Electrolyte additive for electrolytic copper foil, and high-tensile strength and high-elongation electrolytic copper foil and production method therefor

By using electrolyte additives such as organic divalent sulfide, collagen, sulfur-containing heterocyclic structure brightener and nitrogen-containing polymer leveling agent in the electrolyte, copper foil with high tensile strength and high elongation will be generated, and the solution is solved. The problems of coating wrinkle and expansion fracture in lithium-ion battery manufacturing have improved production efficiency and safety.

WO2024244098A1PCT designated stage expired Publication Date: 2024-12-05JIUJIANG TELFORD ELECTRONICS MATERIAL CO LTD

Patent Information

Application Number
PCT/CN2023/104536
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-01
Filing Date
2023-06-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing copper foil is coated and wrinkled during the manufacturing process of lithium-ion batteries and expanded and broken during use, resulting in low production efficiency and safety risks.

Method used

Using an electrolytic solution additive for electrolytic copper foil, including organic divalent sulfide, collagen, brightener with sulfur-containing heterocyclic structure, nitrogen-containing polymer leveling agent and ether compound, through specific components in the electrolyte The synergistic effect of the two-dimensional effect of copper foils with high tensile strength and high elongation.

Benefits of technology

It significantly improves the tensile strength and elongation of copper foil, solves the problems of coating wrinkle and expansion fracture, and improves the production efficiency and safety of lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023104536_05122024_PF_FP_ABST
    Figure CN2023104536_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are an electrolyte additive for an electrolytic copper foil, and a high-tensile strength and high-elongation electrolytic copper foil and a production method therefor. The electrolyte additive for the electrolytic copper foil comprises, in parts by weight, 15-60 parts of an organic divalent sulfide, 10-40 parts of collagen, 5-45 parts of a brightener of a sulfur-containing heterocyclic structure, 10-70 parts of a nitrogen-containing polymer leveling agent, 15-40 parts of chloride ions and 20-90 parts of an ether compound. According to the additive of the present application, the organic divalent sulfide is used as a brightener, and the brightener of the sulfur-containing heterocyclic structure is also used; the brightener of the sulfur-containing heterocyclic structure cooperates with the nitrogen-containing polymer leveling agent, so that a copper foil with extremely high tensile strength can be obtained, the elongation of the copper foil is effectively improved, and the copper foil has excellent surface stability.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte additive for electrolytic copper foil, high-resistance and high-elongation electrolytic copper foil and production method thereof Technical Field

[0001] The present invention and the method relate to the field of copper foil, and in particular to an electrolyte additive for electrolytic copper foil, a high-resistance and high-elongation electrolytic copper foil and a production method thereof. Background Art

[0002] As the thickness of lithium battery copper foil becomes thinner, the mechanical properties of the copper foil also undergo great changes, the most significant of which are the decrease in tensile strength and elongation. These two indicators directly affect the production efficiency and safety of lithium-ion battery manufacturing.

[0003] Coating wrinkles. Coating is a critical production process for downstream copper foil battery customers. Coating involves applying negative electrode materials to the copper foil. Low tensile strength can cause the foil to wrinkle or break during the coating process. Customer production lines must clean and maintain coating machines tens of meters long at high temperatures before rewinding the foil and re-coating, severely impacting lithium battery production efficiency.

[0004] Battery expansion. During the charge and discharge process of lithium batteries, the negative electrode material contains materials such as silicon, which will expand to a certain extent. Copper foil, as the negative electrode current collector, carries the negative electrode material and acts as a current conductor. If the copper foil has low elongation, the battery is prone to fracture during the expansion process, shortening the lithium battery's lifespan and affecting battery safety. Therefore, it is necessary to maintain a high elongation while ensuring the tensile strength of the copper foil.

[0005] Among them, the use of electrolyte additives is a key factor influencing the preparation of copper foil. The general copper foil additive formula consists of three parts: brightener, leveler, and displacement agent. They work synergistically to promote the copper foil's excellent structural composition and mechanical properties. Brighteners can effectively promote grain nucleation, resulting in grain refinement and achieving a matte and bright finish. They are mostly sulfur-containing organic compounds. Levelers can promote the growth of copper foil grains at the center. They are mostly proteins of different molecular weights. Displacement agents can make the coating "walk" to all parts of the plated part. They can effectively improve the dispersibility of the plating solution and promote the rapid, effective and uniform action of other additives during the copper plating process. They are mostly polyether substances.

[0006] Summary of the Invention

[0007] The purpose of the present invention is to provide an electrolyte additive for electrolytic copper foil, a high-resistance and high-ductility electrolytic copper foil and a production method thereof, so as to solve the problems of wrinkling of the existing copper foil during coating in the manufacturing process of lithium-ion batteries and expansion and fracture during use.

[0008] The first aspect of the present application provides an electrolyte additive for electrolytic copper foil, which includes, by weight, 15-60 parts of an organic divalent sulfide, 10-40 parts of collagen, 5-45 parts of a brightener containing a sulfur heterocyclic structure, 10-70 parts of a nitrogen-containing polymer leveling agent, 15-40 parts of chloride ions, and 20-90 parts of an ether compound.

[0009] Furthermore, the organic divalent sulfide includes one or more selected from the group consisting of 3,3'-dithiobis-1-propanesulfonic acid disodium salt, 3-mercaptopropanesulfonic acid sodium salt, and mercaptobenzimidazole.

[0010] Furthermore, the weight average molecular weight of the above collagen is 3000-6000.

[0011] Furthermore, the brightener containing a sulfur heterocyclic structure includes one or more selected from the group consisting of tetrahydrothiazolidinethione, diphenylvinylpyridine and 2-hydroxyphenylthiourea.

[0012] Furthermore, the nitrogen-containing polymer leveling agent includes polyethyleneimine compounds, and preferably the nitrogen-containing polymer leveling agent includes one or more selected from the group consisting of polyethyleneimine alkyl compounds, polyethyleneimine alkane or ethoxy polyethyleneimine.

[0013] Furthermore, the above-mentioned ether compounds include crown ether compounds, and preferably the ether compounds include one or more selected from the group consisting of 9-crown-3, 12-crown-4, 15-crown-5, 18-crown-6, benzo-12-crown-4, benzo-15-crown-5, benzo-18-crown-6, and benzo-21-crown-7.

[0014] Furthermore, the electrolyte additives include, by weight, 40-45 parts of an organic divalent sulfide, 20-35 parts of collagen, 30-45 parts of tetrahydrothiazolidinethione, 35-50 parts of a polyethyleneimine compound, 20-30 parts of chloride ions, and 60-70 parts of a crown ether compound, wherein the organic divalent sulfide includes 3,3'-dithiobis-1-propanesulfonic acid disodium salt or 3-mercaptopropanesulfonic acid sodium salt.

[0015] In a second aspect of the present application, a method for producing electrolytic copper foil is provided, comprising the following steps: (1) dissolving a metallic element copper in an electrolyte, wherein the electrolyte comprises a sulfuric acid-copper sulfate solution and an additive, wherein the additive is any one of the electrolyte additives described above; (2) electrolyzing the metallic element copper to obtain a raw foil; and (3) washing and passivating the raw foil to obtain a copper foil.

[0016] Furthermore, the copper ion concentration in the above electrolyte is 75g / L-100g / L, and / or the sulfuric acid concentration is 90g / L-140g / L.

[0017] Furthermore, the content of the above-mentioned organic divalent sulfide in the electrolyte is 15 mg / L-60 mg / L; the content of collagen in the electrolyte is 10 mg / L-40 mg / L; the content of tetrahydrothiazolidinethione in the electrolyte is 5 mg / L-45 mg / L; the content of nitrogen-containing polymer leveling agent in the electrolyte is 10 mg / L-70 mg / L; the content of ether compound in the electrolyte is 20 mg / L-90 mg / L; and the content of chloride ion in the electrolyte is 15-40 ppm.

[0018] Furthermore, the electrolysis conditions are selected from any one or more of the following: the electrolysis temperature is 40°C-60°C, the upper flow rate of the electrolyte is 40m 3 / h-50m 3 / h, the current density of electrolysis is 6000A / m 2 -7000A / m 2 .

[0019] In a third aspect of the present application, an electrolytic copper foil is provided, which satisfies at least two of the following conditions: tensile strength between 480 MPa and 550 MPa, elongation of 6 to 8, grain size of 0.4 μm to 0.5 μm, and twin ratio of 52% to 70%.

[0020] In a fourth aspect of the present application, an electrolytic copper foil is provided, which is obtained by any of the above-mentioned production methods.

[0021] The additive of the present application not only uses an organic divalent sulfide as a brightener, but also uses a brightener containing a sulfur heterocyclic structure. The brightener containing a sulfur heterocyclic structure works synergistically with a nitrogen-containing polymer leveling agent to obtain a copper foil with extremely high tensile strength and effectively improve the elongation of the copper foil. At the same time, this type of copper foil has excellent surface stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the specific embodiments of the present invention, the following briefly introduces the drawings required for describing the specific embodiments.

[0023] FIG1 is an EBSD photograph of the thickness of the copper foil prepared in Example 3.

[0024] FIG2 is an EBSD photograph of the thickness of the copper foil prepared in Comparative Example 2.

[0025] FIG3 is a TEM image of the copper foil prepared in Example 3.

[0026] Note: The present invention refers to the double-bright copper foil with M (matte) side and S (glossy) side. The S side is the side that is in contact with the cathode roller, and the other side is the M side. DETAILED DESCRIPTION

[0027] In order to make the present invention more clearly explained, the present invention will be further described in detail below. Obviously, the embodiments described are only some embodiments of the present invention, rather than all embodiments. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present invention are within the scope of protection of the present invention.

[0028] The first embodiment of the present application provides an electrolyte additive for electrolytic copper foil, which includes, by weight, 15-60 parts of an organic divalent sulfide, 10-40 parts of collagen, 5-45 parts of a brightener containing a sulfur heterocyclic structure, 10-70 parts of a nitrogen-containing polymer leveling agent, 15-40 parts of chloride ions, and 20-90 parts of an ether compound.

[0029] The additive of the present application not only uses an organic divalent sulfide as a brightener, but also uses a brightener containing a sulfur heterocyclic structure. The brightener containing a sulfur heterocyclic structure works synergistically with a nitrogen-containing polymer leveling agent to obtain a copper foil with extremely high tensile strength and effectively improve the elongation of the copper foil. At the same time, this type of copper foil has excellent surface stability.

[0030] The reason for this is that, in the aforementioned proportions, the combination of this sulfur-heterocyclic brightener, collagen, and nitrogen-containing polymer levelers creates a smoother, denser copper foil structure, producing numerous nanocrystalline regions. This enhances the fine-grain strengthening effect and promotes the formation of numerous twins within the copper foil. This synergistic effect significantly increases the probability and proportion of nanotwin formation. The combined effects of fine grains and nanotwins enhance both the copper foil's tensile strength and its elongation.

[0031] In summary, this application uses the theoretical principles of grain refinement and increasing the proportion of nano-twins, breaking through the limitations of traditional formulas. It innovatively adopts specific additives and optimized ratios to reduce the introduction of impurities. On the one hand, it generates a large number of nanocrystalline areas, while at the same time increasing the twin ratio of the copper foil and generating a clear nano-twin structure, ensuring the tensile strength of the copper foil while maintaining a high elongation, thereby effectively solving the problems of existing copper foil wrinkling during coating in the manufacturing process of lithium-ion batteries and expansion and fracture during use.

[0032] The above-mentioned organic divalent sulfide forms a cuprous complex with the surface of the copper foil during the electroplating process and is adsorbed on the copper deposition site, playing a catalytic role in promoting deposition, thereby being able to reduce the roughness of the copper foil within a certain concentration and significantly improve the tensile strength and elongation of the copper foil. The organic divalent sulfide used in this application can be selected from commonly used sulfur-containing organic compounds as brighteners, including but not limited to sodium polydisulfide dipropane sulfonate, sodium 4-[[2-(acetylamino)ethyl]dithio]-1-butanesulfinate, thiamine disulfide compounds, 2-substituted hydrazono-1,3-dithiocyclopentane, ethylenethiourea, 3,3'-dithiobis-1-propanesulfonic acid disodium salt, 3-mercaptopropanesulfonic acid sodium salt, and mercaptobenzimidazole. Both mercapto and sulfonate groups can combine with metal ions to form complexes and accelerate the reducibility of metal ions. In addition, mercapto groups have the effect of enhancing the toughness of the coating, and sulfonate groups have the effect of reducing liquid surface tension, improving coating properties and antioxidant properties. In some embodiments, the organic divalent sulfide comprises one or more selected from the group consisting of 3,3'-dithiobis-1-propanesulfonic acid disodium salt, 3-mercaptopropanesulfonic acid sodium salt, and mercaptobenzimidazole. These preferred organic divalent sulfides not only form complexes with copper ions during the electroplating process, thereby covering the surface of the copper ions and promoting their reduction and deposition, ultimately forming a dense and uniformly distributed electroplated layer, but also have the following advantages:

[0033] 1. It can better control the physical properties of the plating solution, such as surface tension and viscosity, thereby improving the uniformity and coordination of the plating solution, and thus improving the quality of the electroplating coating.

[0034] 2. Improve the electroplating efficiency of the plating solution: It can effectively promote electrochemical reactions, improve electrode reaction efficiency and reaction rate, shorten electroplating time, and thus improve production efficiency. At the same time, these additives also have the effect of reducing side reactions and improving the efficiency of copper ion use, thereby narrowing the battery potential range, saving electricity, and reducing production costs.

[0035] 3. Improving the adhesion of electroplated coatings: These additives act as surfactants in the plating solution, reducing the liquid's surface tension and interfacial energy, thereby facilitating the interaction between the plating solution and the substrate and improving the coating's adhesion. Furthermore, these compounds can control the redox potential during the electroplating process, filling defects on the electrode surface and further enhancing the adhesion and stability of the coating.

[0036] 4. Environmentally friendly: Small amounts are used during the electroplating process, reducing the environmental impact of the plating solution. Furthermore, these additives combine with copper ions during the electroplating process to form stable complexes, thereby reducing the concentration of copper ions in the plating solution and reducing the generation of pollutants, thus meeting environmental protection requirements.

[0037] 5. Economical: These additives are used in small quantities and are low-cost during the electroplating process. They can effectively increase the plating rate and make the distribution of the electroplated coating more uniform, thereby saving materials and energy, reducing production costs, and improving production efficiency. In addition, they can improve the quality and adhesion of the electroplated coating, reduce residue and scrap rates, and further improve the economic benefits of production.

[0038] The collagen used in this application is conventional commercial collagen. In order to improve the dispersibility of collagen in the electrolyte, in some embodiments, the weight average molecular weight of the collagen is selected to be 3000-6000.

[0039] The sulfur-containing heterocyclic brightener used in this application can be selected from conventional brighteners of this type. In some embodiments, the sulfur-containing heterocyclic brightener includes one or more selected from the group consisting of tetrahydrothiazolidinethione, diphenylvinylpyridine, and 2-hydroxyphenylthiourea. In particular, tetrahydrothiazolidinethione and nitrogen-containing polymer levelers offer a more synergistic effect, further enhancing the tensile strength of copper foil (>700 MPa) and more effectively increasing its elongation. Furthermore, such copper foil exhibits excellent surface stability.

[0040] The cations of nitrogen-containing polymer levelers readily adsorb on active sites, and unsaturated bonds enhance adsorption. Under convection electroplating conditions, this reduces surface microprofile fluctuations and surface roughness, significantly improving the tensile strength and elongation of the copper foil. To further enhance the aforementioned benefits of nitrogen-containing polymer levelers, in some embodiments, the nitrogen-containing polymer leveler comprises a polyethyleneimine compound, preferably one or more selected from the group consisting of polyethyleneimine alkyl compounds, polyethyleneimine alkane, or ethoxypolyethyleneimine. This application does not have specific requirements for the molecular weight of the nitrogen-containing polymer leveler.

[0041] Ether compounds are used as moving agents, which are conducive to uniform copper plating. Conventional ether polymers and crown ether compounds can be used for the ether compounds of this application. Crown ether compound molecules have uncharged ring structures, so they have good non-ionicity during electroplating, can further reduce the resistivity and liquid surface tension of the electroplating solution, and promote the reduction of metal ions; when crown ether compounds interact with ions, multilayer coordination often occurs, and a complex that is more stable than other ether polymers can be formed, which more effectively improves the catalytic performance of the electroplating solution; the water solubility of crown ether compounds is better than other ether polymers, and they are easily dissolved in water to form a stable electroplating solution, without any pollution to the environment during the electroplating process; crown ether compounds can more efficiently form complexes with metal ions, can more efficiently deposit on the metal surface during the electroplating process, and form a uniform, dense metal coating. Therefore, crown ether compounds have the advantages of good non-ionicity, strong multilayer coordination, good water solubility, and strong film-forming ability in electroplating, which can further improve the electrochemical properties of the electroplating solution and obtain high-quality metal coatings. In some embodiments, the above-mentioned ether compounds include crown ether compounds, and preferably the ether compounds include one or more selected from the group consisting of 9-crown-3, 12-crown-4, 15-crown-5, 18-crown-6, benzo-12-crown-4, benzo-15-crown-5, benzo-18-crown-6, and benzo-21-crown-7.

[0042] In some embodiments, the chloride ions are provided by hydrochloric acid or a chloride salt, preferably sodium chloride or potassium chloride, with hydrochloric acid being preferred. Chloride ions act as an anode activator and a stress reliever for the coating, aiding in anode dissolution and synergistically working with additives to brighten and smooth the coating while also reducing tensile stress in the coating.

[0043] In some embodiments, the weight parts of the organic divalent sulfide include, but are not limited to, 15, 20, 25, 30, 35, 40, 45, 55, or 60 parts.

[0044] In some embodiments, the collagen includes, but is not limited to, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, or 40 parts.

[0045] In some embodiments, the brightener containing a sulfur heterocyclic structure includes but is not limited to 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts or 45 parts.

[0046] In some embodiments, the nitrogen-containing polymer leveler includes, but is not limited to, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 55 parts, 60 parts, 65 parts, or 70 parts.

[0047] In some embodiments, the chloride ion includes, but is not limited to, 15, 20, 25, 30, 35, or 40 parts.

[0048] In some embodiments, the ether compound includes, but is not limited to, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, or 90 parts.

[0049] In some embodiments, the electrolyte additive includes, by weight, 40-45 parts of an organic divalent sulfide, 20-35 parts of collagen, 30-45 parts of tetrahydrothiazolidinethione, 35-50 parts of a polyethyleneimine compound, 20-30 parts of chloride ions, and 60-70 parts of a crown ether compound, wherein the organic divalent sulfide includes 3,3'-dithiobis-1-propanesulfonic acid disodium salt or 3-mercaptopropanesulfonic acid sodium salt. The synergistic effect of crown ether compounds and thiazolidinethione can significantly increase the rate and efficiency of electrochemical reactions, promote the reduction and uniform deposition of metal ions, improve the electrochemical properties of the electroplating solution, enhance the stability of the electrochemical reaction, and promote the mass transfer and diffusion of the solution. The promotion of the reduction of metal ions helps to form a uniform, dense, and bright metal coating, thereby improving the corrosion resistance, wear resistance, and heat resistance of the coating. Compared with traditional electroplating solution systems, the synergistic effect of crown ether compounds and thiazolidinethione can reduce the use of harmful substances, reduce carbon emissions, and be more environmentally friendly. In summary, the synergistic effect of crown ether compounds and thiazolidinethione can improve the efficiency of electrochemical reactions, improve the electroplating solution system, improve the performance of the coating, and achieve environmentally friendly production.

[0050] A second embodiment of the present application provides a method for producing electrolytic copper foil, comprising the following steps: (1) dissolving a metallic element copper in an electrolyte, wherein the electrolyte comprises a sulfuric acid-copper sulfate solution and an additive, wherein the additive is any one of the electrolyte additives described above; (2) electrolyzing the metallic element copper to obtain a raw foil; and (3) washing and passivating the raw foil to obtain a copper foil.

[0051] The production method of the present application adopts the above-mentioned specific additives, which generate a large number of nanocrystalline areas during electrolysis, while increasing the twin ratio of the copper foil and generating a clear nanotwin structure, ensuring the tensile strength of the copper foil while maintaining a high elongation.

[0052] In some embodiments of the present application, the copper ion concentration in the electrolyte is 75 g / L-100 g / L, and / or the sulfuric acid concentration is 90 g / L-140 g / L, to improve the stability of electrolysis.

[0053] In some embodiments of the present application, the content of the organic divalent sulfide in the electrolyte is 15 mg / L-60 mg / L; the content of collagen in the electrolyte is 10 mg / L-40 mg / L; the content of tetrahydrothiazolidinethione in the electrolyte is 5 mg / L-45 mg / L; the content of the nitrogen-containing polymer leveler in the electrolyte is 15 mg / L-70 mg / L; the content of the ether compound in the electrolyte is 20 mg / L-90 mg / L; and the content of chloride ions in the electrolyte is 10-40 ppm. By controlling the content of each component in the electrolyte within the above ranges during the electrolysis process, a full synergistic effect of each component is achieved, thereby simultaneously improving the tensile strength and elongation of the copper foil.

[0054] The electrolysis conditions of this application can refer to the conventional copper foil electrolysis conditions, that is, the use of the electrolyte additives of this application does not require changes to the conventional electrolysis conditions, so its applicability is relatively wide. In some embodiments, the electrolysis conditions are selected from any one or more of the following: the electrolysis temperature is 40°C-60°C, the upper flow rate of the electrolyte is 40m 3 / h-50m 3 / h, the current density of electrolysis is 6000A / m 2 -7000A / m 2 . To promote the full play of the role of electrolyte additives.

[0055] The washing and passivation after electrolysis can refer to the commonly used washing process and passivation process in electrolytic copper foil, which will not be described in detail in this application.

[0056] A third embodiment of the present application provides an electrolytic copper foil that meets at least two of the following conditions: a tensile strength between 480 MPa and 550 MPa, an elongation of 6 to 8, a grain size of 0.4 μm to 0.5 μm, and a twinning ratio of 52% to 70%. The electrolytic copper foil of the present application exhibits both high tensile strength and high elongation, effectively addressing the issues of conventional copper foil wrinkling during coating and expansion and fracture during use during lithium-ion battery manufacturing.

[0057] The above tensile strength and elongation are obtained by testing the copper foil at room temperature (about 25°C) using a HY-0230 universal material testing machine manufactured by Shanghai Hengyi Precision Instrument Co., Ltd. in accordance with the test method GB / T29847-2013.

[0058] A fourth embodiment of the present application provides an electrolytic copper foil produced using any of the aforementioned production methods. The electrolytic copper foil produced by the production method of the present application has both high tensile strength and high elongation, thereby effectively solving the problems of conventional copper foils such as wrinkling during coating and expansion and fracture during use during lithium-ion battery manufacturing.

[0059] The following examples and comparative examples further illustrate the beneficial effects of the present application. Where specific techniques or conditions are not specified in the examples, the techniques or conditions described in the literature in the art or in the product instructions were used. Reagents or instruments used without manufacturer specified are commercially available conventional products.

[0060] Example 1

[0061] A sulfuric acid-copper sulfate solution prepared by dissolving elemental copper metal in sulfuric acid is used as an electrolytic electrolyte, and additives are added thereto; the resulting electrolyte has a copper ion concentration of 86 g / L, a sulfuric acid concentration of 110 g / L, a 3,3'-dithiobis-1-propanesulfonic acid disodium salt concentration of 45 mg / L, a collagen (molecular weight of 5000-6000) concentration of 22 mg / L, a tetrahydrothiazolidinethione concentration of 45 mg / L, a polyethyleneimine octadecyl urea (CAS No.: 6844125-8) concentration of 35 mg / L, a 27-crown-9 and a benzo-30-crown-10 concentration of 60 mg / L, and a chloride ion concentration of 20 ppm (chloride ions are provided by hydrochloric acid); the electrolysis temperature is 55°C, and the upper flow rate of the electrolyte is 45 m 3 / h, electrolysis current density is 6500A / m 2 After electrolysis reaction, the obtained raw foil is washed, passivated and dried to obtain uncut finished lithium battery copper foil.

[0062] Example 2

[0063] A sulfuric acid-copper sulfate solution prepared by dissolving elemental copper metal in sulfuric acid is used as an electrolytic electrolyte, and additives are added thereto. The copper ion concentration in the obtained electrolyte is 89 g / L, the sulfuric acid concentration is 115 g / L, the combined concentration of 3,3'-dithiobis-1-propanesulfonic acid disodium salt and 3-mercaptopropanesulfonic acid sodium salt in a mass ratio of 1:1 is 40 mg / L, the collagen (molecular weight 5000-6000) concentration is 25 mg / L, the tetrahydrothiazolidinethione concentration is 35 mg / L, the ethoxypolyethyleneimine (CAS No.: 26658-46-8) concentration is 35 mg / L, the 12-crown-4 concentration is 70 mg / L, and the chloride ion concentration is 22 ppm (chloride ions are provided by hydrochloric acid); the electrolysis temperature is 55°C, the upper liquid flow rate of the electrolyte is 45 m 3 / h, electrolysis current density is 6500A / m 2 After electrolysis reaction, the obtained raw foil is washed, passivated and dried to obtain uncut finished lithium battery copper foil.

[0064] Example 3

[0065] A sulfuric acid-copper sulfate solution prepared by dissolving elemental copper metal in sulfuric acid is used as an electrolytic electrolyte, and additives are added thereto; the copper ion concentration in the obtained electrolyte is 90 g / L, the sulfuric acid concentration is 120 g / L, the combined concentration of 3,3'-dithiobis-1-propanesulfonic acid disodium salt and 3-mercaptopropanesulfonic acid sodium salt in a mass ratio of 2:1 is 45 mg / L, the collagen (molecular weight 5000-6000) concentration is 20 mg / L, the tetrahydrothiazolidinethione concentration is 30 mg / L, the ethoxypolyethyleneimine (CAS No.: 26658-46-8) concentration is 35 mg / L, the 12-crown-4 concentration is 60 mg / L, and the chloride ion concentration is 30 ppm (chloride ions are provided by hydrochloric acid); the electrolysis temperature is 55°C, and the upper liquid flow rate of the electrolyte is 45 m 3 / h, the electrolysis current density is 7000A / m 2 After electrolysis reaction, the obtained raw foil is washed, passivated and dried to obtain uncut finished lithium battery copper foil.

[0066] Example 4

[0067] A sulfuric acid-copper sulfate solution prepared by dissolving elemental copper metal in sulfuric acid is used as an electrolytic electrolyte, and additives are added thereto; the resulting electrolyte has a copper ion concentration of 100 g / L, a sulfuric acid concentration of 130 g / L, a 3-mercaptopropanesulfonic acid sodium salt concentration of 50 mg / L, a collagen (molecular weight 5000-6000) concentration of 35 mg / L, a tetrahydrothiazolidinethione concentration of 38 mg / L, a PVAM polyvinylamine (CAS: 183815-54-5) concentration of 35 mg / L, an 18-crown-6 concentration of 60 mg / L, and a chloride ion concentration of 30 ppm (chloride ions are provided by hydrochloric acid); the electrolysis temperature is 60°C, and the upper flow rate of the electrolyte is 45 m 3 / h, the electrolysis current density is 7000A / m 2 After electrolysis reaction, the obtained raw foil is washed, passivated and dried to obtain uncut finished lithium battery copper foil.

[0068] Example 5

[0069] The only difference from Example 3 is that the total concentration of 3,3'-dithiobis-1-propanesulfonic acid disodium salt and 3-mercaptopropanesulfonic acid sodium salt is 15 mg / L, and the rest is the same as Example 3.

[0070] Example 6

[0071] The only difference from Example 3 is that the total concentration of 3,3'-dithiobis-1-propanesulfonic acid disodium salt and 3-mercaptopropanesulfonic acid sodium salt is 60 mg / L, and the rest is the same as Example 3.

[0072] Example 7

[0073] The only difference from Example 3 is that the concentration of collagen (molecular weight 5000-6000) is 10 mg / L, and the rest is the same as Example 3.

[0074] Example 8

[0075] The only difference from Example 3 is that the concentration of collagen (molecular weight 5000-6000) is 40 mg / L, and the rest is the same as Example 3.

[0076] Example 9

[0077] The only difference from Example 3 is that the concentration of collagen (molecular weight 3000-4000) is 20 mg / L, and the rest is the same as Example 3.

[0078] Example 10

[0079] The only difference from Example 3 is that the concentration of tetrahydrothiothione is 5 mg / L, and the rest is the same as Example 3.

[0080] Example 11

[0081] The only difference from Example 3 is that the concentration of ethoxypolyethyleneimine (CAS No.: 26658-46-8) is 10 mg / L, and the rest is the same as Example 3.

[0082] Example 12

[0083] The only difference from Example 3 is that the concentration of ethoxypolyethyleneimine (CAS No.: 26658-46-8) is 70 mg / L, and the rest is the same as Example 3.

[0084] Example 13

[0085] The only difference from Example 3 is that the concentration of ethoxypolyethyleneimine (CAS No.: 26658-46-8) is 50 mg / L, and the rest is the same as Example 3.

[0086] Example 14

[0087] The only difference from Example 3 is that the chloride ion concentration is 10 ppm (hydrochloric acid is used to provide chloride ions), and the rest is the same as Example 3.

[0088] Example 15

[0089] The only difference from Example 3 is that the chloride ion concentration is 40 ppm (hydrochloric acid is used to provide chloride ions), and the rest is the same as Example 3.

[0090] Example 16

[0091] The only difference from Example 3 is that the concentration of 12-crown-4 is 20 mg / L, and the rest is the same as Example 3.

[0092] Example 17

[0093] The only difference from Example 3 is that the concentration of 12-crown-4 is 70 mg / L, and the rest is the same as Example 3.

[0094] Example 18

[0095] The only difference from Example 3 is that fatty alcohol polyoxyethylene ether M (CAS: 37335-03-8) is used to replace 12-crown-4 at an equal concentration, and the rest is the same as Example 3.

[0096] Example 19

[0097] The only difference from Example 3 is that the copper ion concentration in the electrolyte is 65 g / L, and the rest is the same as Example 3.

[0098] Example 20

[0099] The only difference from Example 3 is that the sulfuric acid concentration is 90 g / L, and the rest is the same as Example 3.

[0100] Example 21

[0101] The only difference from Example 3 is that the sulfuric acid concentration is 140 g / L, and the rest is the same as Example 3.

[0102] Example 22

[0103] The only difference from Example 3 is that the electrolysis temperature is 40° C., and the rest is the same as Example 3.

[0104] Example 23

[0105] The only difference from Example 3 is that the upper flow rate of the electrolyte is 40m 3 / h, and the rest is the same as in Example 3.

[0106] Example 24

[0107] The only difference from Example 3 is that the upper flow rate of the electrolyte is 50m 3 / h, and the rest is the same as in Example 3.

[0108] Example 25

[0109] The only difference from Example 3 is that the electrolysis current density is 6000A / m 2 , the rest is the same as Example 3.

[0110] Example 26

[0111] Same as Example 1, except that the current density in the electrolyte is 7000 A / m 2 .

[0112] Comparative Example 1

[0113] The process is the same as Example 1, except that 3,3'-dithiobis-1-propanesulfonic acid disodium salt is not added to the electrolyte.

[0114] Comparative Example 2

[0115] The same as Example 3, except that 12-crown-4 was not added to the electrolyte.

[0116] Comparative Example 3

[0117] The process is the same as Example 3, except that 3,3'-dithiobis-1-propanesulfonic acid disodium salt and 3-mercaptopropanesulfonic acid sodium salt are not added to the electrolyte.

[0118] Comparative Example 4

[0119] The only difference from Example 3 is that the total concentration of 3,3'-dithiobis-1-propanesulfonic acid disodium salt and 3-mercaptopropanesulfonic acid sodium salt is 10 mg / L, and the rest is the same as Example 3.

[0120] Comparative Example 5

[0121] The only difference from Example 3 is that the total concentration of 3,3'-dithiobis-1-propanesulfonic acid disodium salt and 3-mercaptopropanesulfonic acid sodium salt is 70 mg / L, and the rest is the same as Example 3.

[0122] Comparative Example 6

[0123] The only difference from Example 3 is that tetrahydrothiazolidinethione is not added, and the rest is the same as Example 3.

[0124] Comparative Example 7

[0125] The only difference from Example 3 is that the concentration of tetrahydrothiothione is 50 mg / L, and the rest is the same as Example 3.

[0126] Comparative Example 8

[0127] The only difference from Example 3 is that ethoxypolyethyleneimine (CAS No.: 26658-46-8) is not added, and the rest is the same as Example 3.

[0128] Comparative Example 9

[0129] The only difference from Example 3 is that the concentration of ethoxypolyethyleneimine (CAS No.: 26658-46-8) is 80 mg / L, and the rest is the same as Example 3.

[0130] Comparative Example 10

[0131] The only difference from Example 3 is that the concentration of 12-crown-4 is 100 mg / L, and the rest is the same as Example 3.

[0132] During the implementation of the above embodiments and comparative examples, each parameter was controlled as much as possible at the corresponding set value. However, as the reaction progresses and the substance is consumed, the concentration and electrical performance parameters will fluctuate within the allowable range in practice.

[0133] The microstructure and basic physical properties of the electrolytic copper foils prepared in Examples 1-26 and Comparative Examples 1-10 were tested. The testing methods for the microstructure and basic physical properties are as follows:

[0134] EBSD (Electrode Backscatter Diffraction) Testing: The microstructure of copper foil samples from various examples and comparative examples was observed using a C-Swift EBSD detector manufactured by Oxford Instruments. The EBSD images of Example 3 and Comparative Example 2 are shown in Figures 1 and 2. Figure 1 shows a large number of nanocrystalline and twin regions, while Figure 2 shows larger grains with only a small number of nanocrystalline and twin regions. The TEM image of Example 3, shown in Figure 3, shows a distinct nanoscale twin structure.

[0135] Glossiness test: According to the test method GB / T 13891, a WGG60-E gloss meter manufactured by Costar Optoelectronic Instrument Co., Ltd. was used to measure the glossiness of the copper foil along the length direction of the M surface at an incident angle of 60°.

[0136] Tensile strength and elongation test: According to the test method GB / T29847-2013, the tensile strength and elongation of the copper foil were tested at room temperature (about 25°C) using a HY-0230 universal material testing machine manufactured by Shanghai Hengyi Precision Instrument Co., Ltd.

[0137] The test results of the microstructure and basic physical properties of the electrolytic copper foils prepared in each embodiment and each comparative example are shown in Table 1.

[0138] Table 1 Performance test results of electrolytic copper foil

[0139] In summary, a reasonable additive formulation and ratio can effectively control the grain growth pattern of copper foil during the electroplating process, generating a large number of nanocrystals and nanotwins, enhancing the copper foil's tensile strength while maintaining good plasticity. By controlling grain size and forming nanotwins, the strength and toughness of copper foil can be effectively improved. When the grain size decreases to a certain level, the interfacial energy will occupy an increasingly large proportion of the total material volume, and the bulk density between grains will also increase. This increases the density of grain boundaries, shortening the diffusion distance, and making dislocations more easily blocked by grain boundaries, increasing the resistance to plastic deformation. The presence of nanotwin interfaces makes the material less prone to fracture, thereby supporting plastic deformation at high strain rates. The diffuse stress field exerted by the nanotwin interfaces can also hinder the movement of matrix atoms, thereby improving strength and toughness. At this time, the bending and twisting of the grain boundaries help limit the relative displacement between grains, improve the material's ductility, and play a role in mechanical strengthening.

[0140] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and components may be substituted with equivalents without departing from the scope of the present application. In particular, the various technical features described in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but encompasses all technical solutions within the scope of the claims.

Claims

1. An electrolyte additive for electrolytic copper foil, characterized in that: In parts by weight, the electrolyte additive includes: 15-60 parts of organic divalent sulfide, 10-40 parts of collagen, 5-45 parts of brightener containing sulfur heterocyclic structure, 10-70 parts of nitrogen-containing polymer leveling agent, 15-40 parts of chloride ion and 20-90 parts of ether compound.

2. The electrolyte additive according to claim 1, characterized in that: The organic divalent sulfide includes one or more selected from the group consisting of 3,3'-dithiobis-1-propanesulfonic acid disodium salt, 3-mercaptopropanesulfonic acid sodium salt, and mercaptobenzimidazole.

3. The electrolyte additive according to claim 1 or 2, characterized in that: The weight average molecular weight of the collagen is 3000-6000.

4. The electrolyte additive according to any one of claims 1 to 3, characterized in that The brightener containing a sulfur heterocyclic structure includes one or more selected from the group consisting of tetrahydrothiazolidinethione, diphenylvinylpyridine and 2-hydroxyphenylthiourea.

5. The electrolyte additive according to any one of claims 1 to 4, characterized in that The nitrogen-containing polymer leveler includes polyethyleneimine compounds, and preferably the nitrogen-containing polymer leveler includes one or more selected from the group consisting of polyethyleneimine alkyl compounds, polyethyleneimine alkane or ethoxy polyethyleneimine.

6. The electrolyte additive according to any one of claims 1 to 5, characterized in that The ether compounds include crown ether compounds, and preferably the ether compounds include one or more selected from the group consisting of 9-crown-3, 12-crown-4, 15-crown-5, 18-crown-6, benzo-12-crown-4, benzo-15-crown-5, benzo-18-crown-6, and benzo-21-crown-7.

7. The electrolyte additive according to any one of claims 1 to 6, characterized in that: In parts by weight, the electrolyte additive includes: 40-45 parts of organic divalent sulfide, 20-35 parts of collagen, 30-45 parts of tetrahydrothiazolidinethione, 35-50 parts of polyethyleneimine compounds, 20-30 parts of chloride ions and 60-70 parts of crown ether compounds, wherein the organic divalent sulfide includes 3,3'-dithiobis-1-propanesulfonic acid disodium salt or 3-mercaptopropanesulfonic acid sodium salt.

8. A method for producing an electrolytic copper foil, characterized in that: The steps include: (1) dissolving a single metal copper in an electrolyte, wherein the electrolyte comprises a sulfuric acid-copper sulfate solution and an additive, wherein the additive is the electrolyte additive according to any one of claims 1 to 7; (2) electrolyzing the metal element copper to obtain raw foil; (3) Washing and passivating the original foil to obtain copper foil.

9. The production method according to claim 8, characterized in that: The copper ion concentration in the electrolyte is 75 g / L-100 g / L, and / or the sulfuric acid concentration is 90 g / L-140 g / L.

10. The production method according to claim 8 or 9, characterized in that: The content of the organic divalent sulfide in the electrolyte is 15 mg / L-60 mg / L; the content of the collagen in the electrolyte is 10 mg / L-40 mg / L; the content of the tetrahydrothiazolidinethione in the electrolyte is 5 mg / L-45 mg / L; the content of the nitrogen-containing polymer leveling agent in the electrolyte is 10 mg / L-70 mg / L; the content of the ether compound in the electrolyte is 20 mg / L-90 mg / L; the content of the chloride ion in the electrolyte is 15-40 ppm.

11. The production method according to any one of claims 8 to 10, characterized in that The electrolysis conditions are selected from any one or more of the following: The electrolysis temperature is 40℃-60℃, and the electrolyte flow rate is 40m 3 / h-50m 3 / h, The current density of electrolysis is 6000A / m 2 -7000A / m 2 .

12. An electrolytic copper foil, characterized in that: The electrolytic copper foil satisfies at least two of the following conditions: The tensile strength is between 480MPa-550MPa, the elongation is 6-8, the grain size is 0.4μm-0.5μm, and the twin ratio is 52%-70%.

13. An electrolytic copper foil, characterized in that: The electrolytic copper foil is obtained by the production method according to any one of claims 8 to 11.

Citation Information

Patent Citations

  • Preparation method of electrolytic copper foil

    CN108560025A

  • Electrolyte for preparing lithium battery copper foil and production process

    CN108677222A

  • Electrolyte additive for electrolytic copper foil, high-resistance and high-ductility electrolytic copper foil and production method of high-resistance and high-ductility electrolytic copper foil

    CN116590762A

  • Additive for electroylite solution of electroplating process for copper coating with high elongation and electroylite solution of electroplating process for copper coating with high elongation comprising the same

    KR1020130077240A

Cited By

  • Electrolyte for preparing copper foil with high tensile strength, copper foil and preparation method of copper foil

    CN120866890A