Carbon fluoride modification method, modified carbon fluoride and lithium / carbon fluoride battery

By using composite solvents to modify carbon fluoride in lithium/fluorinated carbon batteries, the problem of side reaction between carbon fluorinated carbon and electrolyte is solved, and the battery storage stability is improved and the production cost is reduced. It is suitable for large-scale Large-scale production.

WO2024245458A1PCT designated stage expired Publication Date: 2024-12-05EVE ENERGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/106398
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-11-09
Filing Date
2024-07-19
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The side reaction between carbon fluoride and electrolyte in lithium/fluorinated carbon batteries affects storage stability. The prior art blocks the contact between the positive electrode and the electrolyte but fails to reduce side reactions from the root cause, and the preparation process is complicated and costly. Difficult to apply to large-scale production.

Method used

Modify carbon fluoride by composite solvents (water and ether solvents), and clean unstable components by water and wetting and cleaning of ether solvents, reduce the side reaction between carbon fluoride and electrolyte, and improve material chemistry Stability, simplified process without pre-charge.

Benefits of technology

Effectively reduce the side reaction between carbon fluoride and electrolyte, improve the storage stability of lithium/fluoride carbon batteries, reduce production costs, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024106398_05122024_PF_FP_ABST
    Figure CN2024106398_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a carbon fluoride modification method, modified carbon fluoride and a lithium / carbon fluoride battery. The modification method comprises: mixing carbon fluoride with a composite solvent, subjecting same to a modification treatment, and then performing solid-liquid separation, so as to obtain modified carbon fluoride, wherein the composite solvent comprises water and an ether solvent. The composite solvent is used to modify carbon fluoride; and under the synergistic effect of water and the ether solvent, unstable components in a carbon fluoride material can be removed by means of reaction, thereby improving the chemical stability of the carbon fluoride material and reducing side reactions of carbon fluoride with an electrolyte solution, and therefore the storage stability of a lithium / carbon fluoride battery is improved. The modification method is simple and feasible, does not need the step of pre-charging, and is easy to implement and suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Method for modifying carbon fluoride, modified carbon fluoride and lithium / carbon fluoride battery

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on November 9, 2023, with application number 202311489337.9. The entire contents of the above application are incorporated by reference into this application.

[0002] Technical Field

[0003] The present application relates to the field of battery technology, and in particular to a method for modifying carbon fluoride, modified carbon fluoride, and a lithium / carbon fluoride battery.

[0004] Background Art

[0005] Lithium / carbon fluoride batteries are currently the most energy-dense type of lithium primary battery. Compared to other lithium primary batteries, they offer advantages such as stable discharge, safe storage, and low self-discharge. Therefore, they are suitable for many aspects of production and life, especially in medical devices and military weaponry. Furthermore, these batteries are environmentally friendly, making recycling more convenient and reducing environmental impact.

[0006] However, the carbon fluoride, the active material in the positive electrode of lithium / carbon fluoride batteries, is prone to side reactions with the electrolyte, especially with the organic solvent in the electrolyte, which directly affects the storage stability of the battery. To overcome these drawbacks, CN112993289A discloses a lithium / carbon fluoride battery, its electrolyte, and a method for using it. This method adds a cyclic phosphate to the electrolyte, which can form a passivation layer at the positive electrode to prevent direct contact between the electrolyte and the carbon fluoride. The phosphate can also decompose to generate phosphorus oxide free radicals, which quench hydrogen free radicals in the electrolyte, thereby reducing side reactions between the electrolyte and the electrode and improving the battery's storage performance.

[0007] CN114628670A discloses the use of nitrogen-doped carbon-coated fluorinated carbon in lithium / fluorinated carbon batteries. An aqueous solution of tris(hydroxymethylaminomethane) is used as a buffer solution. A polydopamine fluorinated carbon composite material is first obtained through the self-polymerization reaction of dopamine hydrochloride. The composite material is calcined under an inert atmosphere to obtain a nitrogen-doped carbon-coated fluorinated carbon electrode material. The surface carbon layer is coated to block direct contact between the electrolyte and the fluorinated carbon, thereby reducing the self-discharge phenomenon of the battery and improving the shelf performance of the battery.

[0008] Technical issues

[0009] The above technology has the following shortcomings: 1) The oxidation potential of the phosphate additive is higher than the open circuit voltage of the lithium / carbon fluoride battery. The battery needs to be pre-charged to form a passivation layer of cyclic phosphate on the positive electrode. The charging process may affect the safety performance of the battery and may produce lithium dendrites that pierce the diaphragm; 2) The preparation process of carbon fluoride surface coating is complicated and costly, which is not conducive to large-scale production; 3) Both of the above technical methods slow down the side reaction between the positive electrode and the electrolyte by blocking the direct contact between the positive electrode and the electrolyte, and do not reduce the side reaction between carbon fluoride and the electrolyte from the root.

[0010] Therefore, there is an urgent need to provide a method that can fundamentally reduce the side reaction between carbon fluoride and electrolyte, does not require a pre-charging step, and is suitable for large-scale production.

[0011] The present invention provides a method for modifying carbon fluoride, modified carbon fluoride, and a lithium / carbon fluoride battery. This invention utilizes a composite solvent to modify carbon fluoride. The synergistic effects of water and an ether solvent effectively remove unstable components from the carbon fluoride material, improving the material's chemical stability and reducing side reactions between the carbon fluoride and the electrolyte, thereby enhancing the storage stability of the lithium / carbon fluoride battery. Furthermore, the modification method is simple and feasible, requiring no pre-charging, making it easy to implement and suitable for large-scale production.

[0012] Technical Solutions

[0013] In a first aspect, the present application provides a method for modifying carbon fluoride, the modification method comprising:

[0014] The modified carbon fluoride is obtained by mixing carbon fluoride and a composite solvent, performing a modification treatment, and then performing solid-liquid separation, wherein the composite solvent includes water and an ether solvent.

[0015] In a second aspect, the present application provides a modified fluorinated carbon, which is prepared by the modification method described in the first aspect.

[0016] In a third aspect, the present application provides a lithium / carbon fluoride battery, wherein the positive electrode of the lithium / carbon fluoride battery comprises the modified carbon fluoride described in the second aspect.

[0017] Beneficial effects

[0018] Compared with the related art, the beneficial effects of this application are:

[0019] (1) The present application provides a method for modifying carbon fluoride, wherein a composite solvent is used to pretreat carbon fluoride, wherein water can react and clean unstable components in carbon fluoride, such as unstable CF bonds, atomic fluorine between carbon layers, residual fluorinating agents and catalysts during the fluorination process, and active defect structures on the surface of the material, thereby removing unstable components in carbon fluoride and reducing the side reaction between carbon fluoride and electrolyte. Ether solvents have good affinity with carbon fluoride and can effectively wet carbon fluoride, thus wetting and cleaning the material. Ethers can also react with unstable components in carbon fluoride. Therefore, under the combined action of water and ether solvents, unstable components in carbon fluoride are effectively removed, the chemical stability of the material is improved, the side reaction between carbon fluoride and electrolyte is reduced, the storage stability of lithium / carbon fluoride batteries is improved, and the capacity loss of the battery due to side reactions during storage is avoided.

[0020] (2) The modification method of the present application is simple and feasible, does not require precharging, is easy to implement, has low cost, and is suitable for large-scale production.

[0021] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description.

[0022] BRIEF DESCRIPTION OF THE DRAWINGS

[0023] FIG1 is a CV curve diagram of the modified fluorinated carbon provided in Example 1 of the present application and the unmodified fluorinated carbon provided in Comparative Example 1.

[0024] FIG2 is an infrared spectrum of the modified fluorinated carbon provided in Example 1 of the present application and the unmodified fluorinated carbon provided in Comparative Example 1.

[0025] Modes for Carrying Out the Invention

[0026] In a first aspect, the present application provides a method for modifying carbon fluoride, the modification method comprising:

[0027] The modified carbon fluoride is obtained by mixing carbon fluoride and a composite solvent, performing a modification treatment, and then performing solid-liquid separation, wherein the composite solvent includes water and an ether solvent.

[0028] The present application provides a method for modifying carbon fluoride, wherein a composite solvent is used to pretreat carbon fluoride, wherein water can react and clean unstable components in carbon fluoride, such as unstable C—F bonds, atomic fluorine between carbon layers, residual fluorinating agents and catalysts during the fluorination process, and active defect structures on the surface of the material, thereby removing unstable components in carbon fluoride and reducing the side reaction between carbon fluoride and electrolyte; ether solvents and carbon fluoride have good affinity and can effectively wet carbon fluoride, thus wetting and cleaning the material, and ethers can also react with unstable components in carbon fluoride. Therefore, under the combined action of water and ether solvents, unstable components in carbon fluoride are effectively removed, the chemical stability of the material is improved, the side reaction between carbon fluoride and electrolyte is reduced, the storage stability of lithium / carbon fluoride batteries is improved, and the capacity loss caused by side reactions during storage of the battery is avoided; in addition, the modification method of the present application is simple and feasible, does not require precharging, is easy to implement, has low cost, and is suitable for large-scale production.

[0029] In one embodiment, the ether solvent includes at least one of dimethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether and tetrahydrofuran, and ethylene glycol dimethyl ether can be selected.

[0030] In one embodiment, in the composite solvent, the mass ratio of water to ether solvent is (10-90): (10-90), wherein the selection range of water (10-90) can be, for example, 10, 20, 30, 40, 50, 60, 70, 80 or 90, and the selection range of ether solvent (10-90) can be, for example, 10, 20, 30, 40, 50, 60, 70, 80 or 90, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] In this application, if the mass ratio of water and ether solvent is too low, the modification effect is poor; if the mass ratio of water and ether solvent is too high, since the proportion of water in the composite solvent is too large and carbon fluoride is a hydrophobic material, the carbon fluoride cannot be wetted and modification cannot be performed.

[0032] In one embodiment, the solid-liquid mass ratio of the fluorinated carbon and the composite solvent is (1 / 10-1 / 2):1, for example, it can be 0.1:1, 0.2:1, 0.3:1, 0.4:1 or 0.5:1, etc., but is not limited to the listed values, and other unlisted values ​​within this numerical range are also applicable.

[0033] In the present application, if the solid-liquid ratio of carbon fluoride and the composite solvent is too low, it will lead to waste of resources; if the solid-liquid ratio of carbon fluoride and the composite solvent is too high, it will lead to insufficient treatment and the unstable components in the carbon fluoride will not be completely eliminated.

[0034] In one embodiment, the temperature of the modification treatment is 0-90°C, for example, it can be 0°C, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C or 80°C, etc., but is not limited to the listed values. Other unlisted values ​​within this numerical range are also applicable, and 40-60°C can be selected.

[0035] The present application may choose to carry out the modification treatment at 40-60°C. This is because the modification at high temperature can increase the reactivity of the unstable structure in the carbon fluoride, improve the wettability of the solvent and the carbon fluoride, make the pretreatment reaction more thorough, and be beneficial to the structural stability of the material. If the temperature of the modification treatment is too low, the wettability of the solvent and the carbon fluoride is poor, and the reactivity of the solvent and the active structure in the carbon fluoride is poor, which will result in the unstable components in the carbon fluoride not being completely eliminated and the material remaining unstable; if the temperature of the modification treatment is too high, for power-type fluorinated hard carbon materials, the carbon-fluorine bond on the carbon fluoride surface will be destroyed, the wettability of the electrolyte and the carbon fluoride will be improved, and the release of the semi-ionic bond in the carbon fluoride will be aggravated, the self-discharge of the battery will be aggravated, and the storage performance will deteriorate.

[0036] In one embodiment, the modification treatment time is greater than 0.01h, for example, it can be 0.02h, 0.05h, 0.1h, 0.5h, 1h, 2h, 4h, 6h, 8h, 10h, 15h, 20h, 25h, 30h, 40h, 45h or 48h, etc., but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, and 4h-48h can be selected.

[0037] In one embodiment, the modification process is accompanied by stirring, and the stirring rate is 100-1000 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0038] As an optional technical solution of the present application, the modification method specifically includes:

[0039] The carbon fluoride is added into a composite solvent consisting of water and an ether solvent, and then stirred to carry out modification treatment, and then solid-liquid separation, drying and dispersion are carried out to obtain the modified carbon fluoride.

[0040] Optionally, the solid-liquid separation method includes centrifugation, filtration or natural sedimentation.

[0041] In a second aspect, the present application provides a modified fluorinated carbon, which is prepared by the modification method described in the first aspect.

[0042] In one embodiment, the modified carbon fluoride has a cyclic voltammetry (CV) curve with a reduction peak in the voltage range of 2-3 V. The reduction peak corresponds to the reduction peak of the lithium-carbon fluoride reaction.

[0043] In one embodiment, compared with the infrared spectrum of unmodified fluorinated carbon, the infrared spectrum of the modified fluorinated carbon is 1332 cm -1 CF2 functional group and 1100-1200cm -1 The absorption peak of the semi-ionic CF bond at 877-878 cm -1 and 1427-1697cm -1 The characteristic absorption peak of the inactive defect structure in the wavelength range, such as 1697 cm -1 (C=O), 1631cm -1 (C=C), 1427cm -1 (CH2) and 877cm -1 (Substituents on the benzene ring).

[0044] In a third aspect, the present application provides a lithium / carbon fluoride battery, wherein the positive electrode of the lithium / carbon fluoride battery comprises the modified carbon fluoride described in the second aspect.

[0045] In one embodiment, the lithium / carbon fluoride battery further comprises a lithium metal anode, an electrolyte, and a separator.

[0046] Optionally, the modified carbon fluoride positive electrode, the metal lithium negative electrode and the separator are assembled into a battery cell by lamination or winding.

[0047] In one embodiment, the electrolyte includes an organic solvent and an electrolyte salt.

[0048] In one embodiment, the electrolyte salt includes at least one of lithium perchlorate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), and lithium trifluoromethanesulfonate.

[0049] In one embodiment, the organic solvent includes at least one of ethylene glycol dimethyl ether, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.

[0050] In one embodiment, the concentration of the electrolyte is 0.5-2 mol / L, for example, it can be 0.5 mol / L, 0.7 mol / L, 1 mol / L, 1.5 mol / L or 2 mol / L, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0051] Optionally, the electrolyte solution is prepared by mixing organic solvent components (such as propylene carbonate and ethylene glycol dimethyl ether) in a glove box filled with argon to obtain a mixed solvent, and adding an electrolyte salt to the mixed solvent to obtain the electrolyte solution.

[0052] Optionally, after assembling the battery cell, the electrolyte is injected into the battery cell with an injection coefficient of 1.0-1.6 g / Ah (for example, 1.0 g / Ah, 1.2 g / Ah, 1.4 g / Ah or 1.6 g / Ah, etc.), and after sealing, a lithium / carbon fluoride battery is obtained.

[0053] The numerical range described in this application includes not only the point values ​​listed above, but also any point values ​​between the above numerical ranges that are not listed. Due to limited space and for the sake of simplicity, this application no longer exhaustively lists the specific point values ​​included in the range.

[0054] The technical solution of this application is further explained below through specific implementation methods.

[0055] Example 1

[0056] This embodiment provides a method for modifying carbon fluoride, comprising:

[0057] The carbon fluoride material is added to a composite solvent composed of water and an ether solvent, wherein the ether solvent is ethylene glycol dimethyl ether, the mass ratio of water to ethylene glycol dimethyl ether is 50:50, and the solid-liquid mass ratio of carbon fluoride to the composite solvent is 1:5. Then, stirring is started to make its speed 500r / min, and the modification treatment is carried out at 40°C for 24h, followed by solid-liquid separation. The separated product is placed in a blast oven for drying, and finally the dried modified carbon fluoride particles are dispersed using a powder disperser to obtain modified carbon fluoride powder. Example 2

[0058] This embodiment provides a method for modifying carbon fluoride, comprising:

[0059] The carbon fluoride material is added to a composite solvent composed of water and an ether solvent, wherein the ether solvent is tetrahydrofuran, the mass ratio of water to tetrahydrofuran is 60:40, and the solid-liquid mass ratio of the carbon fluoride and the composite solvent is 1 / 3:1. Then, stirring is started to make its speed 300r / min, and the modification treatment is carried out at 60°C for 10h, followed by solid-liquid separation. The separated product is placed in a blast oven for drying, and finally the dried modified carbon fluoride particles are dispersed by a powder disperser to obtain modified carbon fluoride powder.

[0060] Example 3

[0061] This embodiment provides a method for modifying carbon fluoride, comprising:

[0062] The carbon fluoride material is added to a composite solvent composed of water and an ether solvent, wherein the ether solvent is diethylene glycol dimethyl ether, the mass ratio of water to diethylene glycol dimethyl ether is 50:50, and the solid-liquid ratio of the carbon fluoride and the composite solvent is 1 / 5:1. Then, stirring is started to make its speed 400r / min, and the modification treatment is carried out at 70°C for 24h, followed by solid-liquid separation. The separated product is placed in a blast oven for drying, and finally the dried modified carbon fluoride particles are dispersed using a powder disperser to obtain modified carbon fluoride powder.

[0063] Example 4

[0064] The difference between this embodiment and embodiment 1 is that ethylene glycol dimethyl ether is replaced by tetrahydrofuran.

[0065] The remaining parameters and operating steps are exactly the same as those in Example 1.

[0066] Example 5

[0067] The difference between this embodiment and embodiment 1 is that the solid-liquid mass ratio of carbon fluoride and the composite solvent is adjusted to 0.05:1.

[0068] The remaining parameters and operating steps are exactly the same as those in Example 1.

[0069] Example 6

[0070] The difference between this embodiment and embodiment 1 is that the solid-liquid mass ratio of carbon fluoride and the composite solvent is adjusted to 0.55:1.

[0071] The remaining parameters and operating steps are exactly the same as those in Example 1.

[0072] Example 7

[0073] The difference between this embodiment and embodiment 1 is that the modification temperature is adjusted to -5°C.

[0074] The remaining parameters and operating steps are exactly the same as those in Example 1.

[0075] Example 8

[0076] The difference between this embodiment and embodiment 1 is that the modification temperature is adjusted to 95°C.

[0077] The remaining parameters and operating steps are exactly the same as those in Example 1.

[0078] Comparative Example 1

[0079] This comparative example provides a carbon fluoride material that is the same as that in Example 1, but is not subjected to a composite solvent modification treatment.

[0080] Comparative Example 2

[0081] The difference between this comparative example and Example 1 is that water is omitted from the composite solvent, so that the composite solvent contains only an ether solvent (ie, ethylene glycol dimethyl ether).

[0082] The remaining parameters and operating steps are exactly the same as those in Example 1.

[0083] Performance Testing

[0084] (1) Cyclic voltammetry (CV) test

[0085] The modified fluorinated carbon of Example 1 and the unmodified fluorinated carbon of Comparative Example 1 were fabricated into button cells. After storage at 55°C for 14 days, CV testing was performed. The specific test conditions were: a scan rate of 0.05 mV / s, from the fully charged open circuit voltage of the battery to 1 V.

[0086] Figure 1 shows the CV curves of the unmodified carbon fluoride of Comparative Example 1 and the modified carbon fluoride of Example 1. As can be seen from the figure, the unmodified carbon fluoride material has two reduction peaks in the CV curve. The reduction peak at 2.3V is the side reaction of carbon fluoride with the electrolyte, which proves that the carbon fluoride material is unstable and prone to side reactions with the electrolyte. In addition, the deterioration of the electrolyte reduces the reduction peak current of the lithium-carbon fluoride reaction, shifts the reduction peak of the lithium-carbon fluoride reaction to the left, and increases the polarization of the battery discharge process. The modification process makes the carbon fluoride material stable, the side reaction with the electrolyte basically disappears, the reduction peak of the side reaction disappears, and the storage stability of the battery is improved.

[0087] (2) Infrared spectrum test

[0088] The modified fluorinated carbon of Example 1 and the unmodified fluorinated carbon of Comparative Example 1 were tested by infrared spectroscopy in the range of 4000-400 cm -1 , as shown in Figure 2. The test results show that after pretreatment, the fluorinated carbon material has a -1 (C=O), 1631cm -1 (C=C), 1427cm -1 (CH2), 877cm -1 The characteristic absorption peak at 1332 cm -1 (CF2) and 1100-1200cm -1 (semi-ionic CF bond) is weakened, indicating that there are many defective structures in the unmodified fluorinated carbon material, and some carbon-fluorine bonds are unstable. Pretreatment can eliminate unstable components in the material, improve the stability of the material, and thus improve the storage stability of the battery.

[0089] (3) Storage stability test

[0090] The carbon fluoride material finally provided in the above examples and comparative examples was used as the active material, and was mixed with the conductive agent Super P and the adhesive polyvinylidene fluoride (PVDF) respectively. The active material, the conductive agent and the adhesive were mixed in a mass ratio of 87:8:5 to prepare a high viscosity slurry with a viscosity of 12000cp. The slurry was coated on the carbon-coated aluminum foil, with a coating on the A side and then on the B side. The coating thickness was 100μm, and the electrode load was 120g / m 2 After drying at 100℃, roller pressing, compaction density 1.26g / cm 3 , porosity 52%, cutting or die-cutting into corresponding sizes to obtain a carbon fluoride positive electrode sheet; cutting the lithium ribbon into corresponding sizes to obtain a negative electrode lithium sheet with a thickness of 50 μm; assembling the modified carbon fluoride positive electrode sheet, the metal lithium negative electrode sheet and the separator into a battery cell by lamination, injecting a primary lithium fluoride carbon battery electrolyte into the battery cell, wherein the organic solvent in the electrolyte is propylene carbonate (PC) and ethylene glycol dimethyl ether (DME), the electrolyte salt is lithium trifluoromethanesulfonate LiTFA and lithium perchlorate LiClO4, the electrolyte concentration is 1 mol / L, the injection coefficient is 1.2 g / Ah, and the lithium / carbon fluoride battery is obtained after sealing.

[0091] Test conditions: a) Discharge the lithium / carbon fluoride battery at room temperature at 0.01C with a discharge cutoff voltage of 1.5V, and record the discharge capacity of the new battery. b) Store the new lithium / carbon fluoride battery at 55°C for 14 days, then retest under the above conditions and record the battery's discharge capacity. Calculate the capacity retention as follows: discharge capacity after high-temperature storage / discharge capacity of the new battery * 100%.

[0092] Table 1

[0093]

[0094] analyze:

[0095] The results of Examples 1-3 and Comparative Example 1 show that the present application uses a composite solvent composed of water and an ether solvent to modify the carbon fluoride material. Under the synergistic effect of water and the ether solvent, the unstable components in the carbon fluoride material can be reacted, thereby improving the chemical stability of the material itself and reducing the side reactions between the carbon fluoride and the electrolyte, especially the side reactions between the oxidizing fluorine in the carbon fluoride and ethylene glycol dimethyl ether, thereby improving the storage stability of the lithium / carbon fluoride battery and maintaining stable capacity. As can be seen from Table 1, the capacity retention rate of Examples 1-3 is relatively high, indicating that the modified carbon fluoride material has good stability, the self-discharge of the modified carbon fluoride battery is reduced, and the storage stability is good; the capacity retention rate of Comparative Example 1 is relatively low, indicating that the battery assembled with the unmodified carbon fluoride has a large self-discharge after being stored at high temperature for 14 days and has poor storage stability.

[0096] From the results of Example 1 and Example 4, it can be seen that the use of ethylene glycol dimethyl ether and water as a composite solvent for modification results in a better capacity retention rate and storage stability of the corresponding battery.

[0097] It can be seen from the results of Example 1 and Examples 5-6 that if the solid-liquid mass ratio of carbon fluoride and the composite solvent is too low, it will lead to waste of resources; if the solid-liquid ratio of carbon fluoride and the composite solvent is too high, it will lead to insufficient treatment, the unstable components in the carbon fluoride are not completely eliminated, and the battery capacity retention rate is low.

[0098] It can be seen from the results of Example 1 and Examples 7-8 that if the temperature of the modification treatment is too low, the wettability of the solvent and carbon fluoride is poor, and the reactivity of the solvent and the active structure in carbon fluoride is poor, which will lead to the unstable components in carbon fluoride not being completely eliminated and the battery capacity retention rate being low; if the temperature of the modification treatment is too high, for power-type fluorinated hard carbon materials, the carbon-fluorine bonds on the surface of carbon fluoride will be destroyed, the wettability of the electrolyte and carbon fluoride will be improved, the release of semi-ionic bonds in carbon fluoride will be aggravated, the self-discharge of the battery will be aggravated, and the storage performance will deteriorate.

[0099] It can be seen from the results of Example 1 and Comparative Example 2 that if only ether solvents are used for modification, the improvement on the storage stability of the battery is limited, and the ether solvent alone cannot significantly improve the storage stability of the battery.

Claims

1. A method for modifying fluorinated carbon, comprising: The carbon fluoride and the composite solvent are mixed, modified, and then solid-liquid separated to obtain the modified carbon fluoride, wherein the composite solvent includes water and an ether solvent.

2. The modification method according to claim 1, wherein: The ether solvent includes at least one of dimethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether and tetrahydrofuran, and ethylene glycol dimethyl ether can be selected.

3. The modification method according to claim 1 or 2, wherein: In the composite solvent, the mass ratio of water to the ether solvent is (10-90):(10-90).

4. The modification method according to any one of claims 1 to 3, wherein: The solid-liquid mass ratio of the carbon fluoride and the composite solvent is (1 / 10-1 / 2):

1.

5. The modification method according to any one of claims 1 to 4, wherein: The temperature of the modification treatment is 0-90°C, and can be optionally 40-60°C.

6. The modification method according to any one of claims 1 to 5, wherein: The modification treatment time is greater than 0.01 h, and can be selected to be 4-48 h.

7. The modification method according to any one of claims 1 to 6, wherein: The modification process is accompanied by stirring, and the stirring rate is 100-1000r / min.

8. The modification method according to any one of claims 1 to 7, wherein: The modification method specifically comprises: The carbon fluoride is added into a composite solvent consisting of water and an ether solvent, and then stirring is started to carry out modification treatment, and then solid-liquid separation, drying and dispersion are carried out to obtain the modified carbon fluoride.

9. A modified fluorinated carbon, wherein: The modified fluorinated carbon is prepared by the modification method described in any one of claims 1 to 8.

10. The modified fluorinated carbon according to claim 9, wherein In the cyclic voltammetry curve of the modified fluorinated carbon, there is a reduction peak in the voltage range of 2-3V.

11. A lithium / carbon fluoride battery, wherein: The positive electrode of the lithium / carbon fluoride battery comprises the modified carbon fluoride according to claim 9 or 10.

12. The lithium / carbon fluoride battery according to claim 11, wherein: The lithium / carbon fluoride battery also includes a lithium metal negative electrode, an electrolyte and a separator.

13. The lithium / carbon fluoride battery according to claim 12, wherein: The concentration of the electrolyte is 0.5-2 mol / L.

Citation Information

Patent Citations

  • Lithium / carbon fluoride battery and electrolyte and use method thereof

    CN112993289A

  • Application of nitrogen-doped-carbon-coated carbon fluoride in lithium / carbon fluoride battery

    CN114628670A

  • Silicon dioxide modified carbon fluoride material and preparation method thereof

    CN105655588A

  • Modified perfluorocarbon battery and methods for preparing positive electrode pieces and positive electrode materials for modified perfluorocarbon battery

    CN107959026A

  • Preparation method and application of carbon fluoride material

    CN111204735A