Battery and electric device
By using LixNi(1-y-z)CoyMzO2-b positive electrode active material and optimized electrolyte components in lithium-ion batteries, the problem of degradation of battery cycle performance under high charging cutoff voltage is solved, and the cycle stability and service life of the battery are significantly improved. .
Patent Information
- Application Number
- PCT/CN2023/094855
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-21
AI Technical Summary
Lithium-ion batteries have poor cycling performance under high charging cutoff voltage and have poor stability, mainly due to the collapse or damage of the positive electrode active material, which leads to poor cycling stability.
LixNi(1-y-z)CoyMzO2-b is used as the positive electrode active material, and nitrile compounds are added to the electrolyte to define the content of cobalt elements and cyano groups, and combined with hexafluorophosphate and vinyl carbonate to optimize the electrolyte components to Improve the stability and battery circulation performance of the positive electrode active material.
It effectively reduces the growth rate of DC internal resistance during the battery cycle, reduces the content of free cobalt ions in the electrolyte, reduces the side reaction of solvents, and improves the cycle stability and service life of the battery under high charging cut-off voltage.
Smart Images

Figure CN2023094855_21112024_PF_FP_ABST
Abstract
Description
Batteries and electrical devices Technical Field
[0001] The present application belongs to the field of battery technology, and specifically relates to a battery and an electrical device. Background Art
[0002] Lithium-ion batteries are not only used in energy storage systems such as hydropower, thermal, wind, and solar power plants, but are also widely used in electric vehicles such as electric bicycles, electric motorcycles, and electric cars, as well as in military equipment and aerospace. With the increasing demand for battery energy density, increasing the upper voltage limit (charge cutoff voltage) of ternary materials is an effective solution. However, as the voltage increases, the battery's cycle performance decreases.
[0003] Summary of the Invention
[0004] In view of the technical problems existing in the background technology, the present application provides a battery that can alleviate the problem of poor battery cycle stability under high charging cut-off voltage.
[0005] In order to achieve the above object, the first aspect of the present application provides a battery, the battery comprising a positive electrode sheet and an electrolyte, wherein the positive electrode sheet comprises Li x Ni (1-y-z) Co y M z O 2-b , wherein M includes at least one element selected from Mn, Al, Fe, Ti, Mg, Cr, Ga, Cu, Zn, Nb and Zr, 0<x≤1.2, 0.18≤y≤0.25, 0≤z≤0.2, 1-yz≥0.55, 0≤b≤0.2; the electrolyte includes a nitrile compound, and based on the total mass of the electrolyte, the content of cyanide in the electrolyte is w%, w>0 and satisfies 0.04≤y / w≤0.4.
[0006] The battery of this application comprises Li x Ni (1-y-z) Co y M z O 2-b The invention relates to a positive electrode sheet of a positive electrode active material and an electrolyte including a nitrile compound, by limiting the content of cobalt element in the positive electrode active material and the content of cyanide group in the electrolyte to satisfy 0.04≤y / w≤0.4 (0.18≤y≤0.25, the content of cyanide group in the electrolyte is w%). On the one hand, the growth rate of (DC internal resistance) DCR during the battery cycle can be reduced, and on the other hand, the content of free cobalt ions in the electrolyte can be reduced, the side reaction of the solvent can be reduced, and the stability of the positive electrode active material can be improved, thereby improving the cycle stability of the battery under high charge cut-off voltage.
[0007] In some embodiments, 0.1≤y / w≤0.3. Thus, the cycle stability of the battery at a high charge cut-off voltage can be improved while reducing the DCR growth rate of the battery.
[0008] In some embodiments, 0.5≤w≤5, preferably 0.5≤w≤2. Thus, the free cobalt ions in the electrolyte can be effectively complexed, the side reaction of the solvent can be reduced, and the cycle stability of the battery at a high charge cut-off voltage can be improved.
[0009] In some embodiments, 0.18≤y≤0.2. This can effectively reduce the growth rate of DCR during battery cycling and improve the cycling stability of the battery at high charge cut-off voltage.
[0010] In some embodiments, the nitrile compound comprises a polynitrile compound, and optionally, the carbon chain length between two adjacent cyano groups in the polynitrile compound does not exceed 8 carbon atoms. Thus, the molecular structure of the polynitrile compound is stable, thereby facilitating the stability of the electrolyte.
[0011] In some embodiments, the polynitrile compound includes a bisnitrile compound. Thus, the bisnitrile compound can be adsorbed in parallel on the surface of the positive electrode active material, thereby stabilizing the positive electrode electrolyte interface film (CEI film) on the surface of the positive electrode sheet, thereby improving the cycle stability of the battery.
[0012] In some embodiments, the nitrile compound comprises a mononitrile compound, and optionally, the carbon chain length of the mononitrile compound does not exceed 4 carbon atoms. Thus, the molecular structure of the mononitrile compound is stable, thereby facilitating the stability of the electrolyte.
[0013] In some embodiments, the electrolyte further comprises hexafluorophosphate and ethylene carbonate, wherein the hexafluorophosphate content is n%, and the ethylene carbonate content is m%, based on the total mass of the electrolyte, where n>0, m>0, and 2≤m / n≤2.5. This effectively reduces the risk of ethylene carbonate oxidation at the positive electrode.
[0014] In some embodiments, m and n satisfy at least one of the following conditions: 15≤m≤30, preferably 20≤m≤30; 8≤n≤15, preferably 10≤n≤14. This can effectively reduce the risk of ethylene carbonate being oxidized at the positive electrode.
[0015] In some embodiments, 0.1≤w / m≤0.2. This can increase the service life of the positive electrode and the negative electrode and improve the cycle stability of the battery.
[0016] In some embodiments, the Li x Ni (1-y-z) Co yM z O 2-b The specific surface area is ≤3m 2 / g. Thus, the occurrence of side reactions in the electrolyte can be reduced.
[0017] In some embodiments, the water content in the electrolyte is ≤0.002% based on the total mass of the electrolyte, thereby improving the integrity of the CEI membrane and the cycle stability of the battery.
[0018] In some embodiments, the content of hydrofluoric acid in the electrolyte is ≤0.015% based on the total mass of the electrolyte, thereby improving the integrity of the CEI membrane and the cycle stability of the battery.
[0019] The second aspect of the present application provides an electrical device, comprising the battery according to the first aspect of the present application, so that the electrical device has excellent cycle stability.
[0020] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become obvious from the description below, or will be learned through practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiment below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the drawings to represent the same components. In the drawings:
[0022] FIG1 is a schematic structural diagram of a battery according to an embodiment of the present application;
[0023] FIG2 is a schematic structural diagram of a battery module according to an embodiment of the present application;
[0024] FIG3 is a schematic structural diagram of a battery pack according to an embodiment of the present application;
[0025] FIG4 is an exploded view of FIG3 ;
[0026] FIG5 is a schematic diagram of an embodiment of an electric device using a battery as a power source.
[0027] Explanation of reference numerals: 1: secondary battery; 2: battery module; 3: battery pack; 4: upper case; 5: lower case. DETAILED DESCRIPTION
[0028] The following embodiments of the technical solution of the present application are described in detail. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only used as examples and are not intended to limit the scope of protection of the present application.
[0029] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0030] For the sake of clarity, only some numerical ranges are specifically disclosed herein. However, any lower limit may be combined with any upper limit to form an unspecified range; and any lower limit may be combined with other lower limits to form an unspecified range, and similarly, any upper limit may be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value may itself serve as a lower limit or upper limit and be combined with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.
[0031] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.
[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.
[0033] Currently, market developments indicate that lithium-ion batteries are becoming increasingly widely used. They are not only used in energy storage systems such as hydropower, thermal power, wind power, and solar power plants, but are also widely used in electric vehicles like electric bicycles, electric motorcycles, and electric cars, as well as in military equipment and aerospace. As the application of lithium-ion batteries continues to expand, market demand is also growing.
[0034] Cathode active materials are the core and key materials of lithium-ion batteries. Ternary materials are one of the most widely used cathode active materials. As cathode active materials in lithium-ion batteries, ternary materials can increase the battery's energy density. However, as the voltage increases, as lithium ions are released, ternary materials are prone to collapse or damage, resulting in poor stability of the ternary materials, which in turn affects the battery's cycling stability.
[0035] In order to alleviate the problem of collapse or damage of ternary materials, the composition of the positive active material and the electrolyte can be optimized to improve the stability of the positive active material, thereby improving the cycle stability of the battery. Specifically, after the voltage of the lithium-ion battery is increased, as lithium ions are released into the electrolyte, vacancies appear on the surface of the positive active material, causing the positive active material to collapse or break. The cobalt ions in the positive active material can increase the diffusion rate of lithium ions. When the lithium ions on the surface of the positive active material are released into the electrolyte, the lithium ions inside the positive active material can diffuse to the surface of the positive active material to replenish the released lithium ions, thereby preventing the positive active material from collapsing, improving the stability of the positive active material, and thereby improving the cycle stability of the battery. However, excessive cobalt content will catalyze the oxidation of the solvent in the electrolyte and deteriorate the life of the battery, while the cyano group can effectively complex the free cobalt ions, prevent the free cobalt ions from oxidizing the solvent, and reduce the side reactions of the solvent.
[0036] The battery disclosed in the embodiments of the present application can be used in electrical devices that use the battery as a power source or various energy storage systems that use the battery as an energy storage element. The electrical device can be, but is not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, and the like. Among them, the electric toy can include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, and the like, and the spacecraft can include airplanes, rockets, space shuttles, and spacecraft, and the like.
[0037] The first aspect of the present application provides a battery, the battery comprising: a positive electrode plate and an electrolyte, wherein the positive electrode plate comprises Li x Ni (1-y-z) Co y M z O 2-b , wherein M includes at least one element selected from Mn, Al, Fe, Ti, Mg, Cr, Ga, Cu, Zn, Nb and Zr, 0<x≤1.2, 0.18≤y≤0.25, 0≤z≤0.2, 1-yz≥0.55, 0≤b≤0.2; the electrolyte includes a nitrile compound, and based on the total mass of the electrolyte, the content of cyanide in the electrolyte is w%, w>0 and satisfies 0.04≤y / w≤0.4.
[0038] Without wishing to be bound by any theory, this application employs x Ni (1-y-z) Co y M z O 2-bIn batteries with positive electrode sheets containing a nitrile compound and an electrolyte containing a nitrile compound, a corresponding amount of cobalt in the positive electrode material (0.18≤y≤0.25) can significantly improve the electronic and ionic impedances of the positive electrode material, thereby suppressing the DCR growth rate during battery cycling. At the same time, a corresponding amount of cobalt in the positive electrode material (0.18≤y≤0.25) can increase the diffusion rate of lithium ions in the positive electrode material. At high charge cut-off voltages, as lithium ions are released from the surface of the positive electrode material, lithium ions located within the positive electrode material can quickly diffuse to the surface of the positive electrode material, thereby reducing the probability of collapse or damage of the positive electrode material, improving the stability of the positive electrode material, and improving the cycle stability of the battery at high charge cut-off voltages. However, if the cobalt content is too high, the free cobalt ions have a strong catalytic effect and can catalyze the oxidation of the solvent in the electrolyte, causing gas production and shortening the battery life. Moreover, the free cobalt ions are easily dissolved in the electrolyte. The dissolved cobalt ions are reduced at the negative electrode, which may block the transmission of lithium ions. By adding nitrile compounds to the electrolyte, the cyanide groups in the nitrile compounds can effectively complex the free cobalt ions in the electrolyte, inhibiting the dissolution of cobalt ions in the electrolyte, and stably fixing the free cobalt ions on the surface of the positive electrode active material. At the same time, the complexed cobalt ions lose their catalytic properties, thereby reducing the side reactions of the solvent. In this application, the cobalt content in the positive electrode active material (0.18≤y≤0.25) and the cyanide content in the electrolyte (w%) satisfy 0.04≤y / w≤0.4. On the one hand, it can reduce the growth rate of DCR during the battery cycle; on the other hand, it can reduce the content of free cobalt ions in the electrolyte, reduce the side reactions of the solvent, and at the same time improve the stability of the positive electrode active material and improve the cycle stability of the battery at a high charge cut-off voltage.
[0039] In the present application, "nitrile compound" refers to a compound including a cyano group in its structure.
[0040] In this application, the cyano content is quantitatively analyzed by gas chromatography with reference to GB / T-9722-2006 General Rules for Gas Chromatography. The cyano groups in the electrolyte are separated in the chromatographic column and a detection signal spectrum of each component is generated. The retention time is used for component qualitative analysis, and a standard solution is prepared to correct the peak area to achieve quantitative analysis of the cyano groups.
[0041] In some embodiments, the positive electrode active material Li x Ni (1-y-z) Co y M z O 2-b 0<x≤1.2, for example, 0.2≤x≤1.2, 0.4≤x≤1, 0.5≤x≤0.8, 0.6≤x≤0.7, etc. Thus, the positive electrode active material includes lithium ions in such a content that the battery has a higher capacity.
[0042] It should be noted that in the positive electrode sheet, battery, or electrical device, lithium ions are consumed during the battery formation and cycling processes, so the measured lithium content x in the positive electrode active material may be less than 1. At the same time, if the positive and negative electrode sheets are replenished with lithium, the measured lithium content x in the positive electrode active material may be greater than 1 after the battery formation and cycling processes.
[0043] In some embodiments, the positive electrode active material Li x Ni (1-y-z) Co y M z O 2-b , 0.18≤y≤0.25, for example, 0.19≤y≤0.24, 0.2≤y≤0.23, 0.21≤y≤0.22, etc. In other embodiments, the above-mentioned positive electrode active material Li x Ni (1-y-z) Co y M z O 2-b , 0.18≤y≤0.2. Therefore, the inclusion of the cobalt element at this content in the positive electrode active material can significantly improve the electronic impedance and ionic impedance of the positive electrode active material, suppress the DCR growth rate during the battery cycle, and at the same time, the cobalt element at this content in the positive electrode active material can increase the diffusion rate of lithium ions in the positive electrode active material. At a high charge cut-off voltage, as lithium ions are released from the surface of the positive electrode active material, lithium ions located inside the positive electrode active material can quickly diffuse to the surface of the positive electrode active material, thereby reducing the probability of collapse or damage of the positive electrode active material, improving the stability of the positive electrode active material, and improving the cycle stability of the battery at a high charge cut-off voltage.
[0044] In some embodiments, the positive electrode active material Li x Ni (1-y-z) Co y M z O 2-b , 0≤z≤0.2, for example, 0≤z≤0.1, 0.05≤z≤0.1, 0.1≤z≤0.15, 0.15≤z≤0.2, etc., and 1-yz≥0.55, for example, 0.55≤1-yz≤0.82, 0.58≤1-yz≤0.8, 0.6≤1-yz≤0.78, 0.62≤1-yz≤0.75, 0.65≤1-yz≤0.72, 0.68≤1-yz≤0.7, etc. Thus, the positive electrode active material of this composition has excellent energy density.
[0045] In some embodiments, the positive electrode active material Li x Ni(1-y-z) Co y M z O 2-b , 0≤b≤0.2, for example, 0.05≤b≤0.2, 0.1≤b≤0.2, 0.15≤b≤0.2, etc.
[0046] It should be noted that in the positive electrode sheet, battery or electrical device, due to the battery cycling process, the oxygen element in the positive electrode active material is lost, so the measured oxygen element content 2-b in the positive electrode active material may be less than 2.
[0047] In some embodiments, the positive electrode active material Li x Ni (1-y-z) Co y M z O 2-b Specific surface area BET≤3m 2 / g, for example, BET≤0.5m 2 / g, BET≤1m 2 / g, BET≤1.5m 2 / g, BET≤2m 2 / g, BET≤2.5m 2 / g, etc. This can reduce the occurrence of side reactions in the electrolyte.
[0048] In this application, the specific surface area of the positive electrode active material can be tested by referring to the following method: using the American Microelectronics multi-station fully automatic specific surface area and pore analyzer GeminiVII2390, take about 7g of the sample and put it into a 9cc long tube with a bulb, degas at 200℃ for 2h, and then put it into the host for testing to obtain the BET (specific surface area) data of the positive electrode active material.
[0049] In some embodiments, the cobalt content y in the positive electrode active material and the cyanide content w% in the electrolyte in the above-mentioned battery satisfy 0.04≤y / w≤0.4, for example, 0.05≤y / w≤0.35, 0.1≤y / w≤0.3, 0.15≤y / w≤0.25, 0.2≤y / w≤0.25, etc.
[0050] This application limits the cobalt content y in the positive electrode active material of the above-mentioned battery and the cyanide content w% in the electrolyte to 0.04≤y / w≤0.4. On the one hand, it can reduce the growth rate of DCR during battery cycling. On the other hand, it can reduce the content of free cobalt ions in the electrolyte, reduce solvent side reactions, and at the same time improve the stability of the positive electrode active material, thereby improving the cycle stability of the battery at high charge cut-off voltage. In other embodiments, the cobalt content y in the positive electrode active material of the above-mentioned battery and the cyanide content w% in the electrolyte meet 0.1≤y / w≤0.3.
[0051] In some embodiments, the cyanide content in the electrolyte of the battery is w%, which satisfies 0.5≤w≤5, for example, 1≤w≤4.5, 1.5≤w≤4, 2≤w≤3.5, 2.5≤w≤3, etc. In other embodiments, the cyanide content in the electrolyte of the battery is w%, which satisfies 0.5≤w≤2.
[0052] The electrolyte including the above-mentioned content of cyanide can effectively complex the free cobalt ions in the electrolyte, inhibit the dissolution of cobalt ions in the electrolyte, and stably fix the free cobalt ions on the surface of the positive electrode active material. At the same time, the complexed cobalt ions lose their catalytic properties, thereby reducing the side reactions of the solvent and improving the battery cycle performance.
[0053] In some embodiments, the nitrile compound in the electrolyte may include at least one of a single nitrile compound and a polynitrile compound. For example, when the nitrile compound includes a single nitrile compound, in some specific embodiments, the length of the carbon chain in the single nitrile compound does not exceed 4 carbons. The single nitrile compound molecule of this carbon chain length is not easy to decompose in the electrolyte, which can improve the stability of the single nitrile compound, and then improve the stability of the electrolyte, further improving the complexation of free cobalt ions. In other embodiments, the single nitrile compound may include acetonitrile, propionitrile and acrylonitrile etc.
[0054] It should be noted that the “polynitrile compound” in the present application refers to a nitrile compound having two or more cyano groups.
[0055] In some embodiments, the nitrile compound includes a polynitrile compound. In some specific embodiments, the carbon chain length between two adjacent cyano groups in the polynitrile compound does not exceed 8 carbon atoms. Polynitrile compound molecules with this carbon chain length are not easily decomposed in the electrolyte, which can improve the stability of the polynitrile compound, thereby improving the stability of the electrolyte and further improving the complexation effect on free cobalt ions. In other embodiments, the polynitrile compound may include a dinitrile compound, a trinitrile compound, etc., and the trinitrile compound includes 1,3,6-hexanetrinitrile. In some embodiments, the polynitrile compound includes a dinitrile compound, for example, the dinitrile compound may include at least one of malononitrile, succinonitrile, suberonitrile, and adiponitrile.
[0056] The dinitrile compounds of the present application can be adsorbed in parallel on the surface of the positive electrode active material. Both ends of the dinitrile compound molecular chain are adsorbed on the surface of the positive electrode active material, which can improve the stability of the CEI film on the surface of the positive electrode sheet to a certain extent, thereby improving the cycle stability of the battery. In other embodiments, the dinitrile compound includes at least one of succinonitrile and suberonitrile.
[0057] In some embodiments, the electrolyte of the present application further includes: hexafluorophosphate and ethylene carbonate. Based on the total mass of the electrolyte, the hexafluorophosphate content is n%, and the ethylene carbonate content is m%, where m and n satisfy n>0, m>0, and 2≤m / n≤2.5, for example, 2.1≤m / n≤2.5, 2.2≤m / n≤2.5, 2.3≤m / n≤2.5, 2.4≤m / n≤2.5, etc. The ethylene carbonate content and the hexafluorophosphate content satisfying the above ratio can, on the one hand, simultaneously utilize the film-forming properties of ethylene carbonate at the negative electrode and the property of hexafluorophosphate to improve the conductivity of the electrolyte, and on the other hand, reduce the oxidation of ethylene carbonate on the surface of the positive electrode, thereby improving the cycle stability of the battery. In some specific embodiments, the electrolyte can include lithium hexafluorophosphate.
[0058] In the present application, the content of hexafluorophosphate is detected and quantified by ion chromatography in the electrolyte. For details, please refer to JY / T-020 General Rules for Ion Chromatography.
[0059] In some embodiments, the content m% of ethylene carbonate in the electrolyte satisfies 15≤m≤30, such as 16≤m≤29, 17≤m≤28, 18≤m≤27, 19≤m≤26, 20≤m≤25, 21≤m≤24, 22≤m≤23, etc. In some embodiments, the content m% of ethylene carbonate in the electrolyte satisfies 20≤m≤30. The ethylene carbonate content in this application can form a stable (solid electrolyte interface) SEI film on the surface of the negative electrode, thereby improving the cycle stability of the battery.
[0060] In some embodiments, the hexafluorophosphate content n% in the electrolyte satisfies 8≤n≤15, such as 9≤n≤14, 10≤n≤13, 11≤n≤12, etc. In other embodiments, the hexafluorophosphate content n% in the electrolyte satisfies 10≤n≤14. The hexafluorophosphate content in this application can effectively increase the conductivity of the electrolyte, thereby improving the kinetic performance of the battery.
[0061] In some embodiments, the cyanide content w% and the ethylene carbonate content m% in the above-mentioned electrolyte satisfy 0.1≤w / m≤0.2, for example, 0.11≤w / m≤0.19, 0.12≤w / m≤0.18, 0.13≤w / m≤0.17, 0.14≤w / m≤0.16, 0.14≤w / m≤0.15, etc.
[0062] The present application limits the content w% of the cyano group in the electrolyte and the content m% of the ethylene carbonate to satisfy 0.1≤w / m≤0.2. The cyano group can improve the cycle performance of the battery to a certain extent and reduce the growth rate of the battery DCR. The ethylene carbonate improves the film-forming performance of the negative electrode. The cyano group and the ethylene carbonate play a synergistic role. While the cyano group effectively complexes the free cobalt ions and the film-forming properties of the ethylene carbonate on the negative electrode are exerted, the service life of the positive electrode and the negative electrode can be improved.
[0063] In some embodiments, the lithium salt in the above-mentioned electrolyte may include, in addition to lithium hexafluorophosphate, one or more of lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSi), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0064] In some embodiments, the solvent in the electrolyte may include, in addition to ethylene carbonate, propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE). One or more of the following.
[0065] In some embodiments, the electrolyte further includes additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives capable of improving certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature performance.
[0066] In some embodiments, the water content in the electrolyte is ≤0.002% based on the total mass of the electrolyte, thereby improving the integrity of the CEI membrane and the cycle performance of the battery.
[0067] In this application, "water content in electrolyte" refers to the water content per unit mass of electrolyte. The test method for "water content in electrolyte" is: inject the electrolyte into the electrolytic cell that has reached equilibrium, and after the indicator electrode detects H2O, electrode oxidation occurs. - I2 is a quantitative chemical reaction between I2 and H2O, so the water content is calculated. According to HG / T4067-2015 Determination of Water in Hexafluorophosphate Electrolyte 5.9, the quantitative reaction formula of I2 and H2O is: H2O+I2+SO2+3C5H5N=2C5H5N·HI+C5H5N·SO3. The amount of water is calculated by the amount of iodine consumed.
[0068] In some embodiments, the content of hydrofluoric acid in the electrolyte is ≤0.015% based on the total mass of the electrolyte, thereby improving the integrity of the CEI membrane and the cycle performance of the battery.
[0069] In this application, "hydrofluoric acid content in electrolyte" refers to the content of hydrofluoric acid in electrolyte per unit mass. "Hydrofluoric acid content in electrolyte" adopts acid-base titration hydrofluoric acid content analysis (SYA). Under dry environment, the free acid in electrolyte is titrated with triethylamine standard solution, and the HF content is calculated as follows: HF (ppm) = (V2-V1) / 1000*C*20 / m*1000000 = (V2-V1)*C / m*20,000; where: 0.01 - concentration of SYA standard solution, 0.02mol / L; V0 - volume reading of burette before starting titration, ml; V - volume reading of burette at the end point after adding electrolyte sample, ml; 20 - molar molecular weight of HF, g / mol; m - amount of electrolyte weighed, g; 20000 - coefficient for conversion to ug / g.
[0070] In some embodiments, the positive electrode sheet generally includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, and the positive electrode active material layer includes the above-mentioned positive electrode active material.
[0071] The positive electrode current collector may be a conventional metal foil or a composite current collector (a metal material may be disposed on a polymer substrate to form a composite current collector). As an example, the positive electrode current collector may be an aluminum foil.
[0072] The positive electrode active material layer in the positive electrode sheet may also optionally include a binder, a conductive agent and other optional additives.
[0073] As an example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, Super P (SP), graphene, and carbon nanofibers.
[0074] As an example, the adhesive may include one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB).
[0075] A battery is a battery that can be recharged to activate the active materials after discharge and continue to be used.
[0076] Typically, a battery consists of a positive electrode, a negative electrode, a separator, and an electrolyte. During the battery's charge and discharge processes, active ions are inserted and removed between the positive and negative electrodes. The separator is placed between the positive and negative electrodes to isolate them. The electrolyte conducts ions between the positive and negative electrodes.
[0077] In a battery, the negative electrode plate generally includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode active material.
[0078] The negative electrode current collector may be a conventional metal foil or a composite current collector (for example, a metal material may be disposed on a polymer substrate to form a composite current collector). As an example, the negative electrode current collector may be a copper foil.
[0079] The specific type of the negative electrode active material is not limited, and active materials that can be used for the negative electrode of the battery known in the art can be used, and those skilled in the art can choose according to actual needs. As an example, the negative electrode active material may include but is not limited to one or more of artificial graphite, natural graphite, hard carbon, soft carbon, silicon-based materials and tin-based materials. The silicon-based material may include one or more of elemental silicon, silicon oxide compounds (such as silicon monoxide), silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may include one or more of elemental tin, tin oxide compounds, and tin alloys. These materials can all be obtained through commercial channels.
[0080] In some embodiments, to further improve the energy density of the battery, the negative electrode active material may include a silicon-based material.
[0081] The negative electrode active material layer may also optionally include a binder, a conductive agent, and other optional auxiliary agents.
[0082] As an example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0083] As an example, the adhesive may include one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB).
[0084] As examples, other optional additives may include thickeners and dispersants (eg, sodium carboxymethyl cellulose CMC-Na), and PTC thermistor materials.
[0085] As the above-mentioned isolation membrane, the present application has no special restrictions, and any well-known porous structure isolation membrane with electrochemical stability and mechanical stability can be selected according to actual needs. For example, it can be a single-layer or multi-layer film containing one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride.
[0086] The embodiment of the present application has no particular limitation on the shape of the battery, which can be cylindrical, square or any other shape. FIG1 shows a secondary battery 1 with a square structure as an example.
[0087] In some embodiments, the secondary battery may include an outer packaging for encapsulating the positive electrode sheet, the negative electrode sheet, and the electrolyte.
[0088] In some embodiments, the outer packaging may include a housing and a cover. The housing may include a bottom plate and side plates connected to the bottom plate, with the bottom plate and side plates enclosing a receiving cavity. The housing may have an opening communicating with the receiving cavity, and the cover may be positioned over the opening to seal the receiving cavity.
[0089] The positive electrode sheet, negative electrode sheet, and separator can be wound or laminated to form an electrode assembly. The electrode assembly is encapsulated in the housing. The electrolyte is infiltrated into the electrode assembly. The number of electrode assemblies in a battery can be one or more, and can be adjusted according to needs.
[0090] In some embodiments, the outer packaging of the battery may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell.
[0091] The outer packaging of the battery may also be a soft bag, such as a bag-type soft bag. The material of the soft bag may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0092] In some embodiments, the batteries can be assembled into a battery module, and the number of sodium-ion batteries contained in the battery module can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module.
[0093] Figure 2 shows an example battery module 2. Referring to Figure 2 , within the battery module 2, multiple secondary batteries 1 may be arranged sequentially along the length of the battery module 2. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 1 may be secured together using fasteners.
[0094] The battery module 2 may further include a housing having a housing space, wherein the housing space accommodates a plurality of secondary batteries 1. In some embodiments, the battery modules may be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0095] Figures 3 and 4 illustrate an example battery pack 3. Referring to Figures 3 and 4 , the battery pack 3 may include a battery box and multiple battery modules 2 disposed within the battery box. The battery box comprises an upper case 4 and a lower case 5. The upper case 4 can be placed over the lower case 5 to form an enclosed space for accommodating the battery modules 2. The multiple battery modules 2 can be arranged in any manner within the battery box.
[0096] [Electrical devices]
[0097] The present application also provides an electrical device, which includes at least one of the battery, battery module and battery pack. The battery, battery module or battery pack can serve as a power source for the electrical device, and can also serve as an energy storage unit for the electrical device. The electrical device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck), an electric train, a ship, a satellite, and an energy storage system.
[0098] The electrical device may select a secondary battery, a battery module or a battery pack according to its usage requirements.
[0099] Figure 5 shows an example of an electric device. This device includes a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the battery, a battery pack or battery module can be used.
[0100] As another example, electric devices may include mobile phones, tablet computers, and laptop computers. These electric devices are generally required to be lightweight and thin, and may use batteries as power sources.
[0101] In order to make the technical problems, technical solutions and beneficial effects solved by the embodiments of the present application clearer, the following will be further described in detail with reference to the embodiments and drawings. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is in no way intended to limit the present application and its applications. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0102] Example 1
[0103] 1. Preparation of positive electrode sheet
[0104] The polyvinylidene fluoride binder is fully dissolved in N-methylpyrrolidone, and the carbon black conductive agent and the positive electrode active material Li are added. x Ni (1-y-z) Co y M z O 2-b A uniformly dispersed positive electrode slurry (the mass ratio of polyvinylidene fluoride binder, carbon black conductive agent and positive electrode active material is 10:10:80) was prepared (its composition is shown in Table 1). The positive electrode slurry was evenly coated on the upper and lower surfaces of the aluminum foil, and then transferred to a vacuum drying oven for complete drying. The obtained electrode sheet was rolled and then punched to obtain the positive electrode sheet.
[0105] 2. Preparation of negative electrode sheet
[0106] Artificial graphite, carbon nanotube material and binder sodium carboxymethyl cellulose are added to water in a mass ratio of 8:1:1 and stirred to form a uniform negative electrode slurry. The negative electrode slurry is coated on the upper and lower surfaces of the copper foil, and then transferred to a vacuum drying oven for complete drying, and then punched to obtain the negative electrode sheet.
[0107] 3. Preparation of electrolyte
[0108] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), nitrile compounds and lithium hexafluorophosphate LiPF6 were dissolved in ethylene carbonate and ethyl methyl carbonate, with a mass ratio of ethylene carbonate to ethyl methyl carbonate being 3:7 (the content and type of nitrile compounds, and the contents of lithium hexafluorophosphate and ethylene carbonate are shown in Table 1), and stirred uniformly to obtain an electrolyte.
[0109] 5. Isolation film
[0110] Polypropylene film is used as the isolation film.
[0111] 6. Preparation of lithium-ion batteries
[0112] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets to serve as an isolation, and then wound to obtain an electrode assembly; the electrode assembly is placed in an outer package, and the prepared electrolyte is injected into the dried lithium-ion battery. After vacuum packaging, standing, formation, and shaping processes, a lithium-ion battery is obtained.
[0113] The differences between Examples 2-19 and Comparative Examples 1-4 and Example 1 are shown in Table 1.
[0114] Table 1
[0115] The lithium-ion batteries obtained in Examples 1-19 and Comparative Examples 1-4 were tested for cycle capacity retention, DCR growth rate, BET of the positive electrode active material, water content in the electrolyte, and hydrofluoric acid content in the electrolyte at 45°C. The test results are shown in Table 2.
[0116] Battery cycle capacity retention rate at 1.45℃
[0117] Under 45°C cycling conditions, charge at a constant current rate of 0.5C to a charge cut-off voltage of 4.5V, then charge at a constant voltage to a current of ≤0.05C, let it rest for 5 minutes, and then discharge at a constant current rate of 0.33C to a discharge cut-off voltage of 2.5V, let it rest for 5 minutes, and record the battery capacity at this time as C0. Follow this method for 600 cycles of charge and discharge, and record the battery capacity after 600 cycles as C1.
[0118] The cycle capacity retention rate of the battery at 45°C = C1 / C0×100%.
[0119] 2. Calculation method of battery DCR growth rate
[0120] Before cycling the battery, adjust the SOC to 50%. Then, discharge it at 4C for 30 seconds. The pre-discharge voltage is recorded as V1, and the post-discharge voltage is recorded as V2. Calculate DCR1 = (V1 - V2) / I (where I corresponds to the 4C discharge current). After 300 cycles, remove the battery. Test DCR2 using the same protocol, calculating ΔDCR = (DCR2 - DCR1) / DCR1, where ΔDCR represents the rate of increase in the battery's DCR.
[0121] 3. BET test method for positive electrode active materials
[0122] Using the American Microelectronics multi-station fully automatic specific surface area and pore analyzer GeminiVII2390, about 7g of sample was taken and placed in a 9cc long tube with a bulb, degassed at 200℃ for 2h, and then placed in the host for testing to obtain the BET (specific surface area) data of the positive electrode active material.
[0123] 4. Test method for water content in electrolyte
[0124] The electrolyte is injected into the electrolytic cell to reach equilibrium. After the indicator electrode detects H2O, electrode oxidation occurs. - I2 is a quantitative chemical reaction between I2 and H2O, so the water content is calculated. According to HG / T4067-2015 Determination of Water in Hexafluorophosphate Electrolyte 5.9, the quantitative reaction formula of I2 and H2O is: H2O+I2+SO2+3C5H5N=2C5H5N·HI+C5H5N·SO3. The amount of water is calculated by the amount of iodine consumed.
[0125] 5. Test method for hydrofluoric acid content in electrolyte
[0126] The hydrofluoric acid content (SYA) was analyzed by acid-base titration: in a dry environment, the free acid in the electrolyte was titrated with a standard triethylamine solution, and the HF content was calculated as follows: HF (ppm) = (V2-V1) / 1000*C*20 / m*1000000 = (V2-V1)*C / m*20,000; where: 0.01 is the concentration of the SYA standard solution, 0.02 mol / L; V0 is the volume reading of the burette before the start of titration, ml; V is the volume reading of the burette at the end point after the electrolyte sample is added, ml; 20 is the molar molecular weight of HF, g / mol; m is the amount of electrolyte weighed, g; 20000 is the coefficient for conversion to ug / g.
[0127] Table 2
[0128] Conclusion: As can be seen from Table 2, the cycle capacity retention rate at 45°C of the lithium ion batteries corresponding to Examples 1-19 is significantly higher than that of Comparative Examples 1-4, and the DCR growth rate of the lithium ion batteries corresponding to Examples 1-19 is significantly lower than that of Comparative Examples 1-4, indicating that the battery of the present application has excellent cycle stability at a high charge cut-off voltage.
[0129] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A battery comprising a positive electrode sheet and an electrolyte, wherein: The positive electrode sheet includes Li x Ni (1-y-z) Co y M z O 2-b , wherein M includes at least one element selected from the group consisting of Mn, Al, Fe, Ti, Mg, Cr, Ga, Cu, Zn, Nb and Zr, 0<x≤1.2, 0.18≤y≤0.25, 0≤z≤0.2, 1-yz≥0.55, 0≤b≤0.2; The electrolyte includes a nitrile compound. Based on the total mass of the electrolyte, the content of cyanide in the electrolyte is w%, w>0 and satisfies 0.04≤y / w≤0.
4.
2. The battery according to claim 1, wherein 0.1≤y / w≤0.
3.
3. The battery according to claim 1 or 2, wherein: 0.5≤w≤5, preferably 0.5≤w≤2.
4. The battery according to any one of claims 1 to 3, wherein 0.18≤y≤0.2。 5. The battery according to any one of claims 1 to 4, wherein The nitrile compound includes a polynitrile compound. Optionally, the carbon chain length between two adjacent cyano groups in the polynitrile compound does not exceed 8 carbons.
6. The battery according to claim 5, wherein The polynitrile compounds include dinitrile compounds.
7. The battery according to any one of claims 1 to 6, wherein The nitrile compound includes a mononitrile compound, and optionally, the length of the carbon chain in the mononitrile compound does not exceed 4 carbons.
8. The battery according to any one of claims 1 to 7, wherein The electrolyte further includes hexafluorophosphate and ethylene carbonate. Based on the total mass of the electrolyte, the content of the hexafluorophosphate is n%, and the content of the ethylene carbonate is m%, n>0, m>0 and 2≤m / n≤2.
5.
9. The battery according to claim 8, wherein m and n satisfy at least one of the following conditions: 15≤m≤30, preferably 20≤m≤30; 8≤n≤15, preferably 10≤n≤14.
10. The battery according to claim 8 or 9, wherein 0.1≤w / m≤0.
2.
11. The battery according to any one of claims 1 to 10, wherein The Li x Ni (1-y-z) Co y M z O 2-b The specific surface area is ≤3m 2 / g.
12. The battery according to any one of claims 1 to 11, wherein Based on the total mass of the electrolyte, the water content in the electrolyte is ≤0.002%.
13. The battery according to any one of claims 1 to 12, wherein Based on the total mass of the electrolyte, the content of hydrofluoric acid in the electrolyte is ≤0.015%.
14. An electrical device comprising the battery according to any one of claims 1 to 13.
Citation Information
Patent Citations
Lithium ion secondary battery with high energy density
CN102394311A
Non-aqueous electrolyte capable of improving safety performance of battery
CN102496738A
Lithium ion battery and application thereof
CN113299972A
Electrochemical device and electronic device
CN114068910A
Secondary battery