Nonaqueous electrolyte power storage element
The non-aqueous electrolyte energy storage element with a specific graphite-to-silicon-based active material ratio and adherence to certain formulas addresses capacity loss in silicon-based active materials, ensuring high capacity retention through suppression of crystalline phase accumulation.
Patent Information
- Application Number
- PCT/JP2026/017034
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-04-29
- Publication Date
- 2026-11-12
AI Technical Summary
Non-aqueous electrolyte energy storage devices using silicon-based active materials experience a decrease in capacity after repeated charging and discharging, particularly influenced by the reaction potential of the negative electrode, leading to a decrease in capacity with shallow discharge depths.
A non-aqueous electrolyte energy storage element comprising a positive electrode and a negative electrode with a specific ratio of graphite and silicon-based active material, where the silicon-based active material is silicon oxide, a silicon-carbon composite, or elemental silicon, and adhering to specific formulas to maintain a high capacity retention rate.
The solution ensures high capacity retention after charge-discharge cycles, suppressing the accumulation of the crystalline phase in the silicon-based active material, thereby maintaining discharge capacity regardless of discharge depth.
Smart Images

Figure JP2026017034_12112026_PF_FP_ABST
Abstract
Description
Non-aqueous electrolyte energy storage element
[0001] This invention relates to a non-aqueous electrolyte energy storage element.
[0002] Non-aqueous electrolyte secondary batteries, such as lithium-ion batteries, are widely used in electronic devices like personal computers and communication terminals, as well as automobiles, due to their high energy density. Generally, non-aqueous electrolyte secondary batteries consist of a pair of electrodes electrically isolated by a separator, and a non-aqueous electrolyte interposed between these electrodes. They are configured to charge and discharge by transferring charge-transporting ions between the two electrodes. Besides non-aqueous electrolyte secondary batteries, capacitors such as lithium-ion capacitors and electric double-layer capacitors are also widely used as non-aqueous electrolyte energy storage elements.
[0003] Non-aqueous electrolyte energy storage devices are known that use silicon-based active materials containing silicon elements, such as elemental silicon or silicon oxide, as the negative electrode active material (see Patent Document 1). Silicon-based active materials have advantages such as a larger discharge capacity per unit mass compared to carbon materials such as graphite (carbon-based active materials).
[0004] Japanese Patent Publication No. 2015-053152
[0005] Non-aqueous electrolyte energy storage devices using silicon-based active materials may experience a decrease in capacity after repeated charging and discharging. In particular, as will be discussed later, the likelihood of this capacity decrease is influenced by the reaction potential of the negative electrode (especially the silicon-based active material) during charging and discharging. Therefore, the capacity may decrease more easily after repeated charging and discharging depending on the discharge depth of the negative electrode.
[0006] The present invention aims to provide a non-aqueous electrolyte energy storage element using a silicon-based active material, which has a high capacity retention rate after charge-discharge cycles.
[0007] A non-aqueous electrolyte energy storage element according to one aspect of the present invention comprises a positive electrode and a negative electrode containing graphite and a silicon-based active material, wherein the content of the silicon-based active material relative to the total of the graphite and the silicon-based active material is 30% by mass or more and 70% by mass or less, and the silicon-based active material is silicon oxide, a silicon-carbon composite or elemental silicon, and when the silicon-based active material is silicon oxide, the following formula (1a) is satisfied, when the silicon-based active material is a composite, the following formula (1b) is satisfied, and when the silicon-based active material is elemental silicon, the following formula (1c) is satisfied. y ≤ 0.0031x + 0.6035 ... (1a) y ≤ 0.0033x + 0.5629 ... (1b) y ≤ 0.0055x + 0.5247 ... (1c) (In equations (1a), (1b), and (1c), x is the content (mass %) of the silicon-based active material relative to the total amount of graphite and silicon-based active material. y is the ratio of the actual charge amount of the negative electrode to the theoretical charge amount of the negative electrode (charge depth of the negative electrode).)
[0008] According to one aspect of the present invention, it is possible to provide a non-aqueous electrolyte energy storage element that has a high capacity retention rate after charge-discharge cycles.
[0009] Figure 1 is a perspective view showing a non-aqueous electrolyte energy storage element according to one embodiment of the present invention. Figure 2 is a schematic diagram showing an energy storage device equipped with multiple non-aqueous electrolyte energy storage elements according to one embodiment of the present invention. Figure 3 is the charging curve of a test battery using a negative electrode unipolarity of Reference Examples 1 to 4. Figure 4 is a graph showing the relationship between the silicon oxide content (mass%) relative to the total of graphite and silicon oxide (x) and the ratio of the actual charge amount of the negative electrode to the theoretical charge amount of the negative electrode (charge depth of the negative electrode) (y) for each non-aqueous electrolyte energy storage element of the examples and comparative examples.
[0010] First, an overview of the non-aqueous electrolyte energy storage elements disclosed herein will be provided.
[0011] (1) A non-aqueous electrolyte energy storage element according to one aspect of the present invention comprises a positive electrode and a negative electrode containing graphite and a silicon-based active material, wherein the content of the silicon-based active material relative to the total of the graphite and the silicon-based active material is 30% by mass or more and 70% by mass or less, and the silicon-based active material is silicon oxide, a composite of silicon and carbon, or elemental silicon, and if the silicon-based active material is silicon oxide, the following formula (1a) is satisfied, if the silicon-based active material is a composite, the following formula (1b) is satisfied, and if the silicon-based active material is elemental silicon, the following formula (1c) is satisfied. y ≤ 0.0031x + 0.6035 ... (1a) y ≤ 0.0033x + 0.5629 ... (1b) y ≤ 0.0055x + 0.5247 ... (1c) (In equations (1a), (1b), and (1c), x is the content (mass %) of the silicon-based active material relative to the total amount of graphite and silicon-based active material. y is the ratio of the actual charge amount of the negative electrode to the theoretical charge amount of the negative electrode (charge depth of the negative electrode).)
[0012] The non-aqueous electrolyte energy storage element described in (1) above has a high capacity retention rate after charge-discharge cycles. More specifically, the non-aqueous electrolyte energy storage element described in (1) above has a high capacity retention rate after charge-discharge cycles, regardless of the depth of discharge during discharge. The reason for this is not clear, but the following reasons are speculated. In this specification, the reduction reaction in which charge transport ions such as lithium ions are absorbed into the negative electrode active material (graphite and silicon-based active material) is called "charging," and the oxidation reaction in which charge transport ions are released from the negative electrode active material is called "discharging." For example, when the charge transport ions in the silicon-based active material are lithium ions, when charged, it becomes an amorphous alloy phase (e.g., a-Li x It changes to Si, and further to 0.05V vs. Li / Li + When charged to a potential lower than that, the crystalline phase (for example, c-Li 15 Si 4 ) changes to ). When discharge is performed while the crystalline phase is present, a two-phase coexistence reaction proceeds in which the crystalline phase changes to an amorphous alloy phase, resulting in 0.45V vs. Li / Li + A plateau is observed in the vicinity. Immediately before this plateau is observed (for example, 0.25 to 0.45 V vs. Li / Li) +) region is further on the front side (for example, 0.05 to 0.25 V vs. Li / Li + ) region, the potential increase rate accompanying the progress of the discharge reaction when discharging at a constant current is larger. Therefore, when the discharge of the non-aqueous electrolyte power storage element ends in the region immediately before the plateau is observed, the discharge capacity decreases by reaching the discharge end voltage of the non-aqueous electrolyte power storage element at a shallower discharge depth than when no crystal phase is present. Also, at about 0.45 V vs. Li / Li + If discharge is not performed until a potential higher than that is reached, the amorphous alloy phase remains. The amorphous alloy phase has higher electron conductivity than a silicon-based active material in an unalloyed state (such as simple silicon). Therefore, when charging is performed with the amorphous alloy phase remaining, the reaction between the amorphous alloy phase and lithium or the like proceeds, making it easier to generate a crystal phase. Then, as charge and discharge are repeated, the crystal phase accumulates, and the potential increase rate immediately before the plateau is observed increases, so the discharge end voltage of the non-aqueous electrolyte power storage element is reached at a shallower discharge depth, and the discharge capacity gradually decreases. As described above, particularly when charge and discharge with a shallow discharge depth are repeated, the accumulation of the crystal phase progresses, and the discharge capacity may decrease. In contrast, in the non-aqueous electrolyte power storage element described in the above (1), by satisfying any of the formulas (1a) to (1c), the negative electrode potential at the state of charge is at the potential at which the silicon-based active material changes into a crystal phase (for example, 0.050 V vs. Li / Li + ) or higher. For this reason, in the case of the non-aqueous electrolyte power storage element described in the above (1), the silicon-based active material hardly changes into a crystal phase even in a charged state, so accumulation of the crystal phase hardly occurs even if charge and discharge are repeated regardless of the discharge depth. For such reasons, it is presumed that the non-aqueous electrolyte power storage element described in the above (1) has a high capacity retention rate after charge-discharge cycles.
[0013] Here, we will explain the procedure for deriving equation (1c) from equation (1a), focusing on equation (1a). Negative electrodes (Reference Examples 1 to 4) were prepared using graphite and silicon oxide as negative electrode active materials, with the silicon oxide content (mass%) (x) relative to the total of graphite and silicon oxide as shown in Table 1. A test battery was assembled using these negative electrodes as the working electrode and a metallic lithium electrode as the counter electrode, and charged with a current of 1 / 3C. The obtained charging curve is shown in Figure 3. Based on the above charging curve, the voltage of the test battery was 0.050V (potential of the metallic lithium electrode was 0.000V vs. Li / Li + Therefore, the negative electrode potential is 0.050V vs. Li / Li + The charging depth (SOC, where the theoretical charge amount of the negative electrode is considered to be 100% SOC) reached was determined, and the upper limit of the negative electrode charging depth was calculated by setting SOC 0% to 0 and SOC 100% to 1. The results are shown in Table 1. By approximating the relationship between the silicon oxide content (mass%) (x) relative to the total of graphite and silicon oxide and the upper limit of the negative electrode charging depth (y) with a linear equation, we obtained y = 0.0031x + 0.6035 and derived equation (1a). Equations (1b) and (1c) were obtained using the same procedure.
[0014]
[0015] The "actual charge amount of the negative electrode" is determined by the following procedure: Discharge the non-aqueous electrolyte energy storage element with a discharge current of 0.05C until it reaches the discharge termination voltage for normal use. Charge it with a constant current of 0.05C until it reaches the charge termination voltage for normal use, bringing it to a fully charged state. Record the amount of charge at this time. Discharge the non-aqueous electrolyte energy storage element with a discharge current of 0.05C until it reaches the discharge termination voltage for normal use. Disassemble the element, remove the negative electrode, cut out the removed negative electrode to use as the working electrode, and assemble a test battery with a metallic lithium electrode as the counter electrode. Discharge (residual discharge) the assembled test battery as follows: Use a discharge current equivalent to 0.05C for the discharge capacity (mAh) of the working electrode calculated based on the theoretical discharge capacity (mAh / g) per unit mass of the negative electrode active material, and perform constant current discharge until it reaches 2.0V. The remaining discharge capacity of the negative electrode is calculated by dividing the discharge capacity at this time by the area of the negative electrode that was cut out as the working electrode, and multiplying it by the charge / discharge area of the non-aqueous electrolyte energy storage element. "Charge / discharge area" refers to the area of the part where the positive electrode and negative electrode face each other and are effectively used for charging and discharging. The sum of the recorded amount of charge and the remaining discharge capacity of the negative electrode is called the "actual amount of charge of the negative electrode". "Normal use" refers to the case in which the non-aqueous electrolyte energy storage element is used by adopting the charge / discharge conditions recommended or specified for the non-aqueous electrolyte energy storage element, and, if equipment for using the non-aqueous electrolyte energy storage element is provided, it refers to the case in which the non-aqueous electrolyte energy storage element is used by applying that equipment.
[0016] The "theoretical charge amount of the negative electrode" is determined by the following procedure. For the test battery used in the measurement of the "actual charge amount of the negative electrode" described above, after performing the residual discharge described above, charging is performed as follows: The charging current is set to a current equivalent to 0.1C for the discharge capacity (mAh) of the working electrode, which is calculated based on the theoretical discharge capacity (mAh / g) per unit mass of the negative electrode active material, and constant current charging is performed until the voltage reaches 0.01V. The amount of charge at this time is divided by the area of the negative electrode that has been cut out as the working electrode, and the theoretical charge amount of the negative electrode is obtained by multiplying this by the chargeable and dischargeable area of the non-aqueous electrolyte energy storage element.
[0017] (2) In the non-aqueous electrolyte energy storage element described in (1) above, y may be 0.3000 or more in formulas (1a), (1b), and (1c).
[0018] According to the non-aqueous electrolyte energy storage element described in (2) above, the ratio of the actual amount of charge in the negative electrode to the theoretical amount of charge in the negative electrode (the charging depth of the negative electrode) is sufficiently large, which allows for an increase in energy density.
[0019] (3) In the non-aqueous electrolyte energy storage element described in (1) or (2) above, the total content of graphite and silicon-based active material relative to all negative electrode active materials contained in the negative electrode may be 90% by mass or more.
[0020] According to the non-aqueous electrolyte energy storage element described in (3) above, the negative electrode active material is mainly composed of graphite and silicon-based active material, which allows for a more substantial effect of high capacity retention after charge-discharge cycles.
[0021] (4) In the non-aqueous electrolyte energy storage element described in any one of (1) to (3) above, the negative electrode potential in the charged state during normal use is 0.050V vs. Li / Li + That's fine too.
[0022] According to the non-aqueous electrolyte energy storage element described in (4) above, the negative electrode potential in the charged state during normal use is 0.050V vs. Li / Li + As a result of the above, the accumulation of the crystalline phase in the silicon-based active material is further suppressed, leading to a higher capacity retention rate after charge-discharge cycles.
[0023] A non-aqueous electrolyte energy storage element, a method for manufacturing a non-aqueous electrolyte energy storage element, an energy storage device, and other embodiments according to one embodiment of the present invention will be described in detail below.
[0024] <Non-aqueous electrolyte energy storage element> A non-aqueous electrolyte energy storage element according to one embodiment of the present invention comprises a positive electrode, a negative electrode, a non-aqueous electrolyte, and a container for housing them. The non-aqueous electrolyte energy storage element may further include a separator interposed between the positive electrode and the negative electrode to electrically insulate them. The positive electrode, the negative electrode, and any separator typically constitute an electrode body. At least a portion of the non-aqueous electrolyte is usually present in a state of being impregnated into the electrode body. The non-aqueous electrolyte energy storage element according to one embodiment of the present invention may further include other components.
[0025] For example, the non-aqueous electrolyte energy storage element 1 shown in Figure 1, according to one embodiment of the present invention, comprises an electrode body 2, a non-aqueous electrolyte (not shown), and a rectangular parallelepiped container 3 that houses them. The non-aqueous electrolyte energy storage element 1 in Figure 1 further comprises a positive electrode lead 4, a positive electrode external terminal 5, a negative electrode lead 6, and a negative electrode external terminal 7. The positive electrode lead 4 and the negative electrode lead 6 are housed together with the electrode body 2, etc., inside the container 3. The positive electrode external terminal 5 and the negative electrode external terminal 7 are provided outside the container 3. The positive electrode constituting the electrode body 2 is electrically connected to the positive electrode external terminal 5 via the positive electrode lead 4. The negative electrode constituting the electrode body 2 is electrically connected to the negative electrode external terminal 7 via the negative electrode lead 6.
[0026] The non-aqueous electrolyte energy storage element of the present invention may also be a non-aqueous electrolyte secondary battery. The following will describe in detail the main components constituting the non-aqueous electrolyte energy storage element according to one embodiment of the present invention, focusing on the case where the non-aqueous electrolyte energy storage element is a non-aqueous electrolyte secondary battery (particularly a lithium-ion secondary battery), but this is not intended to limit the scope of application of the present invention.
[0027] Furthermore, the lower and upper limits of each numerical range described in the embodiments of the present invention can be combined in any way (however, the upper limit is greater than the lower limit).
[0028] (Positive electrode) The positive electrode comprises a positive electrode substrate and a positive electrode active material layer laminated directly to the positive electrode substrate or via an intermediate layer. Typically, the positive electrode has a portion where the positive electrode substrate is exposed. This exposed portion of the positive electrode substrate is usually connected to the positive electrode lead described above. The positive electrode may have a shape such as a sheet, plate, or strip.
[0029] The thickness of the positive electrode is set appropriately according to the application of the non-aqueous electrolyte energy storage element. The average thickness of the positive electrode may be, for example, 30 μm or more and 1,000 μm or less. The lower limit of the average thickness of the positive electrode may be 50 μm, 100 μm, or 200 μm. The upper limit of the average thickness of the positive electrode may be 500 μm, 400 μm, 300 μm, 200 μm, or 100 μm. The average thickness of the positive electrode is the average thickness of the portion in which the positive electrode active material layer is laminated directly onto the positive electrode substrate or via an intermediate layer. If both portions exist in which the positive electrode active material layer is laminated on both sides of the positive electrode substrate and portions in which the positive electrode active material layer is laminated on only one side of the positive electrode substrate, then the average thickness of the portion in which the positive electrode active material layer is laminated on both sides of the positive electrode substrate shall be used. Furthermore, in this specification, "average thickness" means the average value of the thickness measured at any five locations.
[0030] The positive electrode substrate is conductive. In this specification, "having conductivity" means that the volume resistivity is 10 -2 This means that the volume resistivity is Ω·cm or less. The volume resistivity shall be the value measured in accordance with JIS-H-0505 (1975). On the other hand, in this specification, "not conductive" or "having (electrical) insulating properties" means that the above volume resistivity is 10 7 This means it is greater than or equal to Ω·cm.
[0031] Examples of materials for the positive electrode substrate include metals such as aluminum, titanium, iron, and their alloys (stainless steel, etc.). Among these, aluminum or aluminum alloys are preferred from the viewpoint of high potential resistance, high electronic conductivity, and cost.
[0032] The positive electrode substrate has a shape such as a sheet, plate, or strip. Examples of positive electrode substrate forms include foil, vapor-deposited film, mesh, and porous material, with foil being preferred. The positive electrode substrate may also be, for example, aluminum foil or aluminum alloy foil.
[0033] The average thickness of the positive electrode substrate may be, for example, 3 μm or more and 50 μm or less. The lower limit of the average thickness of the positive electrode substrate may be 5 μm, 8 μm, 10 μm, or 15 μm. The upper limit of the average thickness of the positive electrode substrate may be 40 μm, 30 μm, 20 μm, or 15 μm.
[0034] The intermediate layer is a layer placed between the positive electrode substrate and the positive electrode active material layer. The intermediate layer includes, for example, a conductive agent and a binder. When the intermediate layer contains a conductive agent, the contact resistance between the positive electrode substrate and the positive electrode active material layer can be reduced. Examples of conductive agents and binders used in the intermediate layer are the same as those used in the positive electrode active material layer, which will be described later.
[0035] The positive electrode active material layer contains a positive electrode active material. The positive electrode active material layer may optionally contain conductive agents, binders, thickeners, fillers, and other optional components. The positive electrode active material layer may be formed from a positive electrode mixture containing the positive electrode active material and other optional components. The positive electrode active material layer may be provided on only one side of a positive electrode substrate having a shape such as a sheet, or on both sides.
[0036] For the positive electrode active material, known positive electrode active materials can be used. For lithium-ion secondary batteries, materials capable of intercalating and releasing lithium ions are typically used. Examples of positive electrode active materials include lithium transition metal composite oxides, polyanion compounds, chalcogen compounds, sulfur-based materials, and lithium oxide. One or more positive electrode active materials can be used.
[0037] Examples of transition metal elements included in lithium transition metal composite oxides include nickel, cobalt, and manganese. Lithium transition metal composite oxides may also contain typical metal elements such as aluminum. An example of a lithium transition metal composite oxide is α-NaFeO 2 Examples include lithium transition metal composite oxides having a type crystal structure and lithium transition metal composite oxides having a spinel-type crystal structure.
[0038] α-NaFeO 2 Li is a lithium transition metal composite oxide having a type crystal structure. 1+α Ma 1-α O 2Examples include those represented as follows: (Ma is a metallic element other than lithium, containing one or more transition metal elements. 0 ≤ α < 1.) It is preferable that Ma contains one or more of Ni, Co, and Mn. The total content of Ni, Co, and Mn relative to Ma ((Ni + Co + Mn) / Ma) is preferably 90 mol% or more, and more preferably 98 mol% or more.
[0039] Li is a lithium transition metal composite oxide having a spinel-type crystal structure. β Mb 2 O 4 Examples include those expressed as follows: (Mb is a metallic element other than lithium, containing one or more transition metal elements. 0 < β ≤ 1.2.) Mb preferably contains Mn. The Mn content relative to Mb (Mn / Mb) is preferably 50 mol% or more, and more preferably 80 mol% or more.
[0040] A polyanionic compound is a compound composed of a polyanion (i.e., a polyvalent oxo acid anion) and a cation. Preferably, the polyanionic compound contains lithium cations and transition metal cations. An example of a polyanionic compound is LiFePO. 4 LiMnPO 4 LiMn x Fe 1-x PO 4 (0<x<1), LiNiPO 4 LiCoPO 4 Li 3 V 2 (PO 4 ) 3 Li 2 MnSiO 4 Li 2 CoPO 4 Examples include F. The surface of the polyanionic compound particles may be coated with other materials (for example, carbon materials as described later).
[0041] Examples of chalcogen compounds include titanium disulfide, molybdenum disulfide, and molybdenum dioxide.
[0042] Examples of sulfur-based materials include elemental sulfur, metal sulfides such as lithium sulfide, organic disulfide compounds, and organic sulfur compounds such as carbon sulfide compounds.
[0043] The atoms or polyanions in these materials, which are the positive electrode active materials, may be partially substituted with atoms or anions of other elements. These materials may also be coated on the surface with other materials.
[0044] A lithium transition metal composite oxide is preferred as the positive electrode active material, and α-NaFeO 2 Lithium transition metal composite oxides having a specific crystal structure are more preferred.
[0045] The positive electrode active material is usually in particulate form. The average particle size of the positive electrode active material is preferably, for example, 0.1 μm or more and 20 μm or less. Setting the average particle size of the positive electrode active material above the lower limit facilitates the manufacture and handling of the positive electrode active material. Setting the average particle size of the positive electrode active material below the upper limit improves the electronic conductivity of the positive electrode active material layer. When a composite material of the positive electrode active material and other materials is used, the average particle size of the composite material is considered the average particle size of the positive electrode active material. "Average particle size" refers to the value (D50) at which the volume-based integrated distribution, calculated according to JIS-Z-8819-2 (2001), is 50%, based on the particle size distribution measured by laser diffraction / scattering on a dilution of particles diluted with a solvent, in accordance with JIS-Z-8825 (2013). For obtaining particles of the positive electrode active material and the negative electrode active material described later with predetermined particle sizes, known methods using, for example, pulverizers and classifiers can be employed.
[0046] The content of the positive electrode active material in the positive electrode active material layer is preferably 50% by mass or more and 99% by mass or less, more preferably 70% by mass or more and 98% by mass or less, and may also be 80% by mass or more and 95% by mass or less. By setting the content of the positive electrode active material within the above range, it is possible to achieve both high energy density and manufacturability in the positive electrode active material layer.
[0047] Conductive agents are typically components made of conductive materials. Even if the volume resistivity of a conductive agent cannot be directly measured, the volume resistivity is 10 -2Materials whose conductivity is known to be Ω·cm or less are classified as conductive agents. Examples of conductive agents include carbon materials, metals, and conductive ceramics. A carbon material is a material whose main constituent element is carbon. The main constituent element is the element with the highest mass content. For example, the carbon content in a carbon material may be 80% by mass or more, 90% by mass or more, 95% by mass, 99% by mass, or 99.9% by mass or more. It is preferable that the carbon material is a carbon material other than a non-carbonized polymer compound. Examples of carbon materials include graphite, non-graphitic carbon, and graphene-based carbon. Examples of non-graphitic carbon include carbon nanofibers, pitch-based carbon fibers, and carbon black. Examples of carbon black include furnace black, acetylene black, and Ketjen black. Examples of graphene-based carbon include graphene, carbon nanotubes (CNT), and fullerene. Conductive agents can take the form of powder or fibers. One or more conductive agents can be used. These materials may also be used as a composite conductive agent. For example, a composite material of carbon black and CNTs may be used.
[0048] The content of the conductive agent in the positive electrode active material layer is preferably 0.1% by mass or more and 10% by mass or less, more preferably 1% by mass or more and 9% by mass or less, and even more preferably 3% by mass or more and 8% by mass or less. The upper limit of the conductive agent content may be 5% by mass, 4% by mass, or 3% by mass. By setting the conductive agent content within the above range, it is possible to increase the energy density of the non-aqueous electrolyte energy storage element.
[0049] Examples of binders include water-based binders and organic solvent-based binders.
[0050] A water-based binder is a binder that dissolves or disperses in water. A water-based binder may be one in mass or more that dissolves or disperses in 100 parts by mass of water at 20°C. When forming a positive electrode active material layer using a positive electrode mixture paste in which the dispersion medium is water or a mixed solvent mainly composed of water, a water-based binder (a water-soluble or water-dispersible polymer material) can be used. Examples of water-based binders include polyethylene oxide, polypropylene oxide, polyvinyl alcohol, polyacrylic acid, polymethacrylic acid, polytetrafluoroethylene, styrene-butadiene rubber, polyethylene, polypropylene, nitrile-butadiene rubber, and cellulose.
[0051] An organic solvent-based binder is a binder that dissolves or disperses in an organic solvent (e.g., N-methylpyrrolidone). An organic solvent-based binder may be a binder that dissolves or disperses at 1 part by mass or more per 100 parts by mass of an organic solvent (e.g., N-methylpyrrolidone) at 20°C. When forming a positive electrode active material layer using a positive electrode mixture paste in which the dispersion medium is an organic solvent or a mixed solvent mainly composed of an organic solvent, an organic solvent-based binder (a polymer material having solubility or dispersibility in an organic solvent) can be used. Examples of organic solvent-based binders include polyvinylidene fluoride, copolymers of vinylidene fluoride and hexafluoropropylene, copolymers of ethylene and vinyl alcohol, polyacrylonitrile, polyphosphazene, polysiloxane, polyvinyl acetate, polymethyl methacrylate, polystyrene, polycarbonate, polyamide, polyimide, polyamideimide, crosslinked polymers of cellulose and chitosan pyrrolidone carboxylate, and derivatives of chitosan.
[0052] The binder may be a fluororesin (polytetrafluoroethylene, polyvinylidene fluoride, etc.), a polyolefin (polyethylene, polypropylene, etc.), an elastomer (ethylene propylene diene rubber, styrene butadiene rubber, fluororubber, etc.), a polysaccharide polymer (cellulose, chitosan derivatives, etc.), etc. One or more types of binders may be used.
[0053] The binder content in the positive electrode active material layer is preferably 0.1% by mass or more and 10% by mass or less, more preferably 1% by mass or more and 9% by mass or less, and even more preferably 3% by mass or more and 8% by mass or less. The upper limit of the binder content may be 5% by mass, 4% by mass, or 3% by mass. By setting the binder content within the above range, the positive electrode active material can be stably maintained. The technology disclosed herein can also be implemented in a form in which the positive electrode active material layer does not contain a binder.
[0054] Examples of thickening agents include polysaccharide polymers such as carboxymethylcellulose and methylcellulose. If the thickening agent has a functional group that reacts with lithium, etc., this functional group may be deactivated beforehand by methylation or the like. The thickening agent may also function as a binder. One or more types of thickening agents can be used. When the positive electrode active material layer contains a thickening agent, the content of the thickening agent in the positive electrode active material layer is preferably 0.1% by mass or more and 8% by mass or less, more preferably 5% by mass or less, and even more preferably 2% by mass or less. The technology disclosed herein can also be carried out in a form in which the positive electrode active material layer does not contain a thickening agent.
[0055] The filler is not particularly limited. The filler may be a component other than the positive electrode active material, conductive agent, binder, and thickener, and may be a component that is intentionally included. The filler may be included as a component that fills gaps in the positive electrode active material layer, or it may be included for other purposes. The filler may be an organic substance such as a polyolefin, or an inorganic substance such as an inorganic oxide, hydroxide, or carbonate. One or more types of fillers may be used. When the positive electrode active material layer contains a filler, the filler content in the positive electrode active material layer can be 0.1% by mass or more and 8% by mass or less, usually preferably 5% by mass or less, and more preferably 2% by mass or less. The technology disclosed herein can also be carried out in a form in which the positive electrode active material layer does not contain a filler.
[0056] The positive electrode active material layer may further contain other components besides the positive electrode active material, conductive agent, binder, thickener, and filler. These other components may include those unintentionally present in the positive electrode active material layer. Furthermore, the positive electrode active material layer may contain impurities unintentionally present as these other components, insofar as they achieve the effects of the present invention. The upper limit of the content of these other components in the positive electrode active material layer may be 10% by mass, or 5%, 2%, 1%, 0.1%, or 0.01% by mass. The upper limit of the content of unintentionally present components in the positive electrode active material layer may be 10% by mass, or 5%, 2%, 1%, 0.1%, or 0.01% by mass. The upper limit of the content of unintentionally present impurities in the positive electrode active material layer may be 10% by mass, or 5%, 2%, 1%, 0.1%, or 0.01% by mass.
[0057] The thickness of the positive electrode active material layer is set appropriately according to the type of positive electrode active material, the application of the non-aqueous electrolyte energy storage element, etc. The average thickness of one positive electrode active material layer may be, for example, 5 μm or more and 1,000 μm or less. The lower limit of the average thickness of one positive electrode active material layer may be 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, or 100 μm. The upper limit of the average thickness of one positive electrode active material layer may be 800 μm, 500 μm, 200 μm, 100 μm, 80 μm, 60 μm, or 40 μm. The mass per unit area of one positive electrode active material layer may be, for example, 4 mg / cm². 2 100mg / cm or more 2 The following is also acceptable: The lower limit of the mass per unit area of one positive electrode active material layer is 6 mg / cm². 2 , 8 mg / cm 2 or 10 mg / cm² 2 It may also be the case that the upper limit of the mass per unit area of one positive electrode active material layer is 50 mg / cm². 2 , 20 mg / cm 2 , 15 mg / cm 2 , 12 mg / cm 2 or 10 mg / cm² 2 That's fine.
[0058] The porosity of the positive electrode active material layer may be, for example, 20% or more and 50% or less. The lower limit of the porosity of the positive electrode active material layer may be 25%, 30%, or 35%. The upper limit of the porosity of the positive electrode active material layer may be 45%, 40%, or 35%. The "porosity (%)" of the positive electrode active material layer and the negative electrode active material layer described later is calculated by taking the apparent volume (volume including voids) of the positive (negative) electrode active material layer as V 1 Let V be the sum of the actual volumes of each material constituting the positive (negative) electrode active material layer. 2 In that case, (1-V 2 / V 1 It is calculated using the formula ) × 100. V is the sum of the actual volumes of each material constituting the positive (negative) electrode active material layer. 2 This can be calculated from the content of each material in the positive (negative) electrode active material layer and the true density of each material.
[0059] (Method for Manufacturing a Positive Electrode) A positive electrode can be manufactured by known methods. A positive electrode can be manufactured, for example, by applying a paste-like positive electrode mixture (positive electrode mixture paste) directly to a positive electrode substrate or via an intermediate layer, and drying it to form a positive electrode active material layer. The positive electrode mixture paste usually contains a positive electrode active material, other optional components, and a dispersion medium. After drying, the positive electrode active material layer may be pressed or otherwise subjected to other processes.
[0060] (Negative electrode) The negative electrode comprises a negative electrode substrate and a negative electrode active material layer laminated directly to the negative electrode substrate or via an intermediate layer. Typically, the negative electrode has a portion where the negative electrode substrate is exposed. This exposed portion of the negative electrode substrate is usually connected to the negative electrode lead described above. The negative electrode may have a shape such as a sheet, plate, or strip.
[0061] The thickness of the negative electrode is set appropriately according to the application of the non-aqueous electrolyte energy storage element. The average thickness of the negative electrode may be, for example, 30 μm or more and 1,000 μm or less. The lower limit of the average thickness of the negative electrode may be 50 μm, 100 μm, or 200 μm. The upper limit of the average thickness of the negative electrode may be 500 μm, 400 μm, 300 μm, 200 μm, or 100 μm. The average thickness of the negative electrode is the average thickness of the portion in which the negative electrode active material layer is laminated directly to the negative electrode substrate or via an intermediate layer. If there are portions in which the negative electrode active material layer is laminated on both sides of the negative electrode substrate and portions in which the negative electrode active material layer is laminated on only one side of the negative electrode substrate, then the average thickness of the portion in which the negative electrode active material layer is laminated on both sides of the negative electrode substrate shall be used.
[0062] The negative electrode substrate is electrically conductive. Examples of materials for the negative electrode substrate include metals such as copper, nickel, iron, and their alloys (such as stainless steel), as well as carbon materials. Among these, copper or copper alloys are preferred.
[0063] The negative electrode substrate has a shape such as a sheet, plate, or strip. Examples of negative electrode substrate forms include foil, vapor-deposited film, mesh, and porous material, with foil being preferred. The negative electrode substrate may also be, for example, copper foil or copper alloy foil.
[0064] The average thickness of the negative electrode substrate may be, for example, 2 μm or more and 35 μm or less. The lower limit of the average thickness of the negative electrode substrate may be 3 μm, 4 μm, 5 μm, or 10 μm. The upper limit of the average thickness of the negative electrode substrate may be 30 μm, 20 μm, 15 μm, or 10 μm.
[0065] The configuration of the negative electrode intermediate layer is not particularly limited; for example, it can be selected from the configurations exemplified for the positive electrode intermediate layer.
[0066] The negative electrode active material layer contains graphite and silicon-based active material. The negative electrode active material layer may optionally contain other negative electrode active materials other than graphite and silicon-based active material, conductive agents, binders, thickeners, fillers, and other optional components. The conductive agents, binders, thickeners, fillers, and other optional components can be selected from the materials exemplified above for the positive electrode. The negative electrode active material layer may be formed from a negative electrode mixture containing the negative electrode active material and other optional components. The negative electrode active material layer may be provided on only one side of a negative electrode substrate having a shape such as a sheet, or on both sides.
[0067] Graphite is a component that functions as the negative electrode active material. "Graphite" refers to the average lattice plane spacing (d) of the (002) plane, which is determined by X-ray diffraction before charging / discharging or during the discharge state. 002 This refers to carbon materials with a n-scale of 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite.
[0068] Here, the "discharge state" of the carbon material refers to a state in which sufficient lithium ions that can be absorbed and released during charging and discharging are released from the carbon material, which is the negative electrode active material. For example, in a half-cell using a negative electrode containing a carbon material as the negative electrode active material as the working electrode and a metallic lithium electrode as the counter electrode, this is a state in which the open-circuit voltage is 0.7V or higher.
[0069] The average particle size of the graphite is preferably, for example, 1 μm to 100 μm, more preferably 4 μm to 50 μm, and even more preferably 8 μm to 30 μm. Setting the average particle size of the graphite above the lower limit makes it easier to manufacture or handle the graphite. Setting the average particle size of the graphite below the upper limit improves the electronic conductivity of the negative electrode active material layer.
[0070] The lower limit of the graphite content in the negative electrode active material layer is preferably 20% by mass, more preferably 30% by mass, and may be 40%, 50%, or 60% by mass. The upper limit of the graphite content in the negative electrode active material layer is preferably 80% by mass, more preferably 70% by mass, and may be 60%, 50%, or 40% by mass.
[0071] Silicon-based active materials are components that function as negative electrode active materials and contain the element silicon. Silicon-based active materials include silicon oxide, a silicon-carbon composite, or elemental silicon. Among these, silicon oxide is preferred from the viewpoint of increasing capacity retention. Furthermore, elemental silicon is preferred from the viewpoint of increasing energy density.
[0072] For example, silicon dioxide is SiO x Examples include those expressed as (0 < x < 2, preferably 0.8 ≤ x ≤ 1.2).
[0073] A silicon-carbon composite is typically a composite in which silicon is supported within the pores of porous carbon. Silicon may also be supported on the surface of the porous carbon. Porous carbon is a carbon material that is porous. The silicon supported on the porous carbon may be elemental silicon or a silicon compound, but elemental silicon is preferred. Furthermore, the silicon-carbon composite may have silicon particles whose surfaces are coated with a carbon material. The silicon in the silicon particles may be elemental silicon or a silicon compound. The silicon content in the silicon-carbon composite is preferably 40% to 70% by mass, more preferably 45% to 65% by mass, and even more preferably 50% to 60% by mass. The silicon-carbon composite can be manufactured by known methods.
[0074] Elemental silicon is a substance consisting substantially only of the element silicon, or may consist solely of the element silicon. However, at least a portion of the surface of the elemental silicon particles may be oxidized or otherwise affected. Furthermore, trace amounts of other elements may be present. Preferably, the element silicon content in elemental silicon is, for example, 99% by mass or more in the discharged state.
[0075] The average particle size of the silicon-based active material may be, for example, 1 nm or more and 100 μm or less. The lower limit of the average particle size of the silicon-based active material may be 10 nm, 100 nm, 1 μm, 5 μm, or 10 μm. The upper limit of the average particle size of the silicon-based active material may be 30 μm, 20 μm, 10 μm, 5 μm, or 1 μm. Setting the average particle size of the silicon-based active material to be above the lower limit makes it easier to manufacture or handle the silicon-based active material. Setting the average particle size of the silicon-based active material to be below the upper limit improves the electronic conductivity of the negative electrode active material layer.
[0076] The lower limit of the silicon-based active material content in the negative electrode active material layer is preferably 20% by mass, more preferably 30% by mass, and may be 40%, 50%, or 60% by mass. The upper limit of the silicon-based active material content in the negative electrode active material layer is preferably 80% by mass, more preferably 70% by mass, and may be 60%, 50%, or 40% by mass.
[0077] The lower limit of the silicon-based active material content (x in formulas (1a) to (1c)) relative to the total of graphite and silicon-based active material in the negative electrode active material layer is 30% by mass, preferably 35% by mass, and may be 40% or 45% by mass. By setting the silicon-based active material content relative to the total of graphite and silicon-based active material to be above the above lower limit, the negative electrode potential in the charged state tends to increase. Therefore, by setting the silicon-based active material content relative to the total of graphite and silicon-based active material to be above the above lower limit, and setting the ratio of the theoretical charge amount of the negative electrode to the charge amount of the positive electrode (N / P) within an appropriate range, the negative electrode potential in the charged state can be set to 0.050 V vs. Li / Li + This can be achieved, and the capacity retention rate after charge-discharge cycles of the non-aqueous electrolyte energy storage element can be sufficiently increased. The upper limit of the silicon-based active material content relative to the total of graphite and silicon-based active material in the negative electrode active material layer is 70% by mass, preferably 60% by mass, and may be 50% by mass or 40% by mass.
[0078] The negative electrode active material layer may contain negative electrode active materials other than graphite and silicon-based active materials. Examples of other negative electrode active materials include conventionally known negative electrode active materials other than graphite and silicon-based active materials. However, the lower limit of the total content of graphite and silicon-based active materials relative to all negative electrode active materials contained in the negative electrode (or negative electrode active material layer) is preferably 90% by mass, more preferably 95% by mass, and even more preferably 99% by mass. The total content of graphite and silicon-based active materials relative to all negative electrode active materials contained in the negative electrode (or negative electrode active material layer) may be 100% by mass. By constructing the negative electrode active material substantially from graphite and silicon-based active materials alone, the negative electrode potential in the charged state is 0.050 V vs. Li / Li + This makes it easier to achieve the above, and the capacity retention rate after charge-discharge cycles of the non-aqueous electrolyte energy storage element can be sufficiently increased.
[0079] The lower limit of the total content of graphite and silicon-based active material in the negative electrode active material layer is preferably 80% by mass, more preferably 90% by mass, and even more preferably 94% by mass. The upper limit of the above total content is preferably 99% by mass, more preferably 98% by mass, and even more preferably 97% by mass. By setting the total content of graphite and silicon-based active material within the above range, it is possible to achieve both high energy density and manufacturability in the negative electrode active material layer.
[0080] The lower limit of the negative electrode active material content in the negative electrode active material layer is preferably 80% by mass, more preferably 90% by mass, and even more preferably 94% by mass. The upper limit of the above content is preferably 99% by mass, more preferably 98% by mass, and even more preferably 97% by mass. By setting the negative electrode active material content within the above range, it is possible to achieve both high energy density and manufacturability in the negative electrode active material layer.
[0081] When the negative electrode active material layer contains a conductive agent, the content of the conductive agent in the negative electrode active material layer is preferably 1% by mass or more and 10% by mass or less, and more preferably 3% by mass or more and 9% by mass or less. The content of the conductive agent in the negative electrode active material layer may be 5% by mass or less, 2% by mass or less, 1% by mass or less, 0.5% by mass or less, or 0.1% by mass or less. The technology disclosed herein can also be carried out in a form in which the negative electrode active material layer does not contain a conductive agent.
[0082] When the negative electrode active material layer contains a binder, the binder content in the negative electrode active material layer is preferably 0.1% by mass or more and 10% by mass or less, and more preferably 0.5% by mass or more and 8% by mass or less. The binder content in the negative electrode active material layer may be 5% by mass or less, or 2% by mass or less. The technology disclosed herein can also be carried out in a form in which the negative electrode active material layer does not contain a binder.
[0083] When the negative electrode active material layer contains a thickening agent, the content of the thickening agent in the negative electrode active material layer is preferably 0.1% by mass or more and 10% by mass or less, and more preferably 0.5% by mass or more and 8% by mass or less. The content of the thickening agent in the negative electrode active material layer may be 5% by mass or less, or 2% by mass or less. The technology disclosed herein can also be carried out in a form in which the negative electrode active material layer does not contain a thickening agent.
[0084] The filler in the negative electrode active material layer is a component other than the negative electrode active material, conductive agent, binder, and thickener, and may be a component that is intentionally included. The filler may be included as a component that fills gaps in the negative electrode active material layer, or it may be included for other purposes. When the negative electrode active material layer contains a filler, the filler content in the negative electrode active material layer can be 0.1% by mass or more and 8% by mass or less, usually preferably 5% by mass or less, and more preferably 2% by mass or less. The technology disclosed herein can also be carried out in a form in which the negative electrode active material layer does not contain a filler.
[0085] The lower limit of the total content of graphite, silicon-based active material, binder, and thickener in the negative electrode active material layer is preferably 90% by mass, but may be 95% by mass, 97% by mass, 98% by mass, 99% by mass, 99.5% by mass, or 99.9% by mass. The upper limit of the total content of graphite, silicon-based active material, binder, and thickener in the negative electrode active material layer may be 100% by mass.
[0086] The negative electrode active material layer may further contain other components besides the negative electrode active material (graphite, silicon-based active material, and other negative electrode active materials), conductive agent, binder, thickener, and filler. These other components may include those unintentionally present in the negative electrode active material layer. Furthermore, the negative electrode active material layer may contain impurities unintentionally present as these other components, insofar as they achieve the effects of the present invention. The upper limit of the content of these other components in the negative electrode active material layer may be 10% by mass, 5% by mass, 2% by mass, 1% by mass, 0.1% by mass, or 0.01% by mass. The upper limit of the content of unintentionally present components in the negative electrode active material layer may be 10% by mass, 5% by mass, 2% by mass, 1% by mass, 0.1% by mass, or 0.01% by mass. The upper limit for the amount of unintentionally contained impurities in the negative electrode active material layer may be 10% by mass, or it may be 5% by mass, 2% by mass, 1% by mass, 0.1% by mass, or 0.01% by mass.
[0087] The thickness of the negative electrode active material layer is set appropriately according to the type of negative electrode active material, the application of the non-aqueous electrolyte energy storage element, etc. The average thickness of one negative electrode active material layer may be, for example, 5 μm or more and 1,000 μm or less. The lower limit of the average thickness of one negative electrode active material layer may be 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, or 100 μm. The upper limit of the average thickness of one negative electrode active material layer may be 800 μm, 500 μm, 200 μm, 100 μm, 80 μm, 60 μm, or 40 μm. The mass per unit area of one negative electrode active material layer may be, for example, 2 mg / cm². 2 50mg / cm or more 2 The following is also acceptable: The lower limit of the mass per unit area of one negative electrode active material layer is 3 mg / cm². 2 , 4 mg / cm 2 , 5 mg / cm 2or 6 mg / cm 2 It may also be the case that the upper limit of the mass per unit area of one negative electrode active material layer is 30 mg / cm². 2 , 20 mg / cm 2 , 15 mg / cm 2 , 12 mg / cm 2 or 10 mg / cm² 2 That's fine.
[0088] The porosity of the negative electrode active material layer may be, for example, 30% to 70%. The lower limit of the porosity of the negative electrode active material layer may be 35%, 40%, or 45%. The upper limit of the porosity of the negative electrode active material layer may be 60%, 50%, or 40%.
[0089] (Method for Manufacturing the Negative Electrode) The negative electrode can be manufactured by known methods. The negative electrode can be manufactured, for example, in the same way as the method for manufacturing the positive electrode described above, by applying a paste-like negative electrode mixture (negative electrode mixture paste) directly to the negative electrode substrate or via an intermediate layer, and drying it to form a negative electrode active material layer. After drying, the negative electrode active material layer may be pressed or otherwise subjected to the process.
[0090] (Regarding formulas (1a) to (1c), etc.) In a non-aqueous electrolyte energy storage element according to one embodiment of the present invention, when the silicon-based active material is silicon oxide, the following formula (1a) is satisfied; when the silicon-based active material is a composite of silicon and carbon, the following formula (1b) is satisfied; and when the silicon-based active material is elemental silicon, the following formula (1c) is satisfied. y ≤ 0.0031x + 0.6035 ... (1a) y ≤ 0.0033x + 0.5629 ... (1b) y ≤ 0.0055x + 0.5247 ... (1c) In formulas (1a), (1b), and (1c), x is the content (mass%) of the silicon-based active material relative to the total of graphite and the silicon-based active material. y is the ratio of the actual charge amount of the negative electrode to the theoretical charge amount of the negative electrode (charge depth of the negative electrode).
[0091] In a non-aqueous electrolyte energy storage element according to one embodiment of the present invention, the capacity retention rate after charge-discharge cycles is high by satisfying any of the equations (1a) to (1c).
[0092] In equations (1a) to (1c), the upper limit of y (the ratio of the actual charge amount of the negative electrode to the theoretical charge amount of the negative electrode (charge depth of the negative electrode)) is preferably 0.7000, more preferably 0.6700, and even more preferably 0.6400. When y is below the above upper limit, the negative electrode potential in the charged state increases, and the capacity retention rate after charge-discharge cycles of the non-aqueous electrolyte energy storage element can be further increased.
[0093] In equations (1a) to (1c), the lower limit of y (the ratio of the actual charge amount of the negative electrode to the theoretical charge amount of the negative electrode (charge depth of the negative electrode)) is preferably 0.3000, more preferably 0.3500, even more preferably 0.4000, even more preferably 0.4500, and may also be 0.5000, 0.5500, 0.5800, or 0.6000. By having y be equal to or greater than the above lower limit, it is possible to increase the energy density of the non-aqueous electrolyte energy storage element.
[0094] The value of y (the ratio of the actual charge amount of the negative electrode to the theoretical charge amount of the negative electrode (the charge depth of the negative electrode)) can be adjusted by the type of positive electrode active material, the content of the positive electrode active material in the positive electrode active material layer, the mixing ratio of graphite and silicon-based active material, the content of the negative electrode active material in the negative electrode active material layer, the ratio of the mass per unit area of one negative electrode active material layer to the mass per unit area of one positive electrode active material layer, and so on.
[0095] In one embodiment of the present invention, the ratio of the mass per unit area of one negative electrode active material layer to the mass per unit area of one positive electrode active material layer (negative electrode active material layer / positive electrode active material layer) may be, for example, 0.25 or more and 0.45 or less, or 0.30 or more and 0.40 or less.
[0096] (Separator) A known separator can be used. Examples of separators include a separator consisting only of a substrate layer, or a separator in which an inorganic layer containing inorganic particles and a binder is formed on one or both sides of the substrate layer.
[0097] Examples of the substrate layer form of the separator include woven fabric, nonwoven fabric, and porous resin film. Among these forms, porous resin film is preferred from the viewpoint of strength, and nonwoven fabric is preferred from the viewpoint of liquid retention of non-aqueous electrolytes. The material of the substrate layer of the separator is not particularly limited as long as it has insulating properties, but resins such as polyolefins (polyethylene, polypropylene, etc.), polyimide, and aramid are preferred.
[0098] Examples of inorganic compounds constituting the inorganic particles include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, and magnesium oxide; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; sparingly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium titanate; covalent crystals such as silicon; mineral resource-derived materials such as talc, zeolite, kaolin, bentonite, and mica, or their artificial counterparts. One or more types of inorganic particles can be used. The average particle size of the inorganic particles is preferably, for example, 0.5 μm to 10 μm. The inorganic particle content in the inorganic layer is preferably 50% to 99% by mass, and more preferably 80% to 98% by mass.
[0099] Examples of binders used in the inorganic layer include those similar to those exemplified in the positive electrode active material layer.
[0100] The porosity of the separator may be, for example, 20% or more and 80% or less. The lower limit of the separator's porosity may be 30%, 40%, or 50% from the viewpoint of discharge performance, etc. The upper limit of the separator's porosity may be 70%, 60%, or 50% from the viewpoint of strength, etc. In this specification, "porosity" refers to a volume-based value and means a measurement value obtained using a mercury porosimeter.
[0101] The average thickness of the separator may be, for example, 10 μm or more and 40 μm or less, or 15 μm or more and 30 μm or less.
[0102] A polymer gel composed of a polymer and a non-aqueous electrolyte may be used as a separator. A polymer gel may also be used in combination with a porous resin film, nonwoven fabric, etc., as described above, as a separator.
[0103] (Electrode Body) As the electrode body, known structures such as wound electrode bodies and laminated electrode bodies can be used.
[0104] A wound electrode has a structure in which the positive electrode and negative electrode are wound together while being insulated. The wound electrode may be cylindrical or flattened. The electrode 2 of the non-aqueous electrolyte energy storage element 1 in Figure 1 is a flattened wound electrode. A wound electrode can be manufactured, for example, by the following procedure. First, a laminate is obtained by stacking a positive electrode, a separator, and a negative electrode, each formed in a strip shape. A wound electrode is obtained by winding this laminate.
[0105] A laminated electrode body has a structure in which one or more positive electrodes and one or more negative electrodes are stacked in an insulated state. For example, a laminated electrode body can be obtained by stacking a positive electrode, a separator, and a negative electrode, each formed in a rectangular shape.
[0106] Other electrode structures can also be used, such as those in which at least one of the positive and negative electrodes is folded in a bellows-like manner and stacked.
[0107] (Non-aqueous electrolyte) Known non-aqueous electrolytes can be used as the non-aqueous electrolyte. A non-aqueous electrolyte is a medium that carries charge transport ions (e.g., lithium ions) between the positive electrode and the negative electrode and substantially does not contain water. The water content in the non-aqueous electrolyte may be, for example, 10,000 ppm or less, 5,000 ppm or less, 500 ppm or less, 100 ppm or less, preferably 50 ppm or less, and more preferably 20 ppm or less. Examples of non-aqueous electrolytes include non-aqueous electrolyte solutions and solid electrolytes. Non-aqueous electrolyte solutions and solid electrolytes may be used in combination.
[0108] (Non-aqueous electrolyte) A non-aqueous electrolyte contains a non-aqueous solvent and an electrolyte salt dissolved in this non-aqueous solvent.
[0109] Any known non-aqueous solvent can be used. Examples of non-aqueous solvents include carbonates, esters, ethers, amides, and nitriles. Examples of carbonates include cyclic carbonates and linear carbonates. Examples of esters include carboxylic acid esters, phosphate esters, and sulfonic acid esters. As non-aqueous solvents, compounds in which some of the hydrogen atoms contained in these compounds are substituted with halogen atoms may also be used. One or more non-aqueous solvents can be used.
[0110] A cyclic carbonate is a carbonate having a ring structure containing a carbonate group (-O-C(=O)-O-). Examples of cyclic carbonates include ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, vinylethylene carbonate, chloroethylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, styrene carbonate, 1-phenylvinylene carbonate, and 1,2-diphenylvinylene carbonate. A cyclic carbonate may be a saturated cyclic carbonate such as ethylene carbonate, or an unsaturated cyclic carbonate such as vinylene carbonate. "Saturated" means not having carbon-carbon unsaturated bonds (carbon-carbon double bonds and carbon-carbon triple bonds). "Unsaturated" means having carbon-carbon unsaturated bonds. As the cyclic carbonate, saturated cyclic carbonates are preferred, and ethylene carbonates are more preferred.
[0111] A chain-like carbonate refers to a carbonate that does not have a ring structure containing a carbonate group. Examples of chain-like carbonates include diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, diphenyl carbonate, trifluoroethyl methyl carbonate, and bis(trifluoroethyl) carbonate. The chain-like carbonate may be a saturated chain-like carbonate such as dimethyl carbonate, or an unsaturated chain-like carbonate such as diphenyl carbonate. A saturated chain-like carbonate is preferred as the chain-like carbonate, and ethyl methyl carbonate is more preferred.
[0112] The non-aqueous solvent preferably contains a carbonate, and more preferably contains a cyclic carbonate and a chain carbonate. The content of the carbonate in the non-aqueous solvent is preferably 80 vol% or more and 100 vol% or less, may be 99 vol% or more and 100 vol% or less, or may be 100 vol%. By using the cyclic carbonate, dissociation of the electrolyte salt can be promoted to increase the ionic conductivity of the non-aqueous electrolytic solution. By using the chain carbonate, the viscosity of the non-aqueous electrolytic solution can be kept low. When the cyclic carbonate and the chain carbonate are used in combination, the volume ratio of the cyclic carbonate to the chain carbonate (cyclic carbonate:chain carbonate) is, for example, preferably in the range of 5:95 to 50:50.
[0113] As the electrolyte salt, a known electrolyte salt can be used. Examples of the electrolyte salt include lithium salts, sodium salts, potassium salts, magnesium salts, onium salts and the like. Among these, lithium salts are preferred. One or two or more electrolyte salts can be used.
[0114] As the lithium salt, LiPF 6 , LiPO 2 F 2 , LiBF 4 , LiClO 4 and other inorganic lithium salts, LiN(SO 2 F) 2 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 C 2 F 5 ) 2 , LiN(SO 2 CF 3 )(SO 2 C 4 F 9 ) and other imide salts, LiB(C 2 O 4 ) 2 , LiBF 2 (C 2 O 4 ), LiPF 2 (C 2 O 4 )2 Examples include lithium oxalate salts such as LiN(SO4). 2 F) 2 This also applies to inorganic lithium salts. Among these, inorganic lithium salts are preferred, and LiPF 6 This is more preferable. In some cases, an imide salt may also be preferable.
[0115] The electrolyte salt content in the non-aqueous electrolyte is 0.1 mol / dm³ at 20°C and 1 atm. 3 2.5mol / dm or more 3 The following is preferred: 0.3 mol / dm 3 2.0mol / dm or more 3 The following is more preferable: 0.5 mol / dm 3 More than 1.7mol / dm 3 The following is even more preferable: 0.7 mol / dm 3 1.5mol / dm or more 3 The following is particularly preferable. By setting the electrolyte salt content within the above range, the ionic conductivity of the non-aqueous electrolyte can be increased.
[0116] The non-aqueous electrolyte may contain additives in addition to the non-aqueous solvent and electrolyte salt. One or more types of additives may be used. When additives are used in the non-aqueous electrolyte, the additive content in the non-aqueous electrolyte is preferably 0.01% by mass or more and 10% by mass or less, more preferably 0.1% by mass or more and 7% by mass or less, even more preferably 0.2% by mass or more and 5% by mass or less, and particularly preferably 0.3% by mass or more and 3% by mass or less.
[0117] (Solid Electrolyte) The solid electrolyte can be selected from any material that has ionic conductivity, such as lithium, sodium, and calcium, and is solid at room temperature (e.g., 20°C). Examples of solid electrolytes include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, halide solid electrolytes, and polymer solid electrolytes. One or more types of solid electrolytes can be used.
[0118] (Container) The container houses the electrode body and non-aqueous electrolyte in its internal space. The container material can be a metal material such as aluminum or stainless steel, or a resin material, with metal materials being preferred from the viewpoint of strength, etc. A composite material of metal and resin materials can also be used.
[0119] The shape of the container is not particularly limited, but it can be cylindrical, rectangular (square), disc-shaped, etc. The container may also be in the form of a sheet or other shape formed from a metal-resin composite film.
[0120] (Negative electrode potential in the charged state during normal use) In a non-aqueous electrolyte energy storage element according to one embodiment of the present invention, the lower limit of the negative electrode potential in the charged state during normal use is 0.050V vs. Li / Li + Preferably, 0.055V vs. Li / Li + More preferably, 0.060V vs. Li / Li + Or 0.065V vs. Li / Li + This is even more preferable. When the negative electrode potential in the charged state during normal use is above the above lower limit, the accumulation of the crystalline phase in the silicon-based active material is further suppressed, and the capacity retention rate after charge-discharge cycles of the non-aqueous electrolyte energy storage element is further increased.
[0121] The upper limit of the negative electrode potential in the normal charging state is 0.100V vs. Li / Li + Preferably, 0.090V vs. Li / Li + More preferable is 0.080V vs. Li / Li + Or 0.075V vs. Li / Li + This is even more preferable. By keeping the negative electrode potential below the above upper limit in the charged state during normal use, it is possible to increase the discharge capacity of the non-aqueous electrolyte energy storage element, increase the energy density, and so on.
[0122] The negative electrode potential in the normal charging state can be adjusted by the mixing ratio of graphite and silicon-based active material, the amount of negative electrode active material in the negative electrode active material layer, and the ratio of the positive electrode's charge amount to the negative electrode's theoretical charge amount.
[0123] (Shape and application of non-aqueous electrolyte energy storage element) The shape of the non-aqueous electrolyte energy storage element according to one embodiment of the present invention is not particularly limited. The non-aqueous electrolyte energy storage element may be, for example, a cylindrical battery, a prismatic battery, a flat battery, a coin cell battery, a button cell battery, etc.
[0124] The applications of the non-aqueous electrolyte energy storage element according to one embodiment of the present invention are not particularly limited. The non-aqueous electrolyte energy storage element can be used, for example, as a power source for automobiles such as electric vehicles, hybrid vehicles, and plug-in hybrid vehicles, as a power source for electronic devices such as personal computers and communication terminals, and as a power storage power source.
[0125] The non-aqueous electrolyte energy storage element according to one embodiment of the present invention can be used individually or in combination. The non-aqueous electrolyte energy storage element may be used individually when the required output and required voltage are small. On the other hand, when at least one of the required output and required voltage is large, the non-aqueous electrolyte energy storage element may be used as an energy storage device in combination with other non-aqueous electrolyte energy storage elements. In an energy storage device in which multiple non-aqueous electrolyte energy storage elements are combined, at least one of the non-aqueous electrolyte energy storage elements included in the energy storage device may be a non-aqueous electrolyte energy storage element according to one embodiment of the present invention. The energy storage device will be described in detail later.
[0126] In the non-aqueous electrolyte energy storage element according to one embodiment of the present invention, the container may be restrained to maintain a certain thickness, or it may not be restrained in such a way. Alternatively, the container may be restrained to have a certain load applied to it. When the container is restrained, expansion of the container due to charge-discharge cycles, etc., may be suppressed, and a decrease in charge-discharge performance may be suppressed. When the container is restrained, the electrode body inside the container may or may not have a load applied to it. For example, the non-aqueous electrolyte energy storage element or energy storage device may be provided with a restraining member that performs such restraint.
[0127] <Method for Manufacturing a Non-Aqueous Electrolyte Energy Storage Element> A non-aqueous electrolyte energy storage element according to one embodiment of the present invention can be manufactured by a known method. The method for manufacturing the non-aqueous electrolyte energy storage element includes, for example, preparing a positive electrode, preparing a negative electrode, preparing a non-aqueous electrolyte, and housing the positive electrode, negative electrode, and non-aqueous electrolyte in a container. The manufacturing method may also include preparing a separator, and manufacturing an electrode body using the positive electrode, negative electrode, and separator. Housing the positive electrode, negative electrode, and non-aqueous electrolyte in a container may be equivalent to housing the electrode body and non-aqueous electrolyte in a container.
[0128] Preparing the positive electrode may also mean manufacturing the positive electrode. The positive electrode can be manufactured by the method described above. Preparing the negative electrode may also mean manufacturing the negative electrode. The negative electrode can be manufactured by the method described above. Preparing the non-aqueous electrolyte may also mean preparing the non-aqueous electrolyte. The non-aqueous electrolyte can be prepared, for example, by dissolving an electrolyte salt in a non-aqueous solvent. The positive electrode, negative electrode, separator, non-aqueous electrolyte, etc., may be prepared by purchase or other means.
[0129] The electrode body (or positive and negative electrode) and the non-aqueous electrolyte can be housed in a container by known methods. If the non-aqueous electrolyte is a non-aqueous electrolyte solution, for example, the electrode body (or positive and negative electrode) can be housed in the container first, and then the non-aqueous electrolyte solution can be injected through an inlet provided in the container. The inlet is sealed after the non-aqueous electrolyte solution is injected. The method for manufacturing the non-aqueous electrolyte energy storage element may further include initial charging and discharging of the assembled uncharged / discharged energy storage element.
[0130] The non-aqueous electrolyte energy storage element according to one embodiment of the present invention may be manufactured by other methods. For example, if the non-aqueous electrolyte energy storage element according to one embodiment of the present invention is an all-solid-state battery, it may be manufactured by pressing the forming materials of the positive electrode, separator, and negative electrode individually or collectively.
[0131] <Energy Storage Device> The energy storage device 30 in Figure 2 comprises a plurality of energy storage units 20. Each energy storage unit 20 comprises a plurality of electrically connected non-aqueous electrolyte energy storage elements 1. The energy storage device 30 may also include busbars (not shown) for electrically connecting the plurality of non-aqueous electrolyte energy storage elements 1, busbars (not shown) for electrically connecting the plurality of energy storage units 20, etc. The energy storage unit 20 or the energy storage device 30 may also include a condition monitoring device (not shown) for monitoring the state of one or more non-aqueous electrolyte energy storage elements 1.
[0132] <Other Embodiments> The non-aqueous electrolyte energy storage element of the present invention is not limited to the embodiments described above, and various modifications may be made without departing from the spirit of the present invention. For example, the configuration of one embodiment may be added to the configuration of another embodiment, and a part of the configuration of one embodiment may be replaced with the configuration of another embodiment or with well-known technology. Furthermore, a part of the configuration of one embodiment may be deleted. Also, well-known technology may be added to the configuration of one embodiment.
[0133] In the above embodiment, a case in which a non-aqueous electrolyte energy storage element is used as a rechargeable non-aqueous electrolyte secondary battery was described, but the type, shape, dimensions, capacity, etc. of the non-aqueous electrolyte energy storage element are arbitrary. The present invention can also be applied to various secondary batteries, electric double-layer capacitors, lithium-ion capacitors, and other capacitors.
[0134] In the above embodiment, an electrode body in which a separator is interposed between the positive electrode and the negative electrode was described, but the electrode body does not need to have a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other, with a non-conductive layer formed on the active material layer of either the positive electrode or the negative electrode. Thus, the positive electrode and the negative electrode may further have layers other than the base material, intermediate layer, and active material layer. Furthermore, the positive electrode and the negative electrode do not need to have a layered structure.
[0135] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0136] [Example 1] (Preparation of positive and negative electrodes) As the positive electrode active material, α-NaFeO 2LiNi is a lithium transition metal composite oxide having a type crystal structure. 3/5 Mn 1/5 Co 1/5 O 2 The following was prepared. A positive electrode mixture paste was made containing the above positive electrode active material, acetylene black (AB) as a conductive agent, and polyvinylidene fluoride (PVDF) as a binder in a mass ratio (based on solid content) of 93:4:3, with N-methylpyrrolidone (NMP) as the dispersion medium. This positive electrode mixture paste was applied to a strip of aluminum foil as the positive electrode substrate and dried to volatilize the NMP. After pressurizing this with a roller press to form the positive electrode active material layer, the positive electrode was obtained by vacuum drying.
[0137] As a mixture of negative electrode active material and conductive agent, a mixture of graphite, silicon oxide (SiO), a silicon-based active material, and single-walled carbon nanotubes (SWCNTs) as a conductive agent was prepared in a mass ratio of 64.97:34.98:0.05. That is, the content of silicon oxide (mass%) (x) relative to the total of graphite and silicon oxide, which are the negative electrode active materials, was set to 35 mass%. A negative electrode mixture paste was prepared by containing the above mixture (mixture of negative electrode active material and conductive agent), styrene-butadiene rubber (SBR) as a binder, and carboxymethylcellulose (CMC) as a thickener in a mass ratio of 97:2:1 (on a solid content basis), with water as the dispersion medium. This negative electrode mixture paste was applied to a strip-shaped copper foil current collector as the negative electrode base material and dried to evaporate the water. After pressurizing this with a roller press machine to form the negative electrode active material layer, the negative electrode was obtained by vacuum drying.
[0138] In the fabrication of the positive and negative electrodes, the amount of positive electrode mixture paste applied per unit area was adjusted so that the ratio of the mass per unit area of one negative electrode active material layer to the mass per unit area of one positive electrode active material layer (negative electrode active material layer / positive electrode active material layer (mass ratio)) was 0.36. According to this design, the ratio of the actual charge amount of the negative electrode to the theoretical charge amount of the negative electrode in the resulting non-aqueous electrolyte energy storage element (negative electrode charge depth) (y) is 0.6300, and the negative electrode potential in the charged state of the resulting non-aqueous electrolyte energy storage element is 0.068V vs. Li / Li + We have confirmed that this will be the case.
[0139] (Preparation of non-aqueous electrolyte) 100 parts by mass of a mixed solvent obtained by mixing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 30:35:35 is mixed with 2 parts by mass of fluoroethylene carbonate (FEC) to make a non-aqueous solvent, to which lithium hexafluorophosphate (LiPF) is added as the electrolyte salt. 6 ) 1.0 mol / dm 3 A non-aqueous electrolyte was prepared by mixing the components to achieve the specified content.
[0140] (Fabrication of Non-Aqueous Electrolyte Energy Storage Element) A microporous polyolefin membrane with an inorganic layer formed on one side was prepared as a separator. An electrode body was fabricated by laminating the positive electrode and the negative electrode via this separator. The lamination was carried out so that the inorganic layer of the separator and the positive electrode faced each other. This electrode body was placed in a container made of a metal-resin composite film, the non-aqueous electrolyte was injected into the container, and then the container was sealed by heat welding.
[0141] (Initial Charge and Discharge) The obtained non-aqueous electrolyte energy storage element was subjected to three initial charge and discharge cycles at 25°C in the following manner. In the first cycle, constant current and constant voltage charging was performed with a charging current of 0.2C, a charging termination voltage of 4.25V, and a total charging time of 7 hours, followed by a 10-minute rest period. Subsequently, constant current discharge was performed with a discharge current of 0.2C and a discharge termination voltage of 2.75V, followed by a 10-minute rest period. In the second and third cycles, constant current and constant voltage charging was performed with a charging current of 1C, a charging termination voltage of 4.25V, and a total charging time of 3 hours, followed by a 10-minute rest period. Subsequently, constant current discharge was performed with a discharge current of 1C and a discharge termination voltage of 2.75V, followed by a 10-minute rest period. The initial charge and discharge was performed by the above procedure. This obtained the non-aqueous electrolyte energy storage element of Example 1.
[0142] [Example 2, Comparative Examples 1 and 2] The silicon dioxide content (mass%) (x) relative to the total of graphite and silicon dioxide (SiO), which are the negative electrode active materials, was set as shown in Table 2. In addition, the amount of positive electrode mixture paste and negative electrode mixture paste applied per unit area was adjusted so that the ratio of the mass per unit area of one negative electrode active material layer to the mass per unit area of one positive electrode active material layer (negative electrode active material layer / positive electrode active material layer (mass ratio)) was the value shown in Table 2. In each example and comparative example, the mass per unit area of one positive electrode active material layer and the mass per unit area of one negative electrode active material layer were adjusted so that the energy density of each non-aqueous electrolyte energy storage element obtained was equal. Except for these points, the non-aqueous electrolyte energy storage elements of Example 2 and Comparative Examples 1 and 2 were obtained in the same manner as in Example 1. Furthermore, in each example and comparative example, it was confirmed that the ratio of the actual charge amount of the negative electrode to the theoretical charge amount of the negative electrode in each obtained non-aqueous electrolyte energy storage element (negative electrode charge depth) (y), and the negative electrode potential in the charged state of the obtained non-aqueous electrolyte energy storage element are the values shown in Table 2. Figure 4 shows a graph illustrating the relationship between the silicon oxide content (mass%) relative to the total of graphite and silicon oxide (x) and the ratio of the actual charge amount of the negative electrode to the theoretical charge amount of the negative electrode (negative electrode charge depth) (y) in each non-aqueous electrolyte energy storage element of the examples and comparative examples. In addition, Figure 4 also shows a straight line represented by the equation (1a) y = 0.0031x + 0.6035.
[0143] (Evaluation) Capacity retention rate in charge-discharge cycles (1) 10-100% SOC cycle The non-aqueous electrolyte energy storage elements obtained in Examples 1 and 2 and Comparative Examples 1 and 2 were subjected to charge-discharge cycle tests in the following manner. Constant current and constant voltage charging was performed in a constant temperature bath at 25°C with a charging current of 1.0C, a charging termination voltage of 4.25V, and a total charging time of 3 hours, followed by a 10-minute rest period. After that, constant current discharge was performed with a discharge current of 1.0C, followed by a 10-minute rest period. Discharge was performed until the closed-circuit voltage reached 90% of the discharge capacity of the third cycle in the initial charge-discharge cycle. This charge-discharge was performed 50 times. The percentage of the discharge capacity at the 50th cycle relative to the discharge capacity at the 1st cycle in the above charge-discharge cycle test was determined as the capacity retention rate in the 10-100% SOC cycle. The results are shown in Table 2.
[0144] (2) The charge-discharge cycle test was performed in the same manner as in "(1) 10-100% SOC cycle," except that the 25-100% SOC cycle discharge was performed until the closed-circuit voltage reached 75% of the discharge capacity of the third cycle in the initial charge-discharge cycle. The capacity retention rate in the 25-100% SOC cycle was then determined. The results are shown in Table 2.
[0145] (3) The charge-discharge cycle test was performed in the same manner as in "(1) 10-100% SOC cycle," except that the 35-100% SOC cycle discharge was performed until the closed-circuit voltage reached 65% of the discharge capacity of the third cycle in the initial charge-discharge cycle. The capacity retention rate in the 35-100% SOC cycle was then determined. The results are shown in Table 2.
[0146] In each charge-discharge cycle test, a capacity retention rate of 93.5% or higher was considered high. Table 2 also shows the negative electrode potential at the end of discharge (SOC 10%, 25%, or 35%) in each charge-discharge cycle test.
[0147]
[0148] As shown in Table 2, the non-aqueous electrolyte energy storage element of Comparative Example 1 had a low capacity retention rate in the 10-100% SOC cycle. This was due to a negative electrode potential of 0.45 V vs. Li / Li+ Discharge does not reach a potential higher than this, and the accumulation of the crystalline phase progresses within the negative electrode active material layer, just before a plateau is observed (0.25 to 0.45 V vs. Li / Li + This is thought to be because the discharge occurred in a state where the rate of potential increase accompanying the progress of the discharge reaction was large in the region of ), and the discharge ended in this region. In addition, the non-aqueous electrolyte energy storage element of Comparative Example 1 showed high capacity retention rates in the 25-100% SOC cycle and the 35-100% SOC cycle. This is because the negative electrode potential was just before a plateau was observed (0.25 to 0.45 V vs. Li / Li + This is thought to be because discharge did not occur in the region where the rate of potential increase accompanying the progress of the discharge reaction was large. In other words, it is thought that the capacity retention rate was high because the two-phase coexistence reaction in which the crystalline phase of the silicon-based compound changes to an amorphous alloy phase was unlikely to occur.
[0149] Furthermore, in the non-aqueous electrolyte energy storage element of Comparative Example 2, the capacity retention rate was high in the 10-100% SOC cycle, but the capacity retention rate was low in the 25-100% SOC cycle and the 35-100% SOC cycle. This is because, in the case of the 25-100% SOC cycle and the 35-100% SOC cycle, the negative electrode potential was 0.45V vs. Li / Li + Discharge does not reach a potential higher than this, and the accumulation of the crystalline phase progresses within the negative electrode active material layer, just before a plateau is observed (0.25 to 0.45 V vs. Li / Li + This is thought to be because the discharge occurred in a state where the potential increase accompanying the progress of the discharge reaction was large in the region of ), and the discharge ended in this region.
[0150] Thus, in each of the comparative examples of non-aqueous electrolyte energy storage elements, the capacity retention rate after the charge-discharge cycle test was low depending on the depth of discharge. In contrast, in each of the non-aqueous electrolyte energy storage elements of Examples 1 and 2, the capacity retention rate after the charge-discharge cycle test was high regardless of the depth of discharge and the negative electrode potential at the end of discharge (SOC 10%, 25%, or 35%). This is because the content of silicon-based active material (mass%) relative to the total of graphite and silicon-based active material (x) and the ratio of the theoretical amount of charge of the negative electrode to the amount of charge of the positive electrode (negative electrode charge depth) (y) were within an appropriate range, and the potential at which the negative electrode potential in the charged state changes to the crystalline phase of the silicon-based active material (0.050V vs. Li / Li) + This is thought to be because the result was above that.
[0151] This invention can be applied to non-aqueous electrolyte energy storage elements used as power sources for electronic devices such as personal computers and communication terminals, as well as for automobiles and industrial applications.
[0152] 1. Non-aqueous electrolyte energy storage element 2. Electrode body 3. Container 4. Positive electrode lead 5. Positive electrode external terminal 6. Negative electrode lead 7. Negative electrode external terminal 20. Energy storage unit 30. Energy storage device
Claims
1. A non-aqueous electrolyte energy storage element comprising a positive electrode and a negative electrode containing graphite and a silicon-based active material, wherein the content of the silicon-based active material relative to the total of the graphite and the silicon-based active material is 30% by mass or more and 70% by mass or less, the silicon-based active material is silicon oxide, a silicon-carbon composite, or elemental silicon, and if the silicon-based active material is silicon oxide, it satisfies the following formula (1a), if the silicon-based active material is a composite, it satisfies the following formula (1b), and if the silicon-based active material is elemental silicon, it satisfies the following formula (1c). y ≤ 0.0031x + 0.6035 ... (1a) y ≤ 0.0033x + 0.5629 ... (1b) y ≤ 0.0055x + 0.5247 ... (1c) (In equations (1a), (1b), and (1c), x is the content (mass %) of the silicon-based active material relative to the total amount of graphite and silicon-based active material. y is the ratio of the actual charge amount of the negative electrode to the theoretical charge amount of the negative electrode (charge depth of the negative electrode).) 2. The non-aqueous electrolyte energy storage element according to claim 1, wherein in formulas (1a), (1b), and (1c) above, y is 0.3000 or more.
3. The non-aqueous electrolyte energy storage element according to claim 1 or claim 2, wherein the total content of the graphite and silicon-based active material relative to all negative electrode active materials contained in the negative electrode is 90% by mass or more.
4. Negative electrode potential in the normal charging state is 0.050V vs. Li / Li + The non-aqueous electrolyte energy storage element according to claim 1 or claim 2.