Positive electrode active material for non-aqueous electrolyte secondary battery, positive electrode for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery

The use of a lithium transition metal composite oxide with a sulfonic acid compound on its surface addresses the challenges of maintaining battery capacity and reducing reaction resistance in non-aqueous electrolyte secondary batteries, improving exposure resistance and reaction efficiency.

WO2024247736A1PCT designated stage expired Publication Date: 2024-12-05PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018088
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-05-16
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Non-aqueous electrolyte secondary batteries face challenges in maintaining battery capacity and reducing reaction resistance, especially when exposed to different atmospheres, with existing techniques not effectively addressing these issues.

Method used

A positive electrode active material comprising a lithium transition metal composite oxide with a layered structure and a sulfonic acid compound on its surface, where the sulfonic acid compound contains 70 mol% or more Ni, and a specific ammonia content, is used to enhance exposure resistance and reduce reaction resistance.

Benefits of technology

The proposed solution effectively improves exposure resistance and reduces reaction resistance in non-aqueous electrolyte secondary batteries, as demonstrated by the specific acid consumption range and ammonia content, leading to enhanced battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018088_05122024_PF_FP_ABST
    Figure JP2024018088_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a non-aqueous electrolyte secondary battery in which reaction resistance is reduced while improving exposure resistance. A positive electrode active material for a non-aqueous electrolyte secondary battery according to the present invention contains: a lithium transition metal composite oxide; and a sulfonic acid compound that is present on the surface of the lithium transition metal composite oxide and is represented by general formula I. When the lithium transition metal composite oxide is added to an alkali solution and subsequently distilled, the distillate is absorbed by sulfuric acid, and the result is analyzed by ion chromatography, a predetermined amount of ammonia is detected. When a filtrate of an aqueous dispersion of the lithium transition metal composite oxide is titrated with hydrochloric acid, the acid consumption amount to a first inflection point of a pH curve is defined as X mol / g, and the acid consumption amount to a second inflection point is defined as Y mol / g, Y - X and X - (Y - X) are each within a predetermined range. (In the formula, A represents a group 1 element or a group 2 element, R represents a hydrocarbon group, and n is 1 or 2.)
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode active material for non-aqueous electrolyte secondary battery, positive electrode for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery

[0001] The present disclosure relates to a positive electrode active material for a non-aqueous electrolyte secondary battery, a positive electrode for a non-aqueous electrolyte secondary battery, and a non-aqueous electrolyte secondary battery.

[0002] In recent years, the applications of non-aqueous electrolyte secondary batteries have expanded to include power sources for electric vehicles and power storage devices for utilizing natural energy. The characteristics required of the positive electrode active material used in non-aqueous electrolyte secondary batteries also change depending on the application. For example, Patent Document 1 discloses a technology for reducing the amount of gas generated during storage in a charged state in a non-aqueous electrolyte secondary battery using a water-free positive electrode active material.

[0003] Japanese Patent Application Laid-Open No. 2020-511642

[0004] However, non-aqueous electrolyte secondary batteries may experience a decrease in battery capacity due to the atmosphere to which they are exposed. Furthermore, reducing the reaction resistance of non-aqueous electrolyte secondary batteries is important for achieving excellent output characteristics. The technology described in Patent Document 1 does not address the suppression of the decrease in battery capacity due to exposure or the reduction of reaction resistance, and there is still room for improvement.

[0005] An object of the present disclosure is to provide a nonaqueous electrolyte secondary battery with improved exposure resistance and reduced reaction resistance.

[0006] A positive electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a lithium transition metal composite oxide and a sulfonic acid compound present on the surface of the lithium transition metal composite oxide, wherein the lithium transition metal composite oxide has a layered structure and contains 70 mol % or more of Ni relative to the total number of moles of metal elements excluding Li, and the sulfonic acid compound is represented by general formula I. When the lithium transition metal composite oxide is added to an alkaline solution and then distilled, and the distillate is absorbed into sulfuric acid and analyzed by ion chromatography, ammonia is detected at 2 ppm or more and 200 ppm or less relative to the lithium transition metal composite oxide. When an aqueous dispersion obtained by dispersing 1 g of the lithium transition metal composite oxide in 70 ml of pure water is titrated with hydrochloric acid, the value of Y-X is 50 μmol / g or more and 300 μmol / g or less, and the value of X-(Y-X) is 150 μmol / g or less, where X mol / g is the amount of acid consumed up to a first inflection point on a pH curve and Y mol / g is the amount of acid consumed up to a second inflection point. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)

[0007] A positive electrode for a nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure includes the positive electrode active material.

[0008] A non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a positive electrode containing the above-described positive electrode active material, a negative electrode, and a non-aqueous electrolyte.

[0009] According to the positive electrode active material for a non-aqueous electrolyte secondary battery according to one aspect of the present disclosure, the reaction resistance of the non-aqueous electrolyte secondary battery can be reduced while improving the exposure resistance thereof.

[0010] 1 is a longitudinal cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment of the present invention;

[0011] As described above, in non-aqueous electrolyte secondary batteries, it is an important challenge to improve exposure resistance while reducing reaction resistance. The present inventors have discovered that by allowing ammonia and a predetermined sulfonic acid compound to coexist on the surface of a lithium transition metal composite oxide that satisfies a predetermined acid consumption range, it is possible to specifically improve exposure resistance while reducing reaction resistance. Hereinafter, an example of an embodiment of the present disclosure will be described in detail with reference to the drawings.

[0012] An example of an embodiment of a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail below. In the following description, specific numerical values, materials, and designs may be used as examples. However, other numerical values, materials, and designs may be used as long as the effects of the present disclosure are obtained. A cylindrical battery in which a wound electrode assembly is housed in a cylindrical exterior body will be exemplified below. However, the electrode assembly is not limited to the wound type and may be a laminated type in which multiple positive electrodes and multiple negative electrodes are alternately stacked one by one with separators interposed therebetween. Furthermore, the exterior body is not limited to a cylindrical shape and may be, for example, rectangular or coin-shaped, or may be a battery case made of a laminate sheet including a metal layer and a resin layer.

[0013] FIG. 1 is an axial cross-sectional view of a cylindrical secondary battery 10 according to an embodiment. As shown in FIG. 1 , the secondary battery 10 includes a wound electrode assembly 14, an electrolyte, and an exterior body 16 that accommodates the electrode assembly 14 and the electrolyte. The electrode assembly 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a wound structure in which the positive electrode 11 and the negative electrode 12 are spirally wound with the separator 13 interposed therebetween. The exterior body 16 is a cylindrical metal container with a bottom and an opening on one axial side, and the opening of the exterior body 16 is closed by a sealing body 17. Hereinafter, for convenience of explanation, the sealing body 17 side of the battery will be referred to as the top, and the bottom side of the exterior body 16 will be referred to as the bottom.

[0014] The positive electrode 11, negative electrode 12, and separator 13 constituting the electrode assembly 14 are all rectangular, elongated bodies that are spirally wound in the longitudinal direction and alternately stacked in the radial direction of the electrode assembly 14. The separator 13 isolates the positive electrode 11 and the negative electrode 12 from each other. The negative electrode 12 is formed to be slightly larger than the positive electrode 11 to prevent lithium precipitation. That is, the negative electrode 12 is formed to be longer than the positive electrode 11 in the longitudinal and lateral directions. The two separators 13 are formed to be at least slightly larger than the positive electrode 11 and are arranged, for example, to sandwich the positive electrode 11. The electrode assembly 14 includes a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like. In the electrode assembly 14, the longitudinal direction of the positive electrode 11 and the negative electrode 12 is the winding direction, and the lateral direction of the positive electrode 11 and the negative electrode 12 is the axial direction. That is, the end faces in the lateral direction of the positive electrode 11 and the negative electrode 12 form the end faces in the axial direction of the electrode body 14 .

[0015] Insulating plates 18 and 19 are disposed above and below the electrode body 14. In the example shown in Fig. 1 , the positive electrode lead 20 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and the negative electrode lead 21 passes outside the insulating plate 19 and extends toward the bottom side of the exterior body 16. The positive electrode lead 20 is connected to the underside of an internal terminal plate 23 of the sealing body 17 by welding or the like, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the internal terminal plate 23, serves as the positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom surface of the exterior body 16 by welding or the like, and the exterior body 16 serves as the negative electrode terminal.

[0016] A gasket 28 is provided between the exterior body 16 and the sealing body 17 to ensure airtightness inside the battery. The exterior body 16 has a grooved portion 22 formed on its side surface that protrudes inward and supports the sealing body 17. The grooved portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior body 16, and supports the sealing body 17 on its top surface. The sealing body 17 is fixed to the top of the exterior body 16 by the grooved portion 22 and the open end of the exterior body 16 that is crimped to the sealing body 17.

[0017] The sealing body 17 has a structure in which, in order from the electrode body 14 side, an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are stacked. Each member constituting the sealing body 17 has, for example, a disk or ring shape, and each member except for the insulating member 25 is electrically connected to one another. The lower valve body 24 and the upper valve body 26 are connected at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks, pushing the upper valve body 26 toward the cap 27, thereby interrupting the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.

[0018] The positive electrode 11, the negative electrode 12, the separator 13, and the non-aqueous electrolyte that constitute the secondary battery 10 will be described in detail below, with the positive electrode 11 being particularly described below.

[0019] [Positive Electrode] The positive electrode 11 includes, for example, a positive electrode core and a positive electrode mixture layer formed on the surface of the positive electrode core. The positive electrode mixture layer is preferably formed on both sides of the positive electrode core. The positive electrode core may be a foil of a metal, such as aluminum or an aluminum alloy, that is stable within the potential range of the positive electrode 11, or a film with such a metal disposed on the surface. The thickness of the positive electrode core is, for example, 10 μm to 30 μm. The positive electrode mixture layer includes, for example, a positive electrode active material, a conductive agent, and a binder. The thickness of the positive electrode mixture layer is, for example, 10 μm to 150 μm on one side of the positive electrode current collector. The positive electrode 11 can be produced, for example, by applying a positive electrode mixture slurry containing a positive electrode active material, a conductive agent, a binder, etc. to the surface of the positive electrode current collector, drying the coating, and then rolling it to form a positive electrode mixture layer on both sides of the positive electrode current collector.

[0020] Examples of the conductive agent contained in the positive electrode mixture layer include carbon black (CB) such as acetylene black (AB) and ketjen black, carbon nanotubes (CNT), graphene, graphite, and other carbon-based materials. These may be used alone or in combination of two or more. The content of the conductive agent in the positive electrode mixture layer is, for example, 0.1% by mass or more and 10% by mass or less with respect to the total mass of the positive electrode mixture layer.

[0021] Examples of binders contained in the positive electrode mixture layer include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide-based resins, acrylic-based resins, and polyolefin-based resins. These may be used alone or in combination of two or more. The content of the binder in the positive electrode mixture layer is, for example, 0.1% by mass or more and 10% by mass or less with respect to the total mass of the positive electrode mixture layer.

[0022] The positive electrode active material contained in the positive electrode mixture layer 31 includes a lithium transition metal composite oxide. The lithium transition metal composite oxide includes, for example, secondary particles formed by aggregation of primary particles. When the lithium transition metal composite oxide is added to an alkaline solution, distilled, and the distillate is absorbed in sulfuric acid and analyzed by ion chromatography, ammonia is detected at a concentration of 2 ppm to 200 ppm relative to the mass of the lithium transition metal composite oxide. Furthermore, when the filtrate of an aqueous dispersion obtained by dispersing 1 g of lithium transition metal composite oxide in 70 ml of pure water is titrated with hydrochloric acid, where X mol / g is the acid consumption up to the first inflection point of the pH curve and Y mol / g is the acid consumption up to the second inflection point, the value of Y-X is 50 μmol / g to 300 μmol / g, and the value of X-(Y-X) is 150 μmol / g or less. This allows the surface of the lithium transition metal composite oxide to be adequately protected without the need for a water washing treatment after firing. On the surfaces of the primary particles constituting the lithium transition metal composite oxide, for example, ammonium compounds are present in an amount of 2 ppm to 200 ppm relative to the mass of the composite oxide.

[0023] The lithium transition metal composite oxide has a layered structure. Examples of the layered structure of the lithium transition metal composite oxide include a layered structure belonging to the space group R-3m and a layered structure belonging to the space group C2 / m. From the viewpoints of increasing capacity and crystalline structure stability, the lithium transition metal composite oxide preferably has a layered structure belonging to the space group R-3m. The layered structure of the lithium transition metal composite oxide may include a transition metal layer, a Li layer, and an oxygen layer.

[0024] The lithium transition metal composite oxide contains 70 mol% or more of Ni relative to the total number of moles of metal elements excluding Li. This allows for a high capacity battery. The Ni content may be, for example, 80 mol% or more and 98 mol% or less. The lithium transition metal composite oxide may contain, in addition to Ni, one or more elements selected from the group consisting of Co, Al, and Mn. The contents of Co, Al, and Mn in the lithium transition metal composite oxide are each, for example, 0 mol% or more and 30 mol% or less relative to the total number of moles of metal elements excluding Li. Furthermore, the total content of Co, Al, and Mn is, for example, 0 mol% or more and 30 mol% or less.

[0025] The lithium transition metal composite oxide is, for example, a compound represented by the general formula Li a Ni x M1 y M2 z O 2-b (wherein 0.8≦a≦1.2, 0.70≦x≦0.98, 0≦y≦0.30, 0≦z≦0.10, 0≦b≦0.05, x+y+z=1, M1 is one or more elements selected from the group consisting of Co, Al, and Mn, and M2 is one or more elements selected from the group consisting of Sr, Ca, Nb, Ti, Zr, and W). The proportion of metal elements contained in the lithium transition metal composite oxide can be measured, for example, by inductively coupled plasma atomic emission spectrometry (ICP-AES).

[0026] The BET specific surface area of ​​the lithium transition metal composite oxide is 0.9 m 2 / g or less is preferable, and 0.8m 2 The BET specific surface area of ​​the composite oxide is, for example, 0.5 m 2 / g or more 0.8m 2 / g or less. The BET specific surface area is measured according to the BET method described in JIS R1626. Specifically, the BET nitrogen adsorption isotherm of the dried composite oxide particles is measured using an automatic specific surface area / pore distribution analyzer (Autosorb iQ3-MP, manufactured by Quantachrome), and the specific surface area is calculated from the amount of nitrogen adsorption using the BET multipoint method.

[0027] The particle size of the primary particles constituting the lithium transition metal composite oxide is, for example, 0.02 μm or more and 2 μm or less. The particle size of the primary particles is measured as the diameter of the circumscribed circle in a particle image observed with a scanning electron microscope (SEM). The average particle size of the secondary particles of the lithium transition metal composite oxide is, for example, 2 μm or more and 30 μm or less. Here, the average particle size refers to the volume-based median diameter (D50). D50 refers to the particle size at which the cumulative frequency in the volume-based particle size distribution is 50% from the smallest particle size, and is also called the median diameter. The particle size distribution of the secondary particles can be measured using a laser diffraction particle size distribution analyzer (e.g., MT3000II, manufactured by Microtrac-Bell Corporation) using water as a dispersion medium.

[0028] As described above, when the filtrate of an aqueous dispersion obtained by dispersing 1 g of lithium transition metal composite oxide in 70 ml of pure water is titrated with hydrochloric acid, the value of Y-X is 50 μmol / g or more and 300 μmol / g or less, and the value of X-(Y-X) is 150 μmol / g or less, where X mol / g is the acid consumption up to the first inflection point of the pH curve and Y mol / g is the acid consumption up to the second inflection point. That is, the lithium transition metal composite oxide contains a water-soluble alkali component that can be titrated with acid. The value of Y-X is preferably 70 μmol / g or more and 250 μmol / g or less, more preferably 80 μmol / g or more and 220 μmol / g or less. The value of X-(Y-X) is preferably 80 μmol / g or less, more preferably 50 μmol / g or less.

[0029] The lithium transition metal composite oxide contains an alkaline component in an amount corresponding to the above-mentioned acid consumption amount. Examples of the alkaline component include lithium hydroxide (LiOH) and lithium carbonate (Li 2 CO 3) and the like. The lithium transition metal composite oxide also contains an ammonium compound in an amount of 2 ppm to 200 ppm in terms of ammonia molecules. The ammonium compound is, for example, ammonia or an ammonium salt. The lithium carbonate, lithium hydroxide, and ammonium compound may be present at the interface between each primary particle inside the composite oxide particles and on the surface of secondary particles formed by aggregation of the primary particles. It is preferable that these are present uniformly throughout the surface of the primary particles, without being unevenly distributed in a part of the surface.

[0030] A specific method for quantifying the water-soluble alkaline component extracted from the lithium transition metal composite oxide is as follows. The titration method described below is generally referred to as the Warder method. (1) 1 g of lithium transition metal composite oxide is added to 30 ml of pure water and stirred to prepare a suspension in which the active material is dispersed in water. (2) The suspension is filtered, and pure water is added to make a measuring cup to bring the total volume to 70 ml to obtain a filtrate containing the water-soluble alkaline component eluted from the active material. (3) While measuring the pH of the filtrate, hydrochloric acid is added dropwise to the filtrate to determine the amount of hydrochloric acid (titration amount) X mol / g consumed up to the first inflection point (near pH 8) of the pH curve and the amount of hydrochloric acid consumed up to the second inflection point (near pH 4) Y mol / g. The inflection points are the peak positions of the differential value with respect to the titration amount.

[0031] The amount of ammonium compounds present on the surface of the primary particles can be quantified by ion chromatography. The specific measurement method is as follows: (1) 1 g of lithium transition metal composite oxide is transferred to a distillation flask and 300 ml of pure water is added. (2) 10 ml of a 30% aqueous sodium hydroxide solution is added to the aqueous dispersion of the lithium transition metal composite oxide to make an alkaline solution, and then boiling stones are added and distilled. (3) The boiled and evaporated solution is cooled and collected, added to 40 ml of sulfuric acid (25 mmol / L), and the volume is adjusted to 200 ml with pure water to obtain a sample solution. (4) The sample solution is measured by ion chromatography, and the amount of ammonium ions detected is converted to the amount of ammonia in the sample.

[0032] At least one surface coating agent selected from a zirconium compound, a tungsten compound, a phosphorus compound, a boron compound, and a rare earth compound may be attached to the surface of the primary particles of the lithium transition metal composite oxide. The surface coating agent is attached to at least one of the surfaces of the primary particles present inside the composite oxide particles, i.e., inside the secondary particles, and the surfaces of the primary particles present on the surface of the composite oxide particles, i.e., the surfaces of the secondary particles. The presence of the surface coating agent suppresses gas generation during charged storage, etc., without causing problems such as capacity reduction. The surface coating agent is preferably present evenly throughout the primary particle surface, rather than being concentrated in a specific area. Furthermore, the content of these agents, in terms of the metal elements constituting the compound, is preferably 0.01 mol% to 0.5 mol% relative to the total moles of metal elements excluding Li in the lithium transition metal composite oxide.

[0033] The zirconium compound, tungsten compound, phosphorus compound, boron compound, and rare earth compound may be any of oxides, nitrides, hydroxides, etc. Specific examples include zirconium oxide, tungsten oxide, lithium tungstate, lithium phosphate, boron oxide, lithium tetraborate, samarium hydroxide, erbium hydroxide, samarium oxide, erbium oxide, etc. The presence of these compounds attached to the surfaces of primary particles present inside or on the surfaces of secondary particles, and the content in terms of metal elements can be observed and measured using a scanning electron microscope (SEM) and an inductively coupled plasma (ICP) optical emission spectrometer.

[0034] The lithium transition metal composite oxide is produced through a first step of synthesizing a metal hydroxide containing Ni, Co, Mn, Al, etc., for example, by a coprecipitation method, a second step of subjecting the metal hydroxide to an oxidizing roasting heat treatment to obtain a metal oxide, and a third step of mixing the metal oxide with lithium hydroxide and calcining the mixture (synthesis step). The lithium transition metal composite oxide obtained in the third step may be washed with water, but is preferably used in a substantially unwashed state.

[0035] In the third step, the mixture is calcined at a temperature of 700°C or higher. The preferred calcination temperature range is 700°C or higher and 900°C or lower. Calcination is preferably carried out in an oxygen stream. In the third step, from the viewpoint of discharge capacity, an excess of lithium source (lithium hydroxide) is used relative to the stoichiometric ratio of the target product. For example, a stoichiometric ratio of 1 to 1.1 times that of the composite oxide is preferred.

[0036] The synthesis process for the lithium transition metal composite oxide is not limited to the above-described process, and may also include, for example, a known synthesis method in which a precursor obtained by co-precipitating or mixing a compound such as a hydroxide, oxide, or carbonate containing at least one element selected from Ni, Co, Mn, Al, and M (M is at least one element selected from Ca, Sr, W, Mg, Mo, Nb, Ti, Si, Mn, and Zr) is mixed with a Li source and calcined to obtain a lithium transition metal composite oxide. When the precursor does not contain a compound such as M, these compounds such as M may be mixed and calcined when the precursor and Li source are mixed and calcined. Furthermore, these compounds may be pulverized to appropriately change the particle shape or particle size, or the water content, including hydrates, may be adjusted before use.

[0037] The process for producing the lithium transition metal composite oxide preferably further includes a fourth step of adding a compound serving as an ammonia source and a compound serving as a carbonate source. In the fourth step, a compound serving as an ammonia source and a carbonate source, such as ammonium carbonate, may be added. In the fourth step, an aqueous solution of ammonium carbonate is, for example, added dropwise or sprayed onto the anhydrous lithium transition metal composite oxide, followed by heat treatment at a temperature lower than the calcination temperature in the third step. An example of the heat treatment conditions is a temperature of 200°C to 500°C and a heating time of 1 hour to 4 hours. Because excess Li exists on the particle surfaces of the anhydrous lithium transition metal composite oxide, adding ammonium carbonate to the particle surfaces, for example, produces lithium carbonate and ammonium compounds.

[0038] The positive electrode active material contains, in addition to a lithium transition metal composite oxide, a sulfonic acid compound represented by the following general formula I. The sulfonic acid compound is present on the surface of the lithium transition metal composite oxide. By including a lithium transition metal composite oxide containing a predetermined amount of an ammonia compound and an alkali component, and the sulfonic acid compound present on the surface of the lithium transition metal composite oxide, the surface of the positive electrode active material is appropriately protected, thereby achieving both improved exposure resistance and reduced reaction resistance. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.)

[0039] The positive electrode mixture layer may contain other positive electrode active materials in addition to the positive electrode active material of the present embodiment described above. Examples of other positive electrode active materials include a lithium transition metal composite oxide in which one or more of the ammonia amount, Y-X, and X-(Y-X) are outside the predetermined range, a positive electrode active material containing a lithium transition metal composite oxide with an Ni content of less than 70 mol%, and a positive electrode active material in which no sulfonic acid compound is present on the surface of the lithium transition metal composite oxide.

[0040] In the above general formula I, A is preferably a Group 1 element, more preferably Li. This can further reduce the DC resistance. Note that when A is a Group 1 element, n=1.

[0041] In general formula I, R is preferably an alkyl group. R is more preferably an alkyl group having 5 or less carbon atoms, further preferably an alkyl group having 3 or less carbon atoms, and particularly preferably a methyl group. In addition, in R, some of the hydrogen atoms bonded to the carbon atoms may be substituted with fluorine. However, in R, not all of the hydrogen atoms bonded to the carbon atoms are substituted with fluorine. The smaller the molecular weight of R, the smaller the DC resistance can be.

[0042] Examples of sulfonic acid compounds include lithium methanesulfonate, lithium ethanesulfonate, lithium propanesulfonate, sodium methanesulfonate, magnesium methanesulfonate, and lithium fluoromethanesulfonate.

[0043] The amount of the sulfonic acid compound contained in the positive electrode 11 is preferably 0.1% by mass or more and 2% by mass or less, and more preferably 0.25% by mass or more and 1.0% by mass or less, relative to the mass of the lithium transition metal composite oxide.

[0044] The presence of the sulfonic acid compound in the positive electrode 11 can be confirmed by Fourier transform infrared spectroscopy (FT-IR). In the infrared absorption spectrum obtained by FT-IR, the positive electrode 11 exhibits a peak at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 It may have an absorption peak at at least one point in the vicinity.

[0045] In the infrared absorption spectrum obtained by FT-IR, for example, the positive electrode 11 containing lithium methanesulfonate has a peak at 1238 cm -1 , 1175 cm -1 , 1065 cm -1 , 785 cm -1 It has an absorption peak around 1238 cm -1 , 1175 cm -1 , 1065 cm -1 The peak around 785 cm is an absorption peak due to the SO stretching vibration of lithium methanesulfonate. -1 The peak in the vicinity is an absorption peak due to the C-S stretching vibration derived from lithium methanesulfonate.

[0046] In the case of the positive electrode 11 containing a sulfonic acid compound other than lithium methanesulfonate, an absorption peak derived from the sulfonic acid compound can be identified, similar to the case of the positive electrode 11 containing lithium methanesulfonate. The presence of the sulfonic acid compound in the positive electrode 11 can also be confirmed by ICP, atomic absorption spectroscopy, X-ray photoelectron spectroscopy (XPS), synchrotron XRD measurement, TOF-SIMS, H-NMR, or the like.

[0047] The positive electrode active material can be prepared, for example, by adding a sulfonic acid solution to an anhydrous lithium transition metal composite oxide and adhering the sulfonic acid compound to the surface of the lithium transition metal composite oxide (addition step). The sulfonic acid solution is, for example, a methanesulfonic acid solution prepared by dissolving methanesulfonic acid in water. Li compounds remain on the surface of the lithium transition metal composite oxide, and even when a sulfonic acid solution is added, a sulfonic acid compound containing Li is formed. A Li compound or a Li compound solution may be added to the lithium transition metal composite oxide together with the sulfonic acid solution, or a mixed solution prepared by premixing the sulfonic acid solution with the Li compound or Li compound solution may be added to the lithium transition metal composite oxide. The Li compound is, for example, LiOH, and the Li compound solution is, for example, a LiOH solution prepared by dissolving LiOH in water. The amounts of the Li compound and sulfonic acid solution added to the lithium transition metal composite oxide preferably satisfy the relationship of 0≦Li compound / sulfonic acid≦1.3 in molar ratio. After the adding step, a drying step may be carried out, for example, under a vacuum atmosphere.

[0048] [Negative Electrode] The negative electrode 12 may have, for example, a negative electrode core and a negative electrode mixture layer formed on the surface of the negative electrode core, or a metal Li foil may be used as the negative electrode 12. Alternatively, the negative electrode 12 may have a negative electrode core, and lithium metal may be deposited on the surface of the negative electrode core upon charging. When the negative electrode 12 has a negative electrode mixture layer, the negative electrode mixture layer is preferably formed on both sides of the negative electrode core. The negative electrode core may be a foil of a metal stable within the potential range of the negative electrode 12, such as copper or a copper alloy, or a film with such a metal disposed on the surface. The thickness of the negative electrode core is, for example, 5 μm or more and 30 μm or less. The negative electrode mixture layer includes, for example, a negative electrode active material and a binder. The thickness of the negative electrode mixture layer is, for example, 10 μm or more and 150 μm or less on one side of the negative electrode core. The negative electrode 12 can be produced, for example, by applying a negative electrode mixture slurry containing a negative electrode active material, a binder, etc. to the surface of a negative electrode core, drying the coating, and then rolling it to form a negative electrode mixture layer on both sides of the negative electrode core.

[0049] The negative electrode active material contained in the negative electrode mixture layer is not particularly limited as long as it can reversibly absorb and release lithium ions, and generally, carbon materials such as graphite are used. Graphite may be any of natural graphite such as flake graphite, lump graphite, and amorphous graphite, or artificial graphite such as lump artificial graphite and graphitized mesophase carbon microbeads. Furthermore, metals that alloy with Li, such as Si and Sn, metal compounds containing Si, Sn, and lithium-titanium composite oxides may also be used as the negative electrode active material. Furthermore, those provided with a carbon coating may also be used. For example, SiO x (0.5≦x≦1.6) or Li 2y SiO (2+y) A Si-containing compound in which fine particles of Si are dispersed in a lithium silicate phase represented by (0<y<2) may be used in combination with graphite.

[0050] Examples of binders contained in the negative electrode mixture layer include styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more.

[0051] [Separator] A porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator 13 include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may have a single-layer structure or a multi-layer structure. Furthermore, a highly heat-resistant resin layer such as an aramid resin may be formed on the surface of the separator 13.

[0052] A filler layer containing an inorganic filler may be formed at the interface between the separator 13 and at least one of the positive electrode 11 and the negative electrode 12. Examples of inorganic fillers include oxides and phosphate compounds containing metal elements such as Ti, Al, Si, and Mg. The filler layer can be formed by applying a slurry containing the filler to the surface of the positive electrode 11, the negative electrode 12, or the separator 13.

[0053] [Non-aqueous electrolyte] The non-aqueous electrolyte has, for example, lithium ion conductivity. The non-aqueous electrolyte may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.

[0054] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent that can be used include esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these. The non-aqueous solvent may contain a halogen-substituted compound in which at least a portion of the hydrogen atoms in these solvents are substituted with halogen atoms such as fluorine. Examples of the halogen-substituted compound include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, and fluorinated chain carboxylic acid esters such as methyl fluoropropionate (FMP).

[0055] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylic acid esters such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).

[0056] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, and methyl phenyl ether. and chain ethers such as ethyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.

[0057] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiClO 4 , LiBF 4 , LiPF 6 , LiAlCl 4 , LiSbF 6 , LiSCN, LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiB 10 Cl 10 , lower aliphatic lithium carboxylates, LiCl, LiBr, LiI, phosphates, borates, and imide salts. Examples of phosphates include lithium difluorophosphate (LiPO 2 F 2Examples of the borate salt include lithium bis(oxalato)borate (LiBOB) and lithium difluoro(oxalato)borate (LiDFFOB). Examples of the imide salt include lithium bisfluorosulfonylimide (LiN(FSO 2 ) 2 ), lithium bistrifluoromethanesulfonyl imide (LiN(CF 3 SO 2 ) 2 ), lithium trifluoromethanesulfonate nonafluorobutanesulfonate imide (LiN(CF 3 SO 2 ) (C 4 F 9 SO 2 )), lithium bispentafluoroethanesulfonyl imide (LiN(C 2 F 5 SO 2 ) 2 Among these, LiPF is preferred from the viewpoint of ionic conductivity, electrochemical stability, etc. 6 The concentration of the lithium salt may be, for example, 4 mol or less, or 3 mol or less, preferably 1.8 mol or less, and more preferably 0.8 mol or more and 1.8 mol or less, per 1 L of the non-aqueous solvent.

[0058] The non-aqueous electrolyte may contain an additive such as an unsaturated carbonate ester, an acid anhydride, a phenol compound, a benzene compound, a nitrile compound, an isocyanate compound, a sultone compound, a sulfate compound, a borate ester compound, a phosphate ester compound, or a phosphite ester compound.

[0059] Examples of unsaturated cyclic carbonates include vinylene carbonate, 4-methylvinylene carbonate, 4,5-dimethylvinylene carbonate, 4-ethylvinylene carbonate, 4,5-diethylvinylene carbonate, 4-propylvinylene carbonate, 4,5-dipropylvinylene carbonate, 4-phenylvinylene carbonate, 4,5-diphenylvinylene carbonate, vinylethylene carbonate, and divinylethylene carbonate. One type of unsaturated cyclic carbonate may be used alone, or two or more types may be used in combination. Some of the hydrogen atoms in the unsaturated cyclic carbonate may be substituted with fluorine atoms. The acid anhydride may be an anhydride formed by intermolecular condensation of multiple carboxylic acid molecules, but is preferably an acid anhydride of a polycarboxylic acid. Examples of polycarboxylic acid anhydrides include succinic anhydride, maleic anhydride, and phthalic anhydride.

[0060] Examples of phenolic compounds include phenol, hydroxytoluene, etc. Examples of benzene compounds include fluorobenzene, hexafluorobenzene, cyclohexylbenzene (CHB), etc.

[0061] Examples of nitrile compounds include adiponitrile, pimelonitrile, propionitrile, and succinonitrile. Examples of isocyanate compounds include methyl isocyanate (MIC), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), and bisisocyanatomethylcyclohexane (BIMCH). Examples of sultone compounds include propane sultone and propene sultone. Examples of sulfate compounds include ethylene sulfate, ethylene sulfite, dimethyl sulfate, and lithium fluorosulfate. Examples of borate ester compounds include trimethyl borate and tris(trimethylsilyl)borate. Examples of phosphate ester compounds include trimethyl phosphate and tris(trimethylsilyl)phosphate. Examples of phosphite ester compounds include trimethyl phosphite and tris(trimethylsilyl)phosphite.

[0062] As the solid electrolyte, for example, a solid or gel-like polymer electrolyte, an inorganic solid electrolyte, etc. can be used. As the inorganic solid electrolyte, a material known in all-solid-state lithium ion secondary batteries, etc. (for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a halogen-based solid electrolyte, etc.) can be used. The polymer electrolyte includes, for example, a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. As the matrix polymer, for example, a polymer material that absorbs the non-aqueous solvent and gels is used. As the polymer material, for example, a fluororesin, an acrylic resin, a polyether resin, etc. can be used.

[0063] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to the following examples.

[0064] Example 1 Preparation of Positive Electrode Active Material [Ni 0.90 Co 0.05 Al 0.05 ](OH) 2A metal hydroxide represented by the formula (I) was calcined at 500°C for 8 hours to obtain a metal oxide. The metal oxide and LiOH were mixed in a molar ratio of 1:1.02, and the mixture was calcined at 800°C for 3 hours under an oxygen stream to obtain a lithium transition metal composite oxide (calcined product). The calcined product was secondary particles formed by aggregation of primary particles. An aqueous ammonium carbonate solution was sprayed onto the anhydrous calcined product, and then heated at 200°C for 3 hours to obtain a lithium transition metal composite oxide. The acid consumption amounts Y-X and X-(Y-X) per 1 g of lithium transition metal composite oxide were determined by the Warder method, and the ammonia amount was determined by the chromatographic analysis. The spraying conditions for the aqueous ammonium carbonate solution were adjusted so that these values ​​were as shown in Table 1 (the same applies hereinafter).

[0065] A methanesulfonic acid solution was added to the lithium transition metal composite oxide (addition step). The concentration of the methanesulfonic acid solution was 10 mass %, and the amount of methanesulfonic acid added was 0.5 mass % relative to the total mass of the lithium transition metal composite oxide. After the addition step, a drying step was performed under a vacuum atmosphere to obtain the positive electrode active material of Example 1. Fourier transform infrared spectroscopy (FT-IR) confirmed the presence of lithium methanesulfonate on the surface of the positive electrode active material.

[0066] The positive electrode active material was left for 4 weeks in an environment with a temperature of 25°C and a dew point of -20°C, exposed to dry air at a wind speed of 4 m / s, to prepare an exposed sample. In addition, the positive electrode active material was left for 4 weeks in an environment with a temperature of 25°C and a dew point of -40°C, without being exposed to dry air, to prepare an unexposed sample.

[0067] [Preparation of Positive Electrode] The exposed sample, acetylene black, and polyvinylidene fluoride were mixed in a mass ratio of 85:10:5 and kneaded using an agate mortar and pestle to form thin pellets. The pellets were then rolled to a predetermined thickness using a roller and punched into a predetermined circular shape to form a positive electrode containing the exposed sample. A positive electrode containing the unexposed sample was prepared in the same manner using the unexposed sample.

[0068] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF 6 ) was dissolved in the solution to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.

[0069] [Preparation of Test Cell] A positive electrode containing an exposed sample and a negative electrode made of lithium metal were stacked facing each other with a separator interposed therebetween to prepare an electrode assembly. The electrode assembly and the nonaqueous electrolyte were then inserted into an aluminum coin-shaped outer casing and sealed by crimping with a press to prepare an exposed test cell. An unexposed test cell was prepared in the same manner using a positive electrode containing an unexposed sample.

[0070] [Evaluation of Exposure Resistance] Each of the exposed test cells and unexposed test cells was charged at a constant current of 0.1 C in a temperature environment of 25 ° C until the cell voltage reached 4.3 V (vs. Li), and then charged at a constant voltage of 4.3 V (vs. Li) until the current value reached 0.01 C. After 1 hour, the cell was discharged at a constant current of 0.1 C until the cell voltage reached 2.5 V (vs. Li). Then, again in a temperature environment of 25 ° C, the cell was charged at a constant current of 0.1 C until the cell voltage reached 4.3 V (vs. Li), and then charged at a constant voltage of 4.3 V (vs. Li) until the current value reached 0.01 C. Then, each of the exposed sample and unexposed sample was discharged at a constant current of 0.2 C until the cell voltage reached 2.5 V (vs. Li), and the exposure resistance was calculated using the following formula: Exposure resistance = (discharge capacity of exposed test cell) / (discharge capacity of unexposed test cell)

[0071] [Evaluation of reaction resistance] The test cell was charged at a constant current of 0.1 C in a temperature environment of 25 ° C until the cell voltage reached 4.3 V (vs. Li), and then charged at a constant voltage of 4.3 V (vs. Li) until the current value reached 0.01 C. After 1 hour, the cell voltage was discharged at a constant current of 0.1 C to 2.5 V (vs. Li). Then, again in a temperature environment of 25 ° C, the cell voltage was charged at a constant current of 0.1 C until the cell voltage reached 4.3 V (vs. Li), and then charged at a constant voltage of 4.3 V (vs. Li) until the current value reached 0.01 C. Next, after 2 hours in a temperature environment of 10 ° C, the AC impedance of the test cell was measured using a Solartron 1255B (manufactured by Solartron) at an applied voltage of 10 mV and a measurement frequency range of 0.01 Hz to 200 kHz. A Nyquist diagram was drawn from the measurement data, and the reaction resistance was calculated from the size of the arc between 10 Hz and 0.1 Hz.

[0072] Example 2 A test cell was prepared and evaluated in the same manner as in Example 1, except that in preparing the positive electrode active material, the ammonium carbonate aqueous solution was added first, followed by the addition of tungsten oxide powder. The amount of tungsten oxide added was adjusted to 0.1 mol % in terms of W relative to the total number of moles of metal elements in the composite oxide excluding Li.

[0073] Example 3 A test cell was prepared and evaluated in the same manner as in Example 1, except that in preparing the positive electrode active material, the ammonium carbonate aqueous solution was added first, followed by the samarium sulfate aqueous solution. The amount of samarium sulfate added was adjusted to 0.1 mol % in terms of Sm with respect to the total number of moles of metal elements in the composite oxide excluding Li.

[0074] Example 4 A test cell was prepared and evaluated in the same manner as in Example 1, except that ammonium zirconium carbonate was used instead of ammonium carbonate in the preparation of the positive electrode active material. That is, an aqueous solution of ammonium zirconium carbonate was sprayed onto the anhydrous fired product, followed by heat treatment. The amount of ammonium zirconium carbonate added was adjusted to 0.1 mol % in terms of Zr relative to the total number of moles of metal elements in the composite oxide excluding Li.

[0075] Examples 5 and 6 Test cells were prepared and evaluated in the same manner as in Example 1, except that in the preparation of the positive electrode active material, the spraying conditions of the ammonium carbonate aqueous solution were adjusted so that the amounts of Y-X, X-(Y-X), and ammonia were the values ​​shown in Table 1.

[0076] Comparative Example 1 A test cell was produced and evaluated in the same manner as in Example 1, except that in the preparation of the positive electrode active material, the fired product without washing was used as it was as the positive electrode active material.

[0077] Comparative Example 2 A test cell was prepared and evaluated in the same manner as in Example 1, except that in preparing the positive electrode active material, ammonia water was sprayed instead of the ammonium carbonate aqueous solution.

[0078] Comparative Example 3 A test cell was produced and evaluated in the same manner as in Example 1, except that the addition step was not carried out in the production of the positive electrode active material.

[0079] Comparative Example 4 A test cell was produced and evaluated in the same manner as in Example 1, except that in the preparation of the positive electrode active material, the fired product without washing without water was used as the lithium transition metal composite oxide, and the lithium transition metal composite oxide was washed with water without performing the addition step, and then subjected to a drying step under conditions of 180°C and 2 hours in a vacuum atmosphere. The lithium transition metal composite oxide was washed with water by adding water to give a slurry concentration of 1500 g / L and stirring for 15 minutes.

[0080] Comparative Example 5 A test cell was produced and evaluated in the same manner as in Example 1, except that in the preparation of the positive electrode active material, ammonia water was sprayed instead of the ammonium carbonate aqueous solution, and the lithium transition metal composite oxide was washed with water without performing the addition step, and then subjected to a drying step under conditions of 180°C in a vacuum atmosphere for 2 hours. The lithium transition metal composite oxide was washed with water by adding water to give a slurry concentration of 1500 g / L and stirring for 15 minutes.

[0081] Comparative Example 6 A test cell was produced and evaluated in the same manner as in Example 1, except that in the preparation of the positive electrode active material, the fired product without washing without water was used as the lithium transition metal composite oxide, and the lithium transition metal composite oxide was washed with water before the addition step and then subjected to a drying step under conditions of 180°C in a vacuum atmosphere for 2 hours. The lithium transition metal composite oxide was washed with water by adding water to give a slurry concentration of 1500 g / L and stirring for 15 minutes.

[0082] Example 7 In the preparation of a positive electrode active material, [Ni 0.82 Co 0.15 Al 0.03 ](OH) 2 A test cell was produced in the same manner as in Example 1, except that a nickel-cobalt-aluminum composite hydroxide represented by the following formula was used, and the spraying conditions of the ammonium carbonate aqueous solution were adjusted so that the amounts of Y-X, X-(Y-X), and ammonia would be the values ​​shown in Table 1, and evaluation was performed.

[0083] Comparative Example 7 A test cell was produced and evaluated in the same manner as in Example 7, except that in the preparation of the positive electrode active material, the fired product without washing was used as it was as the lithium transition metal composite oxide.

[0084] Example 8 In the preparation of a positive electrode active material, [Ni 0.90 Co 0.05 Mn 0.05 ](OH) 2 A test cell was produced in the same manner as in Example 1, except that a nickel-cobalt-manganese composite hydroxide represented by the following formula was used, and the spraying conditions of the ammonium carbonate aqueous solution were adjusted so that the amounts of Y-X, X-(Y-X), and ammonia became the values ​​shown in Table 1, and evaluation was performed.

[0085] Comparative Example 8 A test cell was produced and evaluated in the same manner as in Example 8, except that in the preparation of the positive electrode active material, the fired product without washing was used as it was as the lithium transition metal composite oxide.

[0086] The evaluation results of the test cells of the Examples and Comparative Examples are shown in Table 1. In Table 1, the exposure resistance and reaction resistance of the test cells of Examples 1 to 5 and Comparative Examples 1 to 6 are expressed relative to the exposure resistance and reaction resistance of the test cell of Example 6, each of which is set to 100. The exposure resistance and reaction resistance of the test cell of Comparative Example 7 are expressed relative to the exposure resistance and reaction resistance of the test cell of Example 7, each of which is set to 100, and the exposure resistance and reaction resistance of the test cell of Comparative Example 8 are expressed relative to the exposure resistance and reaction resistance of the test cell of Example 8, each of which is set to 100. Table 1 also shows Y-X, X-(Y-X), and the amount of ammonia.

[0087]

[0088] In Table 1, all of the test cells of the examples have superior exposure resistance and lower reaction resistance compared to the corresponding test cells of the comparative examples. This shows that by causing ammonia and a predetermined sulfonic acid compound to coexist on the surface of a lithium transition metal composite oxide that satisfies a predetermined range of acid consumption, it is possible to specifically improve exposure resistance while reducing reaction resistance.

[0089] The present disclosure is further described by the following embodiments. Configuration 1: A positive electrode active material for a non-aqueous electrolyte secondary battery, comprising a lithium transition metal composite oxide and a sulfonic acid compound present on the surface of the lithium transition metal composite oxide, wherein the lithium transition metal composite oxide has a layered structure and contains 70 mol % or more of Ni relative to the total number of moles of metal elements excluding Li, the sulfonic acid compound is represented by general formula I, and when the lithium transition metal composite oxide is added to an alkaline solution and then distilled, and the distillate is absorbed in sulfuric acid and analyzed by ion chromatography, ammonia is detected at 2 ppm to 200 ppm relative to the lithium transition metal composite oxide, and A positive electrode active material for a non-aqueous electrolyte secondary battery, wherein, when a filtrate of an aqueous dispersion obtained by dispersing 1 g of the lithium transition metal composite oxide in 70 ml of pure water is titrated with hydrochloric acid, the value of Y-X is 50 μmol / g or more and 300 μmol / g or less, and the value of X-(Y-X) is 150 μmol / g or less, where X mol / g is the amount of acid consumed up to a first inflection point of a pH curve and Y mol / g is the amount of acid consumed up to a second inflection point. (wherein A is a Group 1 element or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) Configuration 2: The positive electrode active material for a non-aqueous electrolyte secondary battery according to Configuration 1, wherein the lithium transition metal composite oxide contains secondary particles formed by aggregation of primary particles. Configuration 3: The positive electrode active material for a non-aqueous electrolyte secondary battery according to Configuration 1 or 2, wherein A is a Group 1 element. Configuration 4: The positive electrode active material for a non-aqueous electrolyte secondary battery according to Configuration 1 or 2, wherein A is Li. Configuration 5: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein R is an alkyl group. Configuration 6: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 4, wherein R is a methyl group. Configuration 7: The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 6, wherein the amount of the sulfonic acid compound present on the surface of the lithium transition metal composite oxide is 0.1 mass % or more and 2 mass % or less, relative to the mass of the lithium transition metal composite oxide. Configuration 8: A positive electrode for a non-aqueous electrolyte secondary battery, comprising the positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 7. Configuration 9: A non-aqueous electrolyte secondary battery, comprising: a positive electrode comprising the positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 7; a negative electrode; and a non-aqueous electrolyte.

[0090] REFERENCE SIGNS LIST 10 Secondary battery, 11 Positive electrode, 12 Negative electrode, 13 Separator, 14 Electrode body, 16 Exterior body, 17 Sealing body, 18, 19 Insulating plate, 20 Positive electrode lead, 21 Negative electrode lead, 22 Grooved portion, 23 Internal terminal plate, 24 Lower valve body, 25 Insulating member, 26 Upper valve body, 27 Cap, 28 Gasket

Claims

1. A positive electrode active material for a non-aqueous electrolyte secondary battery comprising a lithium transition metal composite oxide and a sulfonic acid compound present on a surface of the lithium transition metal composite oxide, wherein the lithium transition metal composite oxide has a layered structure and contains 70 mol % or more of Ni relative to the total number of moles of metal elements excluding Li, when the lithium transition metal composite oxide is added to an alkaline solution and then distilled, and the distillate is absorbed into sulfuric acid and analyzed by ion chromatography, ammonia is detected at 2 ppm or more and 200 ppm or less relative to the lithium transition metal composite oxide, when a filtrate of an aqueous dispersion obtained by dispersing 1 g of the lithium transition metal composite oxide in 70 ml of pure water is titrated with hydrochloric acid, where X mol / g is the amount of acid consumed up to a first inflection point of a pH curve and Y mol / g is the amount of acid consumed up to a second inflection point, the value of Y-X is 50 μmol / g or more and 300 μmol / g or less and the value of X-(Y-X) is 150 μmol / g or less, The sulfonic acid compound is represented by general formula I, which is a positive electrode active material for a non-aqueous electrolyte secondary battery. (In the formula, A is a Group 1 or Group 2 element, R is a hydrocarbon group, and n is 1 or 2.) 2. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the lithium transition metal composite oxide contains secondary particles formed by aggregation of primary particles.

3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein A is a Group 1 element.

4. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein A is Li.

5. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein R is an alkyl group.

6. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein R is a methyl group.

7. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the amount of the sulfonic acid compound present on the surface of the lithium transition metal composite oxide is 0.1 mass % or more and 2 mass % or less, based on the mass of the lithium transition metal composite oxide.

8. A positive electrode for a non-aqueous electrolyte secondary battery, comprising the positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 7.

9. A non-aqueous electrolyte secondary battery comprising: a positive electrode containing the positive electrode active material for non-aqueous electrolyte secondary batteries according to any one of claims 1 to 7; a negative electrode; and a non-aqueous electrolyte.

Citation Information

Patent Citations

  • U3Si2 pellets coated with a coating that is highly resistant to oxidation by water and steam

    JP2020511642A

  • Method for modifying lithium metal composite oxide powder

    JP2017197405A

  • Positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery

    JP2019169286A

  • Positive electrode active material for non-aqueous electrolyte secondary battery, positive electrode for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery

    WO2019193874A1