A cell of an all-iron flow battery

The all-iron flow battery's efficiency and capacity are improved by using a combination of conductive and non-conductive materials with a hydrophilized carbon black-based mixture, addressing side reactions and membrane damage, resulting in enhanced performance and stability.

WO2024228691A1PCT designated stage expired Publication Date: 2024-11-07R FLO LLC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/UA2023/000022
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-02
Filing Date
2023-05-17
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

All-iron flow batteries face efficiency and capacity issues due to side reactions at the negative electrode, leading to reduced battery performance and potential membrane damage from iron dendrite growth, which existing solutions fail to adequately address.

Method used

The battery design incorporates a negative electrode composed of a combination of conductive and non-conductive materials with a specific thickness ratio and compression degree, where the conductive material is thermally pretreated carbon felt and the non-conductive material is polymeric felt, both impregnated with a hydrophilized carbon black-based mixture, to increase active area and prevent membrane damage.

Benefits of technology

This design enhances the battery's efficiency and capacity by reducing overvoltage, increasing hydrophilicity, and preventing membrane damage, allowing for higher current density and stable operation without iron dendrite growth, achieving a target capacity of over 600 mAh/cm² at 50 mA/cm² current density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure UA2023000022_07112024_PF_FP_ABST
    Figure UA2023000022_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The claimed invention relates to the energy industry, particularly, to electrochemical technologies for energy accumulation and storage, and it relates to a reaction cell of an all-iron flow battery, the cell consists of a negative electrolyte chamber and a positive electrolyte chamber, and the chambers are equipped with electrolyte input and output tools and separated by a membrane, a negative electrode is arranged in the negative electrolyte chamber, the negative electrode is a porous material that is connected to a current collector; a positive electrode is arranged in the positive electrolyte chamber. According to the invention, the electrodes occupy the entire volume of the corresponding chambers, and the negative electrode is made of a conductive material layer that is formed on a side of the current collector and a non-conductive material layer that is formed on a side of the membrane. The layers are mechanically interconnected by compression, and a thickness of the conductive material layer is greater than a thickness of the non-conductive material layer, and surfaces of the conductive layer which are adjacent to the current collector and to the non-conductive layer as well as a surface of the non-conductive layer that is adjacent to the conductive layer are preliminary impregnated with a hydrophilized carbon black-based mixture to a depth that is at most a half of the thickness of the corresponding layers.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] A CELL OF AN ALL-IRON FLOW BATTERY

[0002] FIELD OF THE INVENTION

[0003] The claimed invention relates to the energy industry, particularly, to electrochemical technologies for energy accumulation and storage, and it relates to a reaction cell of an all-iron flow battery.

[0004] PRIOR ART

[0005] Currently, redox flow batteries are one of the most promising technologies for long-term energy storage, especially in view of the demand for using renewable energy sources continues to increase. Flow batteries differ from other electrochemical energy storage technologies in that they utilize liquid electrolyte solutions which are supplied from outside and comprise reagents that participate in reversible electrochemical reactions. A general operation principle of the flow batteries implies the use of redox reactions both for accumulating the energy in a form of chemical energy in liquid electrolyte solutions and for converting the accumulated chemical energy back to the electrical energy. In terms of a structure, the flow batteries consist of a flow cell that is separated by a separator such as an ion-exchange or microporous separator into chambers having positive and negative electrodes arranged therein. The chambers are filled with positive and negative electrolytes, and each of the chambers is connected to a container for storing the corresponding electrolyte, while enabling a closed circulation of the electrolytes between tanks and the cell chambers. The formed closed electrochemical system may accumulate and convert the electrical energy to the chemical energy and vice versa for multiple times, thereby providing its reliability and scaling possibilities. Therefore, the flow batteries are used in network storage systems for decreasing peak loads, balancing loads, controlling charge, providing backup power etc.

[0006] Currently, the most promising option is to use iron-based flow batteries due to the abundance of raw materials, their affordability, as well as environmentally friendly production and usage. Electrochemical reactions involving iron ions which are dissolved in the corresponding electrolytes take place on the positive and negative electrodes of the all-iron flow battery. The positive electrode uses a Fe2+ / Fe3+redox pair, while the negative electrode uses a Fe2+ / Fe° redox pair. Iron chlorides or sulfates solutions (e.g., FeCh, FeCh, FeSO4, FezCSO^s) may be used as redox active compounds of the electrolytes of the all-iron battery, and these solutions are abundant and provide stability of the electrolyte, since the very same electrolyte may be used both for the negative electrolyte and for the positive electrolyte, thereby decreasing cross-contamination issues. Therefore, the all-iron flow batteries decrease the use of toxic raw materials as compared to other redox flow batteries, thereby decreasing an environmental hazard correspondingly.

[0007] The positive electrode and the negative electrode in the redox flow batteries are the most important components which affect the battery performance, capacity, efficiency and overall price, since the electrochemical reactions take place on their surfaces.

[0008] The redox reaction Fe2+ / Fe3+on the positive electrode is kinetically quick. The ferrous iron reduction reaction on the negative electrode of the all-iron battery competes with two side reactions: reduction of hydrogen protons H+, where two hydrogen protons receive two electrons to form gaseous hydrogen, H2, and reduction reaction to reduce Fe3+to Fe2+ions.

[0009] These two side reactions may decrease the overall battery efficiency, since the electrons transmitted to the negative electrode may be spent to produce hydrogen or to reduce iron(III) ions, rather than to reduce iron(II) ions to form metallic iron. Besides, these side reactions may lead to an imbalance of electrolytes which, in turn, leads to loss of the battery capacity.

[0010] Therefore, the battery efficiency largely depends on characteristics of the negative electrode. The characteristics of the negative electrode are a function of kinetics of the electrochemical reactions which take place on its surface, overvoltage of the electrochemical reactions and contact resistance between the electrode and a current collector. Therewith, the battery capacity depends on an amount of the charged iron which can be stored by the negative electrode, and its efficiency is directly associated with an extent of occurrence of the side reactions on the negative electrode.

[0011] Prior art teaches solutions which are aimed at increasing the operation efficiency of the all-iron battery by making various modifications of its electrodes in order to minimize side reactions and to increase capacity. A patent US9614244B2 dated April 4, 2017 teaches a cell of an all-iron battery, the cell consists of a negative electrolyte chamber and a positive electrolyte chamber which are separated by a membrane and equipped with current collectors. A positive electrode is arranged in the positive electrolyte chamber, and the positive electrode is made of a carbon porous material, while a negative electrode is arranged in the negative electrolyte chamber, and the negative electrode is made as a perforated ribbed structure having an oscillating cross section that forms a plurality of mutually offset channels to enable guiding of the electrolyte flow. The folded ribs of the electrode may be made of iron, iron alloy, stainless steel, titanium or carbon or polymeric plate comprising a plurality of conductive inserts which are attached to the polymeric plate between adjacent channels for the electrolyte flow. This structure of the cell of the all-iron battery enables to increase a working surface of the negative electrode in order to provide a larger area being available for deposition of a metallic iron without any need to increase a volume of the cell of the all-iron battery. A drawback of this solution is a formation of an oxide film along the surface of the metal electrode during charging and discharging of the battery, thereby decreasing an iron coating adhesion and, thus, decreasing a maximum capacity of the electrode. Use of metal anodes may lead to destruction of the electrode structure due to occurrence of corrosion side reactions and to imbalance of a charge degree of the electrolytes.

[0012] An alternative solution is disclosed in a patent US11043679B2 dated June 22, 2021 which teaches a cell of an all-iron battery, the cell consists of a negative electrolyte chamber and a positive electrolyte chamber which are equipped with electrolyte input and output means which are separated by an ion-exchange or microporous composite membrane and equipped with current collectors. The chambers are filled with a porous material for providing a flow of electrolytes which are a negative electrode and a positive electrode respectively. Therewith, the porous material is a plastic mesh with a hydrophilic conductive coating in order to provide wetting of a surface of the electrode with the electrolyte and to enable an unhindered occurrence of an iron deposition reaction on its surface, and it has an open area from 15% to 65% and an open volume from 10% to 70%. Said meshy electrode has a low active area, thereby increasing an overvoltage of chemical reactions on its surface and, consequently, cannot provide a satisfactory energy efficiency of the operation of the battery at a high current density. Furthermore, the structure of the cell does not provide any protection of the separator / membrane surface against growth of metal into the membrane, thereby causing irreversible processes of degradation and / or short circuit in the battery.

[0013] SUMMARY OF THE INVENTION

[0014] An underlying objective of the invention is to increase the negative electrode active area in order to increase the capacity of the electrodes in terms of active metal and, thus, the current density, as well as to protect the membrane against possible damage caused by penetration of the metallic iron into its structure.

[0015] This is achieved by filling layers of the negative electrode with active conductive additives, by providing a barrier to avoid growth of metal into the membrane, by making the positive electrode of a conductive porous material and by making the negative electrode of a combination of conductive and non-conductive materials which are arranged in a certain way relative to the membrane and have a certain thickness ratio and a certain compression degree. A technical effect being achieved lies in increasing the operation efficiency of the all-iron flow battery and in increasing the capacity of the negative electrode due to increase of the active area of the electrode and to prevention of the possible damage of the membrane with iron dendrites.

[0016] The objective is achieved by providing a cell of an all-iron battery, the cell consists of a negative electrolyte chamber and a positive electrolyte chamber, and the chambers are equipped with electrolyte input and output tools and separated by an ion-exchange and / or microporous composite membrane, a negative electrode is arranged in the negative electrolyte chamber, the negative electrode is a porous material that is connected to a current collector, and a positive electrode is arranged in the positive electrolyte chamber, the positive electrode is a porous material that is connected to the current collector. According to the claimed invention, the electrodes occupy the entire volume of the corresponding chambers, and the positive electrode consists of a conductive material, while the negative electrode consists of a conductive material layer that is formed on a side of the current collector and a non-conductive material layer that is arranged between the conductive material and the membrane. The negative electrode layers are mechanically interconnected by compression, and a thickness of the conductive material layer is greater than a thickness of the non-conductive material layer. Surfaces of the conductive layer which are adjacent to the current collector and to the non-conductive layer as well as a surface of the non-conductive layer that is adjacent to the conductive layer are preliminary impregnated with a hydrophilized carbon black -based mixture to a depth that is at most a half of the thickness of the corresponding layers.

[0017] According to an exemplary embodiment of the invention, a thermally pretreated carbon felt is used as the conductive material of the electrodes, while a polymeric felt is used as the non-conductive material of the negative electrode.

[0018] According to another exemplary embodiment, the hydrophilized carbon black based mixture may be a composition that consists of an oxidized carbon black and a dispersed sulphonated tetrafluoroethylene-based fluoropolymer-copolymer, and the layers of the negative electrode are impregnated by applying the mixture via spray coating.

[0019] This structure of the cell of the all-iron battery increases the active area of its electrode material, thereby decreasing the overvoltage of the iron plating process which, in turn, increases the operation efficiency of the battery. Also, it increases the electrode area which is necessary for the deposition of the active metal and the free volume of the electrode chamber, thereby enabling to perform the battery charging process while achieving a high capacity in terms of the active substance. Use of the combination of said materials in the negative electrode increases the hydrophilicity of the electrode material, thereby enabling to use a greater active area of the conductive material which, in turn, decreases the overvoltage of the iron plating process which, in turn, increases the operation efficiency of the battery. In turn, the increase of the hydrophilicity of the non-conductive material enables to decrease a pressure loss of the electrolyte in the negative electrode chamber and decreases a surface tension of the electrolyte in a near-electrode layer. The increase of the hydrophilicity further decreases the surface tension of the electrolyte in a diffusion layer of the electrode surface, thereby allowing to decrease a delay time of a gaseous hydrogen bubble which evolves during the battery charging process on the negative electrode surface. Owing to the thermal treatment of the conductive material, it becomes possible to achieve the greater hydrophilicity of the active area of the electrodes due to partial oxidation of the surface and graphite in order to increase a contact between the electrolytes and the electrodes, and, thus, to increase the active working area which, in turn, will decrease the polarization of the electrodes in the working process and increase the battery efficiency.

[0020] DESCRIPTION OF THE FIGURES

[0021] In order to provide a more complete understanding of the invention and advantages thereof, the following description provides an explanation of possible exemplary embodiments on the invention with a reference to the appended figures, wherein identical designations denote identical parts:

[0022] Fig. 1 illustrates a schematic view of the all-iron battery system;

[0023] Fig. 2 illustrates a schematic cross-sectional view of the cell of the all-iron battery;

[0024] Fig. 3 illustrates an enlarged longitudinal sectional view of the structure of the cell of the all-iron battery having the metallic iron coating applied thereon;

[0025] Fig. 4 illustrates a schematic longitudinal sectional view of the cell of the all-iron battery having the fully conductive negative electrode and the metallic iron coating applied thereon;

[0026] Fig. 5 illustrates a plot depicting the achievement of a target capacity of the claimed battery;

[0027] Fig. 6 illustrates plots depicting the charge level of the negative electrode of the claimed battery and of the battery having the fully conductive negative electrode.

[0028] Fig. 7 illustrates plots depicting the charge level of the negative electrode of the claimed battery and of the batteries having the thermally non -treated negative electrode and the thermally treated negative electrode. Main designations:

[0029] 1. Cell of the all-iron flow battery

[0030] 2. Negative electrolyte chamber

[0031] 3. Positive electrolyte chamber

[0032] 4. Membrane of the cell of the all-iron flow battery

[0033] 5. Negative electrolyte circulation circuit

[0034] 6. Positive electrolyte circulation circuit

[0035] 7. Negative electrolyte pump

[0036] 8. Positive electrolyte pump

[0037] 9. Negative electrolyte tank

[0038] 10. Positive electrolyte tank

[0039] 11. Current collector of the positive electrolyte chamber

[0040] 12. Current collector of the negative electrolyte chamber

[0041] 13. Positive electrolyte electrode

[0042] 14. Conductive layer of the negative electrolyte

[0043] 15. Non-conductive layer of the negative electrolyte

[0044] 16. Deposited iron on the negative electrode

[0045] INVENTION IMPLEMENTATION POSSIBILITY

[0046] According to the claimed invention, a cell (1) of an all-iron flow battery is divided into chambers (2, 3) by an ion-exchange and / or microporous membrane (4) and equipped with electrolyte input and output tools for inputting and outputting the electrolytes to / from both chambers. The electrolyte input and output tools are closed electrolyte circuits (5, 6) which are equipped with circulation pumps (7, 8) and connected to a negative electrolyte tank (9) and to a positive electrolyte tank (10) respectively. The electrolytes are fed from the tanks (9, 10) to the corresponding chambers (2, 3), and the electrolytes, in turn, enter the tanks from the chambers. Each of the chambers is equipped with current collectors (11, 12), and a positive electrode (13) is arranged in the positive electrolyte chamber (3), while the positive electrode is a porous conductive material that is connected to the current collector (11) and to the membrane (4), and a negative electrode is arranged in the negative electrolyte chamber (2), while the negative electrode consists of a conductive material layer (14) that is formed on a side of the current collector (12) and of a non-conductive material layer (15) that is formed on a side of the membrane (4). The layers (14) and (15) are mechanically interconnected by compression when mounting the battery cell, and a thickness of the conductive material layer (14) is at least two times greater than a thickness of the non- conductive material layer (15). Surfaces of the conductive layer (14) which are adjacent to the current collector (12) and to the non-conductive layer (15) as well as a surface of the non-conductive layer (15) with the conductive layer (14) are preliminary impregnated with a hydrophilized carbon black -based mixture to depth that is at most a half of the thickness of the corresponding layers (14, 15). Dark particles (16) illustrated in Fig. 3 demonstrate deposition of the metallic iron on the conductive material and on the non-conductive material of the negative electrode.

[0047] Electrodes are formed during formation of the battery cell. Firstly, the conductive felt layer (14) is laid on the current collector, and the conductive felt layer is coated with the hydrophilized carbon black -based mixture on sides which are in a contact with the current collector (12) and with the non-conductive layer (15), then, the mixture-coated side of the non-conductive felt layer (15) is laid on the conductive felt layer (14). The materials are compressed until a compression degree of the negative electrode layers and of the positive electrode layer that is from 10% to 50% of the initial density is achieved. Therewith, both materials constitute the entire area of the electrode and occupy the entire volume of the negative electrode chamber, and their ratio corresponds to their thickness ratio, e.g., 2 mm of the non-conductive felt and 1 mm of the non-conductive felt. The positive electrode (13) is made in the same way, but of the porous conductive material only which occupies the entire volume of the positive electrolyte chamber accordingly.

[0048] The conductive material of the electrodes is a carbon felt, e.g., of trademarks CFD 2.5 EA (Sigracet), GFD 2.5 EA or GFD 4,6 EA (SGL Carbon) which are present on the market which enable electrolyte flow and have the following characteristics: density from 0.05 to 0.2 g / cm3, porosity from 80 to 95%, specific area from 0.5 to 0.7 m2 / g.

[0049] The non-conductive material is a polymeric felt that may be made of polyester or polypropylene. The material chosen by inventors as a suitable one for using during tests is a felt that is usually used in AGM separators of the AMER-GLASS company that provides the electrode material with the following characteristics: density from 0.05 to 0.2 g / cm3, porosity from 80 to 95%, specific area from 0.5 to 0.7 m2 / g.

[0050] The membrane may be an ion-exchange membrane or a microporous membrane, e.g., acid-resistant cation exchange membranes (e.g., Nafion) having a thickness from 50 to 500 pm and acid-resistant anion exchange membranes of the same thickness.

[0051] In order to increase the hydrophilicity of the active area of the electrodes, at least the carbon felt to be used in the negative electrode was thermally treated before use by loading it into a furnace without any preliminary treatment and held at the temperature of 450 °C during 60 - 120 minutes. Owing to partial oxidation of the surface and graphite due to the thermal treatment, the active working area of the electrode and, thus, a greater contact between the electrolyte and the electrode are increased which, in turn, decreases the polarization of the electrode during the working process and increases the battery efficiency.

[0052] The carbon substance of the mixture may be carbon black Vulcan XC-72 or Vulcan XC-72R which is pretreated in nitric acid to provide hydrophilization. The carbon black is treated by oxidizing with a concentrated nitric acid(HNO3) at a ratio of 1 g of the carbon black per 100 ml (65%) of HNO3 at the temperature from 80 to 120 °C during 60-120 minutes until a full oxidation is achieved. Chemical treatment of the carbon black in the nitric acid enables to form a large number of oxygen-containing functional groups on the carbon black surface which provide the surface with hydrophilic properties. A binding agent of the mixture is a sulfonated tetrafluoroethylene-based fluoropolymer-copolymer dispersion (Nation D521, D520) at a ratio of 60-80 wt. % of the carbon black per 20-40 wt.% of the dispersion (Nation 5%). The hydrophilized carbon black-based mixture is applied directly before mounting the electrode in the battery cell. The application is performed via spray coating in air onto the surface of the conductive felt on both sides and onto the surface of the non-conductive felt on one side only. Therewith, in order to achieve the impregnation with the mixture to at most a half of the corresponding layers, the application is performed at 2 mg per 1 cm2at the layer thickness of 2 mm and at 1 mg per 1 cm2of the electrode area at the layer thickness of 1 mm. That is, if the material thickness is 2 mm and the area is 1 cm2, then 2 mg of the mixture will be required, if the thickness is 1 mm and the area is 2 cm2, then 2 mg of the mixture will be required, if the thickness is 2 mm and the area is 2 cm2, then 4 mg of the mixture will be required, etc.

[0053] This treatment enables to increase the conductive area of the electrode material in both layers, while leaving an isolating interlayer on the membrane side that becomes a barrier that protects the membrane against damaging by the metallic iron. Said isolating interlayer increases the maximum capacity of the electrode in terms of the charged metal and avoids the metal from growing into the membrane which occurs when using the fully conductive negative electrode in the cell of the all-iron battery illustrated in Fig. 4.

[0054] At the initial moment of charging of the all-iron flow battery, reduction reaction of the iron Fe2+ions to the metallic iron takes place on the negative electrode (dots 16 in Fig. 3 and Fig. 4) and reduction reaction of H+ions to molecular gaseous hydrogen Hz takes place on the surface of the current collector. During a certain time period, the iron deposited onto the current collector contacts with the conductive material of the negative electrode and “connects” it to the battery electric circuit, thereby causing growth (reduction) of the metallic iron on its surface. During the charging process of the negative conductive layer, its volume is decreased, since it is filled with the metallic iron, while an amount of iron starts to form on the surface of the conductive layer on the membrane side that is greater than in the volume of the conductive layer. Afterwards, most of the reduced iron is formed on the surface of the conductive layer on the side of the non-conductive layer until the battery charging process is completed.

[0055] During charging of the fully conductive negative electrode in the cell of the all-iron battery to reach the capacity of more than 400 mAh / cm2, the dendrites of the metallic iron grow through the cell membrane causing a short circuit at the positive electrode. This process stops the battery operation according to its technical characteristics.

[0056] When using a combination of the conductive and non-conductive electrode materials as disclosed in the claimed invention at said thickness ratio and at said compression degree, upon conduction of chemical, thermal treatment and owing to filling with the active conductive mixture, a risk of the membrane damage is eliminated and it is enabled to charge the electrode with the capacity of more than 400 mAh / cm2, while achieving high technological characteristics (overall, voltaic, current efficiencies). Fig. 5 illustrates a plot depicting the achievement of a target capacity of the claimed battery being 600 mAh / cm2at the current density of 50 mA / cm2as compared to the example of the invention according to US11043679B2 dated June 22, 2021 with the current density of 45 mA / cm2. X-axis of the plot depicts charging and discharging time of the claimed all-iron battery in minutes during which the voltage on the battery terminals was measured, while Y-axis of the plot depicts the voltage on the battery terminals. As seen from the plot, the voltage of the battery charge that is proposed in the solution is lower than the voltage of the battery charge in the solution of US11043679B2 at higher current density, and the discharging voltage of the proposed solution is higher than the one in the solution of the analogue at higher current density. Change of these two parameters is caused by significantly lower overvoltage of the iron deposition or dissolving on modified electrodes due to increase of the active area and to increase of the hydrophilicity of the electrode material, and leads to increase of the energy efficiency of the all-iron flow battery.

[0057] In order to confirm the operation efficiency of the all-iron battery according to the claimed invention, its charging characteristic was tested to compare it to a battery having a negative electrode that is only a conductive graphite felt as illustrated in the plot of Fig. 6.

[0058] X-axis of the plot depicts a charging time of the claimed all-iron battery in minutes, while Y-axis of the plot depicts a variation of a potential of the negative electrode relative to a silver chloride reference electrode during the battery charging. As seen in the plot, a curve of the potential variation as a function of the charging duration for the solution being compared radically changed its nature near a value of 480 minutes which occurs due to growth of the iron dendrites through the membrane. Use of the invention increases the maximum capacity of the negative electrode of the all-iron flow battery in terms of the metallic iron without growing of the dendrite during more than 800 minutes of charging, thereby providing the stable operation of the battery.

[0059] Also, in order to confirm the operation efficiency of the all-iron battery according to the claimed invention, its charging characteristic was tested to compare it to batteries having a negative electrode that is a conductive graphite felt with the thermal treatment and without it, respectively. Their charge and discharge characteristics are illustrated in the plot of Fig. 7.

[0060] X-axis of the plot depicts a charging time of the claimed all-iron battery in minutes, while Y-axis of the plot depicts a variation of a potential of the negative electrode relative to a silver chloride reference electrode during the battery charging. As seen in the plot, a curve of the potential variation as a function of the charging duration for the solutions being compared radically changed its nature near a value of 480 minutes and 650 minutes which occurs due to growth of the iron dendrites through the membrane. Use of the solution as described in the invention increases the maximum capacity of the negative electrode of the all-iron flow battery in terms of the metallic iron without growing of the dendrites during more than 800 minutes of charging, thereby providing the stable operation of the battery. Also, when using the present technical solution, it is observed that the potential of the negative electrode is increased relative to the thermally non-treated and to the thermally treated material without filling, thereby indicating that the electrode polarization is decreased due to increase of the active area of the electrode which eventually increases the energy efficiency of the all-iron flow battery.

[0061] The above-described exemplary embodiments of the invention must be used for illustrative purposes only and must not restrict the scope of the invention, since skilled artisans are able to introduce obvious modifications during implementation of the invention without going beyond its essence. However, the achieved parameters indicate that the implementation of the present technical solution provides the achievement of the higher operation efficiency of the all-iron flow battery at the higher current density for the higher capacity of the negative electrode in terms of the active material.

[0062] The claimed invention enables to provide the reliable cell of the all-iron battery having enhanced electrochemical properties, namely: decreased overvoltage of the iron plating reaction, decreased polarization, increased hydrophilicity, increased active area value, increased capacity in terms of the charged metal being iron which may be scaled in wide range of geometrical dimensions of the electrodes and power depending on a required usage scenario.

Claims

CLAIMS1. A cell of an all-iron battery, the cell consists of a negative electrolyte chamber and a positive electrolyte chamber, and the chambers are equipped with electrolyte input and output tools and separated by a membrane, a negative electrode is arranged in the negative electrolyte chamber, the negative electrode is a porous material that is connected to a current collector; a positive electrode is arranged in the positive electrolyte chamber, the positive electrode is a porous material that is connected to the current collector, wherein the electrodes occupy an entire volume of the corresponding chambers, and the negative electrode consists of a conductive material layer that is formed on a side of the current collector and a non-conductive material layer that is formed on a side of the membrane, and the layers are mechanically interconnected by compression, and a thickness of the conductive material layer is greater than a thickness of the non-conductive material layer, and surfaces of the conductive layer which are adjacent to the current collector and to the non-conductive layer as well as a surface of the non-conductive layer that is adjacent to the conductive layer are preliminary impregnated with a hydrophilized carbon black-based mixture to a depth that is at most a half of the thickness of the corresponding layers.

2. The cell according to claim 1, wherein a thermally pretreated carbon felt is used as the conductive material of the electrodes, while a polymeric felt is used as the non-conductive material of the negative electrode.

3. The cell according to claim 1, wherein the hydrophilized carbon black-based mixture consists of an oxidized carbon black and a dispersed sulphonated tetrafluoroethylene-based fluoropolymer-copolymer.

4. The cell according to claim 1, wherein the impregnation is performed by applying the mixture via spray coating.

Citation Information

Patent Citations

  • Alternative low cost electrodes for hybrid flow batteries

    US11043679B2

  • Redox and plating electrode systems for an all-iron hybrid flow battery

    US9614244B2

  • Methods and system for manufacturing a redox flow battery system by roll-to-roll processing

    US20200052310A1

  • All-iron flow battery and systems

    WO2019246538A1