Method for repairing and regenerating positive electrode material by recovering waste battery in full-chain integrated manner
Through pyrolytic sorting and plasma coating technology, the problems of high consumption and poor performance in the recycling of the positive electrode materials of waste lithium iron phosphate batteries are solved, and low-cost and efficient carbon capture and fluorine recycling are achieved, which improves regeneration Electrochemical properties of materials.
Patent Information
- Application Number
- PCT/CN2023/093431
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-14
AI Technical Summary
When recycling waste lithium iron phosphate battery positive electrode materials, the prior art consumes high, is expensive, and has serious environmental pollution. The regenerated positive electrode materials have poor performance and are difficult to fully restore conductivity.
The positive electrode material powder was obtained by pyrolytic separation, lithium supplement calcination treatment was performed, and organic gas was mixed with silicon tetrafluoride for plasma coating, carbon was fixed in the lithium iron phosphate coating layer, and waste gas was recovered using SiO2 to achieve carbon Capture and fluorine recycling to reduce carbon dioxide emissions and environmental pollution.
It reduces carbon emissions and environmental pollution, improves the electrochemical performance of recycled positive electrode materials, is low in cost, and has less reagent consumption, achieving efficient repair and regeneration of lithium iron phosphate positive electrode materials.
Smart Images

Figure CN2023093431_14112024_PF_FP_ABST
Abstract
Description
A full-chain integrated method for recycling waste batteries and repairing and regenerating positive electrode materials Technical Field
[0001] The present disclosure belongs to the field of resource recycling technology, for example, a method for recycling waste batteries and repairing and regenerating positive electrode materials in an integrated full-chain manner. Background Art
[0002] With the rapid development of the new energy vehicle industry, lithium iron phosphate batteries have emerged as a leader among lithium-ion power batteries due to their advantages, including excellent thermal stability, safety, and cycle stability. However, power batteries have a limited lifespan, and the number of retired lithium iron phosphate power batteries is increasing year by year. Failure to effectively utilize these batteries can lead to resource waste and environmental pollution. "Full-chain integrated recycling," as a key tool in the circular economy, can effectively address these issues.
[0003] The valuable components of lithium iron phosphate batteries are primarily found in the cathode material. Therefore, the integrated, full-chain recycling of lithium iron phosphate batteries primarily involves the recycling and reuse of spent lithium iron phosphate cathode materials. Common recycling methods for lithium iron phosphate cathode materials are pyrometallurgical and hydrometallurgical methods. Both methods involve separating and extracting valuable metals from spent cathode materials, requiring high energy consumption and the consumption of large quantities of acid and alkaline reagents, resulting in high overall recycling costs. Because lithium iron phosphate is relatively inexpensive compared to ternary cathode materials and contains relatively low valuable metal content, traditional recycling methods are not economically viable.
[0004] CN114006070A discloses a method for high-temperature pyrolysis and pneumatic stripping of used lithium batteries. The waste gas generated by the pyrolysis is treated through high-temperature incineration, rapid cooling, water washing, and alkaline washing before being discharged in compliance with emission standards. This method not only consumes energy but also results in large amounts of carbon dioxide emissions, hindering the achievement of the dual carbon goals.
[0005] CN115312903A discloses a method for regenerating waste lithium iron phosphate to prepare rate-type lithium iron phosphate. The method comprises: adding water to waste lithium iron phosphate powder and ferrous disulfide in a molar ratio to prepare a slurry and mixing; adding an acid solution in a molar ratio of waste lithium iron phosphate powder and hydrogen ions to the slurry, and adding water in a solid-liquid ratio to prepare a slurry and stirring; transferring the mixed slurry to an autoclave, sealing it, introducing an oxidizing gas, heating it, stirring it, and then insulating it; filtering the filtrate after the reaction, adding a phosphorus source and a lithium source to the filtrate, adding a dispersant, and then heating it and insulating it; cooling it after insulation, filtering the slurry, washing it, and spraying it to obtain a spray material; and sintering the spray material under a protective atmosphere to obtain a carbon-coated lithium iron phosphate positive electrode material. The regeneration method can replenish lithium in the waste positive electrode material, restore the material morphology, composition, and electrochemical properties, and achieve regeneration of the positive electrode material. The entire regeneration process consumes less reagents, has a short process flow, and reduces environmental pollution. However, the performance of the regenerated positive electrode material is not very ideal. This is because, although the waste positive electrode material has been replenished with lithium, the positive electrode material has poor conductivity and the outer carbon coating has defects during the cycle. It is difficult to completely restore or improve the conductivity of the positive electrode material by only replenishing lithium. Therefore, the electrochemical performance of the regenerated positive electrode material is not ideal.
[0006] In addition to cathode materials, electrolyte is also a major component of spent lithium-ion batteries. During the pyrolysis of battery fragments, the electrolyte decomposes and produces large amounts of organic gases. Currently, direct combustion of these gases is the common method of disposal.
[0007] Summary of the Invention
[0008] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0009] The purpose of the present disclosure is to provide a full-chain integrated method for recycling waste batteries and repairing and regenerating positive electrode materials. The present disclosure not only utilizes the organic gas generated by the decomposition of the electrolyte, but also restores the performance of the lithium iron phosphate positive electrode material. In addition, the entire reaction process only consumes silicon dioxide while fixing the tail gas, with low reagent consumption and low cost.
[0010] To achieve this disclosure purpose, the present disclosure adopts the following technical solutions:
[0011] In a first aspect, the embodiments of the present disclosure provide a method for recycling waste batteries and repairing and regenerating positive electrode materials in an integrated manner. The repair and regeneration method comprises the following steps:
[0012] (1) discharging the discarded batteries and performing pyrolysis separation to obtain cathode material powder;
[0013] (2) performing lithium supplementation calcination treatment on the positive electrode material powder;
[0014] (3) Mixing an organic gas and silicon tetrafluoride to obtain a mixed gas, using the mixed gas to perform plasma coating treatment on the powder obtained by lithium supplementation calcination to obtain a silicon carbide coated positive electrode material, recovering the obtained waste gas using SiO2, and drying the obtained silicon tetrafluoride gas and recycling it.
[0015] After discharge, the discarded batteries described in the embodiment of the present disclosure are disassembled and crushed to obtain pre-treated battery fragments, and the battery fragments are pyrolyzed to obtain waste positive electrode material powder and waste gas.
[0016] In the repair and regeneration method described in the embodiment of the present disclosure, the carbon capture flow can fix carbon in the coating layer of the regenerated lithium iron phosphate, and will not produce carbon dioxide emissions, which is beneficial to reducing carbon emissions. The fluorine circulation flow can realize the recycling of HF, and does not require further collection and treatment of harmful gases, which is beneficial to reducing environmental pollution. The regenerated silicon carbide-coated lithium iron phosphate can repair the damage of the carbon coating layer of the waste lithium iron phosphate, and the coating surface is smoother and the material has excellent electrochemical properties. The entire reaction process only consumes silicon dioxide while fixing the exhaust gas, with low reagent consumption and low cost.
[0017] The reaction equation for recycling the waste gas using SiO2 in the embodiment of the present disclosure is: SiO2+4HF=SiF4+2H2O.
[0018] In one embodiment, the waste batteries in step (1) include any one of waste lithium iron phosphate batteries, waste lithium cobalt oxide batteries or waste ternary batteries, or a combination of at least two of them.
[0019] In one embodiment, the temperature of the pyrolysis treatment in step (1) is 400-600°C, for example, 400°C, 450°C, 500°C, 550°C or 600°C.
[0020] In one embodiment, the pyrolysis treatment time is 3 to 8 hours, for example, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours or 8 hours.
[0021] In one embodiment, the lithium supplementation calcination treatment in step (2) includes testing the lithium deficiency amount of the positive electrode material powder by inductively coupled plasma mass spectrometry (ICP testing), determining the amount of lithium source added, mixing the positive electrode material powder and the lithium source, and calcining after ball milling.
[0022] In one embodiment, when the positive electrode material powder is lithium iron phosphate, a reducing agent is added.
[0023] In one embodiment, the reducing agent includes any one of sucrose, glucose, cellulose or elemental carbon, or a combination of at least two thereof.
[0024] In one embodiment, the amount of the reducing agent added is 1-5% of the mass of the positive electrode material powder, for example, 1%, 2%, 3%, 4% or 5%, etc. Preferably, it is 2-3%.
[0025] In one embodiment, the lithium source includes any one of lithium hydroxide, lithium carbonate, lithium nitrate, lithium oxalate, lithium acetate, lithium dihydrogen phosphate, or lithium hydrogen phosphate, or a combination of at least two thereof.
[0026] In one embodiment, the ball milling time is 0.5 to 2 hours, for example, 0.5 hours, 0.8 hours, 1 hour, 1.5 hours or 2 hours.
[0027] In one embodiment, the calcination temperature is 650-800°C, for example, 650°C, 680°C, 700°C, 750°C or 800°C.
[0028] In one embodiment, the calcination time is 1 to 5 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours or 5 hours.
[0029] In one embodiment, the calcination atmosphere is nitrogen and / or argon.
[0030] In one embodiment, the organic gas in step (3) is obtained by condensing and recovering the waste gas obtained by the pyrolysis in step (1), and collecting it after removing the acidic gas.
[0031] In one embodiment, the organic gas includes any one of C2H4, CH4 or C2H6, or a combination of at least two of them.
[0032] In one embodiment, the volume ratio of the organic gas to silicon tetrafluoride in step (3) is 1:(1-5), for example: 1:1, 1:2, 1:3, 1:4 or 1:5.
[0033] In one embodiment, the flow rate of the mixed gas in step (3) is 50 to 100 mL / min, for example, 50 mL / min, 60 mL / min, 70 mL / min, 80 mL / min, 90 mL / min or 100 mL / min.
[0034] In one embodiment, the electron energy of the plasma coating treatment is 20-30 eV, for example, 20 eV, 22 eV, 25 eV, 38 eV or 30 eV.
[0035] In one embodiment, the temperature of the plasma coating treatment is 350-500° C., for example, 350° C., 380° C., 400° C., 450° C., or 500° C.
[0036] In one embodiment, the waste gas obtained from the plasma coating treatment is recovered using SiO2, and the obtained silicon tetrafluoride gas is dried and recycled.
[0037] In one embodiment, based on the mass of the silicon carbide coated positive electrode material being 100%, the mass fraction of the silicon carbide coating layer is 0.1-2%, for example, 0.1%, 0.5%, 0.8%, 1%, 1.5% or 2%.
[0038] As an optional solution of the present disclosure, the repair and regeneration method includes the following steps:
[0039] (1) discharging the waste battery and performing pyrolysis treatment to obtain waste gas and positive electrode material powder;
[0040] (2) testing the lithium deficiency of the positive electrode material powder by ICP to determine the amount of lithium source to be added, mixing the positive electrode material powder, the lithium source and the reducing agent, calcining at 650-800° C. for 1-5 hours, wherein the amount of the reducing agent added is 1-5% of the mass of the positive electrode material powder, and condensing and recovering the waste gas, removing acidic gases and collecting organic gases;
[0041] (3) The organic gas collected in step (2) and silicon tetrafluoride are mixed in a volume ratio of 1:(1-5) to obtain a mixed gas, and the mixed gas is introduced into a plasma reactor at a flow rate of 50-100 mL / min. The powder obtained by lithium supplementation calcination is subjected to plasma coating treatment under the conditions of an electron energy of 20-30 eV and a constant temperature zone temperature of 350-500° C. to obtain a silicon carbide-coated positive electrode material, and the obtained waste gas is recovered using SiO2, and the obtained silicon tetrafluoride gas is dried and recycled.
[0042] Compared with the prior art, the present disclosure has the following beneficial effects:
[0043] (1) In the repair and regeneration method disclosed in the present invention, the carbon capture flow can fix carbon in the coating layer of the regenerated lithium iron phosphate, and will not produce carbon dioxide emissions, which is beneficial to reducing carbon emissions. The fluorine circulation flow can realize the recycling of HF, and does not require further collection and treatment of harmful gases, which is beneficial to reducing environmental pollution. The regenerated silicon carbide-coated lithium iron phosphate can repair the damage of the carbon coating layer of the waste lithium iron phosphate, and the coating surface is smoother and the material has excellent electrochemical properties. The entire reaction process only consumes silicon dioxide while fixing the exhaust gas, with low reagent consumption and low cost.
[0044] (2) The lithium iron phosphate battery regenerated by the method disclosed herein can achieve a 0.1C gram capacity of more than 152.79 mAh / g, a coulombic efficiency of more than 96.41%, a 1C gram capacity of more than 138.09 mAh / g, and a compaction density of 2.511 g / cm3 above.
[0045] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.
[0047] FIG1 is a schematic diagram of the process flow of the repair and regeneration method described in Example 1 of the present disclosure.
[0048] FIG2 is an XRD diagram of the silicon carbide coated positive electrode material obtained in Example 1 of the present disclosure. DETAILED DESCRIPTION
[0049] The technical solution of the present disclosure is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present disclosure and should not be regarded as specific limitations of the present disclosure.
[0050] Example 1
[0051] This embodiment provides a method for repairing and regenerating a positive electrode material of a battery, the method comprising the following steps:
[0052] (1) discharging, disassembling and crushing the retired power batteries, pyrolyzing the obtained battery fragments at 600° C. for 4 h, and treating the waste gas after pyrolysis in step (2) to collect the waste lithium iron phosphate positive electrode powder;
[0053] (2) Determine the Fe / Li ratio of the waste lithium iron phosphate by ICP testing, mix a lithium source and a reducing agent into the waste lithium iron phosphate positive electrode material, and ball mill it in a ball mill for 1 hour to achieve a Fe / Li ratio of 1:1.05. The lithium source is lithium hydroxide, and the reducing agent is sucrose. The amount of reducing agent added is 3% of the mass of the waste lithium iron phosphate powder. The mixed waste lithium iron phosphate powder is placed in a nitrogen atmosphere and calcined at 750°C for 3 hours. The electrolyte waste gas is condensed and recovered, the acid gas is removed, and the organic gas (main components are C2H4, CH4, C2H6, etc.) is collected in sequence;
[0054] (3) Mixing organic gas with silicon fluoride gas at atmospheric pressure, controlling the gas flow rate to 60 mL / min and the volume ratio of organic gas to silicon fluoride to be 1:2, evenly spreading the powder obtained by calcining lithium supplementation on a porcelain boat, placing the porcelain boat in the constant temperature zone of the reactor, and then passing the mixed gas into the plasma reactor. The electron energy generated by the plasma reactor is set to 25 eV, the constant temperature zone temperature is adjusted to 400°C, and the reaction is carried out for 2 hours to obtain silicon carbide-coated lithium iron phosphate (silicon carbide mass fraction is 1%). The XRD pattern of the silicon carbide-coated lithium iron phosphate is shown in Figure 2. The waste gas is collected and recycled using SiO2. The reaction equation is as follows: SiO2 + 4HF = SiF4 + 2H2O. The obtained silicon tetrafluoride gas is dried and reused.
[0055] Example 2
[0056] This embodiment provides a method for repairing and regenerating a positive electrode material of a battery, the method comprising the following steps:
[0057] (1) discharging, disassembling and crushing the retired power batteries, and subjecting the obtained battery fragments to pyrolysis treatment at 620° C. for 4 h. The waste gas after pyrolysis is treated in step (2), and the waste lithium iron phosphate positive electrode powder is collected;
[0058] (2) Determine the Fe / Li ratio of the waste lithium iron phosphate by ICP testing, mix a lithium source and a reducing agent into the waste lithium iron phosphate positive electrode material, and ball mill it in a ball mill for 1 hour to achieve a Fe / Li ratio of 1:1.02. The lithium source is lithium hydroxide, and the reducing agent is sucrose. The amount of reducing agent added is 3.2% of the mass of the waste lithium iron phosphate powder. The mixed waste lithium iron phosphate powder is placed in a nitrogen atmosphere and calcined at 780°C for 2.5 hours. The electrolyte waste gas is condensed and recovered, the acid gas is removed, and the organic gas (main components are C2H4, CH4, C2H6, etc.) is collected in sequence;
[0059] (3) Mix the organic gas with silicon fluoride gas at atmospheric pressure, control the gas flow rate to 70 mL / min, and the volume ratio of organic gas to silicon fluoride to be 1:3. Evenly spread the powder obtained by calcining the lithium supplement on a porcelain boat, place the porcelain boat in the constant temperature zone of the reactor, and then pass the mixed gas into the plasma reactor. Set the electron energy generated by the plasma reactor to 27 eV, adjust the constant temperature zone temperature to 380°C, and react for 2 hours to obtain silicon carbide-coated lithium iron phosphate (silicon carbide mass fraction is 1.1%). Collect the waste gas and recycle it using SiO2. The reaction equation is as follows: SiO2 + 4HF = SiF4 + 2H2O. The obtained silicon tetrafluoride gas is dried and reused.
[0060] Example 3
[0061] The only difference between this embodiment and embodiment 1 is that the amount of reducing agent added is 1% of the mass of the waste lithium iron phosphate powder, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0062] Example 4
[0063] The only difference between this embodiment and embodiment 1 is that the amount of reducing agent added is 5% of the mass of the waste lithium iron phosphate powder, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0064] Example 5
[0065] The only difference between this embodiment and embodiment 1 is that the electron energy in step (3) is 15 eV, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0066] Example 6
[0067] The only difference between this embodiment and embodiment 1 is that the electron energy in step (3) is 35 eV, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0068] Example 7
[0069] The only difference between this embodiment and embodiment 1 is that the volume ratio of the organic gas to silicon fluoride in step (3) is 2:1, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0070] Example 8
[0071] The only difference between this embodiment and embodiment 1 is that the volume ratio of the organic gas to silicon fluoride in step (3) is 1:10, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0072] Comparative Example 1
[0073] This comparative example provides a method for repairing and regenerating a positive electrode material of a battery, and the repair and regeneration method comprises the following steps:
[0074] S1: Discharge, dismantle and crush retired power batteries;
[0075] S2: Pyrolysis treatment is performed on the battery fragments pre-treated in S1, and the waste gas after pyrolysis is condensed and recovered to collect the waste lithium iron phosphate positive electrode powder;
[0076] S3: Determine the Fe / Li ratio of the waste lithium iron phosphate using ICP testing. A lithium source and a reducing agent are mixed into the waste lithium iron phosphate cathode material and ball milled for 1 hour to achieve a Fe / Li ratio of 1:1.05. The lithium source is lithium hydroxide, and the reducing agent is sucrose. The reducing agent is added in an amount of 10% of the mass of the waste lithium iron phosphate powder. The mixed waste lithium iron phosphate powder is calcined at 750°C for 3 hours under a nitrogen atmosphere. This yields the repaired, regenerated carbon-coated lithium iron phosphate.
[0077] Comparative Example 2
[0078] This comparative example directly uses silicon carbide solid-phase coating of commercial lithium iron phosphate positive electrode material.
[0079] Performance testing:
[0080] The lithium iron phosphate prepared in the examples and comparative examples was thoroughly stirred and mixed with the conductive agent acetylene black and the binder PVDF in a mass ratio of 90:5:5. An appropriate amount of N-methylpyrrolidone was added, and the slurry was coated on an aluminum foil. The positive electrode was prepared by drying at 120°C in a vacuum dryer for 12 hours. A half-cell was assembled with a metal lithium sheet as the negative electrode, and the electrochemical performance was tested. The test results are shown in Table 1:
[0081] Table 1
[0082] As can be seen from Table 1, according to Examples 1-2, the lithium iron phosphate battery regenerated by the method of the present disclosure can have a 0.1C gram capacity of more than 152.79 mAh / g, a coulombic efficiency of more than 96.41%, a 1C gram capacity of more than 138.09 mAh / g, and a compaction density of 2.511 g / cm 3 above.
[0083] By comparing Example 1 with Examples 3-4, it can be seen that in the repair and regeneration method disclosed in the present invention, the amount of the reducing agent added will affect the effect of obtaining the silicon carbide coated positive electrode material. The effect of obtaining the silicon carbide coated positive electrode material is better when the amount of the reducing agent added is controlled at 2-3% of the mass of the positive electrode material powder. If the amount of the reducing agent added is too large, the carbon coating layer of the regenerated lithium iron phosphate will be too thick, which will cause its capacity to decrease. If the amount of the reducing agent added is too low, the valence state of the iron element in the waste lithium iron phosphate cannot be completely reduced, and it is difficult to initially repair the defective carbon coating layer, resulting in the electrochemical performance and cycle stability of the repaired lithium iron phosphate being difficult to meet commercial needs.
[0084] By comparing Example 1 with Examples 5-6, it can be seen that in the repair and regeneration method disclosed in the present invention, the electron energy of the plasma coating treatment will affect the effect of obtaining the silicon carbide coated positive electrode material. The electron energy of the plasma coating treatment is controlled at 20-30 eV, and the effect of obtaining the silicon carbide coated positive electrode material is better. If the electron energy is too large, although the reaction is promoted, the reaction proceeds rapidly and may produce non-specific reactions, reduce the gram capacity and rate performance, and slightly reduce the coulombic efficiency. If the electron energy is too small and the proportion of organic gas is too small, the reaction rate is slow and the product selectivity is affected, the overall electrochemical performance is reduced, and it cannot be ensured that the reaction can occur or the reaction rate is slow.
[0085] By comparing Example 1 with Examples 7-8, it can be seen that in the repair and regeneration method described in the present disclosure, the volume ratio of organic gas to silicon fluoride will affect the effect of preparing the silicon carbide coated positive electrode material. When the volume ratio of organic gas to silicon fluoride is controlled between 1:1 and 1:5, the effect of preparing the silicon carbide coated positive electrode material is better. If the proportion of organic gas is too large, although it promotes the occurrence of the reaction, it will produce a thicker carbon coating layer, reducing the gram capacity of the repair material. If the proportion of organic gas is too small, the reaction rate is slow and the product selectivity is affected.
[0086] From the comparison between Example 1 and Comparative Example 1, it can be seen that the use of silicon carbide to coat the regenerated lithium iron phosphate can repair the defects of the surface coating layer of the waste lithium iron phosphate, which is beneficial to restoring its electrochemical performance.
[0087] By comparing Example 1 and Comparative Example 2, it can be seen that the silicon carbide coated positive electrode material recovered by the repair method described in the present invention has a similar effect to the silicon carbide coated positive electrode material made from commercial lithium iron phosphate, indicating that the repair and recovery method described in the present application has a better recovery effect, and the carbon capture flow can fix carbon in the coating layer of the regenerated lithium iron phosphate, and will not produce carbon dioxide emissions, which is beneficial to reducing carbon emissions. The fluorine circulation flow can realize the recycling of HF, and does not require further collection and treatment of harmful gases, which is beneficial to reducing environmental pollution.
Claims
1. A method for recycling waste batteries and repairing and regenerating positive electrode materials in a full-chain integrated manner, the repair and regeneration method comprising the following steps: (1) discharging the waste batteries and performing pyrolysis separation to obtain positive electrode material powder; (2) performing lithium supplementation calcination treatment on the positive electrode material powder; (3) An organic gas and silicon tetrafluoride are mixed to obtain a mixed gas, and the mixed gas is used to perform plasma coating treatment on the powder obtained by lithium supplementation calcination to obtain a silicon carbide coated positive electrode material.
2. The repair and regeneration method according to claim 1, wherein: The waste batteries in step (1) include any one of waste lithium iron phosphate batteries, waste lithium cobalt oxide batteries or waste ternary batteries, or a combination of at least two of them.
3. The repair and regeneration method according to claim 1 or 2, wherein: The temperature of the pyrolysis treatment in step (1) is 400-600° C. Optionally, the pyrolysis treatment time is 3 to 8 hours.
4. The repair and regeneration method according to any one of claims 1 to 3, wherein: The lithium supplementation calcination treatment in step (2) includes testing the lithium deficiency amount of the positive electrode material powder by an inductively coupled plasma mass spectrometer, determining the amount of lithium source added, mixing the positive electrode material powder and the lithium source, and calcining after ball milling.
5. The repair and regeneration method according to claim 4, wherein: When the positive electrode material powder is lithium iron phosphate, a reducing agent is added; Optionally, the reducing agent includes any one of sucrose, glucose, cellulose or elemental carbon, or a combination of at least two thereof; Optionally, the amount of the reducing agent added is 1 to 5% of the mass of the positive electrode material powder.
6. The repair and regeneration method according to claim 5, wherein: The amount of the reducing agent added is 2-3% of the mass of the positive electrode material powder.
7. The repair and regeneration method according to any one of claims 4 to 6, wherein: The lithium source includes any one of lithium hydroxide, lithium carbonate, lithium nitrate, lithium oxalate, lithium acetate, lithium dihydrogen phosphate or lithium hydrogen phosphate, or a combination of at least two thereof.
8. The repair and regeneration method according to any one of claims 4 to 7, wherein: The ball milling time is 0.5 to 2 hours.
9. The repair and regeneration method according to any one of claims 4 to 8, wherein: The calcination temperature is 650-800°C; Optionally, the calcination time is 1 to 5 hours.
10. The repair and regeneration method according to any one of claims 4 to 9, wherein: The calcination atmosphere is nitrogen and / or argon.
11. The repair and regeneration method according to any one of claims 1 to 10, wherein: The organic gas in step (3) is obtained by condensing and recovering the waste gas obtained by the pyrolysis in step (1), and collecting the waste gas after removing the acidic gas; Optionally, the organic gas includes any one of C2H4, CH4 or C2H6, or a combination of at least two of them.
12. The repair and regeneration method according to any one of claims 1 to 11, wherein: The volume ratio of the organic gas to silicon tetrafluoride in step (3) is 1:(1-5).
13. The repair and regeneration method according to any one of claims 1 to 12, wherein: The flow rate of the mixed gas in step (3) is 50 to 100 mL / min.
14. The repair and regeneration method according to any one of claims 1 to 13, wherein: The electron energy of the plasma coating treatment in step (3) is 20 to 30 eV; Optionally, the temperature of the plasma coating treatment is 350-500° C.; Optionally, the waste gas obtained by the plasma coating treatment is recovered using SiO2, and the obtained silicon tetrafluoride gas is dried and recycled.
15. The repair and regeneration method according to any one of claims 1 to 14, wherein: Taking the mass of the silicon carbide coated positive electrode material as 100%, the mass fraction of the silicon carbide coating layer is 0.1-2%.
16. The repair and regeneration method according to any one of claims 1 to 15, wherein: The repair and regeneration method comprises the following steps: (1) discharging the waste battery and performing pyrolysis treatment to obtain waste gas and positive electrode material powder; (2) testing the lithium deficiency of the positive electrode material powder by ICP, determining the amount of lithium source added, mixing the positive electrode material powder, the lithium source and the reducing agent, calcining at 650-800° C. for 1-5 hours, wherein the amount of the reducing agent added is 1-5% of the mass of the positive electrode material powder, and condensing and recovering the waste gas, removing acidic gas and collecting organic gas for treatment; (3) The organic gas collected in step (2) and silicon tetrafluoride are mixed in a volume ratio of 1:(1-5) to obtain a mixed gas, and the mixed gas is introduced into a plasma reactor at a flow rate of 50-100 mL / min. The powder obtained by lithium supplementation calcination is subjected to plasma coating treatment for 1-5 hours under the conditions of an electron energy of 20-30 eV and a constant temperature zone temperature of 350-500° C. to obtain a silicon carbide coated positive electrode material, and the obtained waste gas is recovered using SiO2, and the obtained silicon tetrafluoride gas is dried and recycled.
Citation Information
Patent Citations
Method for preparing lithium iron phosphate positive material
CN103390750A
Method for removing organic matters from waste lithium ion batteries through gradient pyrolysis
CN113659227A
Lithium cobalt oxide positive electrode material and regeneration and repair method and application thereof
CN113948788A
Method for repairing and modifying positive electrode active material of waste lithium ion battery
CN114204151A
Direct regeneration method of waste lithium iron phosphate positive electrode material
CN114744315A
Cited By
Method for recycling and converting waste lithium cobalt oxide positive electrode material into high-performance lithium supplement agent, high-performance lithium supplement agent and application of high-performance lithium supplement agent
CN119725838A
Separation, purification and regeneration method of waste lithium iron phosphate electrode material
CN119976831A
Method for combined recovery of lithium iron phosphate and ternary battery powder
CN120423582A
Method for modifying and repairing waste lithium iron phosphate positive electrode material by using tetrabutyl silicate and application of method in deep sea field