Process for production of thermoplastic lignocellulose

A two-step process for producing thermoplastic lignocellulose with improved melt-flow properties addresses the limitations of existing methods, enabling injection molding of sustainable consumer goods.

WO2026234570A1PCT designated stage Publication Date: 2026-11-12MCMASTER UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2026/054445
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-06
Filing Date
2026-05-05
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing methods for producing thermoplastic lignocellulose suffer from poor melt-flow properties, making them unsuitable for injection molding, and there is a need for sustainable, moldable thermoplastic resins for consumer goods.

Method used

A two-step process involving pretreatment of lignocellulose with a functionalizing solution followed by reactive extrusion with an anhydride solution to produce thermoplastic lignocellulose with suitable viscosity and flowability for injection molding.

Benefits of technology

The process results in thermoplastic lignocellulose with low viscosity and high flow rate, enabling injection molding into consumer goods, and utilizing sustainable biomass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2026054445_12112026_PF_FP_ABST
    Figure IB2026054445_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Described is a process for the production injection-mouldable thermoplastic extrudates from lignocellulose. The process comprises: a pretreatment step wherein lignocellulose is first mixed with a functionalizing solution to obtain a slurry of pretreated lignocellulose which is then dried to obtain dry pretreated lignocellulose; and a reactive extrusion step, comprising feeding the dry pretreated lignocellulose in a feed zone of a twin screw extruder and feeding an anhydride solution in a subsequent extrusion zone to obtain the thermoplastic lignocellulose extrudate. The process may further comprise washing the thermoplastic lignocellulose to obtain substantially pure thermoplastic lignocellulose. Also described is a thermoplastic lignocellulose obtained by this process(es) and methods of using of the lignocellulose to make consumer goods.
Need to check novelty before this filing date? Find Prior Art

Description

PROCESS FOR PRODUCTION OF THERMOPLASTIC LIGNOCELLULOSE CROSS REFERENCE TO RELATED APPLICATION

[0001] This patent application claims priority to provisional patent application US 63 / 800,732 filed on May 06, 2025 the content of which is incorporated herein by reference in its entirety.FIELD OF THE INVENTION

[0002] The invention relates to the field of thermoplastic, and more particularly to production an injection-mouldable thermoplastic extrudate produced from lignocellulose.BACKGROUND OF THE INVENTION

[0003] It is estimated that over 460 million metric tons of plastic are produced every year with an estimated 20 million metric tons ending up in the environment as plastic litter. Concerningly, less than 10% of plastic is ever recycled. For this reason, bio-plastic alternatives have started to find traction in the market.

[0004] The most abundant natural polymer is lignocellulose making up most plant material. The abundance of forestry biomass makes it an attractive material as an alternative to petrochemical products such as plastics. The successful implementation of forestry biomass in consumer goods has been hampered by the difficulty of processing the forestry biomass into the desired products. Indeed, lignocellulose lacks a melt state necessary to allow for the polymer to be molded into a desired shape. This property of lignocellulose means that it cannot be used as a replacement polymer for traditional petroplastics. Chemical modifications of lignocellulose can allow for a melt temperature resulting in a thermoplastic lignocellulose (TPLC) product. Many approaches to perform the necessary chemical modification on lignocellulose to make it thermoplastic require techniques that are not conducive to commodity scale manufacturing, such as the use of expensive chemical inputs, large quantities of solvents, and / or poor atom economy of reaction.

[0005] Recent advances have made it economically feasible to consider large-scale, commodity manufacturing of TPLC. For instance, international PCT publication WO2023 / 245287 teaches systems, devices and methods for producing thermoplastic lignocellulose. Nevertheless, this technique, as well as many other existing techniques that produce a thermoplastic lignocellulose, suffer from poor melt- flow properties not conducive to injection molding. Many of the existing processes that make thermoplastic lignocellulosics have melt states that are too viscous to be used in injection molding machines, limiting their widespread use in the market.

[0006] Injection molding can be used to produce complex units, minimizes molding costs, and is an efficient way of maximizing the production of a molded product with varying levels of complexity within a short period of time. For these, and many other reasons, it is one of the preferred methods of molding manufacture by industry worldwide. In order for injection molding to be feasible, a polymer requires a low enough viscosity, or a tendency for that viscosity to drop while in motion, so that it may traverse the narrow pathways of a mold. Viscosity is the resistant to flow, and a polymer with too high of a viscosity cannot be economically used in injection molding and will therefore miss out on a big market.

[0007] Accordingly, there is a need for new ways of producing thermoplastic lignocellulose that, in its melt state, has a low enough viscosity and / or high enough flow rate, such that thermoplastic lignocellulose goods can be injection molded.

[0008] There is also a need for sustainably sourced thermoplastic resins with good moldability that can be useful for housings of electrical / electronic products, automotive interior / exterior materials, and various other consumer goods.

[0009] There is further a need for a method of manufacturing thermoplastic consumer goods from sustainable biomass such as lignocellulose by way of injection molding.

[0010] The present invention addresses these needs and other needs as it will be apparent from the review of the disclosure and description of the features of the invention hereinafter.BRIEF SUMMARY OF THE INVENTION

[0011] According to one aspect, the invention relates to a process for producing a thermoplastic lignocellulose extrudate, comprising:a pretreatment step, comprising:(i) mixing lignocellulose with a functionalizing solution to obtain a slurry of pretreated lignocellulose;(ii) drying said slurry of pretreated lignocellulose to obtain dry pretreated lignocellulose;a reactive extrusion step, comprising feeding the dry pretreated lignocellulose in a feed zone of a twin screw extruder and feeding an anhydride solution in a subsequent extrusion zone to obtain said thermoplastic lignocellulose extrudate.

[0012] According to another aspect, the invention relates to a process for producing a substantially pure thermoplastic lignocellulose, comprising:a pretreatment step, comprising:(i) mixing lignocellulose with a functionalizing solution to obtain a slurry of pretreated lignocellulose;(ii) drying said slurry of pretreated lignocellulose to obtain dry pretreated lignocellulose;a reactive step, comprising mixing pieces of dry pretreated lignocellulose with an anhydride solution to obtain thermoplastic lignocellulose; anda washing step comprising washing the thermoplastic lignocellulose to obtain substantially pure thermoplastic lignocellulose.

[0013] According to another aspect, the invention relates to a thermoplastic lignocellulose (extrudate or substantially pure) obtained by a any of the processes described herein.

[0014] According to another aspect, the invention relates to a thermoplastic lignocellulose having one or more of the following features:a. it is injection-moldable;b. it comprises a melt flow index (MFI) or melt flow rate (MFR) of about 2g / 10min to about 40g / 10min;c. it comprises a complex viscosity ranges between 10000Pa.s and 100 OOOPa.s.;d. it comprises esterified lignocellulose as evidenced a peak in the region of ~1750-1720cm'1when analysed by FTIR.

[0015] According to another aspect, the invention relates to a method for manufacturing a consumer good made of lignocellulose, comprising:a. providing a thermoplastic lignocellulose extrudate obtained from a process as defined herein, or providing a substantially pure lignocellulose obtained from a process as defined herein;b. injection molding of the consumer good with the thermoplastic lignocellulose extrudate or the substantially pure lignocellulose.

[0016] According to another aspect, the invention relates a consumer good made of a thermoplastic lignocellulose extrudate obtained from a process as defined herein, or made from a substantially pure lignocellulose obtained a process as defined herein.

[0017] According to another aspect, the invention relates to the use of a thermoplastic lignocellulose extrudate obtained from a process as defined herein, or made from a substantially pure lignocellulose obtained a process as defined herein, for injection molding of consumer goods.

[0018] Additional aspects, advantages and features of the present invention will become more apparent upon reading of the following non-restrictive description of preferred embodiments which are exemplary and should not be interpreted as limiting the scope of the invention.BRIEF DESCRIPTION OF THE FIGURES

[0019] For the invention to be readily understood, embodiments of the invention are illustrated by way of example in the accompanying figures.

[0020] Figure 1 is a flow diagram showing a one-step process as described in the prior art (e.g., WO 2023 / 245287).

[0021] Figure 2 is flow diagram detailing a two-step process in accordance with an embodiment of the present invention, the process improving melt flow into a region that allows for injection moldability.

[0022] Figure 3 is a graph showing viscosity curves comparing thermoplasticflowability of thermoplastic lignocellulose (TPLC) produced via the one-step method (triangle symbols) and two-step method (round symbols), in accordance with Example 5.

[0023] Figure 4 is a graph showing viscosity curves comparing thermoplasticflowability of thermoplastic lignocellulose (TPLC) produced via the two-step method using hyamine (round symbols) or CTAB (triangle symbols), in accordance with Example 5.

[0024] Figure 5A is a spectra of a Fourier Transform Infrared spectroscopy (FTIR) analysis of starting feedstock lignocellulose.

[0025] Figure 5B is a spectra of FTIR analysis of thermoplastic lignocellulose as described in Example 5.

[0026] Figure 6 is a picture of an injection-molded dog-bone manufactured using thermoplastic lignocellulose obtained by the two-step process in accordance with Example 2.

[0027] Further details of the invention and its advantages will be apparent from the detailed description included below.DETAILED DESCRIPTION OF EMBODIMENTS

[0028] In the following description of the embodiments, references to the accompanying figures are illustrations of an example by which the invention may be practised. It will be understood that other embodiments may be made without departing from the scope of the invention disclosed. Unless defined otherwise, all technical andscientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs.General overview

[0029] The invention provides new and inventive means of producing thermoplastic lignocellulose material that has a low enough viscosity and / or high enough flow rate to be injection molded for manufacturing consumer goods.

[0030] The present invention provides a two-step process for producing thermoplastic lignocellulose, wherein the first step adds in a functionalizing agent(s) and lignocellulose fiber and allows time for the ingredient(s) to work their way into the lignocellulose fiber, while a second step focuses on chemical modification reactions of the lignocellulose to make it thermoplastic.

[0031] Advantageously, several types of lignocellulose may be used in accordance to the process of the present invention, including dry cellulose, pulp, lignocellulose waste or a mixture thereof. The lignocellulose may originate from various sources including, but not limited to, agricultural residues (e.g., corn stover, wheat straw, rice husks, and sugarcane bagasse), forestry residues (sawdust, wood chips, and paper mill discards), energy crops (e.g., switchgrass and elephant grass), pulp and paper products (e.g. TMP pulp) and municipal solid waste or recycling streams (e.g., waste from households and industries). The lignocellulose may also have already undergone previous treatments (e.g., pulping, coating, etc.).Two-step process for producing a thermoplastic lignocellulose extrudate

[0032] One aspect of the invention concerns a process for producing a thermoplastic lignocellulose extrudate. In one particular embodiment the method comprises two steps, namely: (1) a pretreatment step, wherein (a) lignocellulose is mixed with a functionalizing solution to obtain an homogenous slurry of pretreated lignocellulose, and (b) the slurry of pretreated lignocellulose is dried to obtain dry pretreated lignocellulose; and (2) a reactive extrusion step to obtain a thermoplastic lignocellulose extrudate.

[0033] FIG. 1 shows a flow diagram showing a one-step process as described in the prior art (e.g., WO 2023 / 245287) while FIG. 2 describes an embodiment of the process of the present invention. The two diagrams together highlight the differences between the prior art and the current discovery.

[0034] Generally, FIG. 1 describes a reactive extrusion (110). The inputs of the reactive extrusion are a lignocellulose that is ideally dried to a moisture content of >5% (111) and a liquid modifier that is produced by mixing together until homogeneous a functionalization agent, sulfuric acid, and an esterification agent (112). These two components are then mixed and reacted in a twin screw extruder (113). The extrudate that comes off the twin screw extruder is a thermoplastic lignocellulose extrudate (114). A washing step (115), comprising washing the thermoplastic lignocellulose to obtain substantially pure thermoplastic lignocellulose, may also be effected.

[0035] FIG. 2 shows the production of a thermoplastic lignocellulose using a two-step process: Step 1 is a pre-treatment of the lignocellulose (210) which is later used in Step 2 (reactive extrusion (220)). The pretreatment step (210) comprises drying the lignocellulose (211) until it ideally has a moisture content equal to or less than 5% w / w and in parallel making an aqueous solution of the functionalization agent (212). The dry lignocellulose from (211) and the functionalization agent solution from (212) are then mixed together in a twin screw extruder (213). The extrudate is left for several hours (214) at room temperature before being dried (215) until it reaches a moisture content of ideally equal to or less than 10% w / w. The dried, pre-treated lignocellulose produced in (215) is then subjected to reactive extrusion (220) in Step 2. In that second step, the dried lignocellulose (221) is mixed and reacted with butyric anhydride (222) in a twin screw extruder (223). The twin screw extruder (223) can be the same or different from twin screw extruder (113), depending on equipment availability. The extrudate that comes off the twin screw extruder (223) is a thermoplastic lignocellulose extrudate (224). A washing step (225), comprising washing the thermoplastic lignocellulose to obtain substantially pure thermoplastic lignocellulose, may also be effected.

[0036] The functionalizing solution used in the first step preferably comprises quaternary ammonium salt(s). The functionalizing solution may or may not be acidic,since an acid may be present in a following step. In embodiments, the functionalizing solution used in the first step is a strongly acidic aqueous solution comprising quaternary ammonium salt(s). Preferably the acid is sulfuric acid and it is used in a range of about 4% w / w to about 14% w / w (e.g. about 3% w / w, or about 4% w / w, or about 5% w / w, or about 6% w / w, or about 7% w / w, or about 8% w / w, or about 9% w / w, or about 10% w / w, or about 11% w / w, or about 12% w / w, or about 13% w / w, or about 14% w / w) based on the total weight of the composition. It may also be envisionable to use other strong acids such as trifluoroacetic acid.

[0037] Envisioned quaternary ammonium salts include those capable to enhance the solubility, disruption, and / or processing efficiency of lignocellulosic biomass. Particular examples include, but are not limited to, benzethonium chloride (hyamine), cetyltrimethylammonium bromide (CTAB), tetramethylammonium chloride (TMAC), tetraalkylammonium salts including but not limited to Tetraethylammonium Chloride (TEAC), Tetrabutylammonium Chloride (TBAC), Tetrapropylammonium Bromide (TPAB), Tetraethylammonium Bromide (TEAB), Tetrabutylammonium Hydrogen Sulfate (TBAHS), Tetraethylammonium Acetate (TEAA). In one particular embodiment the functionalizing solution comprises water, sulfuric acid (about 9 % w / w), and benzethonium chloride (about 33 % w / w)

[0038] In embodiments, the lignocellulose is mixed with the functionalizing solution such that the functionalization agent to lignocellulose ratios range from about 0.5mol to about 7mol of functionalization agent to 1kg of lignocellulose (e.g. about 0.5mol / kg, , or about 1mol / kg,, or about 2.5mol / kg, or about 3.5mol / kg, or about 5mol / kg,or about 6mol / kg,or about 7 mol / kg).The amount of functionalizing agent or solution may depend upon many variables including the solubility of the functionalization agent in water, the starting amount of water in the starting cellulosic material, the desired final amount of water in the slurry to be obtained, etc. Typically, a lower amount of water is desired as this water has to be removed in a next step. In one particular embodiment, 283g of hyamine was added to 1kg of lignocellulose (i.e., about 0.63mol / kg).

[0039] Preferably, the lignocellulose comes in contact with an acid during the process since acid is beneficial for the esterification of lignocellulose. One or more acid(s) may beadded to the pretreatment step and / or to the reactive extrusion step. Example 2 hereinafter provides a non-limitative example having acid in the second part of the process (reactive extrusion) with the first step (pretreatment step) being acid free. In accordance with the present invention, the acid can be added to the first step (pretreatment step), step 2 (reactive extrusion step) or both steps. In all cases, the parameters (e.g., selection of the acid(s), amount of acid(s), introduction in either one or both steps, etc.) should be selected such that the thermoplastic lignocellulose extrudate to be obtained possess a melt flow that will allow for injection moldability.

[0040] In embodiments, the lignocellulose is mixed with the functionalizing solution using any suitable means such as overhead mixing, extrusion, blending, stirring or the like. The lignocellulose is mixed with the functionalizing solution until a homogenous (e.g., evenly mixed) slurry of pretreated lignocellulose is obtained. The duration of the mixing may be of about 5 min to about 24h (e.g. about 5 min, or about 30 min, or about 1 hour, or about 2 hour, or about 4 hour, or about 8 hour, or about 12 hour, or about 15 hour, or about 20 hour, or about 24 hour, or more) typically 30 min, as it may vary depending on various factors such as the ratio of lignocellulose vs the functionalizing solution, the type of lignocellulose, the concentration of functionalizing solution, the mixing methods, etc. In embodiments, at the end of the pretreatment step a homogenous slurry of pretreated lignocellulose is obtained. That slurry preferably comprises a mixture of lignocellulose and quaternary ammonium salt(s). That slurry is also preferably homogenous, i.e. the lignocellulose appears to be evenly wetted throughout.

[0041] The next step of the process consists of drying the slurry of pretreated lignocellulose to obtain dry pretreated lignocellulose. In embodiments, the drying is carried out until a moisture content of the dry pretreated lignocellulose is about 3% w / w to about 15% w / w, or about 5% w / w to about 10% w / w. In embodiments, the drying is carried out until a moisture content of the dry lignocellulose is about less than 15% w / w, or about less than 10% w / w, about less than 7.5% w / w, or about less than 5% w / w, or about less than 4% w / w, or about less than 2.5% w / w. Those skilled in the art would appreciate that a lower moisture content is preferable. A higher moisture content will still work, however it will require more anhydride reagent in the following reactive extrusion step.

[0042] Any suitable method or device can be used for the drying including, but not limited to, air drying, vacuum oven drying, convection drying, rotary drum drying, infrared drying, freeze drying and the like. In embodiments, the drying is carried out at temperature preserving the lignocellulose, for instance in a vacuum at a temperature of about 40°C to about 100°C. In one particular embodiment, the slurry of lignocellulose is dried into a powder in a vacuum oven at about 60°C overnight.

[0043] The next step of the process consists of the reactive extrusion step. That step comprises two sub steps and is carried out in a twin screw extruder having a feed zone, a subsequent extrusion zone and, finally, an extrusion barrel. Particularly, (i) the dry pretreated lignocellulose is first fed into the feed zone of the twin screw extruder, and (ii) an anhydride solution is fed in the extrusion zone. At the end of the extrusion process, in the extrusion barrel, a thermoplastic lignocellulose extrudate is obtained.

[0044] The anhydride solution comprises an anhydride (or a mixture of anhydrides). Examples include alkyl chain anhydrides such as acetic anhydride, propionic anhydride (propanoic anhydride) butyric anhydride, valeric anhydride (pentanoic anhydride), caproic anhydride (hexanoic anhydride), enanthic anhydride (heptanoic anhydride), caprylic octanoic anhydride (octanoic anhydride), pelargonic anhydride (nonanoic anhydride), capric anhydride (decanoic anhydride), and longer alkyl anhydrides. In a preferred embodiments, the anhydride solution comprises acetic anhydride, butyric anhydride and / or or a mixture thereof. More preferably, butyric anhydride is used.

[0045] The anhydride solution is preferably fed in the twin screw extruder within desirable proportion, with respect to the dry lignocellulose provided in the feed zone. In embodiments, the anhydride solution is fed such that about 0.25 L to about 3L of anhydride solution is used per kilogram of lignocellulose powder (e.g. about 0.5 L to about 2L per kg, or about 0.9 L to about 1 ,5L per kg). In one particular embodiment, 1.33L of anhydride is used for 1 kg of lignocellulose.

[0046] Preferably, the temperature of the reactive extrusion step is controlled. Preferably the twin screw extruder comprises several different temperatures zones that can be set to higher or lower temperature. In embodiments the feed zone of the twin screw extruder operates at around ambient temperature, for instance about 20°C to about 25°C.In embodiments the extrusion in the extrusion zone is carried out at a temperature of about 65°C to about 250°C, or about 80°C to about 200°C, or about 100°C to about 150°C, or about 125°C.

[0047] At the end of the extrusion, a thermoplastic lignocellulose extrudate is obtained. That extrudate may be cooled (e.g., to form pellets) and later be shaped into a required form (e.g. by injection molding).

[0048] Preferably, thermoplastic lignocellulose according to the present invention possesses one or more of the following features:a. it is injection-mouldable;b. it comprises a flowability conducive for injection moldability, for instance a melt flow index (MFI) or melt flow rate (MFR) of about 2g / 10min to about 40g / 10min;c. it comprises rheological properties, a complex viscosity ranges between 10 OOOPa.s and 100 OOOPa.s; and / ord. it comprises esterified lignocellulose as evidenced a peak in the region of ~1750-1720cm'1when analysed by FTIR.

[0049] Those skilled in the art will appreciate that present invention is not limited to any particular type of twin screw extruder and that many different models and size of extruders can be used. Examples of known twin screw extruders include, Leistritz™ ZSE-HP 27mm or Coperion™ ZSK25WLE. In the present examples, a twin screw extruder manufactured by Coperion™ ZSK25WLE 40L / D was used successfully.

[0050] The process of the invention may further comprises the step of washing the thermoplastic lignocellulose extrudate. Washing step(s) may be beneficial to improve purity of the thermoplastic lignocellulose and to reduce presence of any undesirable byproduct(s) therein. In one embodiment, the washing comprises washing with 1 M sodium bicarbonate solution followed by washing water, however pure water, and / or organic solvents miscible with water such as acetone, ethanol, tetrahydrofuran (THF), etc. For instance the thermoplastic lignocellulose extrudate may be soaked in 1M sodium bicarbonate solution for 5min to 24h followed by filtration. After the washing is complete the product needs to be dried before being molded.Batch / beaker process for producing a thermoplastic lignocellulose

[0051] Another aspect of the invention concerns a process for producing thermoplastic lignocellulose as a “batch” rather than in a twin screw extruder. In one embodiment the process comprises:a pretreatment step, comprising: (i) mixing lignocellulose with a functionalizing solution to obtain an homogenous slurry of pretreated lignocellulose; (ii) a drying step, comprising drying the slurry of pretreated lignocellulose to obtain dry pretreated lignocellulose;a reactive step, comprising mixing pieces of dry pretreated lignocellulose with an anhydride solution to obtain thermoplastic lignocellulose; anda washing step, comprising washing the thermoplastic lignocellulose to obtain substantially clean and substantially pure thermoplastic lignocellulose.

[0052] In one embodiment the mixing is carried out at a temperature of about 65°C to about 250°C, or about 100°C to about 200°C. In one embodiment the mixing is carried out for at least 15 min (e.g. about 15 min to about 24h).

[0053] In one embodiment the washing comprises washing with 1M sodium bicarbonate solution followed by washing water.

[0054] The resulting thermoplastic lignocellulose was found to have a good flow (i.e. , desirable MFI / MFR and / or rheological properties, as defined hereinabove).Method of manufacturing consumer goods

[0055] Another aspect of the invention concerns the manufacture of consumer goods made of lignocellulose. Particularly, a thermoplastic lignocellulose extrudate as defined herein may be used for manufacturing a consumer good made of lignocellulose.

[0056] Because it possess sufficient flowability, the lignocellulose of the present invention is suitable to injection moldability. Accordingly, the present invention encompasses the uses of a thermoplastic lignocellulose having desirable properties asdefined herein, and / or obtained by the process described herein, for injection molding of consumer goods.

[0057] Accordingly, the present invention further encompasses any consumer good made of lignocellulose obtained from the process described herein. Examples of goods that could be manufactured using the thermoplastic lignocellulose of the invention include, but are not limited to, electrical / electronic products, automotive interior / exterior materials, etc.

[0058] Accordingly, a consumer good made of lignocellulose as defined herein will possess one or more of the following beneficial features: it is predominantly made of nonpetroleum source of material; it is composable and / or it is biodegradable; and it comprises esterified lignocellulose (e.g., as evidenced by strong peak in the region of ~1750-1720cm'1when analysed by FTIR).

[0059] Those skilled in the art will recognize, or be able to ascertain, using no more than routine experimentation, numerous equivalents to the specific procedures, embodiments, claims, and examples described herein. Such equivalents are considered to be within the scope of this invention and covered by the claims appended hereto. The invention is further illustrated by the following examples, which should not be construed as further or specifically limiting.EXAMPLESExample 1: Two-step process in batch (beaker)

[0060] In one particular example, the two-step process of the invention is carried out in batch (beaker). According to this example, 1 ,25g of hyamine is dissolved in water along with 0.67mL of sulfuric acid. The functionalizing solution is then blended with 4.7g of pulp and mixed well using an overhead mixer until it is a homogenous slurry. The pulp is then dried overnight at 60°C until and then broken up into smaller pieces. In the second step, the small pieces of pulp are added to 6mL of butyric anhydride and stirred with an overhead mixer at 120°C for 30min. After the reaction, the product is washed with 1Msodium bicarbonate solution followed by water until pure. The resulting product has good flow (i.e., it possessed an adequate melt flow index (MFI), as defined hereinabove.Example 2: Two-step process in a twin-screw extruder (dry lignocellulose powder)

[0061] According to this particular example, both steps of the process are carried out in a twin screw extruder. 1kg of lignocellulose was fed as powder into a twin screw extruder at its feed zone, a functionalizing solution of 283g hyamine in 848mL of water was injected in a nearby downstream zone at a feed rate of 1.13L / kg (liquid / lignocellulose ratio). The extrudate was then dried in an oven set to 60°C until dry or overnight. The dry lignocellulose powder was then fed into the twin screw extruder Coperion™ ZSK25WLE 40L / D, in the feed zone set at 25°C while the extrusion zones were set at 110°C. The liquid butyric anhydride mixed with 74.3mL of sulfuric acid was injected in a nearby downstream zone with a feed rate of 1.33L / kg (liquid / treated lignocellulose ratio). The extrudate was washed with 1M sodium bicarbonate solution followed by water until the conductivity no longer increased. This extrudate was successfully used for injection molding a consumer thermoplastic product, as described hereinafter in Example 6.Example 3: Two-step process in a twin-screw extruder (lignocellulose pulp)

[0062] According to this particular example, the first step is carried out in a batch vessel whereas the second step uses a twin screw extruder. 100g of lignocellulose pulp was added to a homogeneous functionalizing solution of 32g hyamine and 7.28mL sulfuric acid in 500mL of water. The mixture was stirred until a homogeneous slurry was made and then dried into a powder using a vacuum oven at 60°C overnight. Next day, a homogeneous solution was prepared where 32.2g of hyamine and 7.63mL of sulfuric acid are dissolved in 120mL acetic anhydride. The treated lignocellulose powder was then fed into the twin screw extruder in the feed zone set at 25°C at 1.5kg / h, while the extrusion zones were set at 110°C. The acetic anhydride solution was fed in a subsequent zone with a feed rate of 32 mL / min (liquid / treated lignocellulose ratio). The extrudate was washed with 1M sodium bicarbonate solution followed by water until the conductivity no longer increased.Example 4: Two-step process in a twin-screw extruder (batch vessel)

[0063] In another particular example using a batch vessel and twin screw extruder, 100g of pulp was added to a homogeneous functionalizing solution of 26g cetyltrimethylammonium bromide (CTAB) and 7.28mL sulfuric acid in 500mL of water. The mixture was stirred until a homogeneous slurry was made and then dried into a powder using a vacuum oven at 60°C overnight. Next day, a homogeneous solution was prepared where 26g of CTAB and 7.63mL of sulfuric acid were dissolved in 120mL acetic anhydride. The treated lignocellulose powder was then fed into the twin screw extruder in the feed zone set at 25°C at 1.5kg / h, while the extrusion zones were set at 110°C. The acetic anhydride solution was injected in a nearby downstream zone with a feed rate of 32 mL / min (liquid / treated lignocellulose ratio). The extrudate was washed with 1M sodium bicarbonate solution followed by water until the until the conductivity no longer increased..Example 5: Comparing thermoplastic-flowability of thermoplastic lignocellulose (TPLC) prepared using both one-step and two-step methods.

[0064] Thermoplastic-flowability was compared for thermoplastic lignocellulose (TPLC) prepared using either (i) a one-step method (see examples B-25 in WO 2023 / 245287) and (ii) a two-step method (present Example 2).

[0065] Measuring the viscosity of the thermoplastic lignocellulose (TPLC) was achieved by making circular disk specimens. Circular disk specimens (25 mm diameter, 1.5 mm thickness) were prepared by compression molding at 160 °C under a pressure of 6 MPa. The complex viscosity of each sample was evaluated using a Discovery™ HR-2 hybrid rheometer (TA Instruments, USA) with a parallel-plate geometry. A temperature sweep test was performed from 80 to 200 °C at a heating rate of 5°C / min under a constant oscillation frequency of 1 Hz and shear rate of 0.1 s’1. The shear strain was maintained within the linear viscoelastic region to ensure reliable rheological measurements.

[0066] Viscosity curves were analyzed to compare the thermoplastic-flowability of TPLC produced via the one-step or the two-step methods, providing insights into the effect of processing conditions on material rheology. As shown in Figure 3, the complex viscosity curve of the two step method is significantly lower than the analogous one-stepmethod TPLC. Figure 4, shows that a variety of functionalizing agents such as hyamine and CTAB can produce similar low viscosity results falling within acceptable injection molding ranges.

[0067] The lignocellulose of the present invention was also analyzed by Fourrier Transformation Infrared spectroscopy (FTIR). The spectra was obtained using a Nicolet 6700™ spectrometer using the SmartiTRT™ ATR accessory. The data was collected between a wavenumber range of 4000-600 cm-1. Figures 5A and 5B display the spectra of original feedstock lignocellulose and of thermoplastic lignocellulose obtained in accordance with Example 2. Esterification of the lignocellulose can be seen as a strong peak in the region of ~1735cm-1(Fig. 5B) which does not exist in the original feedstock lignocellulose (Fig. 5A).Example 6: Injection molding of a consumer good

[0068] Thermoplastic lignocellulose (TPLC) prepared in accordance with the two-step process of Example 2 was used to manufacture a dogbone (Figure 5). The injection molding was performed using an Arburg 370A™ injection molding machine with fitted with an ASTM D638 Type I mold and the molding parameters were adjusted to be within the parameters recommended by the manufacturer.

[0069] The injection molded TPLC dogbone obtained had a dark color (i.e. black) and desired suitable properties including proper shape, sufficient rigidity and a smooth surface.

[0070] Headings are included herein for reference and to aid in locating certain sections. These headings are not intended to limit the scope of the concepts described therein, and these concepts may have applicability in other sections throughout the entire specification. Thus, the present invention is not intended to be limited to the embodiments shown herein but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

[0071] The singular forms “a”, “an” and “the” include corresponding plural references unless the context clearly dictates otherwise. Thus, for example, reference to "acompound" includes one or more of such compounds and reference to "the method" includes reference to equivalent steps and methods known to those of ordinary skill in the art that could be modified or substituted for the methods described herein.

[0072] Unless otherwise indicated, all numbers expressing quantities of ingredients, reaction conditions, concentrations, properties, and so forth used in the specification and claims are to be understood as being modified in all instances by the term “about”. At the very least, each numerical parameter should at least be construed in light of the number of reported significant digits and by applying ordinary rounding techniques. Accordingly, unless indicated to the contrary, the numerical parameters set forth in the present specification and attached claims are approximations that may vary depending upon the properties sought to be obtained. Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the embodiments are approximations, the numerical values set forth in the specific examples are reported as precisely as possible. Any numerical value, however, inherently contains certain errors resulting from variations in experiments, testing measurements, statistical analyses, and such.

[0073] It is understood that the examples and embodiments described herein are for illustrative purposes only and that various modifications or changes in light thereof will be suggested to persons skilled in the art and are to be included within the present invention and scope of the appended claims.

Claims

CLAIMS:

1. A process for producing a thermoplastic lignocellulose extrudate, comprising:a pretreatment step, comprising:(i) mixing lignocellulose with a functionalizing solution to obtain a slurry of pretreated lignocellulose;(ii) drying said slurry of pretreated lignocellulose to obtain dry pretreated lignocellulose;a reactive extrusion step, comprising feeding the dry pretreated lignocellulose in a feed zone of a twin screw extruder and feeding an anhydride solution in a subsequent extrusion zone to obtain said thermoplastic lignocellulose extrudate.

2. The process of claim 1, wherein the lignocellulose in the pretreatment step comprises dry cellulose, pulp, lignocellulose, lignocellulose waste or mixtures thereof.

3. The process of claim 1 or 2, wherein the functionalizing solution comprises water, quaternary ammonium salt(s), and optionally sulfuric acid.

4. The process of any one claims 1 to 3, wherein the quaternary ammonium salt is selected from the group consisting of benzethonium chloride (hyamine), cetyltrimethylammonium bromide (CTAB), tetramethylammonium chloride and mixtures thereof.

5. The process of any one claims 1 to 4, wherein said anhydride solution comprises and alkyl chain anhydride.

6. The process of claim 5, wherein the anhydride solution comprises acetic anhydride, butyric anhydride, or a mixture thereof.

7. The process of any one claims 1 to 6, wherein an acid is added to the pretreatment step and / or to the reactive extrusion step.

8. The process of any one claims 1 to 7, wherein said dry pretreated lignocellulose comprises a moisture content of about less than about 15% w / w.

9. The process of any one claims 1 to 8, wherein the feed zone is kept at a temperature of about 25°C.

10. The process of any one claims 1 to 9, wherein extrusion in the extrusion zone is carried out at a temperature of about 65°C to about 250°C.

11. The process of any one claims 1 to 10, further comprising the step of washing the thermoplastic lignocellulose extrudate.

12. The process of claim 11, wherein the washing compriseswashing with 1M sodium bicarbonate solution followed by washing water13. The process of any one claims 1 to 12, wherein the drying step is carried out in an oven.

14. A process for producing a substantially pure thermoplastic lignocellulose, comprising:a pretreatment step, comprising:(i) mixing lignocellulose with a functionalizing solution to obtain a slurry of pretreated lignocellulose;(ii) drying said slurry of pretreated lignocellulose to obtain dry pretreated lignocellulose;a reactive step, comprising mixing pieces of dry pretreated lignocellulose with an anhydride solution to obtain thermoplastic lignocellulose; anda washing step comprising washing the thermoplastic lignocellulose to obtain substantially pure thermoplastic lignocellulose.

15. The process of claim 14, wherein said mixing is carried out at a temperature of about 65°C to about 250°C.

16. The process of claim 14 or 15, wherein said mixing is carried out for about 10 min to about 24h.

17. The process of any one claims 14 to 16, wherein said washing compriseswashing with 1M sodium bicarbonate solution followed by washing water.

18. A thermoplastic lignocellulose obtained by the process of any one of claims 1 to 17.

19. A thermoplastic lignocellulose having one or more of the following features: (a) it is injection-moldable;(b) it comprises a melt flow index (MFI) or melt flow rate (MFR) of about 2g / 10min to about 40g / 10min; and / or(c) it comprises a complex viscosity ranges between 10000Pa.s and 100 OOOPa.s.;(d) it comprises esterified lignocellulose as evidenced a peak in the region of ~1750-1720cm'1when analysed by FTIR.

20. A method for manufacturing a consumer good made of lignocellulose, comprising:(a) providing the thermoplastic lignocellulose extrudate obtained from the process of any one of claims 1 to 13, or providing the substantially pure lignocellulose obtained from the process of any one of claims 14 to 17; (b) injection molding of the consumer good with said thermoplastic lignocellulose extrudate or said substantially pure lignocellulose.

21. A consumer good made of the thermoplastic lignocellulose extrudate obtained from the process of any one of claims 1 to 13, or made from the substantially pure lignocellulose obtained from the process of any one of claims 14 to 17.

22. Use of the thermoplastic lignocellulose extrudate obtained from the process of any one of claims 1 to 13, or use of the substantially pure lignocellulose obtained from the process of any one of claims 14 to 17, for injection molding of consumer goods.