (CNT), graphene, graphite, and other carbon-based particles. These may be used alone or in combination of two or more.
[0051] Examples of binders contained in the positive electrode mixture layer include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyimide-based resins, acrylic-based resins, polyolefin-based resins, polyacrylonitrile (PAN), etc. These may be used alone or in combination of two or more.
[0052] The positive electrode 11, which is an example of the embodiment, can be produced, for example, through a production process of producing a positive electrode active material, a preparation process of preparing a positive electrode slurry containing the positive electrode active material, a conductive agent, and a binder, a coating process of applying the positive electrode slurry to the surface of a positive electrode core and drying it, and a rolling process of rolling the coating film produced in the coating process. Here, an additive is added in the preparation process, which allows the additive to be dispersed in the positive electrode mixture layer.
[0053] [Negative Electrode] The negative electrode 12 may have, for example, a negative electrode core and a negative electrode mixture layer formed on the surface of the negative electrode core, or a metal Li foil may be used as the negative electrode 12. Alternatively, the negative electrode 12 may have a negative electrode core, and lithium metal may be deposited on the surface of the negative electrode core upon charging. When the negative electrode 12 has a negative electrode mixture layer, the negative electrode mixture layer is preferably formed on both sides of the negative electrode core. The negative electrode core may be made of a foil of a metal that is stable within the potential range of the negative electrode 12, such as copper or a copper alloy, or a film with such a metal disposed on the surface layer. The thickness of the negative electrode core is, for example, 5 μm to 30 μm. The negative electrode mixture layer includes, for example, a negative electrode active material and a binder. The thickness of the negative electrode mixture layer is, for example, 10 μm to 150 μm on one side of the negative electrode core. The negative electrode 12 can be produced, for example, by applying a negative electrode mixture slurry containing a negative electrode active material, a binder, etc. to the surface of a negative electrode core, drying the coating, and then rolling it to form a negative electrode mixture layer on both sides of the negative electrode core.
[0054] The negative electrode active material contained in the negative electrode mixture layer is not particularly limited as long as it can reversibly absorb and release lithium ions, and generally, carbon materials such as graphite are used. Graphite may be any of natural graphite such as flake graphite, lump graphite, and amorphous graphite, or artificial graphite such as lump artificial graphite and graphitized mesophase carbon microbeads. Furthermore, metals that alloy with Li, such as Si and Sn, metal compounds containing Si, Sn, and lithium-titanium composite oxides may also be used as the negative electrode active material. Furthermore, those provided with a carbon coating may also be used. For example, SiO x (0.5≦x≦1.6) or Li 2y SiO (2+y) A Si-containing compound in which fine particles of Si are dispersed in a lithium silicate phase represented by (0<y<2) may be used in combination with graphite.
[0055] Examples of binders contained in the negative electrode mixture layer include styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more.
[0056] [Separator] A porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have a single-layer structure or a multi-layer structure. Furthermore, a highly heat-resistant resin layer such as an aramid resin may be formed on the surface of the separator 13.
[0057] A filler layer containing an inorganic filler may be formed at the interface between the separator 13 and at least one of the positive electrode 11 and the negative electrode 12. Examples of inorganic fillers include oxides and phosphate compounds containing metal elements such as Ti, Al, Si, and Mg. The filler layer can be formed by applying a slurry containing the filler to the surface of the positive electrode 11, the negative electrode 12, or the separator 13.
[0058] [Non-aqueous electrolyte] The non-aqueous electrolyte has ion conductivity (for example, lithium ion conductivity). The non-aqueous electrolyte may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.
[0059] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent that can be used include esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these. The non-aqueous solvent may contain a halogen-substituted compound in which at least a portion of the hydrogen atoms in these solvents are substituted with halogen atoms such as fluorine. Examples of the halogen-substituted compound include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, and fluorinated chain carboxylic acid esters such as methyl fluoropropionate (FMP).
[0060] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylic acid esters such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).
[0061] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, and methyl phenyl ether. and chain ethers such as ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.
[0062] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiClO 4 , LiBF 4 , LiPF 6 , LiAlCl 4 , LiSbF 6 , LiSCN, LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiB 10 Cl 10 , lower aliphatic lithium carboxylates, LiCl, LiBr, LiI, phosphates, borates, and imide salts. Examples of phosphates include lithium difluorophosphate (LiPO 2 F 2Examples of the borate salt include lithium bis(oxalato)borate (LiBOB) and lithium difluoro(oxalato)borate (LiDFFOB). Examples of the imide salt include lithium bisfluorosulfonylimide (LiN(FSO 2 ) 2 ), lithium bistrifluoromethanesulfonyl imide (LiN(CF 3 SO 2 ) 2 ), lithium trifluoromethanesulfonate nonafluorobutanesulfonate imide (LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 )), lithium bispentafluoroethanesulfonyl imide (LiN(C 2 F 5 SO 2 ) 2 Among these, LiPF is preferred from the viewpoint of ionic conductivity, electrochemical stability, etc. 6 The concentration of the lithium salt may be, for example, 4 mol or less, or 3 mol or less, preferably 1.8 mol or less, and more preferably 0.8 mol to 1.8 mol per liter of the non-aqueous solvent.
[0063] The non-aqueous electrolyte may contain an additive such as an unsaturated carbonate ester, an acid anhydride, a phenol compound, a benzene compound, a nitrile compound, an isocyanate compound, a sultone compound, a sulfate compound, a borate ester compound, a phosphate ester compound, or a phosphite ester compound.
[0064] Examples of unsaturated cyclic carbonates include vinylene carbonate, 4-methylvinylene carbonate, 4,5-dimethylvinylene carbonate, 4-ethylvinylene carbonate, 4,5-diethylvinylene carbonate, 4-propylvinylene carbonate, 4,5-dipropylvinylene carbonate, 4-phenylvinylene carbonate, 4,5-diphenylvinylene carbonate, vinylethylene carbonate, and divinylethylene carbonate. One type of unsaturated cyclic carbonate may be used alone, or two or more types may be used in combination. Some of the hydrogen atoms in the unsaturated cyclic carbonate may be substituted with fluorine atoms. The acid anhydride may be an anhydride formed by intermolecular condensation of multiple carboxylic acid molecules, but is preferably an acid anhydride of a polycarboxylic acid. Examples of polycarboxylic acid anhydrides include succinic anhydride, maleic anhydride, and phthalic anhydride.
[0065] Examples of phenolic compounds include phenol, hydroxytoluene, etc. Examples of benzene compounds include fluorobenzene, hexafluorobenzene, cyclohexylbenzene (CHB), etc.
[0066] Examples of nitrile compounds include adiponitrile, pimelonitrile, propionitrile, and succinonitrile. Examples of isocyanate compounds include methyl isocyanate (MIC), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), and bisisocyanatomethylcyclohexane (BIMCH). Examples of sultone compounds include propane sultone and propene sultone. Examples of sulfate compounds include ethylene sulfate, ethylene sulfite, dimethyl sulfate, and lithium fluorosulfate. Examples of borate ester compounds include trimethyl borate and tris(trimethylsilyl)borate. Examples of phosphate ester compounds include trimethyl phosphate and tris(trimethylsilyl)phosphate. Examples of phosphite ester compounds include trimethyl phosphite and tris(trimethylsilyl)phosphite.
[0067] As the solid electrolyte, for example, a solid or gel-like polymer electrolyte, an inorganic solid electrolyte, etc. can be used. As the inorganic solid electrolyte, a material known in all-solid-state lithium ion secondary batteries, etc. (for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a halogen-based solid electrolyte, etc.) can be used. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. As the matrix polymer, for example, a polymer material that absorbs the non-aqueous solvent and gels is used. As the polymer material, for example, a fluororesin, an acrylic resin, a polyether resin, etc. can be used.
[0068] Hereinafter, the present disclosure will be further described with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.
[0069] Example 1 Preparation of Positive Electrode Active Material [Ni 0.90 Co 0.05 Al 0.05 ](OH) 2The composite hydroxide represented by the formula (1) was calcined at 500°C for 8 hours to obtain a metal oxide containing Ni, Co, and Al. Next, lithium hydroxide monohydrate (LiOH·H) was added to the composite hydroxide represented by the formula (1) so that the molar ratio of Li to the total amount of Ni, Co, and Al was 1:1.03. 2 O) was mixed to obtain a mixture. Then, this mixture was placed under an oxygen flow (10 cm) with an oxygen concentration of 95%. 3 The mixture was heated from room temperature to 650°C at a temperature increase rate of 2.0°C / min under a temperature of 2 mL / min per kg of the mixture and 5 L / min per kg of the mixture, and then heated from 650°C to 740°C at a temperature increase rate of 0.5°C / min to obtain a lithium-containing transition metal composite oxide (synthesis step).
[0070] Water was added to the obtained lithium-containing transition metal composite oxide so that the slurry concentration was 1500 g / L, and the mixture was stirred for 15 minutes and filtered to obtain a cake-like composition (washing step). Powdered lithium methanesulfonate was then added to the obtained cake-like composition (addition step). The amount of lithium methanesulfonate added was 0.3 mass% relative to the total mass of the lithium-containing transition metal composite oxide. The obtained cake-like composition was then dried under vacuum at 180°C for 2 hours to obtain the positive electrode active material of Example 1 (drying step). The prepared positive electrode active material was then measured by Fourier transform infrared spectroscopy (FT-IR), confirming the presence of lithium methanesulfonate on the surfaces of the secondary particles of the lithium-containing transition metal composite oxide.
[0071] [Fabrication of Positive Electrode] The positive electrode active material, acetylene black (AB), and polyvinylidene fluoride were mixed in a mass ratio of 86:10:4, and TiO 2 was added, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode mixture slurry. 2 The mass of Ti was added so that it was 0.08 mass% relative to the total mass of the positive electrode active material. Next, the positive electrode mixture slurry was applied to a positive electrode core made of aluminum foil, the coating was dried and compressed, and then the positive electrode core was cut to a predetermined electrode size to obtain a positive electrode having a positive electrode mixture layer disposed on both sides of the positive electrode core. Note that an exposed portion was provided in a part of the positive electrode where the surface of the positive electrode core was exposed.
[0072] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF 6 ) was dissolved in the solution to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0073] [Preparation of Test Cell] A positive electrode lead was attached to the exposed portion of the positive electrode, and a negative electrode lead was attached to the lithium metal foil serving as the negative electrode. The positive electrode and the negative electrode were spirally wound with a polyolefin separator interposed therebetween to prepare a wound electrode assembly. This electrode assembly was housed in an exterior body made of an aluminum laminate sheet, and the nonaqueous electrolyte was poured into it. The opening of the exterior body was then sealed to obtain a test cell.
[0074] [Evaluation of Reaction Resistance] The test cell was subjected to constant current charging at 0.2 C in a temperature environment of 25 ° C until the battery voltage reached 4.4 V (vs. Li), and constant voltage charging at 4.4 V until the current value reached 0.02 C. After a 1-hour pause, the cell was discharged at a constant current of 0.2 C until it reached 2.5 V, which was the initial charge / discharge. Next, after a 2-hour pause in a temperature environment of 10 ° C, the cell was subjected to constant voltage charging at 4.4 V with a current value equivalent to 0.01 C using a Solartron 1255B (manufactured by Solartron), and the AC impedance of each cell was measured at an applied voltage of 10 mV and a measurement frequency range of 0.01 to 200 kHz. The value of the reaction resistance was determined from the Nyquist plot (an arc of about 1 Hz to 0.1 Hz).
[0075] [Evaluation of cycle characteristics] The test cell was charged to 4.4 V (vs. Li) at a constant current of 0.2 C in a temperature environment of 25°C, and then charged at a constant voltage of 4.4 V until the current value reached 0.01 C. After a 1-hour rest, the cell was discharged to 2.5 V at a constant current of 0.2 C, which constituted one cycle. The discharge capacity at 0.2 C after 30 cycles was measured. The capacity retention rate was calculated using the following formula: Capacity retention rate = Discharge capacity after 30 cycles / Discharge capacity at first cycle
[0076] Examples 2 to 9 Test cells were prepared and evaluated in the same manner as in Example 1, except that in the preparation of the positive electrode, the composition of the additive was changed as shown in Table 1. The additives were added so that the mass of the elements shown in Table 1 was the amount added relative to the total mass of the positive electrode active material.
[0077] Comparative Example 1 A test cell was produced and evaluated in the same manner as in Example 1, except that lithium methanesulfonate was not added in the addition step of producing the positive electrode active material, and no additive was added in producing the positive electrode.
[0078] Comparative Example 2 A test cell was prepared and evaluated in the same manner as in Example 1, except that no additive was added in the preparation of the positive electrode.
[0079] Comparative Example 3 A test cell was prepared and evaluated in the same manner as in Example 1, except that lithium methanesulfonate was not added in the addition step of preparing the positive electrode active material.
[0080] <Comparative Example 4> A test cell was produced and evaluated in the same manner as in Example 1, except that in the addition step of producing a positive electrode active material, a 10 mass % lithium succinate solution was added instead of lithium methanesulfonate, and the amount of lithium succinate added was 0.5 mass % with respect to the total mass of the lithium-containing transition metal composite oxide.
[0081] The reaction resistance and capacity retention rate of the test cells of the examples and comparative examples are shown in Table 1. Table 1 also shows the composition of the lithium-containing transition metal composite oxide, and the composition and added amount of the added sulfonic acid compound and additive. The reaction resistance and capacity retention rate of the test cells of Examples 1 to 9 and Comparative Examples 1 to 4 shown in Table 1 are expressed relative to the reaction resistance and capacity retention rate of the test cell of Comparative Example 1, which is set to 100. A smaller value for the reaction resistance means a reduced reaction resistance, and a larger value for the capacity retention rate means better cycle characteristics.
[0082]
[0083] As shown in Table 1, the test cells of the examples exhibited reduced reaction resistance and improved cycle characteristics compared to the test cells of the comparative examples. On the other hand, the test cell of comparative example 2, in which a sulfonic acid compound was present on the surface of the secondary particles and no additive was added, exhibited reduced reaction resistance compared to the test cell of comparative example 1, but its cycle characteristics were worse. The test cell of comparative example 3, in which a sulfonic acid compound was not present on the surface of the secondary particles and an additive was added, exhibited improved cycle characteristics compared to the test cell of comparative example 1, but its reaction resistance was increased. The test cell of comparative example 4, in which lithium succinate was present on the surface of the secondary particles instead of a sulfonic acid compound, exhibited increased reaction resistance compared to the test cell of comparative example 1. In other words, the effects of the present disclosure cannot be achieved even if a compound other than a sulfonic acid compound is present on the surface of the secondary particles.
[0084] The present disclosure will be further described by the following embodiments. Configuration 1: A positive electrode for a non-aqueous electrolyte secondary battery, comprising a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core, the positive electrode mixture layer including a positive electrode active material and an additive, the positive electrode active material including a lithium-containing transition metal composite oxide having a layered structure, the lithium-containing transition metal composite oxide being represented by the general formula Li x Ni a Co b Mn c M d O 2-y (wherein 0.8<x<1.2, 0.75≦a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr), and the positive electrode for a non-aqueous electrolyte secondary battery is represented by the formula (I), and the positive electrode is a secondary particle formed by aggregation of primary particles, the sulfonic acid compound represented by formula (I) is present on the surface of the secondary particle, and the additive comprises a compound containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, Ti, and Al. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) Configuration 2: The positive electrode for a non-aqueous electrolyte secondary battery according to Configuration 1, wherein A is a Group 1 element. Configuration 3: The positive electrode for a non-aqueous electrolyte secondary battery according to Configuration 1 or 2, wherein A is Li. Configuration 4: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 3, wherein R is an alkyl group. Configuration 5: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein R is a methyl group. Configuration 6: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 5, wherein in the positive electrode active material, the amount of the sulfonic acid compound present on the surface of the lithium-containing transition metal composite oxide is 0.05 mass % or more and 1.5 mass % or less, relative to the mass of the lithium-containing transition metal composite oxide. Aspect 7: The positive electrode for a non-aqueous electrolyte secondary battery according to any one of Aspects 1 to 6, wherein in the positive electrode mixture layer, the amount of P, Ca, Sr, B, Zr, Er, Ti, and Al contained in the additive is 0.001 mass % or more and 1 mass % or less, relative to the total mass of the positive electrode active material. Aspect 8: A non-aqueous electrolyte secondary battery comprising the positive electrode for a non-aqueous electrolyte secondary battery according to any one of Aspects 1 to 7, a negative electrode, and a non-aqueous electrolyte.
[0085] REFERENCE SIGNS LIST 10 non-aqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 16 exterior body, 17 sealing body, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 grooved portion, 23 internal terminal plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket
Claims
1. A positive electrode for a non-aqueous electrolyte secondary battery having a positive electrode core and a positive electrode mixture layer formed on a surface of the positive electrode core, the positive electrode mixture layer including a positive electrode active material and an additive, the positive electrode active material including a lithium-containing transition metal composite oxide having a layered structure, the lithium-containing transition metal composite oxide being represented by the general formula Li x Ni a Co b Mn c M d O 2-y (wherein 0.8<x<1.2, 0.75≦a≦0.95, 0≦b≦0.15, 0≦c≦0.25, 0≦d≦0.10, 0≦y<0.05, a+b+c+d=1, and M is at least one element selected from the group consisting of W, Mg, Mo, Nb, Ti, Si, Al, and Zr), and the secondary particles are formed by aggregation of primary particles, a sulfonic acid compound represented by formula (I) is present on surfaces of the secondary particles, and the additive comprises a compound containing at least one element selected from the group consisting of P, Ca, Sr, B, Zr, Er, Ti, and Al. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) 2. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein A is a Group 1 element.
3. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein A is Li.
4. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein R is an alkyl group.
5. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein R is a methyl group.
6. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein in the positive electrode active material, the amount of the sulfonic acid compound present on the surface of the lithium-containing transition metal composite oxide is 0.05 mass % or more and 1.5 mass % or less with respect to the mass of the lithium-containing transition metal composite oxide.
7. The positive electrode for a nonaqueous electrolyte secondary battery according to claim 1, wherein in the positive electrode mixture layer, the amount of P, Ca, Sr, B, Zr, Er, Ti, and Al contained in the additive is 0.001 mass % or more and 1 mass % or less with respect to the total mass of the positive electrode active material.
8. A non-aqueous electrolyte secondary battery comprising the positive electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 7, a negative electrode, and a non-aqueous electrolyte.
Citation Information
Patent Citations
Nickel-based active material for lithium secondary batteries, its manufacturing method, and lithium secondary battery including a positive electrode containing the same
JP2022113728A
Preparation method of single crystal lithium-nickel-cobalt-aluminum oxide
CN113564708A
Lithium secondary battery and positive electrode
JP2003173782A
Lithium titanate powder for power storage device electrode, active substance material, and power storage device using the active substance material
JP2018006164A
Positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery