Metal catalyst, method for producing crotonaldehyde, method for producing 1,3-butadiene, method for producing butadiene polymer, and method for producing crosslinked product
A metal catalyst with controlled Lewis acid content in metal oxide composites addresses inefficiencies in butadiene production from biomass, achieving high reactivity and balanced yields in ethanol conversion to crotonaldehyde and 1,3-butadiene.
Patent Information
- Application Number
- PCT/JP2026/016778
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-27
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for producing butadiene from petrochemicals are inefficient, and alternative biomass-based processes require catalysts with improved reactivity to enhance yield and balance generation rates.
A metal catalyst comprising a specific range of Lewis acid content in metal oxide composites containing Group 4 or Group 5 metals and silicon atoms, optimized through a sedimentation method, is used to convert ethanol into crotonaldehyde, crotyl alcohol, and ultimately 1,3-butadiene, with a balanced generation rate and yield.
The catalyst achieves excellent reactivity in synthesizing crotonaldehyde, crotyl alcohol, and 1,3-butadiene, providing a good balance between generation rate and yield, particularly enhancing reaction (2) reactivity.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Metal catalyst, method for producing crotonaldehyde, method for producing 1,3-butadiene, method for producing butadiene polymer, and method for producing crosslinked products
[0001] This disclosure relates to a metal catalyst. This disclosure also relates to a method for producing crotonaldehyde, a method for producing 1,3-butadiene, a method for producing a butadiene polymer, and a method for producing a crosslinked product using the metal catalyst.
[0002] 1,3-Butadiene has traditionally been obtained primarily as a byproduct of the thermal decomposition of naphtha using an ethylene cracker (naphtha cracker) to produce ethylene and propylene. As an alternative to petrochemical raw materials, processes are being researched to produce butadiene by fermenting biomass (corn and sugarcane) via butanediol, butanol, butene, or ethanol.
[0003] For example, Patent Document 1 describes a solid catalyst comprising a metal (A) and a metal oxide (B) supported on a carrier, wherein the metal (A) is at least one metal selected from the group consisting of metals belonging to Group 11 and Group 13, and the metal oxide (B) is an oxide of at least one metal selected from the group consisting of metals belonging to Group 3, Group 4 and Group 5, and a method for producing butadiene from ethanol or a mixture of ethanol and acetaldehyde in the presence of the solid catalyst is described.
[0004] Japanese Patent Publication No. 2021-194553
[0005] The present invention aims to provide a metal catalyst with excellent reactivity.
[0006] The inventors of the present invention conducted studies to achieve the above objective and found that the objective can be achieved by controlling the amount of Lewis acid within a specific range for metal oxide composites containing metal atoms of Group 4 or Group 5 of the periodic table and silicon atoms, thereby completing the present invention.
[0007] In other words, the present invention provides the following metal catalyst.
[0008] [1] A metal oxide complex containing metal atoms and silicon atoms of Group 4 or Group 5 of the periodic table, with a Lewis acid content of 3 × 10 -5 mol / g or more 1×10 -3 A metal catalyst having a Lewis acid content of mol / g or less, wherein the Lewis acid content is a value calculated based on an infrared spectrum obtained by performing Fourier transform infrared spectroscopy on a sample obtained by adsorbing pyridine onto the metal catalyst and then desorbing the pyridine at 100°C. [2] The metal catalyst according to [1], wherein the oxide content of metal atoms of group 4 or 5 of the periodic table is 4 to 25% by mass.
[0009] Furthermore, the present invention provides the following manufacturing method.
[0010] [3] A method for producing crotonaldehyde, comprising the step of contacting the metal catalyst described in [1] or [2] with ethanol. [4] A method for producing 1,3-butadiene, comprising the step of contacting the metal catalyst described in [1] or [2] with ethanol. [5] A method for producing a butadiene polymer, comprising obtaining 1,3-butadiene by the method described in [4] and polymerizing the obtained 1,3-butadiene. [6] A method for producing a crosslinked product, comprising obtaining a butadiene polymer by the method described in [5] and crosslinking the obtained butadiene polymer.
[0011] According to the present invention, a metal catalyst with excellent reactivity can be provided.
[0012] The metal catalysts of this disclosure can be suitably used in the synthesis of 1,3-butadiene (hereinafter sometimes referred to as butadiene). Butadiene synthesis can be carried out, for example, by the following synthesis scheme.
[0013]
[0014] The above synthetic scheme includes reaction (1) for synthesizing acetaldehyde from ethanol, reaction (2) for synthesizing crotonaldehyde from acetaldehyde, reaction (3) for synthesizing crotyl alcohol from crotonaldehyde, and reaction (4) for synthesizing 1,3-butadiene from crotyl alcohol. The metal catalyst of the present disclosure can be suitably used as a reaction catalyst for any of reactions (1) to (4). The metal catalyst of the present disclosure has excellent reactivity in each of reactions (1) to (4), and by using the metal catalyst of the present disclosure, a good balance between the generation rate and the generation yield can be achieved in each of reactions (1) to (4).
[0015] <Metal Catalyst> The metal catalyst of the present disclosure consists of a metal oxide composite containing a metal atom of Group 4 or Group 5 of the periodic table (hereinafter sometimes referred to as "metal atoms of Groups 4 and 5 of the periodic table") and a silicon atom. The metal catalyst of the present disclosure has a Lewis acid amount of 3×10 -5 mol / g or more and 1×10 -3 mol / g or less.
[0016] The Lewis acid amount of the metal catalyst of the present disclosure is 3×10 -5 mol / g or more and 1×10 -3 mol / g or less. Since the Lewis acid amount is relatively large as described above, the metal catalyst of the present disclosure has excellent reactivity in each of reactions (1) to (4) in the above-mentioned synthetic scheme, and is particularly extremely excellent in the reactivity of reaction (2).
[0017] The Lewis acid amount of the metal catalyst of the present disclosure is not particularly limited as long as it is 3×10 -5 mol / g or more and 1×10 -3 mol / g or less, but is preferably 3.5×10 -5 or more, more preferably 4.0×10 -5 or more, and also preferably 5×10 -4 mol / g or less, more preferably 2×10 -4 mol / g or less, and even more preferably 1×10 -4 mol / g or less. From the viewpoint of further enhancing the reactivity of the metal catalyst, particularly further enhancing the reactivity of reaction (2) in the above-mentioned synthetic scheme, the Lewis acid amount is 5×10 -5mol / g or more is particularly preferable, and 6.5×10 -5 mol / g or more is most preferable.
[0018] The amount of Lewis acid per 1 gram of the content in terms of oxide of the metal atoms of Groups 4 and 5 of the periodic table in the metal catalyst of the present disclosure is not particularly limited, but from the viewpoint that the reactivity of the metal catalyst is further enhanced, and in particular, the reactivity of reaction (2) in the aforementioned synthesis scheme is further enhanced, it is 0.3×10 -3 or more and 1×10 -3 mol / g or less, preferably 0.35×10 -3 or more and 1×10 -3 mol / g or less, more preferably 0.4×10 -3 or more and 1×10 -3 mol / g or less, still more preferable.
[0019] Note that the amount of Brønsted acid of the metal catalyst of the present disclosure is not particularly limited, but is preferably 0.1×10 -5 mol / g or more and 10×10 -5 mol / g or less. In addition, the ratio of Lewis acid [L / (B+L)] relative to the total amount of Lewis acid and Brønsted acid for the metal catalyst of the present disclosure is not particularly limited, but is preferably 0.2 to 1, more preferably 0.3 to 1, still more preferably 0.4 to 0.99, particularly preferably more than 0.5 and 0.98 or less, and most preferably 0.55 to 0.97. When the ratio of Lewis acid [L / (B+L)] is within the above range, the reactivity of the metal catalyst is further enhanced, and in particular, the reactivity of reaction (2) in the aforementioned synthesis scheme is further enhanced.
[0020] In the present disclosure, the amount of Lewis acid and the amount of Brønsted acid of the metal catalyst are values calculated based on an infrared spectrum obtained by performing Fourier transform infrared spectroscopy measurement on a sample obtained by adsorbing pyridine to the metal catalyst and then desorbing the pyridine at 100°C. More specifically, the amount of Lewis acid and the amount of Brønsted acid can be measured by the methods described in the Examples.
[0021] Examples of Group 4 and Group 5 metal atoms contained in the metal catalyst of this disclosure include Group 4 metal atoms such as titanium (Ti), zirconium (Zr), and hafnium (Hf); and Group 5 metal atoms such as vanadium (V) and tantalum (Ta). Among these, Group 4 metal atoms are preferred, and Hf is more preferred, from the viewpoint of further increasing the reactivity of the metal catalyst, and in particular, further increasing the reactivity of reaction (2) in the synthesis scheme described above.
[0022] The oxide-based content of metal atoms from groups 4 and 5 of the periodic table in the metal catalyst of this disclosure is not particularly limited, but is preferably 2 to 50% by mass, more preferably 4 to 25% by mass, even more preferably 5 to 20% by mass, and particularly preferably 6 to 16% by mass. When the oxide-based content of metal atoms from groups 4 and 5 of the periodic table is within the above range, the reactivity of the metal catalyst is further increased, and in particular, the reactivity of reaction (2) in the synthesis scheme described above is further increased. From the viewpoint of extremely increasing the reactivity of the metal catalyst, and in particular extremely increasing the reactivity of reaction (2) in the synthesis scheme described above, the oxide-based content of metal atoms from groups 4 and 5 of the periodic table is preferably 8% by mass or more, and more preferably 10% by mass or more. The oxide-based content of metal atoms from groups 4 and 5 of the periodic table can be measured by ICP emission spectrometry.
[0023] For example, if the metal catalyst of this disclosure is a metal oxide composite containing Hf as a metal atom of Group 4 or 5 of the periodic table, the oxide content of the metal atoms of Group 4 or 5 of the periodic table is HfO 2 This represents the converted content. Furthermore, for example, if the metal catalyst of this disclosure is a metal oxide composite containing Ta as a metal atom of Group 4 or 5 of the periodic table, the oxide-converted content of the metal atoms of Group 4 or 5 of the periodic table is the amount of Ta. 2 O 5 This represents the converted content.
[0024] As the metal catalyst of this disclosure, a metal oxide composite represented by the following compositional formula (i) is preferred. a SiO b(i) (In empirical formula (i), M represents a metal atom of group 4 or 5 of the periodic table, a is a value greater than 0, and b is any value.)
[0025] In empirical formula (i), b is a value that depends on the type of M and the value of a. For example, if M is a metal atom of Group 4 of the periodic table, it is preferable that b satisfies a × 2 + 1.9 ≤ b ≤ a × 2 + 2.1. Also, for example, if M is a metal atom of Group 5 of the periodic table, it is preferable that b satisfies a × 2.5 + 1.9 ≤ b ≤ a × 2.5 + 2.1.
[0026] For example, if the metal catalyst of this disclosure contains a metal atom of Group 4 of the periodic table, a metal oxide composite represented by the following compositional formula (ii) is preferred as the metal catalyst of this disclosure. M' x Si y O z (ii) (In empirical formula (ii), M' represents a metal atom of Group 4 of the periodic table, x and y satisfy x + y = 1, 0 < x < 1, and 0 < y < 1, and z is any value.)
[0027] In compositional formula (ii), z is a value that depends on the type of M'. For example, if M' is Hf, it is preferable that z satisfies 1.9 ≤ z ≤ 2.1.
[0028] In the metal catalyst of this disclosure, the molar equivalents of the content of metal atoms from groups 4 and 5 of the periodic table relative to the content of silicon atoms (e.g., a in composition formula (i), x / y in composition formula (ii)) are not particularly limited, but are preferably 0.0055 to 0.49, more preferably 0.011 to 0.16, even more preferably 0.014 to 0.12, and particularly preferably 0.017 to 0.09. Having the above molar equivalents within this range further enhances the reactivity of the metal catalyst, and in particular, further enhances the reactivity of reaction (2) in the synthesis scheme described above. The content of metal atoms from groups 4 and 5 of the periodic table and silicon atoms can be measured by ICP emission spectrometry.
[0029] <Method for Manufacturing Metal Catalysts> The metal catalysts of this disclosure are preferably manufactured by a sedimentation method. That is, the metal catalysts of this disclosure are preferably metal oxide composites obtained by a sedimentation method. By a sedimentation method, the metal catalysts of this disclosure with a relatively high Lewis acid content can be suitably manufactured.
[0030] The reason why the metal catalyst of this disclosure, which has a relatively high amount of Lewis acid, can be suitably obtained by the sedimentation method is not entirely clear, but it is presumed to be for the following reasons. First, in the metal oxide composite obtained by the sedimentation method, which contains metal atoms of groups 4 and 5 of the periodic table and silicon atoms, the metal atoms of groups 4 and 5 of the periodic table are dispersed together with the silicon atoms, so it is thought that there are many M-O-Si bonds (where M represents metal atoms of groups 4 and 5 of the periodic table). Here, it is presumed that the amount of Lewis acid tends to increase as the number of M-O-Si bonds increases, due to the fact that metal atoms of groups 4 and 5 of the periodic table (M) have lower electronegativity than Si. Therefore, it is presumed that the metal catalyst of this disclosure, which contains many M-O-Si bonds and, as a result, has a relatively high amount of Lewis acid, can be suitably obtained by the sedimentation method.
[0031] On the other hand, metal oxide composites obtained by a manufacturing method (supporting method) in which metal atoms of groups 4 and 5 of the periodic table are supported on a silicon oxide support tend to have too little Lewis acid.
[0032] In the sedimentation method, for example, a silicon-containing compound and a compound containing metal atoms from groups 4 and 5 of the periodic table are heated in an aqueous medium in the presence of a homogeneous precipitating agent to obtain a precursor of the metal oxide composite. The metal oxide composite can then be obtained by calcining the obtained precursor.
[0033] Examples of silicon-containing compounds include amorphous silica such as silica gel; alkali metal silicates such as sodium silicate and potassium silicate; and alkoxysilane compounds such as tetramethoxysilane, tetraethoxysilane, and tetrapropoxysilane. Among these, alkoxysilane compounds are preferred, tetramethoxysilane, tetraethoxysilane, and tetrapropoxysilane are more preferred, and tetraethoxysilane is preferred.
[0034] The amount of silicon-containing compound used is preferably 5 to 50 parts per 100 parts by mass of aqueous medium.
[0035] As compounds containing metal atoms from groups 4 and 5 of the periodic table, water-soluble compounds are preferred. For example, when the metal atom from group 4 and 5 of the periodic table is Hf, hafnium tetrachloride is preferably used, and when the metal atom from group 4 and 5 of the periodic table is Ta, tantalum pentachloride is preferably used.
[0036] The amount of compounds containing metal atoms from groups 4 and 5 of the periodic table used can be determined according to the amount of silicon-containing compounds used and the composition of the target metal catalyst.
[0037] The aqueous medium is water, a hydrophilic solvent, or a mixture thereof. The hydrophilic solvent is not particularly limited as long as it mixes well with water and does not undergo phase separation. Examples of hydrophilic solvents include alcohols such as methanol and ethanol; tetrahydrofuran (THF); and dimethyl sulfoxide (DMSO).
[0038] The aqueous medium preferably contains water, more preferably a mixture of water and a hydrophilic solvent, even more preferably a mixture of water and an alcohol, and particularly preferably a mixture of water and ethanol. When a mixture of water and a hydrophilic solvent is used, the mixing ratio (mass ratio) of water to hydrophilic solvent is preferably water:hydrophilic solvent = 10:1 to 1:1.
[0039] Examples of homogeneous precipitating agents include urea and hexamine, with urea being preferred. These can be used individually or in combination of two or more.
[0040] The amount of homogeneous precipitant used is preferably 1 to 30 moles per mole of metal atoms of Group 4 and Group 5 of the periodic table in the compound containing metal atoms of Group 4 and Group 5 of the periodic table used. By using an amount of homogeneous precipitant within the above range, the nuclei of the metal oxide composite precursor can be uniformly generated, thereby improving the uniformity of the metal catalyst of this disclosure.
[0041] The order in which the silicon-containing compound, the compound containing metal atoms from groups 4 and 5 of the periodic table, the aqueous medium, and the homogeneous precipitant are supplied to the reaction vessel is not particularly limited. For example, when a mixture of water and a hydrophilic solvent is used as the aqueous medium, water and the homogeneous precipitant may be supplied to the reaction vessel first, and then a separately prepared mixture of the silicon-containing compound, the compound containing metal atoms from groups 4 and 5 of the periodic table, and the hydrophilic solvent may be supplied.
[0042] When heating a silicon-containing compound and a compound containing metal atoms from groups 4 and 5 of the periodic table in an aqueous medium in the presence of a homogeneous precipitating agent, the heating conditions are not particularly limited as long as a precursor of the metal oxide complex is obtained, but the heating temperature is preferably 80 to 200°C and the heating time is preferably 5 to 48 hours. The heating pressure is not particularly limited. For example, heating may be carried out under atmospheric pressure. Alternatively, heating may be carried out under a pressurized environment of 0.3 MPa or higher.
[0043] A precursor of a metal oxide composite can be obtained by separating the reaction solution obtained by heating from the solid-liquid. The solid-liquid separation method is not particularly limited, and known methods such as filtration, centrifugation, static separation, and drying can be used.
[0044] It is preferable to pulverize the solids obtained by solid separation. The pulverization method is not particularly limited, and known methods can be used. The pulverization may be performed after or before calcination of the metal oxide composite precursor.
[0045] Next, the metal oxide composite precursor obtained as described above is calcined. The calcination conditions are not particularly limited as long as a metal oxide composite can be obtained, but the calcination temperature is preferably 200 to 600°C, more preferably 300 to 600°C, the calcination time is preferably 1 to 20 hours, more preferably 3 to 10 hours, and the calcination atmosphere is preferably an air atmosphere.
[0046] <Methods for Producing Acetaldehyde, Crotonaldehyde, and 1,3-Butadiene> By contacting the metal catalyst of this disclosure with ethanol, acetaldehyde, crotonaldehyde, and butadiene can be produced according to the synthesis scheme described above. Hereinafter, the method for producing acetaldehyde that includes the step of contacting the metal catalyst of this disclosure with ethanol may be referred to as the method for producing acetaldehyde of this disclosure. Similarly, the methods for producing crotonaldehyde and butadiene that include the step of contacting the metal catalyst of this disclosure with ethanol may be referred to as the method for producing crotonaldehyde and the method for producing butadiene of this disclosure, respectively.
[0047] Examples of ethanol include ethanol derived from biomass such as sugarcane or corn, or ethanol derived from petroleum or natural gas, and it is preferable to use ethanol derived from biomass.
[0048] In the methods for producing crotonaldehyde and butadiene according to the disclosure, ethanol alone may be used as a raw material, or a mixture of ethanol and acetaldehyde may be used. Here, the acetaldehyde may be obtained by the method for producing acetaldehyde according to the disclosure, or obtained by other methods.
[0049] When using acetaldehyde obtained by the method for producing acetaldehyde of the present disclosure, the method for producing crotonaldehyde of the present disclosure and the method for producing butadiene of the present disclosure may each comprise the steps of: obtaining acetaldehyde by contacting ethanol with the metal catalyst of the present disclosure; mixing ethanol with the obtained acetaldehyde to obtain a mixture; and contacting the obtained mixture with the metal catalyst of the present disclosure.
[0050] When using a mixture of ethanol and acetaldehyde as a raw material, the mixing ratio of ethanol and acetaldehyde is not particularly limited, but is preferably in the range of 9.9:0.1 to 5:5, more preferably in the range of 9:1 to 5:5, and even more preferably in the range of 7:3 to 5:5, expressed as a molar ratio of "ethanol:acetaldehyde".
[0051] When contacting the metal catalyst of this disclosure with a raw material (ethanol, or a mixture of ethanol and acetaldehyde), known reaction methods such as flow-through and batch reactions can be used. Among these, the flow-through reaction is preferred from the viewpoint of productivity. Examples of methods for contacting the raw material with the metal catalyst include the suspension bed method, the fluidized bed method, and the fixed bed method. The reaction may be carried out in the gas phase or the liquid phase, but it is preferred in the gas phase from the viewpoint of being able to apply a high reaction temperature and further enhance reactivity.
[0052] When the reaction is carried out in the gas phase, the raw material gas may be supplied to the reactor without dilution, or it may be supplied to the reactor after being appropriately diluted with gases such as nitrogen, helium, argon, or water vapor.
[0053] The reaction conditions in the method for producing acetaldehyde according to this disclosure are not particularly limited as long as conditions are met for obtaining acetaldehyde. The reaction temperature is preferably 260 to 500°C, and more preferably 300 to 480°C, from the viewpoint of further increasing reactivity while suppressing degradation of the metal catalyst. The reaction pressure can be appropriately set in a wide range from atmospheric pressure to high pressure, but atmospheric pressure is preferred.
[0054] The reaction conditions in the methods for producing crotonaldehyde and butadiene according to this disclosure are not particularly limited as long as the desired product (crotonaldehyde or butadiene) can be obtained. The reaction temperature is preferably 260 to 500°C, more preferably 300 to 480°C, from the viewpoint of further increasing reactivity while suppressing degradation of the metal catalyst, and the reaction pressure can be appropriately set in a wide range from atmospheric pressure to high pressure, but atmospheric pressure is preferred.
[0055] After the reaction is complete, the reaction product may be separated and purified by means of separation such as distillation, extraction, membrane separation, or a combination thereof.
[0056] <Method for producing butadiene polymer> Butadiene polymer can be produced by polymerizing the butadiene obtained by the above-described production method.
[0057] The polymerization method is not particularly limited, and known methods can be used. The monomer used for polymerization may consist solely of butadiene, or it may be butadiene in addition to other monomers.
[0058] Other monomers besides butadiene can be any compound copolymerizable with butadiene, and are not particularly limited, but examples include the following monomers.
[0059] Conjugated diene compounds other than 1,3-butadiene, such as isoprene, 2,3-dimethyl-1,3-butadiene, 2-phenyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 4,5-diethyl-1,3-octadiene, and 3-butyl-1,3-octadiene.
[0060] Aromatic vinyl compounds such as styrene, methylstyrene, ethylstyrene, t-butylstyrene, α-methylstyrene, α-methyl-p-methylstyrene, chlorostyrene, bromostyrene, methoxystyrene, dimethylaminomethylstyrene, dimethylaminoethylstyrene, diethylaminomethylstyrene, diethylaminoethylstyrene, cyanoethylstyrene, and vinylnaphthalene.
[0061] Chain-like olefin compounds such as ethylene, propylene, and 1-butene; cyclic olefin compounds such as cyclopentene and 2-norbornene; and non-conjugated diene compounds such as 1,5-hexadiene, 1,6-heptadiene, 1,7-octadiene, dicyclopentadiene, and 5-ethylidene-2-norbornene.
[0062] (Meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate.
[0063] Other (meth)acrylic acid derivatives such as (meth)acrylonitrile and (meth)acrylamide.
[0064] The composition of the monomers used is not particularly limited as long as it contains butadiene, and can be determined according to the polymerization method and the composition of the desired butadiene polymer.
[0065] A polymer composition may be produced by adding the required amounts of various additives, such as crosslinking agents, crosslinking accelerators, crosslinking activators, antioxidants, fillers, surfactants, process oils, plasticizers, lubricants, and compatibilizers, to a butadiene polymer according to conventional methods.
[0066] <Method for producing crosslinked products> Crosslinked products can be produced by crosslinking the butadiene polymer obtained by the above-described manufacturing method.
[0067] The crosslinking method is not particularly limited as long as it can crosslink the butadiene polymer, but a preferred method is to prepare a polymer composition containing the butadiene polymer and a crosslinking agent, and then heat the resulting polymer composition to induce a crosslinking reaction. Known conditions can be used for the crosslinking conditions, depending on the desired shape of the crosslinked product. The polymer composition may be pre-formed, or the resulting crosslinked product may be formed after crosslinking.
[0068] The butadiene polymers and crosslinked products obtained as described above can be used in a variety of applications, such as: materials for various parts of a tire, including the cap tread, base tread, carcass, sidewall, and bead; materials for hoses, belts, mats, vibration-damping rubber, and other industrial products; impact-resistant modifiers for resins; resin film cushioning materials; shoe soles; rubber shoes; golf balls; toys; and more.
[0069] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. Unless otherwise specified, "parts" and "%" are based on weight. Various measurements were performed according to the following methods.
[0070] <Oxide content of metal atoms from Groups 4 and 5 of the Periodic Table> Oxides of metal atoms from Groups 4 and 5 of the Periodic Table (HfO) in the metal catalyst 2 or Ta 2 O 5 The content, converted to ), was measured by ICP emission spectrometry.
[0071] <Lewis Acid and Brønsted Acid Amounts> The Lewis acid amount (unit: mol / g) and Brønsted acid amount (unit: mol / g) of the metal catalyst were calculated based on the infrared spectrum obtained by FT-IR transmission measurement of samples obtained by adsorbing pyridine onto a metal catalyst and then desorbing the pyridine at 100°C. The acid amount is calculated using the formula described in Journal of Catalysis Volume 141, Pages 347-354 (1993) [C (mol / g) = 1.42 × absorbance × (radius)]. 2 The calculation was performed according to [weight]. Furthermore, the amount of Lewis acid in the metal catalyst was determined by the oxides (HfO) of metal atoms of groups 4 and 5 of the periodic table in the metal catalyst. 2 or Ta 2 O 5 The amount of Lewis acid per gram of content (unit: mol / g) was also calculated. The specific measurement conditions were as follows: [Conditions] Degassing conditions: Under vacuum, 400°C, 1 hour Pyridine adsorption conditions: 100°C, 10 minutes Desorption conditions: 180°C, 30 minutes
[0072] <Ratio of Lewis Acid [L / (B+L)]> The ratio of Lewis acid [L / (B+L)] to the total amount of Lewis acid and Brønsted acid in the metal catalyst was calculated using the Lewis acid and Brønsted acid amounts of the metal catalyst calculated according to the above.
[0073] <Crotonaldehyde Production Rate> The production rate of crotonaldehyde when acetaldehyde is contacted with a metal catalyst was determined by the following method. The crotonaldehyde production rate determined in this test corresponds to the reaction rate of reaction (2) in the reaction scheme described above. A faster crotonaldehyde production rate indicates that the metal catalyst has superior reactivity.
[0074] A quartz tube (less than 1 cm in length) was packed with 0.1 g of metal catalyst to serve as a fixed-bed flow reactor. Vaporized acetaldehyde and nitrogen were flowed through the quartz tube packed with the metal catalyst at a temperature of 400°C and atmospheric pressure. The flow rate of acetaldehyde was 9.0 × 10⁻⁶. -6 The flow rate was set to L / min, and the nitrogen flow rate was set to 20 cc / min. The vaporized acetaldehyde and nitrogen were supplied by bubbling nitrogen into the acetaldehyde.
[0075] Then, the gas that passed through the quartz tube filled with a metal catalyst was measured using a GC-FID apparatus to determine the rate of crotonaldehyde production (unit: mol / g-cat·h).
[0076] <Production Rate of Clotyl Alcohol and 1,3-Butadiene> The production rates of clotyl alcohol and 1,3-butadiene when crotonaldehyde is contacted with a metal catalyst were determined by the following method. The production rates of clotyl alcohol and 1,3-butadiene determined in this test are the reaction rates of reactions simulating reactions (3) and (4) in the above reaction scheme. Specifically, when ethanol is used in reaction (3), acetaldehyde and crotonaldehyde are produced, which increases the effective supply rate of crotonaldehyde and makes it difficult to determine the production rate of clotyl alcohol and 1,3-butadiene. Therefore, in this test, 1-propanol was used instead of ethanol in reaction (3). The faster the production rate of clotyl alcohol and 1,3-butadiene, the more reactive the metal catalyst is considered to be.
[0077] A quartz tube (less than 1 cm in length) was packed with 0.0025 g of metal catalyst to serve as a fixed-bed flow reactor. Vaporized crotonaldehyde and 1-propanol (crotonaldehyde:1-propanol = 1 mol:1 mol) and nitrogen were flowed through the quartz tube packed with the metal catalyst at a temperature of 400°C and atmospheric pressure. The total flow rate of crotonaldehyde and 1-propanol was 2.0 × 10⁻⁶. -2The flow rate was set to L / min, and the nitrogen flow rate was set to 8 cc / min. The vaporized crotonaldehyde and 1-propanol, along with the nitrogen, were supplied by bubbling nitrogen into a mixed solution of crotonaldehyde and 1-propanol.
[0078] Then, the gas that passed through the quartz tube filled with a metal catalyst was measured using a GC-FID apparatus, and the total production rate of clotyl alcohol and 1,3-butadiene (unit: mol / g-cat·h) was determined.
[0079] <Yield of 1,3-Butadiene> The gas recovered in each example and comparative example was measured using a GC-FID apparatus to determine the rate of 1,3-butadiene production. The yield of 1,3-butadiene was then calculated according to the following formula: Yield of 1,3-butadiene (%) = Number of moles of 1,3-butadiene produced per unit time × 2 ÷ Total number of moles of ethanol and acetaldehyde supplied as raw materials per unit time × 100
[0080] <Example 1> (Synthesis of Metal Catalyst 1) 80 g of water and a predetermined amount of urea were added to a 500 ml Erlenmeyer flask to obtain an aqueous solution. Next, a mixture of 25 g of tetraethoxysilane, 25 g of ethanol, and a predetermined amount of hafnium tetrachloride was added and stirred with a stirrer. Here, the amount of hafnium tetrachloride used was determined by the hafnium oxide content in the resulting metal catalyst (HfO 2 The amount used was set to a converted amount of 7 wt%, and the amount of urea used was 10 molar equivalents per mole of hafnium atoms in the hafnium tetrachloride used. The stirring conditions were 400 rpm, 30°C, and 10 minutes.
[0081] Next, the Erlenmeyer flask was transferred to a preheated oil bath and stirred under reflux at 140°C for 15 hours. After that, the reaction mixture was separated into solid and liquid to obtain a solid. The solid was washed with water on a filtration device until the pH of the filtrate was approximately 7. The washed solid was dried at 110°C for 8 hours and then pulverized. The pulverized material was placed in an oven, heated to 550°C at a rate of 5°C / min, calcined at 550°C for 5 hours, and then cooled to obtain an Hf-Si oxide composite (hereinafter referred to as "metal catalyst 1"). For the obtained metal catalyst 1, the oxide content of metal atoms from Group 4 of the periodic table, the amount of Lewis acid, the amount of Brønsted acid, the ratio of Lewis acid [L / (B+L)], the rate of crotonaldehyde production, and the rates of clotyl alcohol and 1,3-butadiene production were determined according to the method described above. The results are shown in Table 1.
[0082] (Production of acetaldehyde) A quartz tube (less than 1 cm in length) was packed with metal catalyst 1 to serve as a fixed-bed flow reactor. Vaporized ethanol and nitrogen were flowed through the quartz tube packed with metal catalyst 1 at a temperature of 400°C and atmospheric pressure. The flow rate of ethanol was 9.0 × 10⁻⁶. -6 The flow rate of ethanol was set to L / min, and the nitrogen flow rate was set to 20 cc / min. The vaporized ethanol and nitrogen were supplied by bubbling nitrogen into the ethanol. The gas after passing through the quartz tube filled with metal catalyst 1 was recovered. When the recovered gas was measured using a GC-FID apparatus, acetaldehyde was detected. From the above, it was confirmed that acetaldehyde can be produced by contacting metal catalyst 1 with ethanol.
[0083] (Production of crotonaldehyde and 1,3-butadiene) A quartz tube (less than 1 cm in length) was packed with metal catalyst 1 to serve as a fixed-bed flow reactor. Vaporized ethanol and acetaldehyde (ethanol:acetaldehyde = 6 mol:4 mol) and nitrogen were flowed through the quartz tube packed with metal catalyst 1 at a temperature of 400°C and atmospheric pressure. The total flow rate of ethanol and acetaldehyde was 9.0 × 10⁻⁶. -6The flow rate was set to L / min, and the nitrogen flow rate was set to 20 cc / min. The vaporized ethanol and acetaldehyde, along with the nitrogen, were supplied by bubbling nitrogen into a mixed solution of ethanol and acetaldehyde.
[0084] The gas that passed through the quartz tube filled with metal catalyst 1 was then recovered. When the recovered gas was measured using a GC-FID apparatus, crotonaldehyde and 1,3-butadiene were detected. From the above, it was confirmed that crotonaldehyde and 1,3-butadiene can be produced by contacting metal catalyst 1 with ethanol. Furthermore, the yield of 1,3-butadiene was determined using the recovered gas according to the above method. The results are shown in Table 1.
[0085] <Example 2> (Synthesis of metal catalyst 2) The amount of hafnium tetrachloride used is determined by the hafnium oxide content in the resulting metal catalyst (HfO 2 Except for changing the amount (converted amount) to 14 wt% and setting the amount of urea used to 10 molar equivalents per mole of hafnium atoms in the hafnium tetrachloride used, an Hf-Si oxide composite (hereinafter referred to as "metal catalyst 2") was obtained in the same manner as in Example 1. The obtained metal catalyst 2 was measured in the same manner as in Example 1. The results are shown in Table 1.
[0086] (Production of Acetaldehyde) Acetaldehyde was produced in the same manner as in Example 1, except that the obtained metal catalyst 2 was used, and the gas after passing through the quartz tube filled with metal catalyst 2 was recovered. When the recovered gas was measured using a GC-FID apparatus, acetaldehyde was detected. From the above, it was confirmed that acetaldehyde can be produced by contacting metal catalyst 2 with ethanol.
[0087] Crotonaldehyde and 1,3-butadiene were produced in the same manner as in Example 1, except that the obtained metal catalyst 2 was used. The gas after passing through the quartz tube packed with metal catalyst 2 was recovered. When the recovered gas was measured using a GC-FID apparatus, crotonaldehyde and 1,3-butadiene were detected. From the above, it was confirmed that crotonaldehyde and 1,3-butadiene can be produced by contacting metal catalyst 2 with ethanol. Furthermore, the yield of 1,3-butadiene was determined using the recovered gas according to the method described above. The results are shown in Table 1.
[0088] <Comparative Example 1> In Comparative Example 1, metal catalyst 3 was prepared by a supported method. The pore volume of mesoporous silica (manufactured by Fuji Silicia Co., Ltd., product name: CARiACT G-6, average pore size: 6 nm) was determined in advance by nitrogen adsorption / desorption. 1.1 g of hafnium tetrachloride was dissolved in water equal to the pore volume per 9.3 g of mesoporous silica to obtain an aqueous hafnium tetrachloride solution. Then, the above-prepared hafnium tetrachloride solution was added dropwise to 9.3 g of mesoporous silica to impregnate it, and after drying at 110°C for 4 hours, metal catalyst 3 was obtained by calcining at 500°C for 4 hours. The obtained metal catalyst 3 was measured in the same manner as in Example 1. The results are shown in Table 1.
[0089] Crotonaldehyde and 1,3-butadiene were produced in the same manner as in Example 1, except that the obtained metal catalyst 3 was used. The gas after passing through the quartz tube packed with metal catalyst 3 was recovered. Using the recovered gas, the yield of 1,3-butadiene was determined according to the method described above. The results are shown in Table 1.
[0090]
[0091] As is clear from Table 1, it consists of a metal oxide complex containing metal atoms and silicon atoms of Group 4 of the periodic table, and the amount of Lewis acid measured by the method described above is 3 × 10⁻⁶ -5 mol / g or more 1×10 -3 Metal catalysts with a concentration of mol / g or less exhibited excellent reactivity (Examples 1-2). Specifically, using these metal catalysts resulted in a good balance between the production rate and the production rate.
[0092] On the other hand, metal catalysts with too little Lewis acid measured by the method described above exhibited poor reactivity (Comparative Example 1).
[0093] <Example 3> (Synthesis of Metal Catalyst 4) 80 g of water and a predetermined amount of urea were added to a 500 ml Erlenmeyer flask to obtain an aqueous solution. Next, a mixture of 25 g of tetraethoxysilane, 25 g of ethanol, and a predetermined amount of tantalum pentachloride was added and stirred with a stirrer. Here, the amount of tantalum pentachloride used was determined by the tantalum oxide content (Ta) in the resulting metal catalyst. 2 O 5 The amount used was set to a converted amount of 14.6 wt%, and the amount of urea used was 10 molar equivalents per mole of tantalum atoms in the tantalum pentachloride used. The stirring conditions were 400 rpm, 30°C, and 10 minutes.
[0094] Next, the Erlenmeyer flask was transferred to a preheated oil bath and stirred under reflux at 140°C for 15 hours. After that, the reaction mixture was separated into solid and liquid to obtain a solid. The solid was washed with water on a filtration device until the pH of the filtrate was approximately 7. The washed solid was dried at 110°C for 8 hours and then pulverized. The pulverized material was placed in an oven, heated to 550°C at a rate of 5°C / min, calcined at 550°C for 5 hours, and then cooled to obtain a Ta-Si oxide composite (hereinafter referred to as "metal catalyst 4"). Measurements were performed on metal catalyst 4 according to the above method, and the oxides of metal atoms from groups 4 and 5 of the periodic table (Ta 2 O 5 The converted content is 14.6 wt%, and the Lewis acid content is 7.2 × 10 -5 The concentration is mol / g, and the amount of Brønsted acid is 3.3 × 10⁻⁶. -5 It is mol / g, and is an oxide of metal atoms from groups 4 and 5 of the periodic table (Ta 2 O 5 The amount of Lewis acid per gram of the converted content is 0.5 × 10 -3 The concentration was mol / g, and the ratio of Lewis acid content [L / (B+L)] was 0.69.
[0095] (Production of Acetaldehyde) Acetaldehyde was produced in the same manner as in Example 1, except that the obtained metal catalyst 4 was used, and the gas after passing through the quartz tube filled with the metal catalyst 4 was recovered. When the recovered gas was measured using a GC-FID apparatus, acetaldehyde was detected. From the above, it was confirmed that acetaldehyde can be produced by contacting the metal catalyst 4 with ethanol.
[0096] Except for using the obtained metal catalyst 4, crotonaldehyde and 1,3-butadiene were produced in the same manner as in Example 1, and the gas after passing through the quartz tube packed with metal catalyst 4 was recovered. When the recovered gas was measured using a GC-FID apparatus, crotonaldehyde and 1,3-butadiene were detected. From the above, it was confirmed that crotonaldehyde and 1,3-butadiene can be produced by contacting metal catalyst 4 with ethanol. Furthermore, the yield of 1,3-butadiene was determined using the recovered gas according to the above method and was found to be 35.7%. Considering that the yield of 1,3-butadiene was sufficiently high at 35.7%, and in conjunction with the results of Examples 1-2 and Comparative Example 1, it is estimated that the production rate of clotyl alcohol and 1,3-butadiene was sufficiently high in Example 4. Therefore, it is estimated that a good balance between production rate and production rate was achieved in Example 4 as well.
Claims
1. Consists of a metal oxide complex containing metal atoms and silicon atoms from Group 4 or Group 5 of the periodic table, with a Lewis acid content of 3 × 10⁻¹⁶ -5 mol / g or more 1×10 -3 A metal catalyst having a Lewis acid content of mol / g or less, wherein the Lewis acid content is a value calculated based on the infrared spectrum obtained by performing Fourier transform infrared spectroscopy on a sample obtained by adsorbing pyridine onto the metal catalyst and then desorbing the pyridine at 100°C.
2. The metal catalyst according to claim 1, wherein the content of metal atoms of Group 4 or Group 5 of the periodic table, on an oxide basis, is 4 to 25% by mass.
3. A method for producing crotonaldehyde, comprising the step of contacting the metal catalyst described in claim 1 or 2 with ethanol.
4. A method for producing 1,3-butadiene, comprising the step of contacting the metal catalyst described in claim 1 or 2 with ethanol.
5. A method for producing a butadiene polymer, comprising obtaining 1,3-butadiene by the manufacturing method described in claim 4, and polymerizing the obtained 1,3-butadiene.
6. A method for producing a crosslinked product by obtaining a butadiene polymer by the manufacturing method described in claim 5, and crosslinking the obtained butadiene polymer.