Electrolyte, lithium secondary battery, and electrical apparatus

By using the combination of trimethylsilicon, lithium ion and ester groups in lithium ion batteries, a stable interface film is formed, which solves the problem of side reactions in the cathode and anode interface during the cycle of lithium ion batteries, and is significantly Reduces DC resistance and improves battery power and cycling performance.

WO2024230127A1PCT designated stage expired Publication Date: 2024-11-14CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2023/133387
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-05
Filing Date
2023-11-22
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

During the circulation process, the cathode and anode interface side reactions of existing lithium-ion batteries lead to the deposition of electrolyte decomposition products, blocking lithium ion transmission, increasing direct current resistance (DCR), and affecting battery power and cycling performance.

Method used

The electrolyte containing a first additive containing a trimethylsilyl group, a second additive containing a lithium ion and a third additive containing an ester group is used to form a dense and stable interface film at the electrode interface to inhibit side reactions. , reduce initial DCR and improve initial battery power performance and cycling performance.

Benefits of technology

Effectively suppress the cathode and anode interface side reactions in electrochemical energy storage devices, reduce DCR, and improve the battery's power performance, storage performance and cycling performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023133387_14112024_PF_FP_ABST
    Figure CN2023133387_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides an electrolyte, a lithium secondary battery, and an electrical apparatus. The electrolyte comprises additives. The additives comprise a first additive containing a trimethylsilyl group, a second additive containing lithium ions, and a third additive containing an ester group. By means of adding the three additives to the electrolyte, the present application can effectively reduce the initial DCR of the battery, improve the initial power performance, and improve the cycle performance and storage performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte, lithium secondary battery and electrical device Technical Field

[0001] The present application relates to the technical field of lithium batteries, and in particular to an electrolyte, a lithium secondary battery, and an electrical device. Background Art

[0002] Lithium-ion batteries have attracted much attention due to their high specific energy, long cycle life, low self-discharge and good safety performance. Currently, lithium-ion batteries dominate the portable electronics market, and their applications have penetrated into all aspects of daily life, such as cameras, laptops, electric vehicles, etc.

[0003] During the first charge and discharge process of lithium-ion batteries, the electrode material and the electrolyte react at the solid-liquid interface to form a passivation layer covering the surface of the electrode material. This passivation layer is an interface layer that has the characteristics of a solid electrolyte and is an electronic insulator but is Li + An excellent conductor, Li + The passivation layer formed on the anode side is called the solid electrolyte interface (SEI) and the cathode side is called the cathode electrolyte interphase (CEI). High-quality CEI and SEI films can effectively prevent the continuous reaction between the electrode material and the electrolyte at the anode and cathode surfaces, thereby protecting them. Adding appropriate additives to the electrolyte can help form high-quality CEI and SEI films on the anode and cathode surfaces.

[0004] Therefore, there is an urgent need to develop an additive or additive combination that can improve the comprehensive performance of lithium-ion batteries.

[0005] Summary of the Invention

[0006] In view of the above objectives, the first aspect of the present application provides an electrolyte for a lithium secondary battery, comprising additives, wherein the additives include a first additive containing a trimethylsilyl group, a second additive containing lithium ions, and a third additive containing an ester group.

[0007] The first additive containing a trimethylsilyl group can participate in the film formation at the anode interface during the formation and cyclic storage process of the electrochemical energy storage device, and can effectively reduce the initial DCR of the secondary battery and improve the initial power performance of the battery. The third additive containing an ester group can also participate in the film formation at the anode interface during the formation and cyclic storage process of the electrochemical energy storage device, and can effectively inhibit the occurrence of side reactions at the anode interface. The second additive containing lithium ions can participate in the film formation at the cathode interface, effectively inhibiting the occurrence of side reactions at the cathode interface during the cyclic storage process of the electrochemical energy storage device, thereby inhibiting the growth of DCR during the cycle of the electrochemical energy storage device. The combined use of the first additive, the second additive and the third additive can improve the power performance, storage performance and cycle performance of the electrochemical energy storage device.

[0008] In any embodiment, the first additive includes trimethylfluorosilane and / or tris(trimethylsilyl)phosphate.

[0009] In any embodiment, the second additive includes one or more of lithium difluorophosphate, lithium fluorosulfonate, and lithium difluorobisoxalophosphate.

[0010] In any embodiment, the third additive includes a sulfur-containing compound and / or a cyclic carbonate compound. In any embodiment, the third additive includes one or more of vinyl sulfate, 1,3-propane sultone, fluoroethylene carbonate, and vinylene carbonate.

[0011] In any embodiment, the ratio of the mass content W2 of the second additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is 0.02-20.

[0012] In any embodiment, the ratio of the mass content W2 of the second additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is 1-20.

[0013] When the mass content ratio of the first additive to the second additive is within a suitable range, the electrochemical energy storage device can obtain excellent power performance, storage performance and cycle performance.

[0014] In any embodiment, the ratio of the mass content W3 of the third additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is 0.2-40.

[0015] In any embodiment, the ratio of the mass content W3 of the third additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is 2-20.

[0016] When the mass content ratio of the second additive to the third additive is within a suitable range, the electrochemical energy storage device has a reduced DCR value and excellent initial power performance.

[0017] In any embodiment, the additive satisfies one of the following conditions: (1) 0.05%≤W1≤0.5%; (2) 0.01%≤W2≤1%; (3) 0.1%≤W3≤2%.

[0018] In any embodiment, the additive satisfies the following conditions: (1) 0.15%≤W1≤0.5%; (2) 0.01%≤W2≤0.6%; (3) 0.1%≤W3≤1.2%.

[0019] Controlling the mass content of the first additive, the second additive, and the third additive in the film-forming additive in the electrolyte within an appropriate range can effectively inhibit the occurrence of side reactions at the cathode interface and the anode interface of the electrochemical energy storage device, inhibit the growth of the DCR during the cycle of the electrochemical energy storage device, and improve the power performance, storage performance, and cycle performance of the electrochemical energy storage device.

[0020] The electrolyte solution further comprises an electrolyte salt. In any embodiment, the total concentration of the electrolyte salt in the electrolyte solution is 0.6 mol / L to 1.5 mol / L. In any embodiment, the total concentration of the electrolyte salt in the electrolyte solution is 0.8 mol / L to 1.3 mol / L or 0.9 mol / L to 1.2 mol / L.

[0021] The concentration of the electrolyte salt in the electrolyte has good viscosity and excellent ionic conductivity within a suitable range, and the electrolyte can enable the electrochemical energy storage device to have both excellent power performance and good cycle performance and storage performance.

[0022] In any embodiment, the electrolyte salt includes one or more of LiPF6, LiBF4, LiFSI, LiBOB, LiDFOB, LiPO2F2, LiDFOP, LiTFOP, LiAsF6, Li(FSO2)2N, LiCF3SO3, and LiClO4.

[0023] In any embodiment, the electrolyte salt includes LiPF6 and / or LiFSI.

[0024] In any embodiment, the electrolyte salt includes LiPF6 and LiFSI, and the molar ratio of LiPF6 to LiFSI is (2-6):1.

[0025] In any embodiment, the electrochemical energy storage device comprises a secondary battery.

[0026] A second aspect of the present application provides a lithium secondary battery, comprising a positive electrode sheet, a negative electrode sheet, and the electrolyte of the first aspect of the present application.

[0027] In any embodiment, the positive electrode sheet includes a positive electrode active material, the positive electrode active material includes Li d [Ni x Co y X1 z M1 1-x-y-z ]O2, LiMn2O4, Li2MnO3·(1-a)LiAO2, LiM2X2O4 or one or more thereof,

[0028] Wherein, 0.1≤d≤1, X1 includes Mn and / or Al; M1 includes one or more of Co, Ni, Mn, Mg, Cu, Zn, Al, Sn, B, Ga, Cr, Sr, V, Ti, 0≤x<1, 0≤y≤1, 0≤z≤1, x+y+z≤1; A includes one or more of Ni, Co, Mn, 0<a<1; M2 includes one or more of Fe, Mn, Ni, Co; X2O4 h- X2 includes one or more of S, P, As, V, Mo, and W, and h=2 or 3.

[0029] In any embodiment, the film compaction density of the positive electrode sheet is 3.0 g / cm 3 ~3.8g / cm 3 .

[0030] In any embodiment, the film compaction density of the positive electrode sheet is 3.2 g / cm 3 ~3.6g / cm 3 .

[0031] In any embodiment, the negative electrode plate includes a negative electrode active material, and the negative electrode active material includes at least one of artificial graphite, natural graphite, soft carbon, hard carbon, mesophase microcarbon beads, silicon-based materials, and tin-based materials.

[0032] In any embodiment, the negative electrode sheet has a compacted density of 1.2 g / cm 3 ~2.0g / cm 3 .

[0033] In any embodiment, the negative electrode sheet has a compacted density of 1.4 g / cm 3 ~1.7g / cm 3 .

[0034] The compaction density of the positive electrode sheet and the negative electrode sheet of the secondary battery is within an appropriate range, which helps to improve the energy density of the secondary battery and obtain a secondary battery with improved capacity.

[0035] The cathode and anode interfaces of the secondary battery have a passivation film with good performance and low impedance, which gives it good cycle performance and storage performance.

[0036] A third aspect of the present application provides an electrical device comprising the lithium secondary battery of the second aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] FIG1 is a schematic diagram of a lithium secondary battery according to an embodiment of the present application;

[0038] FIG2 is an exploded view of the lithium secondary battery according to one embodiment of the present application shown in FIG1 ;

[0039] FIG3 is a schematic diagram of a battery module according to an embodiment of the present application;

[0040] FIG4 is a schematic diagram of a battery pack according to an embodiment of the present application;

[0041] FIG5 is an exploded view of the battery pack according to an embodiment of the present application shown in FIG4 ;

[0042] 6 is a schematic diagram of an electrical device using a lithium secondary battery as a power source according to an embodiment of the present application;

[0043] Explanation of reference numerals: 1 battery pack; 2 upper case; 3 lower case; 4 battery module; 5 lithium secondary battery; 51 housing; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION

[0044] Below, the embodiments of the electrolyte, lithium secondary battery and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0045] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0046] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0047] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0048] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0049] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0050] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0051] Additives containing trimethylsilyl groups are one of the most widely used additives in lithium-ion battery electrolytes. They can form a film at the battery anode interface, but they cannot inhibit the occurrence of side reactions at the anode interface. During battery cycling, side reactions at the cathode and anode interfaces can cause electrolyte decomposition products to deposit at the cathode and anode interfaces, blocking lithium ion transmission and increasing the DCR, thereby affecting the improvement of battery power performance. These side reactions are often accompanied by the consumption of active lithium, resulting in a decrease in battery cycling performance and storage performance.

[0052] [Electrolyte]

[0053] Based on this, the present application proposes an electrolyte for a lithium secondary battery, comprising additives, wherein the additives include a first additive containing a trimethylsilyl group, a second additive containing lithium ions, and a third additive containing an ester group.

[0054] In this article, the term "electrolyte" refers to the carrier for ion transport in lithium-ion batteries.

[0055] In this article, the term "additive" refers to a component present in a relatively small amount in the electrolyte, which can be a gas, liquid, or solid. Conceptually, the difference between additives, solvents, and lithium salts (or electrolyte salts) lies primarily in their content in the electrolyte.

[0056] As used herein, the term "trimethylsilyl group" refers to a -Si(CH3)3 group.

[0057] In this context, the term "ester group" refers to a -COOR group, where R is selected from substituted or unsubstituted C 1-5 alkyl.

[0058] In this article, the term “C 1-5 "Alkyl" refers to a straight or branched hydrocarbon chain radical consisting solely of carbon and hydrogen atoms, with no unsaturated bonds in the radical, having from one to five carbon atoms, and attached to the remainder of the molecule by a single bond. 1-5 Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, 1-methylethyl (isopropyl), butyl, and pentyl.

[0059] As used herein, the term "substituted" means that at least one hydrogen atom of the compound or chemical moiety is replaced by another chemical moiety, wherein the substituents are independently selected from the group consisting of hydroxyl, thiol, amino, cyano, nitro, aldehyde, halogen, alkenyl, alkynyl, aryl, heteroaryl, C 1-6 Alkyl, C 1-6 Alkoxy.

[0060] In some embodiments, the first additive is trimethylfluorosilane and / or tris(trimethylsilyl)phosphate.

[0061] In some embodiments, the second additive includes one or more of lithium difluorophosphate, lithium fluorosulfonate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), and lithium tetrafluoroborate.

[0062] In some embodiments, the second additive includes one or more of lithium difluorophosphate, lithium fluorosulfonate, and lithium difluorobisoxalophosphate.

[0063] In some embodiments, the third additive includes a sulfur-containing compound and / or a cyclic carbonate compound. In some embodiments, the third additive includes one or more of vinyl sulfate, 1,3-propane sultone, fluoroethylene carbonate, and vinylene carbonate.

[0064] Without being bound by any theory, the electrolyte of the present application incorporates a first additive containing trimethylsilyl groups, which has a high reduction potential. This first additive can preferentially reduce organic solvents and lithium salts in the electrolyte, forming a dense, uniform, and stable interfacial film on the anode surface. The addition of the first additive containing trimethylsilyl groups results in a thinner film on the anode surface, effectively reducing the initial DCR of the battery and improving initial power performance.

[0065] Without being bound by any theory, the third additive in the electrolyte of the present application similarly has a high reduction potential, enabling it to participate in the formation of a film at the anode interface before the organic solvent and lithium salt in the electrolyte are reduced. This can compensate for the insufficient film formation of the first additive and avoid the accumulation of inert substances on the anode surface that are detrimental to lithium ion transport due to anode side reactions such as electrolyte decomposition. Furthermore, the third additive is highly stable and does not generate gas during the formation of the interface film, which does not affect the battery's cycling and storage performance.

[0066] Without being bound by any theory, the second additive in this application can form a dense, stable interfacial film on the surface of the cathode active material before the organic solvent, inhibiting the oxidative decomposition of the organic solvent at the positive electrode, reducing the consumption of active lithium due to side reactions between the cathode active material and the electrolyte, and effectively preventing direct contact between the organic solvent and the cathode active material. Furthermore, the presence of the interfacial film helps reduce the dissolution of transition metals from the cathode active material.

[0067] The combination of the first, second, and third additives not only forms a dense, stable, and uniform interfacial film at the cathode and anode interfaces, but also inhibits cathode and anode side reactions, reducing the consumption of active lithium. Therefore, the electrolyte of the present application enables the battery to have both excellent power performance and good cycle performance and storage performance.

[0068] In the present application, the amounts of the first additive, the second additive, and the third additive may affect the film-forming effects of the cathode and the anode, and thus affect various properties of the battery.

[0069] In some embodiments, the mass content W1 of the first additive in the electrolyte satisfies 0.05%≤W1≤0.5%. In some embodiments, the first additive satisfies 0.05%≤W1≤0.3%, 0.15%≤W1≤0.5%, 0.15%≤W1≤0.3%, or 0.3%≤W1≤0.5%. In some embodiments, the mass content W1 of the first additive is 0.08%, 0.1%, 0.12%, 0.17%, 0.2%, 0.25%, 0.35%, 0.4%, or 0.45%.

[0070] If the first additive content in the electrolyte is too high, due to its inherent low boiling point, it may cause the overall flash point of the electrolyte to decrease, adversely affecting the safety performance of the battery. If the first additive content in the electrolyte is too low, it will not play the role of modifying the negative electrode SEI film, thereby failing to effectively reduce the initial interfacial impedance of the battery and effectively improve the power performance.

[0071] In some embodiments, the mass content W2 of the second additive in the electrolyte satisfies 0.01% ≤ W2 ≤ 1%. In some embodiments, the mass content W2 of the second additive in the electrolyte satisfies 0.05% ≤ W2 ≤ 1%, 0.08% ≤ W2 ≤ 1%, 0.3% ≤ W2 ≤ 1%, 0.6% ≤ W2 ≤ 1%, 0.05% ≤ W2 ≤ 0.6%, 0.08% ≤ W2 ≤ 0.6%, 0.3% ≤ W2 ≤ 0.6%, or 0.05% ≤ W2 ≤ 0.8%. In some embodiments, the mass content W2 of the second additive in the electrolyte is 0.1%, 0.2%, 0.4%, 0.7%, 0.8%, or 0.9%.

[0072] If the content of the second additive in the electrolyte is too high, the electrolyte conductivity may be deteriorated, reducing the electrolyte kinetics. If the content of the second additive in the electrolyte is too low, the film cannot be effectively formed on the positive electrode, and the occurrence of positive electrode interface side reactions during use cannot be effectively suppressed.

[0073] In some embodiments, the mass content W3 of the third additive in the electrolyte satisfies 0.1% ≤ W3 ≤ 2%. In some embodiments, the mass content W3 of the third additive in the electrolyte satisfies 0.1% ≤ W3 ≤ 1.2%, 0.3% ≤ W3 ≤ 2%, 0.4% ≤ W3 ≤ 1.2%, 0.5% ≤ W3 ≤ 1.2%, 0.6% ≤ W3 ≤ 1.2%, 0.3% ≤ W3 ≤ 0.9%, 0.1% ≤ W3 ≤ 0.9%, or 0.1% ≤ W3 ≤ 0.75%. In some embodiments, the mass content W3 of the third additive in the electrolyte is 0.5%, 0.35%, 0.45%, 0.55%, 0.8%, 1%, 1.1%, 1.5%, or 1.8%.

[0074] If the content of the third additive in the electrolyte is too high, it will easily cause the negative electrode film to be too thick, resulting in increased negative electrode interface impedance. If the content of the third additive in the electrolyte is too low, it will not be able to inhibit negative electrode side reactions and protect the negative electrode.

[0075] In some embodiments, the ratio of the mass content W2 of the second additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is 0.02 to 20. In some embodiments, the ratio of W2 to W1 is 1 to 20. In some embodiments, the ratio of the mass content W2 of the second additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is 0.2 to 20, 0.3 to 20, 1.6 to 20, 2 to 20, 3 to 20, 4 to 20, 5 to 20, 10 to 20, or 12 to 20.

[0076] Controlling the ratio of the mass content W2 of the second additive in the electrolyte to the mass content W1 of the first additive in the electrolyte within an appropriate range helps to reduce the amount of additives used in the electrolyte and avoid deterioration of the electrolyte conductivity; at the same time, a dense, stable, and uniform interface film can be formed at the cathode interface, and a uniform interface film can be formed at the anode interface, thereby inhibiting cathode and anode side reactions and reducing the consumption of active lithium, so that the battery can have excellent conductivity, power performance, and good cycle performance and storage performance.

[0077] In the present application, the dosage relationship between the first additive and the third additive can affect the film-forming effect, film thickness and impedance of the anode interface, and ultimately affect the power performance of the battery.

[0078] In some embodiments, the ratio of the mass content W3 of the third additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is 0.2 to 40. In some embodiments, the ratio of W3 to W1 is 2 to 20. In some embodiments, the ratio of the mass content W3 of the third additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is 1 to 40, 1.2 to 40, 2 to 40, 2.5 to 40, 3 to 40, 6 to 40, 1 to 20, 1.2 to 20, 2.5 to 20, 3 to 20, or 6 to 20.

[0079] By controlling the ratio of the mass content W3 of the third additive in the electrolyte to the mass content W1 of the first additive in the electrolyte within an appropriate range, a dense, stable and uniform interface film can be formed at the cathode and anode interfaces, thereby inhibiting anode side reactions and reducing the consumption of active lithium without excessively affecting the impedance of the anode interface, thereby effectively protecting the anode and enabling the battery to have excellent initial power performance.

[0080] In some embodiments, the additive satisfies at least one of the following conditions: (1) 0.05%≤W1≤0.5%; (2) 0.01%≤W2≤1%; (3) 0.1%≤W3≤2%.

[0081] In some embodiments, the additive satisfies the following conditions: (1) 0.15%≤W1≤0.5%; (2) 0.01%≤W2≤0.6%; (3) 0.1%≤W3≤1.2%.

[0082] By controlling the mass content of the first additive, the second additive, and the third additive in the electrolyte within an appropriate range, the electrolyte can enable the battery to have both excellent power performance and good cycle performance and storage performance.

[0083] In some embodiments, the electrolyte further includes an electrolyte salt, such as a lithium salt.

[0084] In some embodiments, the total concentration of the electrolyte salt in the electrolyte (calculated as lithium ion concentration) is 0.6 mol / L to 1.5 mol / L. In some embodiments, the total concentration of the electrolyte salt in the electrolyte is 0.8 mol / L to 1.3 mol / L, 0.6 mol / L to 1.4 mol / L, 0.6 mol / L to 1.3 mol / L, 0.6 mol / L to 1.2 mol / L, 0.7 mol / L to 1.5 mol / L, 0.8 mol / L to 1.5 mol / L, 0.9 mol / L to 1.5 mol / L, 0.8 mol / L to 1.5 mol / L, 0.8 mol / L to 1.4 mol / L, 0.9 mol / L to 1.5 mol / L, 0.9 mol / L to 1.4 mol / L, or 0.9 mol / L to 1.2 mol / L.

[0085] The concentration of the electrolyte salt in the electrolyte is within a suitable range, the electrolyte has a suitable viscosity and excellent ionic conductivity, and the electrolyte can enable the battery to have both excellent power performance and good cycle performance and storage performance.

[0086] In some embodiments, the electrolyte salt includes one or more of LiPF6, LiBF4, LiFSI, LiBOB, LiDFOB, LiPO2F2, LiDFOP, LiTFOP, LiAsF6, Li(FSO2)2N, LiCF3SO3, and LiClO4.

[0087] In some embodiments, the electrolyte salt includes LiPF6 and / or LiFSI.

[0088] In some embodiments, the electrolyte salt includes LiPF6 and LiFSI, and the molar ratio of LiPF6 to LiFSI is (2-6):1.

[0089] The electrolyte for lithium-ion batteries provided in the present application can form a passivation film with good performance at the cathode and anode interfaces of lithium-ion batteries. For example, LiPF6 has poor thermal stability and is easily decomposed to produce HF, which increases the acid content of the electrolyte. The first additive trimethylfluorosilane can bind to the proton hydrogen in HF, reduce the acid content in the electrolyte, and effectively protect the cathode and anode. It can not only inhibit the increase of direct current resistance (DCR) during the cycle and improve power performance, but also significantly improve the cycle performance and storage performance.

[0090] [Lithium secondary battery]

[0091] The present application provides a lithium secondary battery, which includes a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte in any embodiment.

[0092] In some embodiments, the film density of the positive electrode sheet is 3.0 g / cm 3 Above, can be 3.0g / cm 3 ~3.8g / cm 3 In some embodiments, the positive electrode film has a compaction density of 3.2 g / cm 3 ~3.6g / cm 3 In some embodiments, the positive electrode sheet has a compacted density of 3.2 g / cm 3 ~3.5g / cm 3 , 3.3g / cm 3 ~3.6g / cm 3 or 3.3g / cm 3 ~3.5g / cm 3 .

[0093] The compaction density of the positive electrode membrane is within an appropriate range, which helps reduce side reactions at the electrode interface and also helps improve the energy density of the secondary battery. If the positive electrode membrane is compacted too much, the lithium ion transmission channel is reduced, the impedance of the positive electrode increases, the battery polarization becomes larger, and it is easy to cause oxidative decomposition of the electrolyte. If the positive electrode membrane is compacted too little, the active surface area of ​​the positive electrode active material is larger, the reaction area is larger, and the side reactions increase, all of which are detrimental to the battery performance.

[0094] In the lithium secondary battery of the present application, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector and comprising a positive electrode active material. For example, the positive electrode current collector has two surfaces that oppose each other in the thickness direction of the positive electrode current collector, and the positive electrode film layer is disposed on either or both of the two opposing surfaces of the positive electrode current collector.

[0095] In some embodiments, the positive electrode film layer includes a positive electrode active material, which may include one or more of a lithium transition metal oxide, an olivine-structured lithium-containing phosphate, and their respective modified compounds. In the secondary battery of the present application, the modified compound of each of the above-mentioned positive electrode active materials may be a doping modification, a surface coating modification, or a doping and surface coating modification of the positive electrode active material.

[0096] As an example, the lithium transition metal oxide may include one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and modified compounds thereof. As an example, the lithium phosphate containing olivine structure may include one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and modified compounds thereof. These positive electrode active materials may be used alone or in combination of two or more.

[0097] In some embodiments, the positive electrode active material may include one or more of an olivine-structured lithium-containing phosphate and its modified compounds. In other embodiments, the positive electrode active material may be one or more of an olivine-structured lithium-containing phosphate and its modified compounds. The use of these positive electrode active materials in the positive electrode film layer can improve the battery's cycle performance and storage performance while improving the battery's rate performance. The operating voltage of the battery using these positive electrode active materials is not high, generally ≤4.3V. Within this voltage range, the first organic solvent and the first additive are used in combination to achieve a better effect, thereby further improving the battery's cycle performance and storage performance.

[0098] In some embodiments, the positive electrode active material includes Li d [Nix Co y X z M 1-x-y-z ]O2, LiMn2O4, Li2MnO3·(1-a)LiAO2, LiM2X2O4 or one or more thereof,

[0099] Wherein, 0.1≤d≤1, X1 includes Mn and / or Al; M1 includes one or more of Co, Ni, Mn, Mg, Cu, Zn, Al, Sn, B, Ga, Cr, Sr, V, Ti, 0≤x<1, 0≤y≤1, 0≤z≤1, x+y+z≤1; A includes one or more of Ni, Co, Mn, 0<a<1; M2 includes one or more of Fe, Mn, Ni, Co; X2O4 h- X2 includes one or more of S, P, As, V, Mo, and W, and h=2 or 3.

[0100] In some embodiments, the positive electrode active material contains at least Ni, Mn and Co, the molar ratio of Ni to (Ni+Mn+Co) is greater than or equal to 0.5 and less than 0.98, and the molar ratio of Co to (Ni+Mn+Co) is greater than 0.01.

[0101] It is understandable that in order to improve the energy density of the battery cell, a higher voltage, such as 4.5V, is usually used. When the battery cell is fully charged, the positive electrode has a high oxidizing property and can easily oxidize the electrolyte, consuming limited active lithium ions, resulting in poor performance of the battery cell. The first additive and the second additive in the embodiment of the present application can form a film at the interface of the negative electrode plate, play a synergistic effect, inhibit the side reactions at the interface of the negative electrode plate, and reduce the interface DCR.

[0102] In the lithium secondary battery of the present application, the positive electrode film layer generally comprises a positive electrode active material and an optional binder and an optional conductive agent. The positive electrode film layer is generally formed by coating the positive electrode slurry on the positive electrode current collector, drying, and cold pressing. The positive electrode slurry is generally formed by dispersing the positive electrode active material, the optional conductive agent, the optional binder, and any other components in a solvent and stirring them evenly. The solvent may be N-methylpyrrolidone (NMP), but is not limited thereto. The type and content of the conductive agent and the binder can be selected according to actual needs. As an example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. As an example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0103] In the lithium secondary battery of the present application, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, the positive electrode current collector may be aluminum foil. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may be selected from one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may be selected from polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.

[0104] In some embodiments, the negative electrode active material includes at least one of artificial graphite, natural graphite, soft carbon, hard carbon, mesophase microcarbon beads, silicon-based materials, and tin-based materials.

[0105] In some embodiments, the negative electrode film has a compaction density of 1.2 g / cm 3 ~2.0g / cm 3 In some embodiments, the negative electrode film has a compaction density of 1.4 g / cm 3 ~1.7g / cm 3 , 1.5g / cm 3 ~1.7g / cm 3 , 1.4g / cm 3 ~1.6g / cm 3 The compaction density of the negative electrode active material is within a suitable range, which helps to reduce the side reactions at the electrode interface and also helps to improve the energy density of the secondary battery.

[0106] In the lithium secondary battery of the present application, the negative electrode film layer generally comprises a negative electrode active material, an optional binder, an optional conductive agent and other optional auxiliary agents. The negative electrode film layer is generally formed by coating a negative electrode slurry on a negative electrode current collector, drying it and cold pressing it. The negative electrode slurry is generally formed by dispersing the negative electrode active material, an optional conductive agent, an optional binder and other optional auxiliary agents in a solvent and stirring them evenly. The solvent may be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto. The type and content of the conductive agent and the binder may be selected according to actual needs. As an example, the conductive agent may include one or more of superconducting carbon, carbon black (such as acetylene black, Ketjen black, etc.), carbon dots, carbon nanotubes, graphene and carbon nanofibers. As an example, the binder may include one or more of styrene-butadiene rubber (SBR), water-soluble unsaturated resin (SR-1B), water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). Other optional additives may include thickeners (e.g., sodium carboxymethyl cellulose CMC-Na), PTC thermistor materials, etc.

[0107] In the lithium secondary battery of the present application, the negative electrode film layer may be disposed on one side of the negative electrode current collector, or may be disposed on both sides of the negative electrode current collector. For example, the negative electrode current collector has two opposite sides in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite sides of the negative electrode current collector.

[0108] In the lithium secondary battery of the present application, the type of negative electrode current collector can be selected according to actual needs.

[0109] In the lithium secondary battery of the present application, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, the negative electrode current collector may be a copper foil. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may be selected from one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may be selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.

[0110] It should be noted that the negative electrode film parameters (e.g., thickness, compaction density, etc.) given in this application refer to the parameters of the negative electrode film layer on a single side of the negative electrode current collector. When the negative electrode film layer is provided on both sides of the negative electrode current collector, the parameters of the negative electrode film layer on either side that meet the requirements of this application are considered to fall within the scope of protection of this application. The ranges for negative electrode film thickness, compaction density, etc. described in this application refer to the parameters of the negative electrode film layer after cold pressing and used in battery assembly.

[0111] In addition, in the lithium secondary battery of the present application, the negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate described in the present application may further include a conductive primer layer (e.g., composed of a conductive agent and a binder) disposed between the negative electrode current collector and the negative electrode film layer. In other embodiments, the negative electrode plate described in the present application also includes a protective layer covering the surface of the negative electrode film layer.

[0112] In the lithium secondary battery of the present application, the type of the separator can be any known porous structure separator with good chemical stability and mechanical stability.

[0113] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer can be the same or different.

[0114] In some embodiments, the outer packaging of the lithium secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0115] The shape of the battery in this application includes but is not limited to cylindrical, square or other arbitrary shapes. For example, FIG1 is a lithium secondary battery 5 with a square structure as an example.

[0116] In some embodiments, referring to Figure 2, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the lithium secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0117] In some embodiments, lithium secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art based on the application and capacity of the battery module.

[0118] Figure 3 shows an example battery module 4. Referring to Figure 3 , within the battery module 4, multiple lithium secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple lithium secondary batteries 5 may be secured using fasteners.

[0119] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of lithium secondary batteries 5 are received in the receiving space.

[0120] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0121] Figures 4 and 5 illustrate an example battery pack 1. Referring to Figures 4 and 5 , the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0122] [Electrical devices]

[0123] The present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0124] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0125] Figure 6 shows an example of an electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.

[0126] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.

[0127] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0128] 1. Preparation of batteries

[0129] Example 1

[0130] 1) Preparation of electrolyte

[0131] In an argon environment (water content <10ppm, oxygen content <1ppm), 0.05g of trimethylfluorosilane, 0.01g of lithium difluorophosphate, and 0.1g of vinyl sulfate were added to 86.76g of organic solvents of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) (EC:EMC=3:7wt% / wt%), and mixed evenly to obtain a mixture. 10g (0.8mol / L) of LiPF6 and 3.08g (0.2mol / L) of LiFSI were slowly added to the mixture, and after the lithium salt was completely dissolved, an electrolyte was obtained.

[0132] 2) Preparation of positive electrode sheet

[0133] The positive electrode active material LiNi 0.6 Co 0.2 Mn 0.2 O2, conductive agent Super P, and binder polyvinylidene fluoride (PVDF) are used to prepare positive electrode slurry in N-methylpyrrolidone (NMP). The solid content in the positive electrode slurry is 50wt%, and the solid content of LiNi 0.5 Co 0.2 Mn 0.3 The mass ratio of O2, Super P, and PVDF is 8:1:1. The positive electrode slurry is coated on the current collector aluminum foil and dried at 85°C before cold pressing. After trimming, cutting, and slitting, it is dried under vacuum conditions at 85°C for 4 hours to obtain the positive electrode sheet.

[0134] 3) Preparation of negative electrode sheet

[0135] Graphite, the negative electrode active material, 3% silicon dioxide (SiO), a conductive agent Super P, a thickener sodium carboxymethyl cellulose (CMC-Na), and a binder styrene-butadiene rubber (SBR) were mixed uniformly in deionized water to create a negative electrode slurry. The solids content of the negative electrode slurry was 30 wt%, and the mass ratio of graphite, SiO, Super P, CMC, and the binder styrene-butadiene rubber (SBR) was 80:3:12:3:2. The negative electrode slurry was coated onto a current collector copper foil and dried at 85°C. The negative electrode sheet was then cold-pressed, trimmed, cut, and slit, and then dried at 120°C under vacuum for 12 hours to produce the negative electrode sheet.

[0136] 4) Isolation film

[0137] A 16 μm polyethylene (PE) film was used as the separator.

[0138] 5) Battery Preparation

[0139] The positive electrode sheet, separator, and negative electrode sheet of Example 1 are stacked in order, with the separator placed between the positive and negative electrode sheets to isolate the positive and negative electrodes. The bare battery cell is wound and the tabs are welded. The bare battery cell is placed in an outer package, and the electrolyte prepared above is injected into the dried battery cell. The process includes packaging, standing, forming, shaping, and capacity testing to obtain the lithium-ion battery product of Example 1 (the battery has a thickness of 4.0 mm, a width of 60 mm, and a length of 140 mm).

[0140] In Examples 2 to 20, the ratio of each additive in the electrolyte was adjusted by adjusting the amount of the additive and the organic solvent, and other parameters remained basically the same as in Example 1. Specific parameters are shown in Table 1.

[0141] In Examples 21 to 26, the types of the first additive, the second additive, or the third additive were adjusted, and other parameters remained basically the same as in Example 13. Specific parameters are shown in Table 1.

[0142] In Examples 27 and 28, the type of positive electrode active material was adjusted, and other parameters remained basically the same as in Example 13. Specific parameters are shown in Table 1.

[0143] In Example 29, the mass contents of the first additive, the second additive, and the third additive were adjusted by adjusting the amounts of additives and the organic solvent. Other parameters remained basically the same as those in Example 13. Specific parameters are shown in Table 1.

[0144] In Comparative Examples 1 to 3, the composition of the electrolyte was adjusted so that the electrolyte contained two of the first additive, the second additive, and the third additive. Specific parameters are shown in Table 1.

[0145] 2. Test Method

[0146] 1. Test of the compaction density of the positive electrode film

[0147] The compaction density of the film layer of the positive electrode sheet is obtained by calculation. Take a positive electrode sheet with a unit area of ​​S, weigh it as M1, the mass of the aluminum foil under the unit area S is M2, measure the thickness of the positive electrode sheet H1, and the thickness of the aluminum foil is H2. Then the compaction density of the film layer of the positive electrode sheet = (M1-M2) / ((H1-H2)×S).

[0148] 2. Negative electrode film compaction density test

[0149] The compaction density of the film layer of the negative electrode sheet is obtained by calculation. Take a negative electrode sheet with a unit area of ​​s, weigh it as m1, the mass of the aluminum foil under the unit area s is m2, measure the thickness of the negative electrode sheet h1, and the thickness of the aluminum foil is h2. The compaction density of the film layer of the negative electrode sheet = (m1-m2) / ((h1-h2)×s).

[0150] 3. Battery cycle performance

[0151] The battery capacity retention rate test process is as follows: at 25°C, the prepared battery is charged to 4.25V at a constant current of 1C, then charged to a current of 0.05C at a constant voltage of 4.25V, left for 10 minutes, and then discharged to 2.8V at 1C. The obtained capacity is recorded as the initial capacity C0. Repeat the above steps for the same battery mentioned above, and at the same time record the discharge capacity Cn of the battery after the nth cycle. Then the battery capacity retention rate after each cycle is Pn = Cn / C0 × 100%. The 500 point values ​​P1, P2...500 are used as the vertical coordinates, and the corresponding number of cycles is used as the horizontal coordinates to obtain a curve graph of the battery capacity retention rate and the number of cycles. During this test process, the first cycle corresponds to n = 1, the second cycle corresponds to n = 2, ... the 500th cycle corresponds to n = 500. The battery capacity retention rate data corresponding to the embodiment or comparative example in Table 1 are the data measured after 500 cycles under the above test conditions, that is, the value of P500. The test process of the comparative example and other embodiments is the same as above.

[0152] 4. Battery storage performance

[0153] At 25°C, the prepared battery was charged with a constant current of 1C to 4.25V, then charged with a constant voltage to a current of 0.05C, allowed to stand for 10 minutes, discharged with 1C to 2.8V, and the discharge capacity D0 was recorded. The battery was then placed in a constant temperature box at 60°C and kept warm for 60 days. The battery cell was taken out and, after the surface temperature of the battery cell returned to room temperature, discharged with 1C to 2.8V. The battery was then charged with 1C to 4.25V, charged with a constant voltage to 0.05C, allowed to stand for 10 minutes, discharged with 1C to 2.8V, and the discharge capacity D1 was recorded. The high temperature storage capacity retention rate of the battery = D1 / D0×100%.

[0154] 5. Power performance test of lithium-ion batteries

[0155] The prepared battery was charged from 1C to 4.25V, then charged to 0.05C at a constant voltage, allowed to stand for 30min, then discharged at 1C for 0.5h, allowed to stand for 30min, and the voltage V1 after standing was recorded. Then, it was discharged at 4C for 30s with a sampling interval of 0.1s, and the voltage V2 at the end of discharge was recorded. The DC resistance of the battery DCR = (V1-V2) / I, I = 4C.

[0156] 3. Analysis of test results of various embodiments and comparative examples

[0157] Batteries of various examples and comparative examples were prepared according to the above methods, and various parameters were measured. The results are shown in Tables 1 and 2 below.

[0158] Table 1

[0159] Table 2

[0160] According to the above results, the lithium-ion batteries in Examples 1 to 29 all contain a first additive, a second additive, and a third additive. The first additive includes one of trimethylfluorosilane and tris(trimethylsilyl)phosphate, the second additive includes one of lithium difluorophosphate, lithium fluorosulfonate, and lithium difluorobis(oxalatophosphate), and the third additive includes one of vinylene carbonate, vinyl sulfate, fluoroethylene carbonate, and 1,3-propane sultone.

[0161] As can be seen from Examples 1 to 4, when the mass content of the first additive is within the range of 0.05% to 0.5%, the prepared battery can achieve a cycle performance and storage performance of not less than 90%, and a DCR of not more than 45mohm. As can be seen from Examples 2 to 4, when the mass content of the first additive is within the range of 0.15% to 0.5%, the cycle performance and storage performance can be further improved.

[0162] As shown in Examples 5-9, when the mass content of the second additive is within the range of 0.01% to 1%, the prepared batteries can achieve cycle performance and storage performance of not less than 90%, and a DCR of not more than 45mohm. As shown in Examples 5-8, when the mass content of the second additive is within the range of 0.01% to 0.6%, the DCR of the battery can be further reduced.

[0163] As shown in Examples 10-15, when the mass content of the third additive is within the range of 0.1% to 2%, the prepared batteries can achieve a cycle performance of not less than 94%, a storage performance of not less than 94%, and a DCR of not more than 25mohm. As shown in Examples 10-14, when the mass content of the third additive is within the range of 0.1% to 1.2%, the DCR, cycle performance, storage performance, and high-temperature storage volume expansion rate of the prepared batteries can be balanced.

[0164] As can be seen from Examples 21 to 24, the first additive is adjusted to tris(trimethylsilyl)phosphate, the second additive is adjusted to lithium difluorobis(oxaloyl)phosphate, and the third additive is adjusted to fluoroethylene carbonate or 1,3-propane sultone. The prepared batteries can obtain a cycle performance and storage performance of not less than 95%, and a DCR of not more than 20 mohm.

[0165] As can be seen from Examples 25 to 28, the second additive is adjusted to lithium fluorosulfonate, the third additive is adjusted to fluoroethylene carbonate, vinylene carbonate, vinyl sulfate, 1,3-propane sultone, and the positive electrode active material is Li[Ni 0.97 Co 0.01 Mn 0.02 ]O2, the prepared battery has excellent performance, and can obtain a cycle performance and storage performance of not less than 95%, and a DCR of not more than 20mohm.

[0166] It can be seen from Examples 1 to 29 that the ratio of the mass content W2 of the second additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is controlled to meet 0.02 to 20, and the ratio of the mass content W3 of the third additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is controlled to meet 0.2 to 40, so that the prepared battery has a lower DCR, higher cycle performance and storage performance.

[0167] In Comparative Examples 1-3, the use of the first, second, or third additives was reduced, and the battery's cycle performance and storage performance were no higher than 90%. Compared with Examples 1-29, it can be seen that the simultaneous use of the three additives in the electrolyte can effectively reduce the battery's DCR and improve the battery's power performance, cycle performance, and storage performance.

[0168] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. An electrolyte for a lithium secondary battery, characterized in that: The additive comprises an additive, wherein the additive comprises a first additive containing a trimethylsilyl group, a second additive containing lithium ions, and a third additive containing an ester group.

2. The electrolyte according to claim 1, characterized in that The first additive includes trimethylfluorosilane and / or tris(trimethylsilyl)phosphate; The second additive includes one or more of lithium difluorophosphate, lithium fluorosulfonate, and lithium difluorobisoxalate phosphate; The third additive includes a sulfur-containing compound and / or a cyclic carbonate compound.

3. The electrolyte according to claim 1 or 2, characterized in that The third additive includes one or more of vinyl sulfate, 1,3-propane sultone, fluoroethylene carbonate, and vinylene carbonate.

4. The electrolyte according to any one of claims 1 to 3, characterized in that The ratio of the mass content W2 of the second additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is 0.02-20.

5. The electrolyte according to any one of claims 1 to 4, characterized in that The ratio of the mass content W2 of the second additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is 1-20.

6. The electrolyte according to any one of claims 1 to 5, characterized in that The ratio of the mass content W3 of the third additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is 0.2-40.

7. The electrolyte according to any one of claims 1 to 6, characterized in that The ratio of the mass content W3 of the third additive in the electrolyte to the mass content W1 of the first additive in the electrolyte is 2-20.

8. The electrolyte according to any one of claims 1 to 7, characterized in that The mass content W1 of the first additive in the electrolyte, the mass content W2 of the second additive in the electrolyte, and the mass content W3 of the third additive in the electrolyte meet at least one of the following conditions: (1)0.05%≤W1≤0.5%; (2)0.01%≤W2≤1%; (3)0.1%≤W3≤2%。 9. The electrolyte according to any one of claims 1 to 8, characterized in that The mass content W1 of the first additive in the electrolyte, the mass content W2 of the second additive in the electrolyte, and the mass content W3 of the third additive in the electrolyte meet the following conditions: (1)0.15%≤W1≤0.5%; (2)0.01%≤W2≤0.6%; (3)0.1%≤W3≤1.2%。 10. The electrolyte according to any one of claims 1 to 9, characterized in that The electrolyte solution also includes electrolyte salt, and the total concentration of the electrolyte salt is 0.6 mol / L to 1.5 mol / L.

11. The electrolyte according to any one of claims 1 to 10, characterized in that The total concentration of the electrolyte salt in the electrolyte solution is 0.8 mol / L to 1.3 mol / L.

12. The electrolyte according to any one of claims 1 to 11, characterized in that The electrolyte salt includes one or more of LiPF6, LiBF4, LiFSI, LiBOB, LiDFOB, LiPO2F2, LiDFOP, LiTFOP, LiAsF6, Li(FSO2)2N, LiCF3SO3, and LiClO4.

13. The electrolyte according to any one of claims 1 to 12, characterized in that The electrolyte salt includes one or more of LiPF6 and LiFSI.

14. The electrolyte according to any one of claims 1 to 13, characterized in that The electrolyte salt includes LiPF6 and LiFSI, and the molar ratio of LiPF6 to LiFSI is (2-6):

1.

15. A lithium secondary battery, characterized in that: The invention comprises a positive electrode sheet, a negative electrode sheet and the electrolyte according to any one of claims 1 to 14.

16. The lithium secondary battery according to claim 15, characterized in that: The positive electrode sheet includes a positive electrode active material, and the positive electrode active material includes Li d [Ni x Co y X1 z M1 1-x-y-z ]O2, LiMn2O4, Li2MnO3·(1-a)LiAO2, LiM2X2O4 or one or more thereof; Wherein, 0.1≤d≤1, X1 includes Mn and / or Al; M1 includes one or more of Co, Ni, Mn, Mg, Cu, Zn, Al, Sn, B, Ga, Cr, Sr, V, Ti, 0≤x<1, 0≤y≤1, 0≤z≤1, x+y+z≤1; A includes one or more of Ni, Co, Mn, 0<a<1; M2 includes one or more of Fe, Mn, Ni, Co; X2O4 h- X2 includes one or more of S, P, As, V, Mo, and W, and h=2 or 3.

17. The lithium secondary battery according to claim 15 or 16, characterized in that: The compacted density of the positive electrode film is 3.0 g / cm 3 ~3.8g / cm 3 .

18. The lithium secondary battery according to any one of claims 15 to 17, characterized in that: The negative electrode plate includes a negative electrode active material, and the negative electrode active material includes at least one of artificial graphite, natural graphite, soft carbon, hard carbon, mesophase micro carbon beads, silicon-based materials, and tin-based materials.

19. The lithium secondary battery according to any one of claims 15 to 18, characterized in that: The compacted density of the negative electrode film is 1.2 g / cm 3 ~2.0g / cm 3 .

20. An electrical device, characterized in that: A lithium secondary battery comprising the lithium secondary battery according to any one of claims 15 to 19.

Citation Information

Patent Citations

  • Lithium-ion secondary battery electrolyte containing trimethylfluorosilane

    CN110112464A

  • Electrolyte and lithium-ion secondary battery using same

    CN110137570A

  • Electrolyte and electrochemical device

    CN110854433A

  • Electrolyte and lithium ion secondary battery

    CN112054240A

  • Non-aqueous electrolyte with both high-temperature characteristic and low impedance, application thereof and lithium ion battery

    CN112531212A

Cited By

  • Battery cell, battery device and energy storage device

    WO2026200073A1