Composite metal cyanide complex catalyst and method for producing same, composite metal cyanide complex slurry catalyst and method for producing same, and polymer production method
A multimetal cyanide complex catalyst with controlled water content and X-ray diffraction peaks is developed to enhance catalytic activity and stability, effectively reducing high molecular weight impurities and maintaining performance in humid environments.
Patent Information
- Application Number
- PCT/JP2024/020110
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2024-05-31
- Publication Date
- 2024-12-05
AI Technical Summary
Multimetal cyanide complex catalysts used in epoxide polymerization tend to produce high molecular weight impurities, leading to reduced catalytic activity and stability, especially when exposed to humid environments.
A multimetal cyanide complex catalyst with controlled water content (8,000 to 140,000 ppm) and specific X-ray diffraction peaks at 2θ = 36° and 47°, and no peak at 2θ = 34°, is produced by coordinating an organic ligand with a reaction product of a metal halide salt and a transition metal cyanide compound, ensuring optimal crystal structure and water resistance.
The catalyst exhibits excellent catalytic activity, suppresses the production of high molecular weight impurities, and maintains activity even in humid conditions, with a catalytic activity life of 140 kg-PO/g-cat and ultra-high molecular weight component content below 1,000 ppm.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Composite metal cyanide complex catalyst and method for producing the same, composite metal cyanide complex slurry catalyst and method for producing the same, and method for producing polymer
[0001] The present invention relates to a composite metal cyanide complex catalyst, a method for producing the composite metal cyanide complex catalyst, a composite metal cyanide complex slurry catalyst, a method for producing the composite metal cyanide complex slurry catalyst, and a method for producing a polymer using the composite metal cyanide complex catalyst. This application claims priority based on Japanese Patent Application No. 2023-090792, filed in Japan on June 1, 2023, the contents of which are incorporated herein by reference.
[0002] Composite metal cyanide complex catalysts (hereinafter also referred to as DMC catalysts) are known as polymerization catalysts for epoxides. Composite metal cyanide complex catalysts have the advantages of being more active than base catalysts such as KOH and of being less likely to produce by-products with unsaturated bonds.
[0003] Various studies have been conducted on DMC catalysts. Patent Document 1 describes a method for increasing the polymerization rate of epoxides without increasing the amount of catalyst used by applying a strong shear force during production to make the DMC catalyst substantially amorphous.
[0004] Patent Document 2 describes an example in which a DMC catalyst obtained by producing a composite metal cyanide in the presence of an organic complexing agent (e.g., t-butyl alcohol) and a polyol having a number-average molecular weight of less than 500 exhibits high activity in epoxide polymerization, resulting in the production of a polyether polyol with an extremely low degree of unsaturation. In contrast, the comparative example in which an organic complexing agent was not used was inactive, and the comparative example in which the polyol was not used showed low activity. Furthermore, regarding the difference in crystal structure, the example shows signals in the X-ray diffraction pattern that are not seen in the two comparative examples.
[0005] In Patent Document 3, moisture is considered to be a catalyst poison that inhibits catalytic activity in DMC catalysts, and a method for producing a DMC catalyst using an organic solvent that is substantially free of water is proposed.
[0006] Japanese Patent Application Laid-Open No. 7-196778 International Publication No. 1997 / 040086 Japanese Patent Application Laid-Open No. 2003-103177
[0007] In the polymerization reaction of epoxides, the use of a DMC catalyst tends to narrow the molecular weight distribution (Mw / Mn) of the polymer, but also tends to produce ultra-high molecular weight components that become impurities. According to the findings of the present inventors, high catalytic activity tends to produce a large amount of ultra-high molecular weight components. The present invention aims to provide a composite metal cyanide complex catalyst that has excellent catalytic activity and can suppress the production of high molecular weight impurities.
[0008] The present inventors have conducted extensive research to solve the above problems and have discovered that by controlling the water content and crystal structure of the DMC catalyst, a DMC catalyst can be obtained that has a long catalyst life (high catalytic activity) and can suppress the production of high-molecular-weight impurities, thereby arriving at the present invention.
[0009] The present invention has the following aspects: [1] A double metal cyanide complex catalyst having a water content of 8,000 to 140,000 ppm as measured by the Karl Fischer method of JIS K0068:2001, and having diffraction peaks at 2θ=36° and 2θ=47°, but not at 2θ=34°, in an X-ray diffraction pattern. [2] A method for producing a double metal cyanide complex catalyst by coordinating an organic ligand to a reaction product obtained by reacting a metal halide salt with a transition metal cyanide compound, wherein after the organic ligand is coordinated, the double metal cyanide complex catalyst has a water content of 8,000 to 140,000 ppm as measured by the Karl Fischer method according to JIS K0068:2001, and the water content of the double metal cyanide complex catalyst is adjusted so that an X-ray diffraction pattern of the double metal cyanide complex catalyst exhibits diffraction peaks at 2θ = 36° and 2θ = 47°, but does not exhibit a diffraction peak at 2θ = 34°. [3] A method for producing the double metal cyanide complex catalyst according to [2], wherein the metal halide salt comprises one or more selected from zinc chloride and zinc bromide. [4] A method for producing the double metal cyanide complex catalyst according to [2] or [3], wherein the organic ligand comprises tert-butyl alcohol. [5] A double metal cyanide complex slurry catalyst comprising the double metal cyanide complex catalyst according to [1] above and a dispersion medium having a water content of 500 ppm or less as measured by the Karl Fischer method of JIS K0068: 2001. [6] The double metal cyanide complex slurry catalyst according to [5] above, in which the content of the double metal cyanide complex catalyst is 0.001 to 60 mass% relative to the total mass of the double metal cyanide complex slurry catalyst.[7] A method for producing a double metal cyanide complex slurry catalyst, comprising: a slurry preparation step of preparing a slurry containing a double metal cyanide complex catalyst and a dispersion medium; and a moisture adjustment step of adjusting the moisture content of the slurry so that the double metal cyanide complex catalyst has a moisture content of 8,000 to 140,000 ppm as measured by the Karl Fischer method of JIS K0068:2001 and the dispersion medium has a moisture content of 500 ppm or less as measured by the Karl Fischer method of JIS K0068:2001, and so that an X-ray diffraction pattern of the double metal cyanide complex catalyst has diffraction peaks at 2θ=36° and 2θ=47° and does not have a diffraction peak at 2θ=34°. [8] The method for producing a double metal cyanide complex slurry catalyst according to [7], wherein the slurry preparation step comprises the steps of reacting a metal halide salt with a transition metal cyanide compound in the presence of water, coordinating an organic ligand to the reaction product in the presence of water to obtain a mixture containing the double metal cyanide complex catalyst and water, removing impurities and water from the mixture, and adding a dispersion medium to prepare a slurry containing the double metal cyanide complex catalyst and the dispersion medium. [9] A method for producing a polymer, comprising polymerizing an epoxide in the presence of the double metal cyanide complex catalyst according to [1].
[0010] According to the present invention, a double metal cyanide complex catalyst can be obtained which has excellent catalytic activity and can suppress the formation of high-molecular-weight impurities.
[0011] In this specification and claims, a numerical range expressed as "to" means a numerical range in which the numerical values before and after "to" are the lower and upper limits. In this specification and claims, the unit of content, "ppm," is based on mass unless otherwise specified.
[0012] In this specification, the water content of the double metal cyanide complex catalyst is the water content measured using a Karl Fischer water content analyzer (for example, product name: CA-07 or CA-200 manufactured by Mitsubishi Analytic Co., Ltd.) based on the 6.4 coulometric titration method of the Karl Fischer titration method in the water content measurement method described in JIS K0068:2001. This water content is the total content (unit: ppm) of water of crystallization (bound water, coordinated water) contained in the crystals of the double metal cyanide complex catalyst and water not contained therein (free water) relative to the mass of the solid double metal cyanide complex catalyst.
[0013] In the case of a composite metal cyanide complex slurry catalyst (hereinafter also referred to as "slurry catalyst") containing a composite metal cyanide complex catalyst and a dispersion medium, the slurry catalyst is used as the measurement subject, and the value measured based on 6.4 coulometric titration of the Karl Fischer titration method in the moisture measurement method described in JIS K0068:2001 using a Karl Fischer moisture meter (for example, manufactured by Mitsubishi Analytic Co., Ltd.) is the moisture content in the slurry catalyst (hereinafter also referred to as "slurry moisture content"). The slurry moisture content is the total amount of moisture contained in the composite metal cyanide complex catalyst and the dispersion medium. The remaining water content, obtained by subtracting the moisture in the dispersion medium from the slurry moisture content, is converted into the water content relative to the solid content in the slurry, and this value is taken as the moisture content of the composite metal cyanide complex catalyst.
[0014] The solid content of the slurry can be determined by the following heat-drying method. Specifically, the slurry catalyst is washed with a solvent (e.g., hexane) that does not coordinate with the composite metal cyanide complex, and the dispersion medium is removed by centrifuging several times. The recovered composite metal cyanide complex is then heat-dried at 100°C for 12 hours, and the mass of the resulting dried product is taken as the mass of the solid content in the slurry catalyst to determine the solid content.
[0015] The solid content in the slurry catalyst may be determined during the process of producing the slurry catalyst. Specifically, in a method for producing the target slurry catalyst by washing a reaction product containing the synthesized composite metal cyanide complex and a by-product salt, adding a predetermined amount of dispersing medium to a filter cake obtained by solid-liquid separation, and removing volatile components such as water, a predetermined amount of the filter cake is removed for measurement, and the mass after drying at 100°C for 12 hours is taken as the mass of the solid content, and the solid content in the slurry catalyst can be determined from the amount of dispersing medium added to the filter cake and the mass of the solid content.
[0016] The X-ray diffraction pattern in this specification is a one-dimensional pattern obtained using CuKα radiation (wavelength: 1.5418 Å) as X-rays, with the horizontal axis representing the diffraction angle (2θ, unit: °) and the vertical axis representing the intensity (arbitrary units). In the X-ray diffraction pattern, a waveform that increases simply from a minimum value to a maximum value, and then decreases simply to reach the minimum value again, is referred to as a diffraction peak. The height from the line connecting the two minimum values to the maximum value is referred to as the peak intensity. In this specification, having a diffraction peak at 2θ = x° means that the maximum value of the diffraction peak exists within a 2θ range of (x - 0.5) degrees or more and less than (x + 0.5) degrees, and that the peak intensity is 1% or more relative to the peak intensity (reference peak intensity) of the diffraction peak at 2θ = 24 degrees. The diffraction peak at 2θ = 24 degrees refers to a diffraction peak whose maximum value exists within a 2θ range of (24 - 0.5) degrees or more and less than (24 + 0.5) degrees. In this specification, "having no diffraction peak at 2θ=x°" means that there is no maximum value within the range of 2θ of (x−0.5)° or more and less than (x+0.5)°, or even if there is a maximum value, the peak intensity is less than 1% of the reference peak intensity.
[0017] In this specification, X-ray diffraction pattern measurements are performed under the following conditions. The measurement sample is a solid. In the case of a slurry catalyst, the dried product obtained by the heat drying method is used as the measurement sample. X-ray: CuKα ray (λ=1.54180 Å) Tube voltage: 45 kV Tube current: 200 mA Light source: Monochromatic light source Measurement angle range: 2θ=10 to 80° Step width: (Δ2θ)=0.010° step scan Scan rate: 20° / min Each peak can be analyzed by analyzing the obtained X-ray diffraction pattern using analysis software (for example, analysis software included with an apparatus such as SmartLab Studio II).
[0018] <Duometal cyanide complex catalyst> The duometal cyanide complex catalyst of this embodiment (hereinafter also referred to as DMC catalyst (A)) is a crystalline solid and contains a reaction product of a metal halide salt and a transition metal cyanide compound, an organic ligand, and water of crystallization (coordinated water, etc.) contained within the crystal. In addition, it may contain impurities unavoidable in the production that are contained in trace amounts in the metal salt, metal compound, etc., and moisture other than water of crystallization. The metal halide salt, transition metal cyanide compound, and organic ligand can be those known in the production of DMC catalysts.
[0019] The DMC catalyst (A) is believed to be represented by the following formula (1): M 1 a [M 2 (CN) b ] c ・d(M 1 e X f )・g(Ligand)・h(H 2 O) ... (1) In formula (1), M 1 e X f is a metal halide salt, M 1 is a metal atom that serves as a cation, X is a halogen atom that serves as a counter anion, and M 2 is a transition metal atom contained in the transition metal cyanide compound and serves as an active site, and Ligand is an organic ligand. a, b, c, d, e, f, g, and h are integers, and a, b, c, e, and f are numbers that result in electrical neutrality.
[0020] Said M 1 Examples of the M include Zn(II), Fe(II), Fe(III), Co(II), Ni(II), Al(III), Sr(II), Mn(II), Cr(III), Cu(II), Sn(II), Pb(II), Mo(IV), Mo(VI), W(IV) and W(VI). 2 Examples of the X include Co(III), Fe(II), Fe(III), Co(II), Co(III), Cr(II), Cr(III), Mn(II), Mn(III), V(IV), and V(V). Examples of the X include Cl, Br, and I. 1 e X f The metal halide salt represented by the formula (I) is preferably at least one selected from zinc chloride, zinc bromide, and zinc iodide. 2 In view of the interatomic distance between X and X, it is more preferable that the compound contains one or more selected from zinc chloride and zinc bromide. Examples of the ligand (organic ligand) include alcohols, ethers, esters, aldehydes, ketones, amides, nitriles and sulfides, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, and polyoxyalkylene poly(or mono)ols. One type of organic ligand may be used, or two or more types may be used. Examples of the alcohol include tert-butyl alcohol, n-butyl alcohol, sec-butyl alcohol, iso-butyl alcohol, tert-pentyl alcohol, iso-pentyl alcohol, and ethylene glycol mono-tert-butyl ether. Examples of the polyoxyalkylene poly(or mono)ol include polypropylene diol. A preferred organic ligand is tert-butyl alcohol.
[0021] Preferred examples of the DMC catalyst (A) include zinc hexacyanocobaltate (Zn) containing an organic ligand, water, zinc chloride, or zinc bromide. 3 [Co(CN) 6 ] 2 ) Its chemical formula is Zn 3 [Co(CN) 6 ] 2 d(ZnCl2 )・g(Ligand)・h(H 2 O) or Zn 3 [Co(CN) 6 ] 2 d(ZnBr 2 )・g(Ligand)・h(H 2 O) is considered.
[0022] The DMC catalyst (A) has a water content of 8,000 to 140,000 ppm as measured by the Karl Fischer method, and in its X-ray diffraction pattern, it has diffraction peaks at 2θ = 36° and 2θ = 47°, but no diffraction peak at 2θ = 34°. DMC catalyst (A) with such a water content and crystal structure can achieve both good catalytic activity and suppression of high-molecular-weight impurities. Furthermore, it has excellent water resistance, meaning that its catalytic activity is unlikely to decrease even when stored in a humid environment. If the water content is too high or too low, the catalytic activity is likely to decrease. If it is too high, it is thought that hydrolysis of active sites by water other than water of crystallization (water not encapsulated in the crystals) is likely to occur. If it is too low, the crystal structure changes due to the reduction in water of crystallization, and the structure that contributes to achieving both good catalytic activity and suppression of high-molecular-weight impurities is likely to be lost. The water content is preferably 9,000 to 120,000 ppm, and more preferably 10,000 to 100,000 ppm.
[0023] The DMC catalyst (A) has diffraction peaks at 2θ = 14 ° and 2θ = 16 ° in the X-ray diffraction pattern, and from the viewpoint of obtaining good catalytic activity, it is preferable that P16 / P14, which represents the ratio of the peak intensity (P16) at 2θ = 16 ° to the peak intensity (P14) at 2θ = 14 °, is smaller than 3. P16 / P14 is thought to vary depending on the number of water molecules encapsulated in the DMC catalyst crystals, and the value of P16 / P14 tends to increase as the number of encapsulated water molecules decreases.
[0024] The DMC catalyst (A) has a transition metal atom (M) that serves as an active site, which is obtained by an EXAFS (Extended X-ray Absorption Fine Structure) analysis of a spectrum measured by an XAFS (X-ray Absorption Fine Structure) method.2 It is preferable that the interatomic distance between the halogen atom (X) derived from the metal salt is 2.20 to 2.40 angstroms (Å). When a halogen atom (X) having an interatomic distance of 2.20 to 2.40 Å is used, good catalytic activity is likely to be obtained. The interatomic distance in the DMC catalyst determined by EXAFS analysis is also described in the literature ("X-RAY SPECTROMETRY", 2015, volume 44, issue 5, pp. 330-338, titled "Structural properties and chemical bonds in double metal cyanide catalysts").
[0025] <Double Metal Cyanide Complex Slurry Catalyst> The slurry catalyst of this embodiment contains a DMC catalyst (A) and a dispersion medium. The content of the DMC catalyst (A) relative to the total mass of the slurry catalyst is, for example, preferably 0.001 to 60 mass%, more preferably 0.003 to 50 mass%, and even more preferably 0.006 to 30 mass%. The slurry catalyst is preferably a slurry obtained by dispersing the DMC catalyst (A) in a dispersion medium, i.e., a slurry containing the DMC catalyst (A) and the dispersion medium, and which may also contain impurities and moisture unavoidable during production.
[0026] The dispersion medium of the slurry catalyst preferably does not substantially contain water. Specifically, the water content of the dispersion medium is preferably 500 ppm or less, more preferably 200 ppm or less, and may be an undetectable amount. The water content of the dispersion medium is the water content (unit: mass ppm) measured by the Karl Fischer measurement method, similar to the water content of the DMC catalyst (A).
[0027] As the dispersion medium for the slurry catalyst, organic solvents known in the art for slurry catalysts can be used. For example, the low-volatility hydroxy compounds described in Japanese Patent No. 3194255 can be used. The hydroxy compound is a hydroxyl group-containing compound having 1 to 8 hydroxyl groups and a molecular weight of 100 to 8000, with compounds having alcoholic hydroxyl groups such as polyether polyol being preferred. When the DMC catalyst (A) is used as a catalyst for producing a polyether polyol by ring-opening polymerization of an epoxide, a polyether polyol is preferred as the dispersion medium for the slurry catalyst because it does not become an impurity in the product (polyether polyol). Furthermore, the initiator (polyether polyol) used in the ring-opening polymerization of the epoxide may also be used as part of the dispersion medium. The number-average molecular weight of the polyether polyol used as the dispersion medium is preferably 100 to 8000, more preferably 600 to 3000. If the number-average molecular weight of the polyether polyol is equal to or greater than the lower limit of the above range, it will not poison the catalyst, and if it is equal to or less than the upper limit, the slurry catalyst will be easier to handle. The hydroxyl value of the polyether polyol used as the initiator is, for example, preferably from 3 to 842 mgKOH / g, and more preferably from 7 to 561 mgKOH / g.
[0028] In particular, when the dispersion medium is the product (polyether polyol), the content of the DMC catalyst (A) relative to the total mass of the slurry catalyst is preferably 1 to 60 mass%, more preferably 3 to 40 mass%, and even more preferably 5 to 30 mass%. In particular, when the dispersion medium contains the initiator (polyether polyol), the content of the DMC catalyst (A) relative to the total mass of the slurry catalyst is preferably 0.003 to 0.02 mass%, more preferably 0.004 to 0.015 mass%, and even more preferably 0.006 to 0.01 mass%.
[0029] <Method for producing a composite metal cyanide complex catalyst> In the method for producing a composite metal cyanide complex catalyst of this embodiment, an organic ligand is coordinated to the reaction product obtained by reacting a metal halide salt with a transition metal cyanide compound to synthesize a composite metal cyanide complex catalyst, and then the water content of the composite metal cyanide complex catalyst is adjusted so that the composite metal cyanide complex catalyst has a specific water content and satisfies a specific X-ray diffraction pattern. The method for synthesizing the composite metal cyanide complex catalyst is not particularly limited, and known methods can be used.
[0030] Preferably, first, a metal halide salt and a transition metal cyanide compound are reacted in the presence of water to obtain a reaction product, and an organic ligand is then coordinated in the presence of water to obtain a mixture containing DMC catalyst (A) and water. Impurities and water are removed from the resulting mixture, and the water content of the resulting solid is reduced to a predetermined range to obtain DMC catalyst (A). As shown in the examples described below, DMC catalysts with a water content exceeding 140,000 ppm tend to exhibit a diffraction peak at 2θ = 34°, making it impossible to achieve both good catalytic activity and suppression of high-molecular-weight impurities. Furthermore, even if the water content of a DMC catalyst has been reduced to a range of 8,000 to 140,000 ppm, when the catalyst comes into contact with water not containing an organic ligand, a diffraction peak appears at 2θ = 34°, and the catalytic activity is significantly reduced or no catalytic activity is exhibited. Furthermore, if the water content is reduced too much, the peak at 2θ = 47° disappears, and the catalyst no longer exhibits catalytic activity. Therefore, in the step of removing water from the mixed solution, the water content of the DMC catalyst is gradually reduced to a predetermined range while avoiding contact with water that does not contain organic ligands, thereby producing a DMC catalyst (A) that has a predetermined crystal structure and can achieve both good catalytic activity and suppression of high-molecular-weight impurities.
[0031] The method for obtaining the mixed solution and the method for removing impurities and water from the mixed solution can be selected from known methods that do not allow the DMC catalyst to come into contact with water containing no organic ligands. The method for removing water from the mixed solution can be, for example, a drying method for obtaining a solid DMC catalyst. However, because conventional drying methods cannot control the water content in the DMC catalyst within the range of 8,000 to 140,000 ppm, a water content adjustment step is provided to control the water content to a level that allows the DMC catalyst to maintain an optimal structure. In the water content adjustment step, it is preferable to strictly control the DMC catalyst so that it does not come into contact with water outside the DMC catalyst. The water content adjustment step may be performed consecutively with the immediately preceding step. When producing a solid DMC catalyst, the water content adjustment step involves, for example, heat drying at a temperature of 160°C or lower, preferably 140°C or lower. The heating time is determined so that the water content in the dried solid is within the range of 8,000 to 140,000 ppm. If necessary, the heating time is determined by monitoring the change in the water content in the solid over time during the heat drying step. Drying conditions of 80 to 140°C for 5 to 24 hours are more preferred. If the drying temperature exceeds the upper limit of the above range, the crystalline structure of the DMC catalyst may not be maintained. In other words, if the drying temperature is equal to or lower than the upper limit of the above range, the crystalline structure of the DMC catalyst is more easily maintained. Heat drying may be performed in an atmospheric atmosphere or a reduced pressure atmosphere, but is preferably performed in an atmospheric atmosphere. In order to avoid contact with moisture as much as possible after heat drying, it is preferable to provide a step of returning the temperature to room temperature in a dry gas (dry nitrogen, etc.) after heat drying. Furthermore, when heat drying is performed in a reduced pressure atmosphere, a step of introducing a dry gas (dry nitrogen, etc.) that does not react with the DMC catalyst to return to normal pressure is preferred in order to avoid contact with moisture as much as possible. Whether heat drying is performed in an atmospheric atmosphere or a reduced pressure atmosphere, it is preferable to avoid contact of the DMC catalyst with moisture as much as possible during the process from stopping heating to lowering the temperature to room temperature. In particular, it is preferable to avoid contact of the DMC catalyst with moisture as much as possible after the temperature has reached near room temperature during the temperature lowering process. Dry gas means a gas in which the water vapor content relative to the total volume of the gas at 25°C is 12 ppm by volume or less.Returning to room temperature and pressure using dry gas is advantageous in that the heat-drying time can be shortened, allowing the moisture content adjustment step to be carried out efficiently. On the other hand, by adjusting the heat-drying temperature and time, it is also possible to control the moisture content in the dried solid to 8,000 to 140,000 ppm. Since there is an upper limit to the heat-drying temperature as mentioned above, the moisture content in the dried solid is essentially controlled by the drying time. The longer the drying time, the easier it is to control the moisture content in the dried solid to 140,000 ppm or less. Furthermore, in this case, even if the temperature and pressure are returned to room temperature and normal pressure using air instead of dry gas, the moisture content in the dried solid may still be 8,000 to 140,000 ppm. However, the longer the drying time, the lower the efficiency of the moisture content adjustment step.
[0032] A preferred embodiment of the method for producing the double metal cyanide complex catalyst of this embodiment is, for example, the following method. First, an aqueous solution of a metal halide salt is reacted with an aqueous solution of a cyanide transition metal compound to produce a reaction product. An aqueous solution of an organic ligand is added to the reaction product and stirred to coordinate the organic ligand, thereby obtaining a mixed solution containing the double metal cyanide complex catalyst and water. The resulting mixed solution is subjected to solid-liquid separation to obtain a solid. Solid-liquid separation can be performed by a method known in the art, such as filtration or centrifugation. The resulting solid is washed with an aqueous solution containing the organic ligand, and this solid-liquid separation operation is performed one or more times, preferably two or more times. The resulting solid is dried so that the moisture content falls within the specified range, and is pulverized as necessary.
[0033] <Method for producing a composite metal cyanide complex slurry catalyst> The method for producing a slurry catalyst of this embodiment includes a slurry preparation step of preparing a slurry containing a composite metal cyanide complex catalyst and a dispersion medium, and a moisture adjustment step of adjusting the moisture content of the slurry so that the moisture content of the composite metal cyanide complex catalyst in the slurry catalyst falls within a specific range, the moisture content of the dispersion medium falls within a specific range, and the composite metal cyanide complex catalyst satisfies a specific X-ray diffraction pattern. The preferred ranges for the moisture content of the composite metal cyanide complex catalyst in the slurry catalyst and the preferred ranges for the moisture content of the dispersion medium are the same as those described above. Furthermore, the preferred ranges for the X-ray diffraction pattern of the composite metal cyanide complex catalyst are also the same as those described above.
[0034] The slurry preparation process is not particularly limited, and known methods can be used. Preferably, a mixture containing a DMC catalyst and water is first prepared by reacting a metal halide salt with a transition metal cyanide compound in the presence of water, followed by coordinating an organic ligand to the resulting reaction product in the presence of water. A method can be used in which impurities and water are removed from the resulting mixture, and a dispersion medium is added to prepare a slurry containing the DMC catalyst and the dispersion medium. The method for obtaining the mixture and the method for removing impurities and water from the mixture can be selected from known methods that do not allow the DMC catalyst to come into contact with water containing no organic ligands. A preferred method for removing water from the mixture is to gradually reduce the water content of the slurry to a predetermined range while avoiding contact with water containing no organic ligands. For example, a solvent substitution method can be used to obtain a slurry catalyst by replacing the water in the mixture with a dispersion medium. However, because conventional solvent substitution methods cannot control the water content in the DMC catalyst within the range of 8,000 to 140,000 ppm, a water content adjustment step is provided to control the water content to a level that allows the DMC catalyst to maintain an optimal structure. In the water content adjusting step, it is preferable to strictly control the slurry so that it does not come into contact with water other than the slurry. The water content adjusting step may be carried out consecutively with the immediately preceding step.
[0035] The moisture content adjustment step when producing a slurry catalyst is preferably performed by, for example, drying the slurry catalyst under reduced pressure at 0 to 160°C for 1 to 24 hours until the moisture content of the DMC catalyst in the slurry catalyst reaches 8,000 to 140,000 ppm, followed by introducing a dry gas (e.g., dry nitrogen) that does not react with the DMC catalyst and returning the pressure to normal to avoid contact with moisture as much as possible. The reduced-pressure drying conditions are more preferably 25 to 140°C for 2 to 10 hours. If the drying temperature exceeds the upper limit of the above range, the crystalline structure of the DMC catalyst may not be maintained. In other words, if the drying temperature is below the upper limit of the above range, the crystalline structure of the DMC catalyst is more easily maintained. Returning to normal pressure with a dry gas can shorten the heat-drying time, which is advantageous in that the moisture content adjustment step can be carried out efficiently. On the other hand, by adjusting the temperature and time of heat-drying, it is also possible to control the moisture content of the DMC catalyst in the dried slurry catalyst to 8,000 to 140,000 ppm. As mentioned above, there is an upper limit to the heat drying temperature, so the moisture content of the DMC catalyst in the slurry catalyst after drying is essentially controlled by the drying time. The longer the drying time, the easier it is to control the moisture content of the DMC catalyst in the slurry catalyst after drying to 140,000 ppm or less. In this case, even if the temperature and pressure are returned to normal in the atmosphere rather than in a dry gas, the moisture content of the DMC catalyst in the slurry catalyst after drying may be 8,000 to 140,000 ppm. However, since the drying time is long, the efficiency of the moisture content adjustment step decreases. In addition, it is preferable to use a dispersion medium that has been dehydrated in advance so that the moisture content of the dispersion medium in the slurry catalyst after the moisture content adjustment step is 500 ppm or less.
[0036] Preferred embodiments of the method for producing a composite metal cyanide complex catalyst according to this embodiment include, for example, the following. First, an aqueous solution of a metal halide salt is reacted with an aqueous solution of a cyanide transition metal compound to produce a reaction product. An aqueous solution of an organic ligand is added to the reaction product and stirred to coordinate the organic ligand, thereby obtaining a mixed solution containing the composite metal cyanide complex catalyst and water. The resulting mixed solution is subjected to solid-liquid separation to obtain a solid. The resulting solid is washed with an aqueous solution containing the organic ligand, and this solid-liquid separation operation is performed at least once, preferably at least twice. A dispersion medium is added to the resulting solid and mixed, and then the uncoordinated organic ligand and water are removed by volatilization. In this way, a slurry in which the DMC catalyst is dispersed in the dispersion medium is obtained. The resulting slurry is subjected to the water content adjustment step to produce a slurry catalyst containing the desired DMC catalyst.
[0037] <Method for Producing Polymer> The DMC catalyst of this embodiment is suitable as a catalyst for producing polymers such as polyether polyols and polyester polyols by polymerizing cyclic ethers such as epoxides. Known methods can be applied to produce polymers using the DMC catalyst. Examples of epoxides include propylene oxide (hereinafter also referred to as "PO") and combinations of PO and ethylene oxide. Polyols such as polyether polyols and polyester polyols are used as raw materials for, for example, various polyurethane coatings, elastomers, sealants, foams, and adhesives.
[0038] According to this embodiment, a DMC catalyst can be obtained that can achieve both good catalytic activity and suppression of high-molecular-weight impurities. For example, a DMC catalyst can be obtained that has catalytic activity such that the catalytic activity life [kg-PO / g-cat] measured by the method described in the catalyst activity life evaluation section of the Examples is 140 kg / g or more, and has an ultra-high molecular weight component content of 1,000 ppm or less as determined by the [Method for measuring the content of ultra-high molecular weight components] of the Examples. The content of the ultra-high molecular weight component is more preferably 950 ppm or less, and even more preferably 900 ppm or less. By reducing the content of the ultra-high molecular weight component, the physical properties (e.g., stability, strength, etc.) of polyols produced using the DMC catalyst and articles produced using the polyol can be improved.
[0039] Furthermore, conventional DMC catalysts have poor water resistance and are prone to a decrease in catalytic activity when stored in a humid atmosphere, but the present embodiment provides a DMC catalyst with excellent water resistance. For example, a DMC catalyst can be obtained in which the rate of decrease in catalytic activity life measured by the method described in the water resistance evaluation section of the Examples is less than 25%.
[0040] <Method for Evaluating DMC Catalysts> The water content and X-ray diffraction pattern of a DMC catalyst are measured, and if the water content is 8,000 to 140,000, the catalyst has diffraction peaks at 2θ = 36 ° and 2θ = 47 °, and no diffraction peak at 2θ = 34 °, the catalyst can be evaluated as having good catalytic activity and producing little high-molecular-weight impurities when used as an epoxide polymerization catalyst. Furthermore, the water content and X-ray diffraction pattern of a DMC catalyst are measured, and if the water content is 8,000 to 140,000, the catalyst has diffraction peaks at 2θ = 36 ° and 2θ = 47 °, and no diffraction peak at 2θ = 34 °, the catalyst can be evaluated as having good water resistance.
[0041] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.
[0042] <Evaluation Method> [X-ray Diffraction Measurement] X-ray diffraction (XRD) measurements were performed using an X-ray diffractometer (manufactured by Rigaku Corporation, device name: SmartLab). X-rays were CuKα rays (λ = 1.54180 Å), the tube voltage and tube current were 45 kV and 200 mA, respectively, and a monochromatic light source was used using a Johansson monochromator with a focused optical system. A high-speed detector (manufactured by Rigaku Corporation, device name: D / teX) was used as the detector, with a measurement angle range of 2θ = 10 to 80°, a step scan with a step width (Δ2θ) = 0.010°, and a scan speed of 20° / min. The obtained X-ray diffraction pattern was analyzed using analysis software, and the presence or absence of diffraction peaks at 2θ = 34°, 36°, and 47° was recorded. In addition, the ratio (P16 / P14) of the peak intensity (P16) at 2θ=16° to the peak intensity (P14) at 2θ=14° was calculated. When P16 / P14 was less than 3, it was judged as "good", and when it was 3 or more, it was judged as "poor".
[0043] [Moisture content measurement] Using a Karl Fischer moisture content meter manufactured by Mitsubishi Analytic Co., Ltd., the moisture content of each sample was measured based on the Karl Fischer titration method 6.4 coulometric titration method in the moisture content measurement method described in JIS K0068:2001. The moisture content in the slurry was measured using the slurry to be measured as a sample. The moisture content in the solid (powder) was measured using the powder to be measured as a sample. The moisture content of the dispersion medium was measured using a sample obtained by increasing or decreasing the moisture content of the dispersion medium alone under the same conditions as the operation of increasing or decreasing the moisture content after adding the dispersion medium during the production process of the slurry catalyst. The moisture content (unit: ppm) in the DMC catalyst (solid content) was calculated using the following formulas (i) and (ii): Amount of water in DMC catalyst=(Sw−Pw×B / 100) / (A / 100) (i) B=100−A (ii) Sw: Amount of water in the slurry (unit: ppm) Pw: Amount of water in the dispersion medium (unit: ppm) A: Solid content of the slurry (unit: mass %) B: Proportion of the dispersion medium in the slurry (unit: mass %)
[0044] [XAFS Measurement] The EXAFS spectrum obtained by Fourier transform of the spectrum measured by the XAFS method is corrected for phase shift, and the transition metal atoms (M 2 The interatomic distance (coordination distance) between the halogen atom (X) and the halogen atom (X) derived from the metal salt was calculated. When the interatomic distance was within the range of 2.20 to 2.40 Å, it was judged as "Good", and when it was outside the range, it was judged as "Poor".
[0045] [Evaluation of catalyst activity life] A 200 mL autoclave was charged with 25 g of polyoxypropylene triol having an Mn of 1,500 and a hydroxyl value of 168 mg KOH / g as an initiator, and the DMC catalyst (slurry or solid) obtained in each example, and PO was added sequentially at a temperature of 120 ° C. The amount of DMC catalyst charged was set so that the metal concentration of the DMC catalyst per 1,000 g of initiator would be the catalyst concentration (unit: ppm) listed in Table 3. The catalyst was determined to have been deactivated when no pressure drop was observed after PO was added. Based on the amount of PO (substrate) charged and the amount of DMC catalyst charged until deactivation, the catalyst activity life [kg-PO / g-cat] (the ratio of the mass (kg) of polymerized polypropylene oxide to 1 g of catalyst) (unit: kg / g) was calculated to evaluate "how well the catalyst functions in terms of mass ratio to the substrate." If no pressure drop was observed after the addition of PO, it was judged to be "inactive."
[0046] [Evaluation of Water Resistance] The DMC catalyst (slurry or solid) obtained in each example was stored for one day in a high humidity atmosphere at a temperature of 40°C and a relative humidity of 80%. Before the start of storage and immediately after the end of storage, the catalyst activity life [kg-PO / g-cat] was measured using the method described above. The rate of decrease (unit: %) of the catalyst activity life (A2) immediately after the end of storage relative to the catalyst activity life (A1) before the start of storage was calculated using the following formula. Based on the obtained rate of decrease, water resistance was evaluated according to the following criteria: Rate of decrease of catalyst activity life = (A1 - A2) / A1 x 100 (Evaluation criteria) ○: Rate of decrease is less than 25%. ×: Rate of decrease is 25% or more.
[0047] [Number average molecular weight (Mn) measurement] The molecular weight of the polyether polyol was analyzed using a GPC system (Tosoh Corporation product name HLC-8320) and an RI detector. Two TSK-GEL Super HZ4000 (4.6 mm x 150 mm) columns and two Super HZ2500 (4.6 mm x 150 mm) columns were connected in series in this order. Tetrahydrofuran (THF) was used as the eluent at a flow rate of 0.35 ml / min, the column temperature was set to 40 ° C., and the number average molecular weight Mn was calculated using a calibration curve created using a polystyrene standard sample (Agilent Technologies product name Easical PS-2, molecular weight range 580 to 400,000).
[0048] [Method for measuring the content of ultra-high molecular weight components (CAD-HPLC method)] Polyether polyols were synthesized using the DMC catalysts obtained in each example according to the method of Production Example 1 below. When the number average molecular weight of the polyether polyol to be measured is W, components with molecular weights ranging from 12 times (12W) to 46 times (46W) that of the polyether polyol were defined as ultra-high molecular weight components. The content of ultra-high molecular weight components relative to the total mass of the polyether polyol was determined using the measurement method described in JP 2019-137810 A.
[0049] Specifically, the content of ultrahigh molecular weight components was measured under the following conditions. Apparatus and detector: High-performance liquid chromatography apparatus (ThemoFisher SCIENTIFIC product name U3000HPLC system, degasser: SRD-3600, pump: DGP3600SD, autosampler: WPS-3000TSL, column compartment: TCC-3000SD, UV-Vis detector: VWD-3400RS, charged aerosol detector: Corona Veo) Eluent: HPLC-grade THF Eluent flow rate: 0.2 mL / min Sample injection amount: 20 μL Column: One upstream column and one downstream column described below were connected in series in this order. The exclusion limit molecular weight of each column is the exclusion limit molecular weight when the molecular weight of polystyrene is measured using HPLC-grade THF as the eluent. Upstream column: Showa Denko K.K. product name Shodex KF-404HQ (a column for organic solvent liquid chromatography whose packing material is a styrene divinylbenzene copolymer with an average particle size of 3 μm, an inner diameter of 4.6 mm, a length of 250 mm, a theoretical plate number of 25,000 or more TP / column, and an exclusion limit molecular weight of 1,000,000). Downstream column: Showa Denko K.K. product name Shodex KF-403HQ (a column for organic solvent liquid chromatography whose packing material is a styrene divinylbenzene copolymer with an average particle size of 3 μm, an inner diameter of 4.6 mm, a length of 250 mm, a theoretical plate number of 25,000 or more TP / column, and an exclusion limit molecular weight of 70,000). (1) The polyether polyol to be tested was dissolved in HPLC-grade THF to a concentration of 0.6% by mass, and then filtered through a syringe filter with a pore size of 0.45 μm to prepare a sample. The sample was analyzed under the above-mentioned HPLC conditions to obtain a chromatogram with retention time on the X-axis and signal intensity on the Y-axis. (2) A calibration curve showing the relationship between molecular weight and retention time was created using a polystyrene standard sample (Agilent Technologies, product name Easical PS-2, molecular weight range 580 to 400,000). (3) Using the calibration curve created in (2), the retention time X1 corresponding to the above 12 W and the retention time X2 corresponding to the above 46 W were determined.(4) The area enclosed by the chromatogram, the baseline, the line X = X1, and the line X = X2 was electronically integrated. (5) A standard solution prepared by dissolving a polystyrene standard sample having a molecular weight of 92,600 (Gas Chromatography Co., Ltd. product name PSS-05 No. 500-16) in HPLC-grade THF to concentrations of 1, 6, 20, and 60 ppm by mass was used as a sample, and analyzed under the above HPLC conditions to obtain a chromatogram. The area enclosed by the obtained chromatogram and the baseline was taken as the area. The area at each concentration was calculated, and a calibration curve with an intercept of zero was created, showing the relationship between the concentration of polystyrene having a molecular weight of 92,600 and the area. (6) Using the calibration curve prepared in (5), the area determined in (4) was converted to the concentration of polystyrene having a molecular weight of 92,600, which was taken as the concentration of the ultra-high molecular weight component in the sample prepared in (1). (7) From the concentration value of the ultra-high molecular weight component obtained in (6), the mass of the ultra-high molecular weight component in the sample prepared in (1) was calculated, and further, the content of the ultra-high molecular weight component relative to the mass of the test substance (polyether polyol) used in preparing the sample was calculated.
[0050] [Production Example 1: Production of Polyether Polyol] PO was subjected to ring-opening addition polymerization to glycerin using a KOH catalyst, and further purified using Kyoward 600S (a synthetic adsorbent, a product name of Kyowa Chemical Industry Co., Ltd.) to produce a polyoxypropylene triol (initiator 1) having an Mn of 1,500 and a hydroxyl value of 112 mgKOH / g. 1,000 g of initiator 1 and the DMC catalyst obtained in each example were added to a reaction vessel to form a reaction solution. The amount of DMC catalyst charged was set so that the metal concentration of the DMC catalyst per 1,000 g of initiator was the catalyst concentration (unit: ppm) listed in Table 3. Next, after replacing the atmosphere in the reaction vessel with nitrogen, the reaction solution was heated with stirring. When the temperature reached 135°C, heating was stopped, and 120 g of PO was supplied to the reaction vessel with continued stirring to cause a reaction. When PO was supplied into the reaction vessel, the internal pressure of the reaction vessel rose once, then gradually decreased, and it was confirmed that it had reached the same internal pressure as the reaction vessel immediately before PO was supplied. During this period, when the internal pressure began to decrease, the temperature of the reaction solution rose once, then gradually decreased. After the temperature increase of the reaction solution stopped, it was cooled to 135°C. Next, while stirring the reaction solution, the temperature was maintained at 135°C, and 4,728 g of PO was supplied into the reaction vessel. The internal pressure stopped changing, and it was confirmed that the reaction had ended. In this way, a polyether polyol was obtained.
[0051] Examples 1 to 11 and 16 Slurry catalysts were produced. Examples 2 to 4 and 8 are working examples, and Examples 1, 5 to 7, 9 to 11 and 16 are comparative examples.
[0052] Example 1 An alkylene oxide ring-opening polymer was produced in advance by ring-opening addition polymerization of PO to propylene glycol in the presence of a KOH catalyst, followed by dealkalization purification to prepare a polyoxypropylene diol having an average of 2 hydroxyl groups per molecule and an Mn of 2,000 (hereinafter referred to as "Polyol P1").
[0053] In this example, a zinc hexacyanocobaltate complex (hereinafter also referred to as "TBA") coordinated with tert-butyl alcohol (hereinafter also referred to as "TBA") (hereinafter also referred to as "TBA-DMC catalyst") was produced by the following method. First, a zinc chloride aqueous solution consisting of 10.2 g of zinc chloride and 10 g of water was placed in a 500 mL flask. While the zinc chloride aqueous solution was stirred at 300 revolutions per minute, a potassium hexacyanocobaltate aqueous solution consisting of 4.2 g of potassium hexacyanocobaltate and 75 g of water was added dropwise to the zinc chloride aqueous solution over 30 minutes. During this time, the liquid in the flask was maintained at 40°C. After the dropwise addition of the potassium hexacyanocobaltate aqueous solution was completed, the liquid in the flask was stirred for an additional 30 minutes, and then a mixture of 80 g of TBA, 80 g of water, and 0.6 g of polyol P1 was added, followed by stirring at 40°C for 30 minutes and then at 60°C for an additional 60 minutes, yielding a mixture containing the TBA-DMC catalyst and water. This mixture also contained a salt (i.e., KCl) produced by the reaction.
[0054] The resulting mixture was filtered under pressure (0.25 MPa) using a 125 mm diameter circular filter plate and quantitative filter paper for fine particles (product name: No. 5C, manufactured by ADVANTEC Corporation), and a solid containing the TBA-DMC catalyst (hereinafter referred to as the "filter cake") was separated. The filter cake was then washed with a mixture of TBA and water to remove salt (i.e., KCl). Specifically, the filter cake was transferred to a flask, and a mixture of 36 g of TBA and 84 g of water was added. The mixture was stirred for 30 minutes, and then filtered under pressure under the same conditions as above. The resulting filter cake was transferred to a flask, and a mixture of 108 g of TBA and 12 g of water was added. The mixture was stirred for 30 minutes, yielding a dispersion (1) in which the TBA-DMC catalyst was dispersed in a mixture of TBA and water.
[0055] The dispersion medium of the obtained dispersion (1) was replaced with polyol P1 to produce a slurry catalyst (catalyst 1). Specifically, dispersion (1) was filtered under pressure under the same conditions as above. Polyol P1 was added to the obtained filter cake so that the solid content was 5% by mass, and then volatile components were distilled off under reduced pressure at 80°C for 3 hours. Air (air) was introduced and the pressure was returned to normal, yielding a slurry catalyst (catalyst 1) in which the TBA-DMC catalyst was dispersed in polyol P1. It is believed that a portion of the polyol P1 contained in the slurry is coordinated to the TBA-DMC catalyst. The water content in the slurry catalyst (catalyst 1) was measured using the above method. In addition, the same amount of polyol P1 as the polyol P1 added as the dispersion medium was prepared, and the volatile components were distilled off under reduced pressure at 80°C for 3 hours. This was used as a sample to measure the water content, which was then used as the water content of the dispersion medium. The water content in the DMC catalyst was determined using the above method. The results are shown in Table 1 (hereinafter, the same applies unless otherwise specified). The uncoordinated polyol P1 was removed from the resulting slurry catalyst using hexane, and the resulting solid sample was subjected to XRD and XAFS measurements using the methods described above. The measurement results are shown in Table 1 (hereinafter, the same applies unless otherwise specified).
[0056] The catalyst slurry was evaluated for catalytic activity life and water resistance by the methods described above. Furthermore, a polyether polyol was produced using the catalyst slurry by the method described in Production Example 1, and the content of the ultra-high molecular weight component was measured. The results are shown in Table 3 (the same applies hereinafter unless otherwise specified).
[0057] In this example, a water content adjustment step was performed to adjust the water content to a lower level than in Example 1. That is, a slurry catalyst (catalyst 1) was prepared in the same manner as in Example 1, and then, as the water content adjustment step, the catalyst was dried under reduced pressure at 115°C for 6 hours to distill off volatile components, and then dry nitrogen was introduced to return the pressure to normal pressure, thereby obtaining a slurry catalyst (catalyst 2). The obtained slurry catalyst was measured in the same manner as in Example 1.
[0058] [Example 3] In this example, a water content adjustment step was provided, and the water content was adjusted to be lower than in Example 1. Specifically, the drying time in the water content adjustment step in Example 2 was changed from 6 hours to 4 hours. A slurry catalyst (Catalyst 3) was obtained in the same manner as in Example 2 except for this. The obtained slurry catalyst was measured in the same manner as in Example 1.
[0059] [Example 4] In this example, a dispersion medium was further added to a slurry catalyst (catalyst 2) produced in the same manner as in Example 2 to produce the target slurry catalyst. That is, polyoxypropylene triol, which is initiator 1 in Production Example 1, was added to the slurry catalyst (catalyst 2) produced in the same manner as in Example 2 so that the solid content was 0.0292 mass%, and then, as a water content adjustment step, the mixture was dried under reduced pressure at 130°C for 3 hours to distill off volatile components, and then dry nitrogen was introduced to return the pressure to normal pressure, thereby producing a slurry catalyst (catalyst 4). The obtained slurry catalyst was measured in the same manner as in Example 1.
[0060] [Example 5] In this example, the water content was adjusted to be even lower than in Example 2. That is, in the same manner as in Example 1, a dispersion (1) in which a TBA-DMC catalyst was dispersed in a mixed solution of TBA and water was prepared and filtered. In Example 1, polyol P1 was added to the obtained filter cake, but in this example, the filter cake was freeze-dried before adding polyol P1. The obtained freeze-dried product was dispersed in polyol P1 so that the solid content was 5% by mass to obtain a slurry catalyst (catalyst 5). The obtained slurry catalyst was measured in the same manner as in Example 1. Note that, since no catalytic activity was observed in the measurement of catalyst activity life, water resistance and the content of ultra-high molecular weight components were not evaluated.
[0061] In this example, a slurry catalyst (Catalyst 6) was produced by increasing the water content of the slurry catalyst (Catalyst 2) of Example 2. That is, the slurry catalyst (Catalyst 2) obtained in Example 2 was left to stand for 7 days in a high humidity atmosphere at an atmospheric temperature of 40°C and a relative humidity of 80%, to obtain a slurry catalyst (Catalyst 6). The obtained slurry catalyst was measured in the same manner as in Example 1.
[0062] [Example 7] In this example, the slurry catalyst (catalyst 2) of Example 2 was contacted with water, and then the water content was reduced to the same level as in Example 2. That is, the slurry catalyst (catalyst 2) obtained in Example 2 was added to 500 g of distilled water, and the mixture was stirred for 1 hour. The water was then distilled off under reduced pressure at 80°C to obtain a slurry catalyst (catalyst 7). The obtained slurry catalyst was measured in the same manner as in Example 1. Since the catalyst did not exhibit catalytic activity in the measurement of catalyst activity life, the water resistance and the content of ultra-high molecular weight components were not evaluated.
[0063] A slurry catalyst (Catalyst 8) was obtained in the same manner as in Example 2, except that 10.2 g of zinc chloride was changed to 16.9 g of zinc bromide. The obtained slurry catalyst was measured in the same manner as in Example 1.
[0064] A slurry catalyst (Catalyst 9) was obtained in the same manner as in Example 6, except that 10.2 g of zinc chloride was changed to 23.9 g of zinc iodide. The obtained slurry catalyst was measured in the same manner as in Example 1.
[0065] [Example 10] In Example 2, 10.2 g of zinc chloride was changed to 7.7 g of zinc fluoride. Because zinc fluoride has low solubility in water, an attempt was made to synthesize a DMC catalyst by solid-phase synthesis, but the resulting product did not exhibit catalytic activity in epoxide polymerization.
[0066] A slurry catalyst (Catalyst 11) was obtained in the same manner as in Example 2, except that 10.2 g of zinc chloride was changed to 14.2 g of zinc nitrate. The obtained slurry catalyst was measured in the same manner as in Example 1.
[0067] [Example 16] In the same manner as in Example 1, a dispersion (1) in which a TBA-DMC catalyst was dispersed in a mixed solution of TBA and water was prepared. Dispersion (1) was filtered under pressure (0.25 MPa) using a circular filter plate with a diameter of 125 mm and quantitative filter paper for fine particles (product name: No. 5C, manufactured by ADVANTEC). Polyol P1 was added to the obtained filter cake so that the solid content was 5% by mass, and then the mixture was dried under reduced pressure at 80°C for 3 hours and then at 115°C for 4 hours to distill off volatile components. Air (air) was introduced and the pressure was returned to normal, yielding a slurry catalyst (catalyst 16) in which the TBA-DMC catalyst was dispersed in polyol P1. The obtained slurry catalyst was measured in the same manner as in Example 1.
[0068] <Examples 12-15, 17-19> Powdered DMC catalysts were produced. Examples 13, 14, and 19 are working examples, and Examples 12, 15, 17, and 18 are comparative examples. [Example 12] Dispersion (1) prepared in the same manner as in Example 1 was filtered under pressure (0.25 MPa) using a circular filter plate with a diameter of 125 mm and quantitative filter paper for fine particles (product name: No. 5C, manufactured by ADVANTEC Co., Ltd.), and the filter cake was separated. The obtained filter cake was dried at 60 ° C. under reduced pressure for 2 hours without adding polyol P1. After drying under reduced pressure, the atmosphere (air) was introduced and the pressure was returned to normal, obtaining a powdered DMC catalyst (catalyst 12). The obtained powdered catalyst was measured in the same manner as in Example 1. The results are shown in Tables 2 and 3 (hereinafter, the same applies unless otherwise specified).
[0069] [Example 13] A filter cake was obtained in the same manner as in Example 12. The obtained filter cake was dried in the air at 100°C for 7 hours without adding polyol P1. After drying in the air, the temperature was returned to room temperature under dry nitrogen to obtain a powdered DMC catalyst (catalyst 13). The moisture content of the powdered DMC catalyst (catalyst 13) was in the range of 8,000 to 140,000 ppm. The obtained powdered catalyst was measured in the same manner as in Example 1.
[0070] [Example 14] A filter cake was obtained in the same manner as in Example 12. The obtained filter cake was dried in the air at 100°C for 5 hours without adding polyol P1. After drying in the air, the temperature was returned to room temperature under dry nitrogen to obtain a powdered DMC catalyst (catalyst 14). The moisture content of the powdered DMC catalyst (catalyst 14) was in the range of 8,000 to 140,000 ppm. The obtained powdered catalyst was measured in the same manner as in Example 1.
[0071] [Example 15] A filter cake was obtained in the same manner as in Example 12. The obtained filter cake was freeze-dried without adding polyol P1 to obtain a powdered DMC catalyst (catalyst 15). The obtained powdered catalyst was measured in the same manner as in Example 1.
[0072] Example 17: First, an aqueous solution containing 81.25 g of zinc chloride was prepared in a 5 L flask. While maintaining the temperature at 45°C, the solution was stirred at 450 rpm to increase dispersion and mixing properties and shear force. An aqueous solution containing 26 g of potassium hexacyanocobaltate (200 g of water) was added dropwise to the zinc chloride aqueous solution over 30 minutes. After the addition was completed, a mixture of 325 g of TBA and 325 g of water was added and stirred at 45°C for 80 minutes. Next, a mixture of 6.5 g of cholate sodium salt, 6.5 g of TBA, and 650 g of water was added and stirred for 20 minutes to obtain a dispersion. 350 g of this dispersion was filtered through a pressure suction filter under a pressure of 2.0 bar. The wet filter cake in the pressure suction filter was then washed under a pressure of 3.0 bar with a mixture of 2 g of cholic acid sodium salt, 70 g of TBA, and 30 g of water. The washed wet filter cake was dried under high vacuum at 100°C for 5 hours, and the atmosphere (air) was introduced to return the pressure to normal, obtaining a powdered DMC catalyst (Catalyst 17). The obtained powdered catalyst was measured in the same manner as in Example 1.
[0073] Example 18 First, a zinc chloride aqueous solution consisting of 10.2 g of zinc chloride and 10 g of water was prepared in a 500 mL flask. While maintaining the temperature at 40°C, the solution was stirred at 450 revolutions per minute to increase dispersion and mixing properties and shear force. An aqueous solution consisting of 4.2 g of potassium hexacyanocobaltate and 75 g of water was added dropwise to the zinc chloride aqueous solution over 30 minutes. After the addition was completed and the mixture was stirred for an additional 30 minutes, a mixture consisting of 80 g of TBA, 80 g of water, and 0.6 g of polyol P1 was added, and the mixture was stirred at 40°C for 30 minutes and then at 60°C for 60 minutes to obtain a mixture containing a TBA-DMC catalyst and water. The resulting mixture was filtered under pressure (0.25 MPa) using a 125 mm diameter circular filter plate and quantitative filter paper for fine particles (No. 5C, manufactured by Advantec Corporation), and a solid containing the TBA-DMC catalyst (hereinafter referred to as the "filter cake") was separated. The resulting filter cake was then transferred to a flask, and a mixed solution consisting of 36 g of TBA and 84 g of water was added. The mixture was stirred for 30 minutes, and then pressure filtered for 15 minutes under the same conditions as above. The resulting filter cake was transferred to a flask, and a mixed solution consisting of 108 g of TBA and 12 g of water was added. The mixture was stirred for 30 minutes, yielding a dispersion (18) in which the TBA-DMC catalyst was dispersed in a mixed solution of TBA and water. The dispersion (18) was filtered under pressure (0.25 MPa) using a 125 mm diameter circular filter plate and quantitative filter paper for fine particles (product name, No. 5C, manufactured by Advantec Corporation), and the filter cake was separated. The washed wet filter cake was dried under high vacuum at 100°C for 5 hours, and then atmospheric air was introduced to return the pressure to normal, yielding a powdered DMC catalyst (Catalyst 18). The resulting powdered catalyst was measured in the same manner as in Example 1.
[0074] [Example 19] In the same manner as in Example 1, a mixed liquid containing a TBA-DMC catalyst and water was prepared. The resulting mixed liquid was subjected to solid-liquid separation using a centrifuge, and a solid containing the TBA-DMC catalyst (hereinafter referred to as the "filter cake") was separated. Next, the filter cake was transferred to a flask, and a mixed liquid consisting of 36 g of TBA and 84 g of water was added and stirred for 30 minutes. The resulting mixed liquid was subjected to solid-liquid separation using a centrifuge. The resulting filter cake was transferred to a flask, and a mixed liquid consisting of 108 g of TBA and 12 g of water was added and stirred for 30 minutes. A dispersion (19) in which the TBA-DMC catalyst was dispersed in a mixed liquid of TBA and water was obtained. The resulting mixture (19) was subjected to solid-liquid separation using a centrifuge, and the filter cake was separated. The resulting filter cake was dried under high vacuum at 100°C for 8 hours without adding polyol P1 to distill off the volatile components, and then dry nitrogen was introduced to return to normal pressure, and a powdered DMC catalyst (catalyst 19) was obtained. The powdery catalyst obtained was measured in the same manner as in Example 1.
[0075]
[0076]
[0077]
[0078] As shown in the results in Tables 1 to 3, the DMC catalysts of Examples 1 and 12 had high catalytic activity in epoxide polymerization, but produced a large amount of ultra-high molecular weight components. The DMC catalysts of Examples 5, 7, 10, and 15 were inactive. The catalysts of Examples 6, 9, and 11 had low activity. The DMC catalysts of Examples 16 to 18 had high catalytic activity in epoxide polymerization, but produced a large amount of ultra-high molecular weight components. In contrast, the DMC catalysts of Examples 2 to 4, 8, 13, 14, and 19, which were prepared by a water content adjustment step to have a water content of 8,000 to 140,000 ppm, diffraction peaks at 2θ = 36° and 47°, and no diffraction peak at 2θ = 34°, had high catalytic activity and were able to reduce the content of ultra-high molecular weight components. Furthermore, they had excellent water resistance, meaning that their catalytic activity was less likely to decrease even when stored in a humid environment.
Claims
1. A composite metal cyanide complex catalyst for epoxide polymerization reaction, the composite metal cyanide complex catalyst containing zinc and cobalt, a water content of 8,000 to 140,000 ppm as measured by Karl Fischer method, and an X-ray diffraction pattern having diffraction peaks at 2θ=36° and 2θ=47°, and no diffraction peak at 2θ=34°.
2. A method for producing a composite metal cyanide complex catalyst for epoxide polymerization reaction, by coordinating an organic ligand to a reaction product obtained by reacting a metal halide salt with a transition metal cyanide compound, wherein the metal of the metal halide salt is zinc, and the transition metal of the transition metal cyanide compound is cobalt, and the water content of the composite metal cyanide complex catalyst is adjusted so that after the organic ligand is coordinated, the water content of the composite metal cyanide complex catalyst is 8,000 to 140,000 ppm as measured by Karl Fischer method, and the X-ray diffraction pattern of the composite metal cyanide complex catalyst has diffraction peaks at 2θ=36° and 2θ=47°, but no diffraction peak at 2θ=34°.
3. The method for producing a double metal cyanide complex catalyst according to claim 2, wherein the metal halide salt comprises at least one selected from the group consisting of zinc chloride and zinc bromide.
4. The method for producing a double metal cyanide complex catalyst according to claim 2 or 3, wherein the organic ligand comprises tert-butyl alcohol.
5. A composite metal cyanide complex slurry catalyst comprising the composite metal cyanide complex catalyst according to claim 1 and a dispersion medium having a water content of 500 ppm or less as determined by the Karl Fischer method.
6. The double metal cyanide complex slurry catalyst according to claim 5, wherein the content of the double metal cyanide complex catalyst is 0.001 to 60 mass % based on the total mass of the double metal cyanide complex slurry catalyst.
7. A method for producing a composite metal cyanide complex slurry catalyst containing a composite metal cyanide complex catalyst for epoxide polymerization reaction, wherein the metal species contained in the composite metal cyanide complex catalyst are zinc and cobalt, the method comprising: a slurry preparation step of preparing a slurry containing the composite metal cyanide complex catalyst and a dispersion medium; and a moisture adjustment step of adjusting the moisture content of the slurry so that the composite metal cyanide complex catalyst has a water content of 8,000 to 140,000 ppm as measured by Karl Fischer method, the dispersion medium has a water content of 500 ppm or less as measured by Karl Fischer method, and the X-ray diffraction pattern of the composite metal cyanide complex catalyst has diffraction peaks at 2θ=36° and 2θ=47° and no diffraction peak at 2θ=34°.
8. A method for producing a complex metal cyanide complex slurry catalyst according to claim 7, wherein the slurry preparation step comprises the steps of reacting a metal halide salt whose metal is zinc with a transition metal cyanide compound whose transition metal is cobalt in the presence of water to obtain a reaction product, coordinating an organic ligand in the presence of water to obtain a mixed liquid containing the complex metal cyanide complex catalyst and water, removing impurities and water from the mixed liquid, and adding a dispersing medium to prepare a slurry containing the complex metal cyanide complex catalyst and the dispersing medium.
9. A method for producing a polymer, comprising polymerizing an epoxide in the presence of the double metal cyanide complex catalyst according to claim 1.
Citation Information
Patent Citations
Dimetal cyanide complex catalyst, its production, and production of epoxide polymer by using it
JP1995196778A
Double metal cyanide complex catalyst and producing method thereof
JP2003103177A
Composition for manufacturing polyurethane foam, polyol system liquid, and manufacturing method of polyurethane foam
JP2019137810A
Curable composition, cured article and laminate
JP2023090792A
Method for preserving complex metal cyanide compounds and method for producing polyethers