Hybrid capacitor

The hybrid capacitor design addresses the limitations of EDLCs by using manganese dioxide, nickel hydroxide, or silver oxide as positive electrodes and activated carbon as negative electrodes, enhancing energy storage and cycle performance through suppression of water electrolysis and dendrite formation.

WO2026235187A1PCT designated stage Publication Date: 2026-11-12SUWA UNIV OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/017590
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-08
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Conventional electric double-layer capacitors (EDLCs) have limited energy storage capacity and use expensive activated carbon, while hybrid capacitors with zinc electrodes face issues like dendrite formation, hydrogen generation, and poor cycle performance due to water reductive decomposition and self-discharge.

Method used

A hybrid capacitor design using manganese dioxide, nickel hydroxide, or silver oxide as positive electrodes, activated carbon as negative electrodes, and an alkaline aqueous solution as electrolyte, which suppresses water electrolysis and dendrite formation, ensuring excellent cycle characteristics.

Benefits of technology

The hybrid capacitor achieves increased energy storage capacity, reduced self-discharge, and improved cycle stability by utilizing high-potential positive electrode materials and controlled negative electrode capacitance, eliminating concerns about dendrite formation and hydrogen generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026017590_12112026_PF_FP_ABST
    Figure JP2026017590_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides a hybrid capacitor which resists causing reductive decomposition and self-discharge of water, and does not generate dendrite during charging and discharging. The present disclosure is directed to a hybrid capacitor including a positive electrode, a separator, a negative electrode, and an electrolyte, wherein the positive electrode includes manganese dioxide and nickel hydroxide, or silver oxide, as a positive electrode active material; the electrolyte includes an electrolyte solution of an alkaline aqueous solution; the negative electrode includes a carbon material as a negative electrode active material; and the negative electrode has an electric capacitance of 1-20% of the capacitance of the positive electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Hybrid Capacitor

[0001] This invention relates to a hybrid capacitor.

[0002] Amid the spread of renewable energy and the electrification of developing countries with underdeveloped power grids, the demand for stationary battery storage systems is rapidly expanding. Unlike batteries for electric vehicles, which require lightness and compactness, safety after installation is paramount for stationary battery storage systems.

[0003] While electric double-layer capacitors (EDLCs), which physically store electricity, can maintain their energy storage capacity almost indefinitely, a challenge lies in the small amount of energy they can store. Furthermore, the activated carbon developed for EDLCs is more expensive than general-purpose activated carbon used in deodorizers and other applications, resulting in a significantly lower energy storage rate per unit of price (Wh / yen) compared to batteries.

[0004] Therefore, a hybrid capacitor using zinc as one of the electrodes has been devised. It is said that by using a hybrid structure, the amount of activated carbon used can be halved while the energy storage capacity can be increased by three to four times. In addition, since an alkaline aqueous solution is used as the electrolyte, the presence of hydrophilic groups and other impurities in the activated carbon is permitted, which has the advantage of allowing the use of inexpensive activated carbon (Patent Documents 1-3, Non-Patent Documents 1-2).

[0005] In a configuration using activated carbon as the positive electrode and zinc as the negative electrode, dendrites are formed from the zinc negative electrode during charging, which may induce an internal short circuit. Therefore, Patent Documents 2 and 3 propose solving this problem by making the separator dendritic.

[0006] Japanese Patent Publication No. 2008-66681, Japanese Patent Publication No. 2020-88164, Japanese Patent Publication No. 2020-88163

[0007] https: / / www.shokubai.co.jp / ja / wpdir / wp-content / uploads / 2022 / 10 / file2_0394.pdf (Website of Nippon Shokubai Co., Ltd.) https: / / jglobal.jst.go.jp / detail?JGLOBAL_ID=202402255732104887, Ogawa, et al., Relationship between cycle life and depth of discharge (DOD) of alkaline zinc storage batteries, Presentation at the 63rd Symposium on Batteries

[0008] However, the challenges of zinc anodes in hybrid capacitors are not limited to this. During charge-discharge cycles, the low potential of zinc makes it prone to hydrogen generation through the reductive decomposition of water, and localized galvanic reactions cause the zinc anode to self-discharge and dissolve, resulting in poor cycle performance.

[0009] Therefore, there is a need for hybrid capacitors that are less prone to water reductive decomposition and self-discharge, do not generate dendrites during charging and discharging, and have excellent cycle characteristics.

[0010] The gist of the present invention is as follows: (1) A hybrid capacitor comprising a positive electrode, a separator, a negative electrode, and an electrolyte, wherein the positive electrode comprises manganese dioxide, nickel hydroxide, or silver oxide as a positive electrode active material, the electrolyte comprises an alkaline aqueous solution, the negative electrode comprises a carbon material as a negative electrode active material, and the negative electrode has an electrical capacity of 1 to 20% of the capacity of the positive electrode. (2) The carbon material comprises 20m 2 (1) above, having a specific surface area of ​​1 / g or more. (3) The hybrid capacitor according to (1) or (2) above, wherein the carbon material is activated carbon, graphite, a naturally derived carbon material, or a combination thereof. (4) The hybrid capacitor according to (1) or (2) above, wherein the carbon material is activated carbon. (5) The hybrid capacitor according to (3) above, wherein the naturally derived carbon material is rice husk charcoal, coffee ground charcoal, rice husk briquette charcoal, rice husk briquette ash, bamboo charcoal, or a combination thereof.

[0011] According to the present invention, it is possible to provide a hybrid capacitor that is less prone to water reduction decomposition and self-discharge, does not generate dendrites during charging and discharging, and has excellent cycle characteristics.

[0012] Figure 1 is a schematic cross-sectional view of a conventional hybrid capacitor. Figure 2 is a schematic cross-sectional view of an example of this hybrid capacitor. Figure 3 is a graph of the cycle characteristics of the hybrid capacitors fabricated in the examples and comparative examples. Figure 4 is a Lagoon plot of the hybrid capacitors fabricated in Examples 1, 9, and 10, the hybrid capacitor fabricated in Comparative Example 1, and the electric double-layer capacitor (ELDC) fabricated in Comparative Example 5, in which the positive and negative electrodes are made of activated carbon. Figure 5 is a graph of the cycle characteristics of the hybrid capacitors fabricated in the examples and comparative examples. Figure 6 is a graph showing the voltage behavior of the EDLC constructed in Comparative Example 5, the hybrid capacitor fabricated in Comparative Example 1, and the hybrid capacitor fabricated in Example 1. Figure 7 is a graph showing the charge and discharge behavior of the hybrid capacitors fabricated in Examples 1, 9, and 10, respectively. Figure 8 is a graph showing the cycle characteristics of the hybrid capacitors fabricated in Examples 1, 9, and 10, the hybrid capacitor fabricated in Comparative Example 1, and the EDLC fabricated in Comparative Example 5.

[0013] This disclosure relates to a hybrid capacitor comprising a positive electrode, a separator, a negative electrode, and an electrolyte, wherein the positive electrode comprises manganese dioxide, nickel hydroxide, or silver oxide as a positive electrode active material, the electrolyte comprises an alkaline aqueous solution, the negative electrode comprises a carbon material as a negative electrode active material, and the negative electrode has an electrical capacitance of 1 to 20% of the capacity of the positive electrode.

[0014] The positive electrode active materials in this hybrid capacitor—manganese dioxide, nickel hydroxide, or silver oxide—function at a high standard electrode potential where water electrolysis does not occur, thus suppressing water electrolysis. Furthermore, unlike conventional EDLCs, the positive electrode active materials—manganese dioxide, nickel hydroxide, or silver oxide—exhibit capacity through chemical reactions rather than physical adsorption of ions, eliminating concerns about self-discharge and dendrite formation during charging and discharging. The carbon material used as the negative electrode active material also does not pose a risk of dendrite formation. Therefore, this hybrid capacitor, which contains manganese dioxide, nickel hydroxide, or silver oxide as the positive electrode active material and a carbon material as the negative electrode, is less prone to water reductive decomposition and self-discharge, and eliminates concerns about dendrite formation during charging and discharging.

[0015] This hybrid capacitor also uses an alkaline aqueous solution as the electrolyte, making it highly safe.

[0016] Figure 1 shows a schematic cross-sectional view of a conventional hybrid capacitor 100. In the conventional hybrid capacitor 100, a positive electrode 10 and a negative electrode 14 are included, and a positive electrode separator 13 and a negative electrode separator 17 are arranged between the positive electrode 10 and the negative electrode 14. The positive electrode 10 includes a positive electrode active material layer 11 and a positive electrode current collector 12, and the positive electrode active material layer 11 is formed by applying activated carbon paste on the positive electrode current collector 12. The negative electrode 14 includes a zinc layer 15, a zinc oxide layer 16, and a negative electrode current collector, and the zinc layer 15 and zinc oxide layer 16 are formed by applying metallic zinc paste and zinc oxide paste on the negative electrode current collector.

[0017] Figure 2 shows a schematic cross-sectional view of an example of the hybrid capacitor 200. The hybrid capacitor 200 includes a positive electrode 20 and a negative electrode 24, and a positive electrode separator 23 and a negative electrode separator 27 may be arranged between the positive electrode 20 and the negative electrode 24. The positive electrode 20 includes a positive electrode active material layer 21 and a positive electrode current collector 22, and the positive electrode active material layer 21 may be formed by coating the positive electrode current collector 22 with manganese dioxide paste, nickel hydroxide paste, or silver oxide paste. The negative electrode 24 includes a negative electrode active material layer 25 and a negative electrode current collector 28, and the negative electrode active material layer 25 may be formed by coating the negative electrode current collector 28 with carbon material paste.

[0018] The positive electrode active material is manganese dioxide, nickel hydroxide, or silver oxide. From the perspective of resource availability, manganese dioxide is preferred, and from the perspective of capacity, nickel hydroxide is preferred. When nickel hydroxide is used as the positive electrode active material, the potential of nickel hydroxide is relatively high, which easily increases the potential difference between the positive electrode and the negative electrode during charging, so that a hybrid capacitor exhibiting high capacity can be obtained.

[0019] Manganese dioxide, nickel hydroxide, or silver oxide preferably has a specific surface area of 10 m 2 / g or more, more preferably 20 m 2 / g or more, still more preferably 30 m 2 / g or more. When manganese dioxide, nickel hydroxide, or silver oxide has the above preferred specific surface area, a more favorable redox reaction can be achieved. The upper limit of the specific surface area of manganese dioxide, nickel hydroxide, or silver oxide is not particularly limited, but if the specific surface area is too large, it affects the workability for pulverization, so it may be 50 m 2 / g or less.

[0020] In the present hybrid capacitor, the positive electrode active material can be prepared on the oxidation side (charging side) or the discharge side, but it is preferable to determine which one is adopted as the starting active material according to material cost, stability, environmental load, and the like.

[0021] Manganese dioxide can be represented by the compositional formula MnO 2 or MnOOH. MnO 2 is on the oxidation side, that is, the charging side, and MnOOH is on the discharge side. When preparing as an active material, MnO 2 is relatively stable, easy to handle, and preferred. MnO 2 has a high oxidation number of +4, can be selected from polymorphs of α-type, β-type, γ-type, δ-type, and λ-type according to the application, and the reaction between Mn 4+ and Mn 3+ is relatively reversible with little deterioration, high stability, low cost, and low environmental load.

[0022] MnO 2 is electrolytic MnO 2 (EMD), chemical MnO2 (CMD), barnesite type MnO 2 (Layered MnO 2 ), or combinations thereof may be included. Electrolytic MnO 2 (EMD) and barnesite-type MnO 2 This is preferable because it easily yields relatively high specific capacity and good cycle characteristics.

[0023] Nickel hydroxide is Ni(OH) 2 Alternatively, it can be represented by the chemical formula NiOOH. NiOOH is the oxidizing side, i.e., the charging side, and Ni(OH) 2 This is the discharge side. When preparing it as the active material, Ni(OH) 2 Ni(OH) is relatively stable, easy to handle, and preferable. 2 When preparing Ni(OH), it can be charged in this hybrid capacitor to produce NiOOH. 2 It is a nickel hydroxide with an oxidation state of +2, and is mainly Ni 2+ and Ni 3+ A reversible oxidation-reduction reaction occurs between the two, resulting in high stability, low cost, and low environmental impact.

[0024] Silver oxide is Ag 2 It can be represented by the empirical formula of O. Ag 2 O is a silver oxide with an oxidation state of +1, and it becomes Ag upon discharge. 2 O is mainly Ag + and Ag 0 A redox reaction occurs between them, resulting in high stability, low cost, and low environmental impact.

[0025] The positive electrode may contain a conductive additive. The conductive additive can be a carbon material such as graphite.

[0026] The positive electrode current collector can be a metal foil, a metal mesh, a metal foam, or the like. Examples of metal foams include nickel foam and stainless steel foam. The material of the positive electrode current collector is not particularly limited, but preferably, it is desirable that the surface is nickel-plated.

[0027] The carbon material for the negative electrode can be activated carbon, graphite, naturally derived carbon material, or a combination thereof. Naturally derived carbon material can be rice husk charcoal, coffee grounds charcoal, rice husk briquette charcoal, rice husk briquette ash, bamboo charcoal, or a combination thereof. Since these carbon materials are relatively inexpensive, it is possible to construct a negative electrode at low cost. Activated carbon is preferred in terms of its high electrical capacity.

[0028] The carbon material for the negative electrode is preferably 20m 2 / g or more, more preferably 300m 2 / g or more, more preferably 400m 2 / g or more, more preferably 500m 2 / g or more, more preferably 750m 2 / g or more, more preferably 1000m 2 It has a specific surface area of ​​10 Wh / kg or more. By having the above-mentioned preferred specific surface area, good electrical capacitance can be ensured. In order to obtain an energy density equivalent to 10 Wh / kg or more, which is known for conventional EDLCs, the carbon material of the negative electrode is 20 m 2 It is preferable that the specific surface area is greater than or equal to / g.

[0029] The negative electrode may further contain a conductive additive. The conductive additive can be carbon black, carbon nanotubes, or the like.

[0030] The carbon material of the negative electrode preferably has electronic conductivity. The electronic conductivity of the carbon material of the negative electrode eliminates the need for a conductive additive. Furthermore, having the aforementioned preferred electronic conductivity allows this hybrid capacitor to have better output performance. More preferably, the carbon material of the negative electrode has conductivity greater than that of the electrolyte. This eliminates the potential difference between the surface and the inside of the electrode. The conductivity of the alkaline aqueous electrolyte is approximately 100 to 400 mS / cm.

[0031] The negative electrode current collector can be a metal whose surface is at least Sn, In, Bi, In, Pb, or Cu, and the metal of the core excluding the surface is not particularly limited.

[0032] In this hybrid capacitor, the negative electrode has a capacitance of 1 to 20% of that of the positive electrode. In this application, the capacitance of the negative electrode includes electric double-layer capacitance and pseudo-capacitance, but can be substantially electric double-layer capacitance. By setting the capacitance of the negative electrode to 1 to 20% of that of the positive electrode, the reversibility of the redox reaction of the positive electrode active material, such as manganese dioxide, nickel hydroxide, or silver oxide, can be maintained.

[0033] When a large volume of manganese dioxide is discharged, manganese dioxide becomes Mn 3 O 4 While irreversible phase changes or the breakdown of manganese dioxide crystals can reduce reversibility, controlling the discharge rate (utilization rate) of manganese dioxide to within 20% allows the manganese dioxide crystals to be maintained, resulting in a reversible redox reaction and good cycle characteristics.

[0034] When nickel hydroxide is overcharged, competitive oxygen evolution reactions occur at the positive electrode, causing water to decompose and potentially degrading its cycle characteristics. However, in this hybrid capacitor, by setting the negative electrode capacitance to 1-20% of the positive electrode capacitance, the utilization rate of the positive electrode active material is suppressed for the entire cell. This allows the charge rate (utilization rate) of nickel hydroxide to be controlled to within 20%, thereby suppressing the oxygen evolution reaction and achieving good cycle characteristics.

[0035] When a large volume of silver oxide is charged and discharged, changes in the electrode shape due to the dissolution and extraction reaction can occur, potentially degrading the cycle characteristics. However, by controlling the discharge rate (utilization rate) of silver oxide to within 20%, the dissolution and extraction reaction can be suppressed, resulting in good cycle characteristics.

[0036] The capacitance of the negative electrode is preferably 2 to 18%, 3 to 16%, or 4 to 14% of the capacitance of the positive electrode.

[0037] For example, manganese dioxide has a theoretical capacity of approximately 309 mAh / g. Activated carbon has a theoretical electrical capacity of approximately 40 mAh / g. Therefore, if the same mass (e.g., 1 g) of manganese dioxide and activated carbon is included in the positive and negative electrodes, the ratio of the capacity of activated carbon to the capacity of manganese dioxide will be approximately 13%. In this way, the discharge rate of manganese dioxide can be limited to the above range. Thus, this hybrid capacitor can be used as a rechargeable energy storage device.

[0038] Nickel hydroxide has a theoretical capacity of approximately 289 mAh / g. Therefore, for example, if the same mass (e.g., 1 g) of nickel hydroxide and activated carbon is included in the positive and negative electrodes, the ratio of the activated carbon's capacity to the nickel hydroxide's capacity will be approximately 14%. In this way, the discharge rate of nickel hydroxide can be limited to the above range.

[0039] Silver oxide has a theoretical capacity of approximately 231 mAh / g. Therefore, for example, if the same mass (e.g., 1 g) of silver oxide and activated carbon is included in the positive and negative electrodes, the ratio of the activated carbon's capacity to the silver oxide's capacity will be approximately 17%. In this way, the discharge rate of silver oxide can be limited to the above range.

[0040] The lower limit of the ratio of the capacitance of manganese dioxide, nickel hydroxide, or silver oxide to the capacitance of the carbon material is 1% from the perspective of the practical capacity of this hybrid capacitor.

[0041] The electrolyte contains an alkaline aqueous solution, which mainly consists of water and may contain LiOH, NaOH, KOH, or a combination thereof. The alkaline aqueous solution may also contain other solvents in addition to water.

[0042] Since this hybrid capacitor does not have concerns about dendrite formation from the negative electrode, the density of the separator does not need to be high, and various conventionally used separators can be used. The separator can be a nonwoven fabric, a non-porous membrane, a cellophane separator, etc. A non-porous membrane can prevent the diffusion of ionic species (manganese compounds, nickel compounds, or silver compounds) even if they are unintentionally generated from the positive electrode containing manganese dioxide, nickel hydroxide, or silver oxide. A cellophane separator is preferred from the viewpoint of thickness and ionic conductivity. The separator may have a Gahl value of, for example, 0.1 to 1000 sec. The separator may have a thickness of, for example, 0.1 to 500 μm.

[0043] (Example 1) (Formation of positive electrode (manganese dioxide electrode)) Specific surface area of ​​34 m² 2 / g of manganese dioxide (MnO 2 A cathode composite paste was prepared by mixing powder (HH-TF, manufactured by Tosoh Corporation), graphite (Bunny Height T-602U, manufactured by Nippon Graphite Co., Ltd.), and SBR resin (styrene-butadiene rubber) (Nalstar SR152, manufactured by Nippon A&L Co., Ltd.) in a mass ratio of 9:5:0.5.

[0044] A 3 cm square (excluding the lead-out portion) piece of foamed Ni was prepared as the positive electrode current collector. The resulting positive electrode composite paste was applied (impregnated) onto the foamed Ni to create a 3 cm square positive electrode (250 mAh).

[0045] (Formation of the negative electrode (activated carbon electrode)) Specific surface area is 1100 m² 2 A negative electrode composite was prepared by mixing activated carbon (Bellfine® AP11-0010, manufactured by AT Electrode Co., Ltd.), graphite (Bunny Height T-602U, manufactured by Nippon Graphite Co., Ltd.), and SBR resin (styrene-butadiene rubber) (Nalstar SR152, manufactured by Nippon A&L Co., Ltd.) in a mass ratio of 75.1:8.1:14.4.

[0046] A 20 μm thick Ni foil was prepared as the negative electrode current collector. The resulting negative electrode composite was coated onto the Ni foil to create a 3 cm square negative electrode (3.75 mAh). The ratio of the negative electrode's capacitance to the positive electrode's capacitance was 1.5%.

[0047] (Preparation of electrolyte) As the electrolyte for the alkaline aqueous solution, a 30 wt% KOH aqueous solution was prepared.

[0048] (Fabrication of Hybrid Capacitor) Using the fabricated positive and negative electrodes and the prepared electrolyte, a two-layer separator was constructed by placing nonwoven fabric (manufactured by Nippon Kodo Paper, VL100) on the positive and negative electrode sides, respectively, to fabricate a hybrid capacitor schematically shown in Figure 2.

[0049] (Example 2) A hybrid capacitor was fabricated in the same manner as in Example 1, except that the amount of negative electrode composite paste applied to the Ni foil was increased to form a negative electrode (25 mAh), and the ratio of the electrical capacitance of the negative electrode to the capacitance of the positive electrode was set to 10%.

[0050] (Example 3) A hybrid capacitor was fabricated in the same manner as in Example 1, except that the amount of negative electrode composite paste applied to the Ni foil was increased to form a negative electrode (50 mAh), and the ratio of the electrical capacitance of the negative electrode to the capacitance of the positive electrode was set to 20%.

[0051] (Example 4) Instead of activated carbon as the carbon material for the negative electrode, a material with a specific surface area of ​​1057 m² was used. 2 A hybrid capacitor was fabricated in the same manner as in Example 1, except that conductive carbon powder (Sony Chemical Co., Ltd.) was used in a quantity of 1 / g, and the amount of negative electrode composite paste applied to the Ni foil was increased to form a negative electrode (12.5 mAh), resulting in a ratio of 5% of the capacitance of the negative electrode to the capacitance of the positive electrode.

[0052] (Example 5) Instead of activated carbon as the carbon material for the negative electrode, a material with a specific surface area of ​​1240 m² was used. 2 A hybrid capacitor was fabricated in the same manner as in Example 1, except that bamboo charcoal weighing 1 / g was heat-treated at 800°C in a nitrogen atmosphere for 2 hours, and the amount of negative electrode composite paste applied to the Ni foil was increased to form a negative electrode (12.5 mAh), resulting in a ratio of 5% of the negative electrode's capacitance to that of the positive electrode.

[0053] (Example 6) Instead of activated carbon as the carbon material for the negative electrode, a material with a specific surface area of ​​406 m² was used. 2A hybrid capacitor was fabricated in the same manner as in Example 1, except that a gram of rice husk charcoal was heat-treated at 800°C in a nitrogen atmosphere for 2 hours, and the amount of negative electrode composite paste applied to the Ni foil was increased to form a negative electrode (12.5 mAh), resulting in a ratio of 5% of the negative electrode's capacitance to the positive electrode's capacitance.

[0054] (Example 7) Instead of activated carbon as the carbon material for the negative electrode, a material with a specific surface area of ​​388 m² was used. 2 A hybrid capacitor was fabricated in the same manner as in Example 1, except that coffee grounds charcoal weighing 1 / g was heat-treated at 800°C in a nitrogen atmosphere for 2 hours, and the amount of negative electrode composite paste applied to the Ni foil was increased to form a negative electrode (12.5 mAh), resulting in a ratio of 5% of the negative electrode's capacitance to the positive electrode's capacitance.

[0055] (Example 8) Instead of activated carbon as the carbon material for the negative electrode, a material with a specific surface area of ​​19.2 m² was used. 2 A hybrid capacitor was fabricated in the same manner as in Example 1, except that natural graphite (manufactured by Nippon Graphite Co., Ltd.) was used in a quantity of 1 / g, and the amount of negative electrode composite paste applied to the Ni foil was increased to form a negative electrode (12.5 mAh), resulting in a ratio of 5% of the negative electrode's capacitance to that of the positive electrode.

[0056] (Example 9) (Formation of positive electrode (nickel electrode)) Specific surface area of ​​30 m² 2 Nickel hydroxide (Ni(OH)) / g 2 A positive electrode composite paste was prepared by mixing powder, graphite (manufactured by Nippon Graphite Co., Ltd., Bunny Height T-602U), and SBR resin (styrene-butadiene rubber) (manufactured by Nippon A&L Co., Ltd., Nalstar SR152) in a mass ratio of 9:5:0.5.

[0057] A 3 cm square (excluding the lead-out portion) piece of foamed Ni was prepared as the positive electrode current collector. The resulting positive electrode composite paste was applied (impregnated) onto the foamed Ni to create a 3 cm square positive electrode (250 mAh).

[0058] Similar to Example 1, but with an increased amount of negative electrode composite paste applied to the Ni foil to form a negative electrode (activated carbon electrode) (12.5 mAh), the ratio of the negative electrode's capacitance to the positive electrode's capacitance was set to 5%, and the electrolyte was prepared in the same manner as in Example 1. Using the fabricated positive and negative electrodes and the prepared electrolyte, a two-layer separator was provided by placing nonwoven fabric (manufactured by Nippon Kodo Paper, VL100) on the positive and negative electrode sides, respectively, to fabricate a hybrid capacitor schematically shown in Figure 2.

[0059] (Example 10) (Formation of positive electrode (silver electrode)) Specific surface area of ​​30 m² 2 / g of silver oxide (Ag 2 O) A positive electrode composite paste was prepared by mixing powder, graphite (manufactured by Nippon Graphite Co., Ltd., Bunny Height T-602U), and SBR resin (styrene-butadiene rubber) (manufactured by Nippon A&L Co., Ltd., Nalstar SR152) in a mass ratio of 9:5:0.5.

[0060] A 3 cm square (excluding the lead-out portion) piece of foamed Ni was prepared as the positive electrode current collector. The resulting positive electrode composite paste was applied (impregnated) onto the foamed Ni to create a 3 cm square positive electrode (250 mAh).

[0061] Similar to Example 1, but with an increased amount of negative electrode composite paste applied to the Ni foil to form a negative electrode (activated carbon electrode) (12.5 mAh), the ratio of the negative electrode's capacitance to the positive electrode's capacitance was set to 5%, and the electrolyte was prepared in the same manner as in Example 1. Using the fabricated positive and negative electrodes and the prepared electrolyte, a two-layer separator was provided by placing nonwoven fabric (manufactured by Nippon Kodo Paper, VL100) on the positive and negative electrode sides, respectively, to fabricate a hybrid capacitor schematically shown in Figure 2.

[0062] (Comparative Example 1) (Formation of positive electrode (activated carbon electrode)) Specific surface area of ​​1000 m 2 A cathode composite paste was prepared by mixing activated carbon (Bellfine AP11-0010, manufactured by AT Electrode Co., Ltd.), graphite (Bunny Height T-602U, manufactured by Nippon Graphite Co., Ltd.), and SBR resin (styrene-butadiene rubber) (Nalstar SR152, manufactured by Nippon A&L Co., Ltd.) in a mass ratio of 75.1:8.1:14.4.

[0063] A 20 μm thick Ni foil was prepared as the positive electrode current collector. The resulting positive electrode composite was coated onto the Ni foil to create a 3 cm square positive electrode (4 mAh).

[0064] (Formation of the negative electrode (zinc electrode)) A zinc negative electrode paste was prepared by mixing zinc powder and SBR resin (styrene-butadiene rubber) (Nalstar SR152, manufactured by Nippon A&L Co., Ltd.) in a mass ratio of 9:1. In addition, a zinc oxide negative electrode paste was prepared by mixing zinc oxide powder and SBR resin (styrene-butadiene rubber) (Nalstar SR152, manufactured by Nippon A&L Co., Ltd.) in a mass ratio of 9:1.

[0065] A 3 cm square (excluding the lead-out portion) Zn-plated SUS mesh was prepared as the negative electrode current collector. A prepared zinc negative electrode paste was applied to the Zn-plated SUS mesh to form a 3 cm square zinc layer (420 mAh), and then a prepared zinc oxide negative electrode paste was applied on top of the zinc layer to form a 3 cm square zinc oxide layer (90 mAh), thereby creating a 3 cm square negative electrode (510 mAh).

[0066] (Preparation of electrolyte) As the electrolyte for the alkaline aqueous solution, a 30 wt% KOH aqueous solution was prepared.

[0067] (Fabrication of Hybrid Capacitor) Using the fabricated positive and negative electrodes and the prepared electrolyte, a two-layer separator consisting of nonwoven fabric (manufactured by Nippon Kodo Paper, VL100) on the positive electrode side and cellophane separator (manufactured by Futamura Chemical, P5-1) on the negative electrode side was placed to fabricate a hybrid capacitor schematically shown in Figure 1.

[0068] (Comparative Example 2) A hybrid capacitor was fabricated in the same manner as in Example 1, except that the amount of positive electrode composite paste applied to foamed Ni was reduced to form the positive electrode (25 mAh), and the ratio of the negative electrode's capacitance to the positive electrode's capacitance was set to 25%.

[0069] (Comparative Example 3) A hybrid capacitor was fabricated in the same manner as in Example 1, except that the amount of positive electrode composite paste applied to foamed Ni was reduced to form the positive electrode (25 mAh), and the ratio of the negative electrode's capacitance to the positive electrode's capacitance was set to 30%.

[0070] (Comparative Example 4) A hybrid capacitor was fabricated in the same manner as in Example 1, except that the amount of positive electrode composite paste applied to foamed Ni was reduced to form the positive electrode (25 mAh), and the ratio of the negative electrode's capacitance to the positive electrode's capacitance was set to 50%.

[0071] (Comparative Example 5 (Preparation of EDLC)) Specific surface area of ​​1000 m² 2 A negative electrode composite paste was prepared by mixing activated carbon (Bellfine AP11-0010, manufactured by AT Electrode Co., Ltd.), graphite (Bunny Height T-602U, manufactured by Nippon Graphite Co., Ltd.), and SBR resin (styrene-butadiene rubber) (Nalstar SR152, manufactured by Nippon A&L Co., Ltd.) in a mass ratio of 75.1:8.1:14.4.

[0072] A 20 μm thick Ni foil was prepared as the negative electrode current collector. The resulting negative electrode mixture was coated onto the Ni foil to create a 3 cm square negative electrode (4 mAh).

[0073] Similar to Example 1, a positive electrode (activated carbon electrode) was formed and an electrolyte was prepared. Using the prepared positive and negative electrodes and the prepared electrolyte, a two-layer separator was created by placing nonwoven fabric (manufactured by Nippon Kodo Paper, VL100) on the positive and negative electrode sides, respectively, thereby fabricating an electric double-layer capacitor (EDLC) in which the positive and negative electrodes are made of activated carbon.

[0074] Table 1 shows the measured electrical double-layer capacitance, energy storage capacity, and energy density for the negative electrode active material used in each example. Energy density was calculated as: capacitance at one electrode × operating voltage of 1.5V ÷ 2 (with two electrodes as the denominator). Larger specific surface area resulted in greater electrical double-layer capacitance and higher energy density.

[0075]

[0076] Figure 3 shows graphs of the cycle characteristics of the hybrid capacitors fabricated in Example 1 and Comparative Example 1. The measurement conditions for the cycle characteristics are shown in Table 2.

[0077]

[0078] The hybrid capacitor fabricated in Comparative Example 1 began to lose capacitance retention after about 1000 cycles, and its capacitance retention rate dropped to about 60% after 4000 cycles. This was because the zinc in the negative electrode dissolved due to self-discharge by the 1000th cycle.

[0079] The hybrid capacitor fabricated in Example 1 showed a capacitance retention rate of over 90% after 4000 cycles.

[0080] Figure 4 shows the Lagoon plots for the hybrid capacitors fabricated in Examples 1, 9, and 10, the hybrid capacitor fabricated in Comparative Example 1, and the electric double-layer capacitor (ELDC) fabricated in Comparative Example 5, in which the positive and negative electrodes are made of activated carbon. The discharge capacity was measured with a fixed discharge power, and the Lagoon plots were obtained by plotting the discharge capacity for each discharge power.

[0081] In the Lagone plot, the horizontal axis represents power density and the vertical axis represents energy density. The energy density and power density of the hybrid capacitors fabricated in Examples 1, 9, and 10, and Comparative Example 1, were normalized by the activated carbon mass. The energy density and power density of the EDLC fabricated in Comparative Example 5 were normalized by the activated carbon mass of the positive electrode. The measurement conditions (power performance) for the Lagone plots are shown in Table 3.

[0082]

[0083] The hybrid capacitors fabricated in Examples 1, 9, and 10 showed significantly higher energy densities compared to the EDLC fabricated in Comparative Example 5, and also showed higher energy densities compared to the hybrid capacitor fabricated in Comparative Example 1.

[0084] Figure 5 shows graphs of the cycle characteristics of the hybrid capacitors fabricated in Examples 2 and 3 and Comparative Examples 2 to 4. The measurement conditions for the cycle characteristics were the same as in Table 2, except that the number of cycles was limited to 100.

[0085] The hybrid capacitors fabricated in Examples 2 and 3, where the ratio of negative electrode capacitance to positive electrode capacitance was 10% and 20%, respectively, maintained their capacitance and operated well up to 100 cycles. On the other hand, the hybrid capacitors fabricated in Comparative Examples 2 to 4, where the ratio of negative electrode capacitance to positive electrode capacitance was 25%, 30%, and 50%, respectively, experienced a rapid decrease in capacitance by 100 cycles.

[0086] Hybrid capacitors fabricated in Examples 4-8 using conductive carbon powder, bamboo charcoal, rice husk charcoal, coffee grounds charcoal, and natural graphite as the negative electrode carbon material also exhibited good cycle characteristics similar to those in Example 1.

[0087] Figure 6 shows the voltage behavior of the EDLC constructed in Comparative Example 5, the hybrid capacitor fabricated in Comparative Example 1, and the hybrid capacitor fabricated in Example 1. Figure 6 evaluates the voltage behavior with respect to time when charged with a constant current. The horizontal axis of Figure 6 represents time (seconds), and the vertical axis represents the potentials of the positive and negative electrodes, respectively.

[0088] During the charging of the EDLC, charge accumulated on both the positive and negative electrodes, causing the potential of the positive electrode to rise and the potential of the negative electrode to fall, resulting in a potential difference between the two electrodes. After charging and a rest period, the potentials of both the positive and negative electrodes returned to 0V upon discharge.

[0089] In the hybrid capacitor fabricated in Comparative Example 1, the potential of the negative electrode, made of zinc, remained almost unchanged during charging and discharging, while the potential of the positive electrode, made of activated carbon, increased during charging and decreased during discharging. Due to the low potential of zinc, when attempting to discharge to a state where the activated carbon of the positive electrode and the zinc of the negative electrode were short-circuited, i.e., a potential difference of 0V, hydrogen generation occurred because the hydrogenation voltage of the activated carbon was low, so the discharge was stopped at a potential difference of 0.2V.

[0090] In the hybrid capacitor fabricated in Example 1, an electrochemical reaction occurs on the positive electrode side, which is made of manganese dioxide. As a result, the potential of the positive electrode hardly changes during charging and discharging, while the potential of the negative electrode, which is made of activated carbon, decreases during charging, rises after a rest period, and returns to a potential difference of 0V during discharge. Since carbon and manganese do not produce side reactions even when at the same potential, it was possible to discharge down to a potential difference of 0V. The upper and lower limits of charging and discharging shown in Figure 6 may vary depending on the reference electrode, but for the negative electrode, it is limited by whether or not hydrogen is generated, and for the positive electrode, it is limited by whether or not oxygen is generated. The hybrid capacitor fabricated in Example 1 has a wide and excellent upper and lower limit of charging and discharging.

[0091] Figure 7 shows the charge and discharge behavior of the hybrid capacitors fabricated in Example 1, Example 9, and Example 10, respectively. In Figure 7, the horizontal axis represents critical capacitance, and the vertical axis represents voltage. The hybrid capacitors fabricated in Example 1, Example 9, and Example 10 all showed good charge and discharge behavior.

[0092] Table 4 shows the charging voltage, discharging voltage, and discharge capacity of the hybrid capacitors fabricated in Examples 1, 9, and 10, the hybrid capacitor fabricated in Comparative Example 1, and the EDLC fabricated in Comparative Example 5. All of the hybrid capacitors fabricated in the examples showed good discharge capacity.

[0093] Figure 8 shows the cycle characteristics of the hybrid capacitors fabricated in Example 1, Example 9, and Example 10, the hybrid capacitor fabricated in Comparative Example 1, and the EDLC fabricated in Comparative Example 5.

[0094] The hybrid capacitor fabricated in Comparative Example 1 had low stability of the zinc anode, and its capacitance decreased over time. The EDLC fabricated in Comparative Example 5 had low capacitance from the start. The hybrid capacitors fabricated in Examples 1, 9, and 10 showed high capacitance and good cycle characteristics.

[0095] 100 Conventional hybrid capacitor 10 Positive electrode 11 Positive electrode active material layer 12 Positive electrode current collector 13 Positive electrode side separator 14 Negative electrode 15 Zinc layer 16 Zinc oxide layer 17 Negative electrode side separator 18 Negative electrode current collector 200 This hybrid capacitor 20 Positive electrode 21 Positive electrode active material layer 22 Positive electrode current collector 23 Positive electrode side separator 24 Negative electrode 25 Negative electrode active material layer 27 Negative electrode side separator 28 Negative electrode current collector

Claims

1. A hybrid capacitor comprising a positive electrode, a separator, a negative electrode, and an electrolyte, wherein the positive electrode comprises manganese dioxide, nickel hydroxide, or silver oxide as a positive electrode active material, the electrolyte comprises an alkaline aqueous solution, the negative electrode comprises a carbon material as a negative electrode active material, and the negative electrode has an electrical capacitance of 1 to 20% of the capacity of the positive electrode.

2. The carbon material is 20m 2 The hybrid capacitor according to claim 1, having a specific surface area of ​​1 / g or more.

3. The hybrid capacitor according to claim 1 or 2, wherein the carbon material is activated carbon, graphite, a naturally derived carbon material, or a combination thereof.

4. The hybrid capacitor according to claim 1 or 2, wherein the carbon material is activated carbon.

5. The hybrid capacitor according to claim 3, wherein the naturally derived carbon material is rice husk charcoal, coffee grounds charcoal, rice husk briquette charcoal, rice husk briquette ash, bamboo charcoal, or a combination thereof.