Novel aqueous zinc ion battery electrolyte additive and application thereof

By using silicon-containing organic compound additives in zinc-ion batteries to form a zinc-philic layer, the problems of zinc surface integrity and dendrites are solved, the cycle performance and capacity retention rate of zinc-ion batteries are improved, and more stable battery operation is achieved.

CN118800980AInactive Publication Date: 2024-10-18GUANGXI UNIV

Patent Information

Application Number
CN202410291957.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-14
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing zinc-ion batteries struggle to maintain the integrity of the zinc surface under stringent conditions, leading to damage to the protective layer, corrosion risk and dendrite formation, reducing battery performance.

Method used

Organic compounds containing silicon, such as tetramethyl orthosilicate, tetraethyl orthosilicate, and tetrapropyl orthosilicate, are used as electrolyte additives for aqueous zinc ion batteries to form a zinc-philic layer containing silicon oxide compounds to inhibit zinc dendrites. Side reactions caused by crystals and water reduce the activity of free water in the electrolyte.

Benefits of technology

Significantly improves the cycle performance and capacity retention rate of zinc-ion batteries, ensuring stable battery performance at high depths of discharge and long-term use, and extending the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004741016660000011
    Figure HDA0004741016660000011
  • Figure HDA0004741016660000012
    Figure HDA0004741016660000012
  • Figure HDA0004741016660000013
    Figure HDA0004741016660000013
Patent Text Reader

Abstract

The invention discloses a novel aqueous zinc ion battery electrolyte additive, namely a silicon-containing organic compound, such as tetramethyl orthosilicate, tetraethyl orthosilicate, tetrapropyl orthosilicate and tetrabutyl orthosilicate. As the surface of the additive has rich oxygen-containing groups, the electrolyte additive provided by the invention is beneficial to in-situ formation of a zinc-loving layer containing a silicon-oxygen compound on a zinc negative electrode, and promotes uniform deposition of zinc ions on the surface of the zinc negative electrode, so that formation and overgrowth of zinc dendrites are effectively inhibited; and moreover, the solvation chemistry of Zn < 2 + > can be changed, the side reaction caused by water is inhibited, and the activity of free water in the electrolyte is reduced. Accordingly, the inventor also develops a corresponding modified aqueous zinc ion battery electrolyte and an aqueous zinc ion battery. Tests show that by using the aqueous zinc ion battery electrolyte additive provided by the invention, the cycle performance and the capacity retention ratio of an aqueous zinc ion battery can be remarkably improved, and a promising method is provided for preparing a high-performance aqueous zinc metal battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aqueous zinc ion batteries, and in particular relates to a novel aqueous zinc ion battery electrolyte additive and application thereof. Background Art

[0002] Compared with aqueous battery systems, current lithium-ion batteries using organic electrolytes face great challenges, including limited lithium resources, safety issues, and environmental concerns. In recent years, rechargeable aqueous zinc-ion batteries (ZIBs) have attracted extensive attention as a promising alternative to lithium-ion batteries due to the attractive advantages of zinc metal anodes and aqueous electrolytes.

[0003] Electrolyte optimization is a simple and convenient way to adjust the Zn electrode / electrolyte interface chemistry. By introducing organic solvents with high donor numbers or high acceptor numbers, the Zn 2+ The coordinated environment reduces the water activity, thereby alleviating the H2O-induced side reactions, thereby improving the rechargeability of the Zn anode. However, the high viscosity and high cost of large volume fraction organic solvents hinder the further development of ZIBs. More importantly, for practical Zn anodes, a key challenge remains unresolved, which is how to maintain the integrity of the Zn surface under stringent conditions to ensure long-term cycling performance after the protective layer is damaged. The rupture of the protective layer will re-expose the fresh Zn anode to the aqueous solution with potential corrosion risks, which may further induce dendrite formation and degrade the battery performance. Therefore, a feasible design strategy for ultrathin in-situ artificial interfacial layers with dynamic repair capabilities for Zn surface cracks and modulated electrolyte environment is a great need for durable and reliable aqueous Zn-ion batteries. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a novel aqueous zinc ion battery electrolyte additive with excellent effect and application thereof.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] Organic compounds containing silicon are used as electrolyte additives for aqueous zinc ion batteries. The additives can effectively inhibit zinc dendrites, inhibit side reactions caused by water, and reduce the activity of free water in the electrolyte.

[0007] A novel aqueous zinc ion battery electrolyte additive is an organic compound containing silicon; the organic compound containing silicon is one of tetramethyl orthosilicate, tetraethyl orthosilicate, tetrapropyl orthosilicate, and tetrabutyl orthosilicate, or a combination thereof.

[0008] The modified aqueous zinc ion battery electrolyte comprises a soluble zinc salt and the above additives.

[0009] The concentration of soluble zinc salt is 1-3 mol / L, and the concentration of additive is 0.01-0.05 mol / L.

[0010] The soluble zinc salt is one of zinc sulfate, zinc chloride, zinc bromide, zinc nitrate, zinc acetate, and zinc trifluoromethanesulfonate, or a combination thereof.

[0011] The soluble zinc salt is zinc sulfate with a concentration of 2 mol / L; the additive is tetraethyl orthosilicate with a concentration of 0.02 mol / L.

[0012] Application of the above-mentioned novel aqueous zinc ion battery electrolyte additive or modified aqueous zinc ion battery electrolyte in the preparation of aqueous zinc ion batteries.

[0013] The aqueous zinc ion battery is prepared by using the modified aqueous zinc ion battery electrolyte as the electrolyte, a zinc metal material as the negative electrode, an intercalation compound as the positive electrode, and a diaphragm to separate the positive electrode and the negative electrode.

[0014] The zinc metal material is one of zinc plate, zinc sheet, zinc foil or three-dimensional zinc foam; the intercalation compound is one of manganese series material, vanadium series material and Prussian blue analogue; the diaphragm is one of glass fiber, qualitative filter paper or polypropylene fiber diaphragm.

[0015] The manganese-based material is MnO2, the vanadium-based material is V2O5, and the Prussian blue analogue is Fe4[Fe(CN)6]3.

[0016] In response to the problems existing in current aqueous zinc-ion batteries, the inventors have developed a new type of aqueous zinc-ion battery electrolyte additive - organic compounds containing silicon, such as tetramethyl orthosilicate, tetraethyl orthosilicate, tetrapropyl orthosilicate, and tetrabutyl orthosilicate. Since these additives have abundant oxygen-containing groups on their surfaces, the provided electrolyte additives are conducive to the in-situ formation of a zinc-philic layer containing silicon-oxygen compounds at the zinc negative electrode, promoting the uniform deposition of zinc ions on the surface of the zinc negative electrode, thereby effectively inhibiting the formation and excessive growth of zinc dendrites; and can change the Zn 2+ The solvation chemistry of the present invention inhibits the side reactions caused by water and reduces the activity of free water in the electrolyte. In addition, the electrolyte additive is stable in nature during use, which helps to develop an aqueous zinc ion battery with excellent performance, safety and stability. Based on this, the inventors have also developed a corresponding modified aqueous zinc ion battery electrolyte and an aqueous zinc ion battery. The present invention is assembled into a Zn||Zn symmetrical battery, and the cycle stability test shows that at 5mA·cm- 2 The battery can be stably cycled for ≥1200 h at a current density of 10000 h and can last for 830 h at a high depth of discharge (DOD) of 80%. The battery is assembled into a Zn||V2O5 full battery using an ultra-thin zinc sheet (10 μm) at 1 Ag. -1, under the conditions of low N / P (2.0) and low E / C (20 μL), the capacity retention rate is still 93.15% after 1000 cycles. Therefore, the use of the aqueous zinc ion battery electrolyte additive provided by the present invention can significantly improve the cycle performance and capacity retention rate of aqueous zinc ion batteries, and provides a promising method for preparing high-performance aqueous zinc metal batteries and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The scanning electron microscope characterization diagram of zinc electrodeposition, in which: a is the Zn anode of Example 1 at 0.5 mA cm -2 a is the scanning electron microscopy characterization of the deposition after the lower cycle, b is the scanning electron microscopy characterization of comparative example 1.

[0018] Figure 2 It is the X-ray diffraction characterization diagram of the cycle zinc anode using Example 1 and Comparative Example 1.

[0019] Figure 3 This is a graph showing the results of testing H2 evolution during zinc stripping / plating using the DEMS in Example 2.

[0020] Figure 4 It is the long cycle polarization curve of the Zn||Zn symmetric battery of the aqueous zinc ion battery of the test electrolyte of Example 3 and the reference electrolyte of Comparative Example 2.

[0021] Figure 5 It is a long cycle performance diagram of the Zn||V2O5 battery of the aqueous zinc ion battery prepared by the test electrolyte of Example 4 and the reference electrolyte of Comparative Example 3. DETAILED DESCRIPTION

[0022] Example 1

[0023] Tetraethyl orthosilicate (TEOS) and 2 mol / L zinc sulfate solution were used to prepare a composite electrolyte for zinc electrodeposition to verify the effect of tetraethyl orthosilicate on inducing uniform deposition of zinc ions.

[0024] The operation is as follows: at room temperature, 14.378 g of zinc sulfate heptahydrate and 0.105 g of tetraethyl orthosilicate are added to 25 ml of deionized water, and ultrasonicated for 20 minutes to completely disperse them to prepare 25 ml of an electrolyte containing 2 mol / L zinc sulfate and 0.02 mol / L tetraethyl orthosilicate.

[0025] The assembled symmetric cell was tested at 0.5 mA cm -2 The deposition morphology after cycling at a current density of Figure 1As shown in (a), due to the presence of the formed SEI protective layer (TEOS can form a zinc-philic protective SEI layer in situ, guide Zn uniform nucleation and inhibit the occurrence of side reactions), zinc is deposited in a layered stacking morphology parallel to the basal plane without obvious dendrites;

[0026] Figure 2 X-ray diffraction characterization of zinc deposition shows that all characteristic peaks match well with the standard phase of metallic zinc (PDF#65-3358), and the Zn(002) peak intensity is the highest, indicating that in this embodiment, the main crystal plane of zinc ion deposition is the Zn(002) crystal plane parallel to the basal plane, and no by-product peaks are observed.

[0027] Comparative Example 1

[0028] At room temperature, 14.378 g of zinc sulfate heptahydrate was added to 25 ml of deionized water and ultrasonicated for 20 min to completely disperse it, thereby preparing 25 ml of an electrolyte solution containing 2 mol / L zinc sulfate.

[0029] The assembled symmetric cell was tested at 0.5 mA cm -2 The deposition morphology after cycling at a current density of Figure 1 As shown in (b), the Zn deposition structure is loose with many disordered clusters and corrosion pits, which may aggravate the corrosion reaction and the accumulation of by-products, eventually leading to battery failure.

[0030] Figure 2 X-ray diffraction characterization of zinc deposition shows that all characteristic peaks match well with the standard phase of metallic zinc (PDF#65-3358), and the Zn(101) peak intensity is the highest, indicating that in this embodiment, the main crystal plane of zinc ion deposition is the Zn(101) crystal plane perpendicular to the basal plane, and the formation of by-product (Zn(OH)2)3(ZnSO4)(H2O)5 is observed.

[0031] Example 2

[0032] In situ differential electrochemical mass spectrometry (DEMS) was used to study the hydrogen production of the aqueous zinc ion batteries prepared in Example 1 and Comparative Example 2.

[0033] Procedure: Before testing, use pure He to release gas for 24 hours (0.5 mL min -1 ) to achieve ultra-high vacuum. -2 Current cycling 5mAh cm -2 A symmetrical cell was used and DEMS was used to analyze the generated gas species (H2 was m / z=2).

[0034] Figure 3The hydrogen evolution during the zinc deposition and stripping process is shown in Figure 2. The hydrogen production suddenly increases during the first discharge process in the basic zinc sulfate electrolyte, and then during the entire 10 h operation, the hydrogen production intensity is much lower in the battery assembled with the electrolyte containing tetraethyl orthosilicate additive.

[0035] Example 3

[0036] Tetraethyl orthosilicate was used as an electrolyte additive for aqueous zinc-ion batteries to prepare Zn||Zn symmetric batteries, and the effect of the additive on improving the service life of zinc electrodes was verified.

[0037] The operation is as follows: at room temperature, 14.378 g of zinc sulfate heptahydrate is added to 25 ml of deionized water and ultrasonicated for 20 minutes to make it completely dispersed, and 25 ml of an electrolyte containing 2 mol / L zinc sulfate and 0.02 mol / L tetraethyl orthosilicate is prepared; zinc foil is used as the positive and negative electrodes, and glass fiber is used as a separator. 120 μL of the above-obtained electrolyte is taken to assemble a CR2032 type button-type symmetrical battery, and a cyclic charge and discharge test is carried out on a Xinwei battery test system, and the working current density is 5 mA cm -2 , with a surface capacity of 1 mAh cm -2 .

[0038] Comparative Example 2

[0039] At room temperature, 11.5 g of zinc sulfate heptahydrate was added to 5 ml of deionized water and ultrasonicated for 20 min to completely disperse it, thereby preparing 25 ml of an electrolyte solution containing 2 mol / L zinc sulfate.

[0040] Using zinc foil as positive and negative electrodes and glass fiber as separator, 120 μL of the above electrolyte was assembled into a CR2032 button-type symmetrical battery, and the cyclic charge and discharge test was carried out on the Xinwei battery test system. The current density was 5 mA cm -2 , with a surface capacity of 1 mAh cm -2 .

[0041] The test results are as follows Figure 4 As shown, the working time of Example 3 using tetraethyl orthosilicate electrolyte additive is 1200h, while Comparative Example 2 has a short circuit after 50h of circulation. The greatly increased working time of Example 3 is due to the SEI layer formed by tetraethyl orthosilicate on the surface of the zinc negative electrode, which improves the zinc deposition / stripping reaction kinetics and thus inhibits the growth of zinc dendrites.

[0042] Example 4

[0043] Aqueous zinc ion batteries were prepared using tetraethyl orthosilicate as an electrolyte additive for aqueous zinc ion batteries, and the effect of tetraethyl orthosilicate electrolyte additive on improving the capacity retention rate and service life of aqueous zinc ion full batteries was tested.

[0044] The operation is as follows: at room temperature, add 14.378g zinc sulfate heptahydrate and 0.105g tetraethyl orthosilicate to 25ml deionized water, ultrasonicate for 20min to make it completely dispersed, and prepare 25ml electrolyte containing 2mol / L zinc sulfate and 0.02mol / L tetraethyl orthosilicate; V2O5 positive electrode preparation process: dissolve vanadium oxide (V2O5, Macklin, 99%, 0.3g) in 10mL 2M sodium chloride (NaCl) aqueous solution, stir continuously for 72h, wash the orange-red gel formed with deionized water and ethanol several times in sequence. Then dry it in a vacuum oven at 80℃ for 12 hours, take it out after cooling, filter the solution, dry it, grind it and set it aside. Take 80 mg of the V2O5 prepared above, mix it with Super P and polyvinylidene fluoride in a mass ratio of 7:2:1, grind it in an agate mortar for 30 minutes, add N-methylpyrrolidone, stir for 12 hours, and then evenly apply it on the surface of titanium foil with a scraper. After it is completely dried, slice it for later use;

[0045] The V2O5 cathode material prepared above was used as the cathode, zinc foil as the anode, and glass fiber as the separator. 120 μL of the electrolyte was taken to assemble a CR2032 aqueous zinc ion button-type full battery. The cyclic charge and discharge test was carried out in the Xinwei battery test system with a current density of 1A. -1 .

[0046] Comparative Example 3

[0047] At room temperature, 14.378g of zinc sulfate heptahydrate was added to 25ml of deionized water and ultrasonicated for 20min to completely disperse it, and 25ml of electrolyte containing 2mol / L zinc sulfate was prepared. 120μL of the electrolyte was taken, and the V2O5 positive electrode material prepared in the same way as in Example 4 was used. Zinc foil was used as the negative electrode and glass fiber was used as the separator to assemble the CR2032 type aqueous zinc ion button-type full battery for cyclic charge and discharge test in the Xinwei battery test system. The current density was 1Ag. -1 .

[0048] Test results such as Figure 5 As shown, Example 4 uses ultra-thin zinc sheets (10 μm) at 1 Ag -1 , the discharge capacity under the conditions of low N / P (2.0) and low E / C (20μL) can maintain 93.15% after 1000 cycles, while the discharge capacity of comparative example 3 decays to death after about 150 cycles. This shows that during the cycle process, the addition of tetraethyl orthosilicate can reduce the formation of zinc dendrites, reduce capacity loss, and improve the reversibility of zinc deposition / stripping reaction.

Claims

1. An organic compound containing silicon is used as an electrolyte additive for aqueous zinc ion batteries, characterized in that The additive can effectively inhibit zinc dendrites, inhibit side reactions caused by water, and reduce the activity of free water in the electrolyte.

2. A novel aqueous zinc ion battery electrolyte additive, characterized in that It is an organic compound containing silicon; the organic compound containing silicon is one of tetramethyl orthosilicate, tetraethyl orthosilicate, tetrapropyl orthosilicate, tetrabutyl orthosilicate or a combination thereof.

3. A modified aqueous zinc ion battery electrolyte, characterized in that The invention comprises a soluble zinc salt and the additive according to claim 2.

4. The modified aqueous zinc ion battery electrolyte according to claim 3, characterized in that: The concentration of the soluble zinc salt is 1-3 mol / L, and the concentration of the additive is 0.01-0.05 mol / L.

5. The modified aqueous zinc ion battery electrolyte according to claim 4, characterized in that: The soluble zinc salt is one of zinc sulfate, zinc chloride, zinc bromide, zinc nitrate, zinc acetate, and zinc trifluoromethanesulfonate, or a combination thereof.

6. The modified aqueous zinc ion battery electrolyte according to claim 4, characterized in that: The soluble zinc salt is zinc sulfate with a concentration of 2 mol / L; and the additive is tetraethyl orthosilicate with a concentration of 0.02 mol / L.

7. Use of the novel aqueous zinc ion battery electrolyte additive according to claim 2 or the modified aqueous zinc ion battery electrolyte according to claim 3 in the preparation of aqueous zinc ion batteries.

8. An aqueous zinc ion battery, characterized in that The modified aqueous zinc ion battery electrolyte according to claim 3 is used as the electrolyte, the zinc metal material is used as the negative electrode, the intercalation compound is used as the positive electrode, and the positive electrode and the negative electrode are separated by a diaphragm.

9. The aqueous zinc ion battery according to claim 8, characterized in that: The zinc metal material is one of zinc plate, zinc sheet, zinc foil or three-dimensional zinc foam; the intercalation compound is one of manganese-based materials, vanadium-based materials, and Prussian blue analogs; and the diaphragm is one of glass fiber, qualitative filter paper or polypropylene fiber diaphragm.

10. The aqueous zinc ion battery according to claim 9, characterized in that: The manganese material is MnO2, the vanadium material is V2O5, and the Prussian blue analog is Fe4[Fe(CN)6]3.

Citation Information

Patent Citations

  • Modified zinc negative electrode plate capable of inhibiting dendritic crystal growth, preparation method and application of modified zinc negative electrode plate

    CN117542947A

  • Method for preparing induced pluripotent stem cells from Basal cells derived from human respiratory tissue

    KR1020240148090A

Cited By

  • Asymmetric barrier material, preparation thereof and application of asymmetric barrier material in aqueous asymmetric zinc metal battery

    CN119601895A

  • Asymmetric barrier materials, preparation thereof and use in aqueous asymmetric zinc metal batteries

    CN119601895B

  • Aqueous zinc ion battery electrolyte and aqueous zinc ion battery

    CN122291728A