Electrolyte solution and lithium-ion battery

By using specific electrolytes of specific compositions, including organic solvents, lithium salts and specific additives in lithium-ion batteries, the side reaction problems caused by the porosity of the negative electrode are solved, and the high-temperature cycling and rate performance of the battery is significantly improved, and the battery is extended cycle life.

WO2024234809A1PCT designated stage expired Publication Date: 2024-11-21ZHUHAI COSMX BATTERY CO LTD

Patent Information

Application Number
PCT/CN2024/081427
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2024-03-13
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The porosity on the surface side of the negative electrode in a lithium-ion battery is higher than that on the negative electrode current collector side, resulting in increased side reaction between the electrolyte and the negative electrode active substance, resulting in a poor high-temperature cycling and rate performance of the battery.

Method used

The electrolyte with specific compositions is adopted, including organic solvents, lithium salts, additive A and additive B. Additive A accelerates the dissociation of lithium salts, improves the conductivity of the electrolyte, and additive B stabilizes the surface of the positive electrode material to form an effective complex protection layer. , additive C forms an interface protective film, optimizing the porosity of the negative electrode active material layer to improve fluidity.

Benefits of technology

It significantly improves the high-temperature cycling performance and rate magnification performance of lithium-ion batteries, extends the cycle life of the battery, and enhances the ionic conductivity and electrochemical performance of the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024081427_21112024_PF_FP_ABST
    Figure CN2024081427_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure relates to the technical field of batteries, and in particular to an electrolyte solution and a lithium-ion battery. The electrolyte solution comprises an organic solvent, a lithium salt, an additive A, i.e., a trinitride compound, and an additive B, i.e., a polynitrile compound. Under the synergistic effect of the additive A and the additive B, not only can the electrolyte solution be prevented from entering a positive electrode active material layer and corroding the positive electrode active material, but the conductivity of ions in the electrolyte solution can also be improved, such that the battery has excellent high-temperature cycle performance and rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte and lithium-ion batteries Technical Field

[0001] The present disclosure relates to the field of battery technology, and in particular to an electrolyte and a lithium-ion battery comprising the electrolyte. Background Art

[0002] Lithium-ion batteries are widely used in various electronic products due to their advantages such as high specific energy density and long cycle life. The negative electrode is an important component of lithium-ion batteries. The negative electrode usually includes a negative electrode current collector and a negative electrode active material layer supported by the negative electrode current collector. Some literature has proposed a method of improving the fluidity of the negative electrode active material layer by adding a non-aqueous electrolyte to the negative electrode active material layer, and the porosity of the negative electrode active material layer on the negative electrode surface side is higher than that on the negative electrode current collector side (for example: Japanese Laid-open Patent Publication 2015-037008). However, the higher porosity on the negative electrode surface side than on the negative electrode current collector side will lead to increased side reactions between the electrolyte and the negative electrode active material, causing the high temperature cycle performance and rate performance of the battery to deteriorate.

[0003] Summary of the Invention

[0004] In view of this, the present disclosure provides an electrolyte and a lithium-ion battery comprising the electrolyte. Under the action of the electrolyte of the present disclosure, the battery of the present disclosure has excellent high-temperature cycle performance and rate performance.

[0005] In order to achieve the above objectives, the present disclosure provides the following technical solutions:

[0006] The present disclosure provides an electrolyte comprising an organic solvent, a lithium salt, an additive A and an additive B;

[0007] The additive A includes a compound as shown in formula (1):

[0008] The additive B includes a compound as shown in formula (2) and / or formula (3):

[0009] wherein m1, m2, m3, n1, n2, and n3 are each independently a positive integer not equal to 0. For example, m1, m2, m3, n1, n2, and n3 are each independently 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, and the like.

[0010] In one example, m1, m2, m3, n1, n2, and n3 are each independently a positive integer from 1 to 3.

[0011] In one example, m1=m2=m3.

[0012] In one example, n1=n2=n3.

[0013] In one example, m1=m2=m3=n1=n2=n3.

[0014] Preferably, the mass percentage of the additive A in the electrolyte is 0.01wt% to 10wt%; for example, 0.01wt%, 0.05wt%, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.2wt%, 1.3wt%, 1.5wt%, 1.6wt%, 1 .8wt%, 2wt%, 2.2wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.8wt%, 3wt%, 3.3wt%, 3.5wt%, 3.8wt%, 4wt%, 4.2wt%, 4.5wt%, 4.8wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt% or any value within the range formed by any two of the above values.

[0015] Preferably, the mass percentage of the additive A in the electrolyte is 0.1 wt% to 1 wt%.

[0016] More preferably, the mass percentage of the additive A in the electrolyte is 0.3 wt %.

[0017] The inventors of the present disclosure have discovered that when the mass percentage of the additive A in the electrolyte is within a specific range, the dissociation of the lithium salt is accelerated and the conductivity of the electrolyte is improved.

[0018] Preferably, the mass percentage of the additive B in the electrolyte is 0.1wt% to 10wt%; for example, 0.1wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2wt%, 2.2wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.8wt%, 3wt%, 3.3wt%, 3.5wt%, 3.8wt%, 4wt%, 4.2wt%, 4.5wt%, 4.8wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt% or any value between the ranges consisting of any two of the above values.

[0019] Preferably, the mass percentage of the additive B in the electrolyte is 0.5 wt% to 2 wt%.

[0020] More preferably, the mass percentage of the additive B in the electrolyte is 1.5 wt %.

[0021] The inventors of the present disclosure have discovered that when the mass percentage of additive B in the electrolyte is within a specific range, it is able to stabilize the surface of the positive electrode material and provide effective complexation protection at the positive electrode.

[0022] In an embodiment of the present disclosure, the additive B includes at least one of the following compounds:

[0023] In an embodiment of the present disclosure, the lithium salt is selected from at least one of lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiPO2F2), lithium difluorooxalatoborate (LiDFOB), lithium bis(trifluoromethylsulfonyl)imide (TFSI), lithium difluorobis(oxalatophosphate), lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium hexafluoroantimonate, lithium hexafluoroarsenate, lithium bis(pentafluoroethylsulfonyl)imide, tris(trifluoromethylsulfonyl)methyllithium or lithium bis(trifluoromethylsulfonyl)imide.

[0024] Preferably, the mass percentage of the lithium salt in the electrolyte is 11 wt% to 18 wt%.

[0025] The inventors of the present disclosure have discovered that specific lithium salts can provide ion transport channels, promote the dissolution and diffusion of lithium ions in the electrolyte, and increase the ionic conductivity of the electrolyte; and when the mass percentage of the lithium salt in the electrolyte is within a specific range, it can effectively improve the electrochemical performance and cycle life of the lithium-ion battery.

[0026] In an embodiment of the present disclosure, the organic solvent includes carboxylate and / or carbonate.

[0027] In an embodiment of the present disclosure, the carboxylate is selected from at least one of the following fluorinated or unsubstituted solvents: propyl acetate, n-butyl acetate, isobutyl acetate, n-amyl acetate, isoamyl acetate, propyl propionate, ethyl propionate, methyl butyrate and ethyl n-butyrate.

[0028] In an embodiment of the present disclosure, the carbonate is selected from at least one of the following fluorinated or unsubstituted solvents: ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.

[0029] In an embodiment of the present disclosure, the electrolyte may further include an additive C, wherein the additive C is selected from at least one of a cyclic carbonate additive, a cyclic sultone additive, a nitrile additive, and a lithium salt additive.

[0030] The inventors of the present disclosure have discovered that when additive C includes a cyclic carbonate additive, the cyclic carbonate additive can be reduced on the surface of the negative electrode to form an interfacial protective film; when additive C includes a cyclic sultone additive, it can participate in film formation, thereby improving the high-temperature performance of the battery; when additive C includes a nitrile additive, it can complex and coordinate on the surface of the positive electrode material to protect the positive electrode; when additive C includes a lithium salt additive, it can form stable interfacial protection on both the positive and negative electrodes.

[0031] In an embodiment of the present disclosure, the cyclic carbonate additive includes at least one of fluoroethylene carbonate, vinylene carbonate, and vinylethylene carbonate.

[0032] In an embodiment of the present disclosure, the cyclic sultone additive is selected from at least one of 1,3-propane sultone, 1,3-propylene sultone, 2,4-butane sultone and 1,4-butane sultone.

[0033] In an embodiment of the present disclosure, the nitrile additive is selected from at least one of saturated polynitriles, unsaturated alkyl polynitriles and oxygen-containing alkyl nitriles.

[0034] In an embodiment of the present disclosure, the lithium salt additive is selected from at least one of lithium difluorooxalatoborate, lithium difluorophosphate, lithium difluorobisoxalatophosphate, and lithium bisoxalatoborate.

[0035] Preferably, the mass percentage of the additive C in the electrolyte is c (unit: wt%), <c≤15。

[0036] The inventors of the present disclosure have discovered that when the mass percentage c of the additive C in the electrolyte is within a specific range, an interface film can be effectively formed to stably protect the battery active material and prevent it from being destroyed.

[0037] The present disclosure also provides a lithium-ion battery, which includes a positive electrode sheet, a negative electrode sheet, a separator and the above-mentioned electrolyte.

[0038] Preferably, the positive electrode active material of the positive electrode sheet includes transition metal lithium oxide.

[0039] In the embodiment of the present disclosure, the chemical formula of the transition metal lithium oxide is Li 1+x Ni y Co z M (1-y-z) O2,

[0040] Among them, -0.1≤x≤1, 0≤y≤1, 0≤z≤1, and 0≤y+z≤1; M is at least one of Mg, Zn, Ga, Ba, Al, Fe, Cr, Sn, V, Mn, Sc, Ti, Nb, Mo and Zr.

[0041] The inventors of the present disclosure have discovered that when the positive electrode active material includes a transition metal lithium oxide and M is a specific element, the electrolyte of the present disclosure is used in combination to further improve the cycle life of the battery.

[0042] In an embodiment of the present disclosure, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on one or both sides of the positive electrode current collector, and the positive electrode active material layer includes the positive electrode active material, a positive electrode conductor and a positive electrode binder.

[0043] Preferably, the mass percentage of each component in the positive electrode active material layer is: 80 wt% to 99.8 wt% of positive electrode active material, 0.1 wt% to 10 wt% of positive electrode conductor and 0.1 wt% to 10 wt% of positive electrode binder.

[0044] Preferably, the mass percentage of each component in the positive electrode active material layer is: 90 wt% to 99.6 wt% of positive electrode active material, 0.2 wt% to 5 wt% of positive electrode conductor and 0.2 wt% to 5 wt% of positive electrode binder.

[0045] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on one side or both sides of the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, a negative electrode conductive agent and a negative electrode binder.

[0046] Preferably, the mass percentage of each component in the negative electrode active material layer is: 80 wt% to 99.8 wt% of the negative electrode active material, 0.1 wt% to 10 wt% of the negative electrode conductor, and 0.1 wt% to 10 wt% of the negative electrode binder.

[0047] Preferably, the mass percentage of each component in the negative electrode active material layer is: 90 wt% to 99.6 wt% of the negative electrode active material, 0.2 wt% to 5 wt% of the negative electrode conductor, and 0.2 wt% to 5 wt% of the negative electrode binder.

[0048] In an embodiment of the present disclosure, the negative electrode active material includes a carbon-based negative electrode material.

[0049] Preferably, the carbon-based negative electrode material includes at least one of artificial graphite, natural graphite, mesocarbon microbeads, hard carbon and soft carbon.

[0050] Preferably, the negative electrode active material may further include a silicon-based negative electrode material.

[0051] Preferably, the silicon-based anode material is selected from at least one of nano-silicon, silicon-oxygen anode material (SiOa, 0 < a < 2), or silicon-carbon anode material.

[0052] Preferably, in the negative electrode active material, the mass ratio of the carbon-based anode material to the silicon-based anode material is 10:0 to 1:19.

[0053] In an embodiment of the present disclosure, the positive electrode conductive agent and the negative electrode conductive agent are each independently selected from at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, carbon nanotubes (including single-walled carbon nanotubes and multi-walled carbon nanotubes), metal powder, and carbon fiber.

[0054] In an embodiment of the present disclosure, the positive electrode binder and the negative electrode binder are each independently selected from at least one of sodium carboxymethyl cellulose, polyvinylidene fluoride, styrene-butadiene rubber, polytetrafluoroethylene, and polyethylene oxide.

[0055] Preferably, the negative electrode active material layer of the negative electrode sheet includes a first region and a second region, and the second region is disposed between the negative electrode current collector and the first region.

[0056] The porosity of the first region is denoted as Q1, and the porosity of the second region is denoted as Q2. Preferably, Q1 / Q2 > 1.

[0057] The inventors of the present disclosure have found that when the porosity on the surface side of the negative electrode is higher than the porosity on the negative electrode current collector side, the negative electrode active material and the electrolyte are likely to come into contact with each other, thereby causing side reactions. The electrolyte is easily decomposed on the surface of the negative electrode active material to form a coating layer. During the charge and discharge process, this coating layer will break as it expands and contracts, resulting in the exposure of the active surface of the negative electrode active material and continued contact with the electrolyte. The electrolyte continuously decomposes at the active surface of the negative electrode active material and forms a coating layer, and so on in a cycle. In the initial stage of the cycle, the negative electrode resistance tends to increase, and the capacity tends to decrease, resulting in poor high-temperature cycle performance and rate performance of the battery.

[0058] However, using the electrolyte of the present disclosure can effectively improve the above problems. When Q1 / Q2 satisfies a specific range, the fluidity of the non-aqueous electrolyte to the negative electrode active material layer can be improved. The improvement of fluidity can not only promote the progress of the battery reaction but also improve, for example, high-rate characteristics, especially the high-rate cycle performance. Additive A in the electrolyte of the present disclosure can be preferentially reduced to form an interface protective film with a lower impedance on the negative electrode in the first region (away from the current collector layer), thereby suppressing the increase caused by side reactions in the later stage of the cycle. The battery has excellent high-temperature cycle performance and rate performance.

[0059] In an embodiment of the present disclosure, Q1 / Q2 is a value greater than 1 and less than 2.

[0060] In an embodiment of the present disclosure, the thicknesses of the first region and the second region may be the same or different, but are preferably the same.

[0061] Compared with the prior art, the present invention has the following beneficial effects:

[0062] The additive A in the electrolyte disclosed herein is an azide compound, which is a zwitterionic compound. Under the action of the dipole moment of the zwitterionic compound, the dissociation of LiPF6 is accelerated. The anionic group PF6 of the dissociated LiPF6 - N in Additive A + The positively charged groups have higher conductivity. In addition, additive A is also a Lewis base compound that can combine with the free acid in the electrolyte to reduce the damage of the free acid to the interface film.

[0063] The additive B in the electrolyte disclosed herein is a polynitrile compound. The cyano group in the additive B can fully complex the cobalt ions in the positive electrode active layer to form a protective layer, thereby preventing the cobalt ions in the positive electrode active layer from dissolving and improving the cycle performance of the lithium ion battery.

[0064] Under the synergistic effect of additives A and B, not only can the electrolyte be prevented from entering the positive electrode active material layer to corrode the positive electrode active material, but the conductivity of the ions in the electrolyte can also be improved, so that the battery has excellent high-temperature cycle performance and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] FIG1 is a schematic structural diagram of the negative electrode sheet disclosed in the present invention.

[0066] Reference numerals are: 10 negative electrode current collector, 20 negative electrode active material layer, 21 first region, 22 second region. DETAILED DESCRIPTION

[0067] The present disclosure discloses an electrolyte and a lithium-ion battery. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the desired results. It is particularly important to point out that all similar replacements and modifications are obvious to those skilled in the art and are deemed to be included in this disclosure. The methods and applications of the present disclosure have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of this disclosure to implement and apply the technology of the present disclosure.

[0068] In the following embodiments, the porosity of the first region and the second region of the negative electrode active material layer is measured as follows:

[0069] Step 1: Obtain the weight fraction, density, initial porosity, particle expansion coefficient, and charge state of each component of the negative electrode; the components of the negative electrode include active material components and inactive material components;

[0070] Step 2: Determine the real-time volume of each component particle based on the weight fraction, density, expansion coefficient and charge state of each component of the negative electrode;

[0071] Step 3: Determine the initial volume of the negative electrode based on the initial porosity of the negative electrode and the initial volume of each component particle;

[0072] Step 4: Determine the real-time volume of the negative electrode based on the weight fraction, density and initial volume of the negative electrode active material component of the negative electrode;

[0073] Step 5: Determine the real-time porosity of the negative electrode based on the real-time volume of the negative electrode and the real-time volume of each component particle.

[0074] The reagents, instruments, and materials used in this disclosure can all be obtained through commercial channels.

[0075] The present disclosure is further described below with reference to the following embodiments:

[0076] Preparation of Lithium Ion Batteries of Examples 1 to 27 and Comparative Examples 1 to 3

[0077] (1) Battery structure

[0078] The battery includes a positive electrode, a separator, a negative electrode and an electrolyte.

[0079] The positive electrode sheet includes a positive electrode current collector and positive electrode active material layers arranged on both sides thereof.

[0080] As shown in Figure 1, the negative electrode sheet includes a negative electrode current collector 10 and negative electrode active material layers 20 arranged on both sides thereof; the negative electrode active material layer includes a first region 21 and a second region 22, and the second region is arranged between the negative electrode current collector and the first region; the porosity of the first region is recorded as Q1, and the porosity of the second region is recorded as Q2 (see Table 2).

[0081] (2) Battery Preparation Method

[0082] The lithium-ion batteries of the embodiments and comparative examples were prepared by the following steps:

[0083] 1) Preparation of positive electrode sheet

[0084] Examples 1 to 26 and Comparative Examples 1 to 3:

[0085] The positive electrode active material lithium cobalt oxide (LiCoO2), polyvinylidene fluoride (PVDF), conductive carbon black SP (super P) and carbon nanotubes (the mass ratio of single-walled carbon nanotubes to multi-walled carbon nanotubes is 1:1) are mixed in a mass ratio of 96:2:1.5:0.5, N-methylpyrrolidone (NMP) is added, and the mixture is stirred under the action of a vacuum mixer until the mixed system becomes a positive electrode active slurry with uniform fluidity; the positive electrode active slurry is evenly coated on both surfaces of an aluminum foil; the coated aluminum foil is dried, and then rolled and slit to obtain the desired positive electrode sheet.

[0086] Example 27:

[0087] The positive electrode active material, lithium cobalt oxide (LiCoO2), was replaced with the same mass of lithium cobalt oxide doped with Mg, Al and Ti, where the doping amounts of Mg, Al and Ti were 2000 ppm, 2000 ppm and 1000 ppm, respectively.

[0088] 2) Negative electrode preparation

[0089] Examples 1 to 11, 13 to 27 and Comparative Examples 1 to 3:

[0090] (1) Preparation of the first slurry: artificial graphite, sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber, SP, and single-walled carbon nanotubes (SWCNTs) as negative electrode active materials were mixed in a mass ratio of 95.5:1.5:1.5:1:0.5, deionized water was added, and a first region negative electrode active slurry was obtained under the action of a vacuum mixer;

[0091] (2) Preparation of the second slurry: artificial graphite, sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber, SP and single-walled carbon nanotubes (SWCNTs) of the negative electrode active material were mixed in a mass ratio of 93.5:3.5:1.5:1:0.5, deionized water was added, and the second region negative electrode active slurry was obtained under the action of a vacuum mixer;

[0092] (3) The second slurry and the first slurry are uniformly coated on the surface of the copper foil in sequence. The thickness of the first slurry coating (i.e., the first region) is d1, and the thickness of the second slurry coating (i.e., the second region) is d2, where d1 = d2. The coated copper foil is dried at room temperature and then transferred to an 80°C oven for drying for 10 hours. The negative electrode sheet is then obtained by cold pressing and slitting.

[0093] Example 12:

[0094] The difference from the above-mentioned preparation of the negative electrode sheet is step (3): the first slurry and the second slurry are uniformly coated on the two surfaces of the copper foil in sequence; the coated copper foil is dried at room temperature, then transferred to an 80°C oven for drying for 10 hours, and then cold pressed and cut to obtain the negative electrode sheet.

[0095] 3) Preparation of electrolyte

[0096] Components of the electrolyte (based on 100% of the total mass of the electrolyte):

[0097] Organic solvent: 61.5wt% to 75.2wt%;

[0098] Lithium salt: lithium hexafluorophosphate (LiPF6), 13 wt%;

[0099] Additive A: 0-1 wt%;

[0100] Additive B: 0-2 wt%;

[0101] Additive C: FEC (fluoroethylene carbonate), 12 wt%.

[0102] Among them, the organic solvent composition is: 5wt% of ethylene carbonate, 10wt% of propylene carbonate, 15wt% of propyl acetate, and 42.5wt% to 45wt% of propyl propionate (the proportion of organic solvent is adjusted based on 100% of the total mass of the electrolyte, and adjusted from propyl propionate, which has the most solvent).

[0103] Note: In Example 20, LiPF6 was replaced with an equal mass of TFSI. In Example 23, FEC was replaced with an equal mass of a combination of FEC and 1,3-propane sultone, wherein the mass ratio of FEC to 1,3-propane sultone was 1:1. In Example 24, FEC was replaced with an equal mass of a combination of FEC and 1,3-propane sultone, wherein the mass ratio of FEC to 1,3-propane sultone was 5:1.

[0104] Table 1 Electrolyte formula

[0105] Table 2 Porosity parameters of negative electrode active material layer

[0106] 4) Preparation of lithium-ion batteries

[0107] The positive electrode sheet, negative electrode sheet, and separator prepared above are stacked in the order of positive electrode sheet, separator, and negative electrode sheet, and then wound to form a battery cell. The battery cell is placed in an outer aluminum foil packaging, and the above electrolyte is injected into the outer packaging. After vacuum packaging, static standing, formation, shaping, and sorting, a lithium-ion battery is obtained. The battery disclosed herein has a charge and discharge range of 3.0V to 4.5V.

[0108] Lithium-ion battery performance testing

[0109] 1) 45℃ cycle performance test

[0110] The batteries of the embodiment and the comparative example were charged and discharged for 1000 cycles at 45°C at a rate of 1C within the charge and discharge cut-off voltage range. The discharge capacity in the first week of the test was calculated as x1mAh, and the discharge capacity in the Nth cycle was calculated as y1mAh. The capacity in the Nth week was divided by the capacity in the first week to obtain the cycle capacity retention rate R1 = y1 / x1 in the Nth week.

[0111] 2) 5C rate discharge test

[0112] First, let the battery rest for 10 minutes after discharging to a certain capacity. Then, discharge it at 0.2C to 3V, let it rest for 10 minutes, then fully charge it at 0.5C, cut off at 0.05C, and discharge it at 0.5C again. Record the discharge capacity as Z1, and let it rest for 10 minutes. Fully charge the battery at 0.5C again, cut off at 0.05C, and discharge it at 5C at 25°C. Record the discharged capacity as Z2. Calculate the rate discharge capacity retention ratio as: Z2 / Z1.

[0113] The lithium-ion batteries obtained in the examples and comparative examples were subjected to a 45°C cycle performance test and a 5C rate discharge test, respectively, using the above method. The test results are as follows:

[0114] Table 3 Performance test results

[0115] The above experimental data show that the combination of additives A and B in the electrolyte can effectively improve the cycle stability of the battery, and the rate discharge data show that the ionic conductivity of the electrolyte can be improved.

[0116] Among them, it can be seen from Examples 1 to 3, 6, and 8 that the optimal dosage of additive A is 0.3% (Example 1).

[0117] By comparing Examples 4 to 7, it can be seen that the optimal usage amount of the additive B polynitrile compound is 1.5% (Example 6). Too much may lead to poor compatibility on the negative electrode side.

[0118] It can be seen from Examples 1 and 9 to 11 that the four compounds of additive B can effectively improve the cycle stability of the battery and the ionic conductivity of the electrolyte.

[0119] In Example 12, the inter-particle porosity Q1 of the first region / the inter-particle porosity Q2 of the second region is less than 1, and the battery cycle stability is poor, and the rate performance is deteriorated.

[0120] Comparing Example 1 with Comparative Examples 1 to 3, it can be seen that the combination of Additive A and Additive B in Example 1 can effectively improve the cycle stability of the battery, and the rate discharge data shows that the ionic conductivity of the electrolyte can be improved.

[0121] The above is only a preferred embodiment of the present disclosure. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present disclosure. These improvements and modifications should also be regarded as within the scope of protection of the present disclosure.

Claims

1. An electrolyte, characterized in that: The electrolyte comprises an organic solvent, a lithium salt, an additive A and an additive B; The additive A comprises a compound as shown in formula (1): The additive B includes a compound as shown in formula (2) and / or formula (3): Among them, m1, m2, m3, n1, n2 and n3 are each independently a positive integer not equal to 0.

2. The electrolyte according to claim 1, characterized in that m1=m2=m3; And / or, n1=n2=n3.

3. The electrolyte according to claim 1 or 2, characterized in that The mass percentage of the additive A in the electrolyte is 0.01wt% to 10wt%.

4. The electrolyte according to any one of claims 1 to 3, characterized in that The mass percentage of the additive A in the electrolyte is 0.1wt% to 1wt%.

5. The electrolyte according to any one of claims 1 to 4, characterized in that The mass percentage of the additive B in the electrolyte is 0.1wt% to 10wt%.

6. The electrolyte according to any one of claims 1 to 5, characterized in that The mass percentage of the additive B in the electrolyte is 0.5wt% to 2wt%.

7. The electrolyte according to any one of claims 1 to 6, characterized in that The additive B comprises at least one of the following compounds:

8. The electrolyte according to any one of claims 1 to 7, characterized in that The lithium salt is selected from at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium bis(trifluoromethylsulfonyl)imide, lithium difluorobis(oxalatophosphate), lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium hexafluoroantimonate, lithium hexafluoroarsenate, lithium bis(pentafluoroethylsulfonyl)imide, tris(trifluoromethylsulfonyl)methyllithium or lithium bis(trifluoromethylsulfonyl)imide.

9. The electrolyte according to any one of claims 1 to 8, characterized in that The mass percentage of the lithium salt in the electrolyte is 11wt% to 18wt%.

10. The electrolyte according to any one of claims 1 to 9, characterized in that The organic solvent comprises carboxylic acid ester and / or carbonate; Preferably, the carboxylic acid ester is selected from at least one of the following fluorinated or unsubstituted solvents: propyl acetate, n-butyl acetate, isobutyl acetate, n-amyl acetate, isoamyl acetate, propyl propionate, ethyl propionate, methyl butyrate and ethyl butyrate; Preferably, the carbonate is selected from at least one of the following fluorinated or unsubstituted solvents: ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate.

11. The electrolyte according to any one of claims 1 to 10, characterized in that The electrolyte further includes an additive C, wherein the additive C is selected from at least one of a cyclic carbonate additive, a cyclic sultone additive, a nitrile additive, and a lithium salt additive; Preferably, the cyclic carbonate additive includes at least one of fluoroethylene carbonate, vinylene carbonate and vinylethylene carbonate; Preferably, the cyclic sultone additive is selected from at least one of 1,3-propane sultone, 1,3-propylene sultone, 2,4-butane sultone and 1,4-butane sultone; Preferably, the nitrile additive is selected from at least one of saturated polynitriles, unsaturated alkyl polynitriles and oxygen-containing alkyl nitriles; Preferably, the lithium salt additive is selected from at least one of lithium difluorooxalatoborate, lithium difluorophosphate, lithium difluorobisoxalatophosphate and lithium dioxalatoborate.

12. The electrolyte according to claim 11, characterized in that The mass percentage of the additive C in the electrolyte is c,0 <c≤15。 13. A lithium ion battery, characterized in that: The lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and the electrolyte according to any one of claims 1 to 12.

14. The lithium ion battery according to claim 13, characterized in that: The positive electrode active material of the positive electrode sheet includes transition metal lithium oxide; Preferably, the chemical formula of the transition metal lithium oxide is Li 1+x Ni y Co z M (1-y-z) O2, Wherein, -0.1≤x≤1, 0≤y≤1, 0≤z≤1, and 0≤y+z≤1; M is Mg, Zn, Ga, Ba, Al, At least one of Fe, Cr, Sn, V, Mn, Sc, Ti, Nb, Mo and Zr.

15. The lithium ion battery according to claim 13 or 14, characterized in that: The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer coated on one side or both sides of the negative electrode current collector, wherein the negative electrode active material layer comprises a first region and a second region, wherein the second region is disposed between the negative electrode current collector and the first region; The porosity of the first region is recorded as Q1, and the porosity of the second region is recorded as Q2, Q1 / Q2>1; Preferably, Q1 / Q2 is a value greater than 1 and less than 2.

Citation Information

Patent Citations

  • Additive for lithium ion battery electrolyte, electrolyte containing same and lithium ion secondary battery

    CN115692841A

  • Electrolyte and lithium ion battery

    CN116417675A

  • Process for the Preparation of Steroidal Carbothioic Acid Derivatives and Intermediates

    US20070270584A1

Cited By

  • Lithium ion secondary battery

    CN119890446A