Polymer coating material as well as preparation method and application thereof
By using a polymer coating material on the negative active material of a lithium-ion battery to form a polymer-conductive material hybrid coating layer, the problems of volume expansion and dispersion are solved, and the cycle stability and production efficiency of the lithium-ion battery are improved.
Patent Information
- Application Number
- CN202310449040.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-10-25
AI Technical Summary
The negative active material of lithium-ion batteries expands severely in volume during the charge and discharge process, causing damage to the material structure, insufficient battery cycle stability, and low negative electrode slurry dispersion and liquid injection efficiency, affecting production efficiency and performance.
A polymer coating material containing active groups is combined with a conductive material to form a polymer-conductive material hybrid coating layer to modify the negative active material, improve its hydrophilicity and conductivity, suppress volume expansion, and improve dispersion sex and infiltration.
It significantly improves the dispersion performance of the negative active material and the cycle performance of the battery, shortens the pulping time, improves the liquid absorption efficiency, and prolongs the cycle stability and conductive performance of the battery.
Smart Images

Figure BDA0004196858400000171 
Figure BDA0004196858400000181 
Figure BDA0004196858400000221
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion battery materials, and in particular relates to a polymer coating material and a preparation method and application thereof. Background Art
[0002] As a green and environmentally friendly new energy source, lithium-ion batteries have the advantages of good reliability, high safety, small size and light weight. They have been widely used in digital products, electric vehicles, military products and other fields. In recent years, in order to meet the needs of future electrification, especially the further development of the digital product industry represented by mobile phones and the electric vehicle industry, the performance improvement of lithium-ion batteries is also facing huge challenges. At present, the market not only has an increasing demand for lithium-ion batteries, but also has higher and higher requirements for the long cycle of lithium-ion batteries.
[0003] Lithium-ion batteries are usually assembled from positive electrodes, negative electrodes, separators and electrolytes. The electrochemical performance of the battery is closely related to each part, especially the positive and negative electrodes have a decisive influence on the performance of lithium-ion batteries; at the same time, the preparation process of the positive and negative electrodes will also directly affect the production progress and product performance of lithium-ion batteries. The conventional method for preparing negative electrode sheets includes: mixing negative electrode active materials, conductive agents, binders and solvents (usually water) to make negative electrode slurry, and then coating the negative electrode slurry on the current collector, and obtaining negative electrode sheets after drying, rolling and other processing steps. In the preparation process of negative electrode slurry, the slurry dispersion process is very important in the production of lithium-ion batteries, and the dispersion time of negative electrode active materials directly determines the production efficiency of lithium-ion batteries. However, the surface of the negative electrode active materials commonly used at present is relatively hydrophobic, and it takes a long time to disperse, which seriously affects the battery production efficiency; moreover, if the dispersibility of the negative electrode active materials in the negative electrode slurry is poor, it will lead to insufficient uniformity of the negative electrode sheet, which will have a negative impact on the performance of lithium-ion batteries.
[0004] Another important process in the production of lithium-ion batteries is to inject electrolyte into the battery, that is, after the positive electrode, negative electrode and separator are made into a battery cell and packaged, the electrolyte is injected into the battery (referred to as the "injection process"). In the injection process, the accuracy of the injection amount and the efficiency of the injection directly determine the consistency and production efficiency of the lithium-ion battery. In the preparation of the battery cell, the negative electrode is wound, stacked, extruded and other processes, resulting in a relatively low liquid absorption efficiency of the electrode, which requires a long time to inject liquid and is prone to uneven absorption, which seriously affects the battery production efficiency and yield rate.
[0005] In addition to the obvious deficiencies in the negative electrode slurry dispersion process and the injection process during the production of lithium-ion batteries, the electrochemical performance of negative electrode active materials also has a lot of room for improvement. The current negative electrode active materials mainly include carbon-based materials and silicon-based materials. Various active materials will undergo different degrees of volume expansion during the charging and discharging process, and the volume expansion of silicon-based materials is particularly serious, which leads to powder separation between materials, damage to the battery pole structure, and difficulty in forming a stable SEI film, resulting in continuous consumption of lithium ions and electrolytes, rapid battery cycle decay, and insufficient cycle stability.
[0006] Therefore, in order to improve the production efficiency of the slurry dispersion process and the liquid injection process and improve the cycle performance of lithium-ion batteries, developing negative electrode materials with better performance is an urgent problem to be solved in this field. Summary of the invention
[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a polymer coating material and a preparation method and application thereof. The polymer coating material has excellent hydrophilicity and conductivity. As a negative electrode active material modifier, it can, on the one hand, improve the hydrophilicity of the negative electrode active material, thereby improving its dispersion performance in the negative electrode slurry, improving the production efficiency of the negative electrode slurry, and improving the wettability and liquid absorption efficiency of the negative electrode plate to the electrolyte; on the other hand, the polymer coating material can effectively inhibit the volume expansion of the negative electrode active material and improve the conductivity at the same time, thereby obtaining a modified negative electrode active material with excellent hydrophilicity, dispersibility, cycle performance, high capacity and rate performance, thereby improving the production efficiency and performance of lithium-ion batteries.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a polymer coating material, which comprises a combination of a polymer and a conductive material; the polymer contains active groups, which comprise a combination of cyano, hydroxyl and strong hydrophilic groups, and the strong hydrophilic groups comprise amino and / or carboxyl groups.
[0010] The polymer coating material provided by the present invention includes a combination of a polymer containing an active group and a conductive material. As a negative electrode active material modifier, it can be coated on the surface of the negative electrode active material to form a modified negative electrode active material having a polymer-conductive material hybrid coating layer. The components of the polymer coating material and its technical effects are as follows: (1) The cyano group in the polymer has a strong adhesion to the negative electrode active material (such as graphite), so that the polymer coating material can be tightly coated on the surface of the negative electrode active material, inhibiting the volume expansion of the negative electrode active material during the charge and discharge process; (2) The polymer contains hydroxyl groups and strong hydrophilic groups and has good hydrophilicity. The polymer coating material is coated on the surface of the negative electrode active material, so that the surface properties of the modified negative electrode active material are more hydrophilic and easier to be evenly dispersed in the negative electrode slurry, which not only greatly shortens the slurrying time, but also can improve the surface uniformity of the negative electrode plate; at the same time, due to this surface hydrophilic property, the negative electrode plate is more wettable to the electrolyte. Good, can greatly improve the electrolyte infiltration speed of the negative electrode plate, shorten the liquid absorption time, and improve the liquid absorption efficiency; (3) in the preparation process of the modified negative electrode active material, the hydroxyl group in the polymer and the strong hydrophilic group (amino group and / or carboxyl group) undergo thermal cross-linking reaction, so that the coating layer on the surface of the modified negative electrode active material has strong water resistance while being hydrophilic, and will not fall off during the preparation process of the negative electrode slurry, so that the surface of the negative electrode active material has a stable coating layer, which inhibits the volume expansion of the negative electrode active material during the cycle; (4) The polymer coating material and the formed coating layer contain conductive materials, have good conductivity, can avoid impedance degradation caused by coating, and make the modified negative electrode active material have good conductivity and rate performance.
[0011] In summary, the present invention, through the design of a polymer containing an active group and its compounding with a conductive material, makes the polymer coating material have excellent hydrophilicity and conductivity, and can be used as a negative electrode active material modifier. On the one hand, the hydrophilicity of the negative electrode active material is improved, its dispersion performance in the negative electrode slurry is improved, the slurrying time is shortened, the production efficiency of the negative electrode slurry is improved, and the wettability and liquid absorption efficiency of the negative electrode electrode sheet to the electrolyte are improved; on the other hand, the polymer coating material can form a stable and reliable coating layer on the surface of the negative electrode active material, effectively inhibit the volume expansion of the negative electrode active material, avoid the impedance degradation caused by the coating, and improve the conductive performance, thereby obtaining a modified negative electrode active material with excellent hydrophilicity, dispersibility, cycle performance, conductivity and rate performance, improving the production efficiency of lithium ion batteries, and improving the cycle performance of lithium ion batteries.
[0012] Preferably, the polymer is coated on the surface of the conductive material.
[0013] It should be noted that, in the polymer coating material, the coating of the conductive material by the polymer may be complete coating or partial coating.
[0014] Preferably, the mass percentage of the conductive material in the polymer coating material is 1-60%, for example, it can be 2%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or 55%, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0015] As a preferred technical solution of the present invention, the mass percentage of the conductive material in the polymer coating material is 1-60%, so that the polymer coating material can form a stable polymer-conductive material hybrid coating layer on the surface of the negative electrode active material, inhibit the volume expansion of the negative electrode active material during the cycle, and improve the structural stability, cycle performance and conductive performance of the material. If the content of the conductive material is too low, the improvement effect on the conductive performance is not obvious, and the material will produce impedance degradation due to the coating; if the content of the conductive material is too high, it will affect the coating effect of the polymer, resulting in the polymer coating material not having a significant inhibitory effect on the volume expansion of the negative electrode active material, and failing to effectively improve the cycle performance.
[0016] Preferably, the conductive material includes any one of polythiophene, polypyrrole, polyaniline, carbon black, carbon nanotubes, carbon fibers, graphene, graphite, Ketjen black, and acetylene black, or a combination of at least two thereof.
[0017] As a preferred technical solution of the present invention, the strong hydrophilic group in the polymer includes a combination of an amino group and a carboxyl group, that is, the active group includes a combination of a cyano group, a hydroxyl group, an amino group and a carboxyl group.
[0018] Preferably, the molar percentage of cyano groups in the active groups is 1-50%, for example, 2%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40% or 45%, as well as specific values between the above points. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific points included in the range.
[0019] Preferably, the molar percentage of hydroxyl groups in the active groups is 1-50%, for example, 2%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40% or 45%, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0020] Preferably, the molar percentage of the strong hydrophilic group in the active group is 1-60%, for example, it can be 2%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or 55%, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0021] Preferably, the molar percentage of the amino group in the active group is 1-20%, for example, it can be 2%, 3%, 5%, 7%, 9%, 10%, 11%, 13%, 15%, 17% or 19%, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0022] Preferably, the molar percentage of carboxyl groups in the active groups is 1-40%, for example, 2%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35% or 38%, as well as specific values between the above points. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific points included in the range.
[0023] As a preferred technical solution of the present invention, the active groups in the polymer include, by molar percentage, cyano group 1-50%, hydroxyl group 1-50%, amino group 1-20%, and carboxyl group 1-40%; thereby, the polymer has good hydrophilicity on the one hand, so that the polymer coating material can improve the hydrophilicity and dispersion performance of the negative electrode active material, improve the production efficiency of the negative electrode slurry, and enhance the wettability and liquid absorption efficiency of the negative electrode electrode sheet to the electrolyte; on the other hand, a specific proportion of cyano groups makes the polymer have good adhesion with the negative electrode active material, so that the polymer coating material is tightly coated on the surface of the negative electrode active material; at the same time, the hydroxyl group can undergo thermal cross-linking reaction with the amino group and the carboxyl group to form a stable coating layer with good water resistance on the surface of the negative electrode active material, thereby inhibiting the volume expansion of the negative electrode active material during the charge and discharge process. If the active groups in the polymer are not a combination of cyano, hydroxyl, amino and carboxyl groups in a specific molar ratio, it will affect the coating and modification effect of the polymer coating material on the negative electrode active material, and it will be impossible to obtain a coating layer with hydrophilicity, water resistance and stability on the surface of the negative electrode active material, which will lead to the modified negative electrode active material being unable to take into account both good hydrophilicity and cycle stability.
[0024] Preferably, the polymerizable monomers of the polymer include a combination of alkenyl nitrile monomers, hydroxyl-containing acrylate monomers, acrylamide monomers and alkenyl carboxylic acid monomers.
[0025] Preferably, the polymerizable monomers include the following components in terms of molar percentage: 1-50% of alkenyl nitrile monomers, 1-50% of hydroxyl-containing acrylate monomers, 1-20% of acrylamide monomers, and 1-40% of alkenyl carboxylic acid monomers.
[0026] As a preferred technical solution of the present invention, the polymer is obtained by copolymerizing alkenyl nitrile monomers, hydroxyl acrylate monomers, acrylamide monomers and alkenyl carboxylic acid monomers in a specific molar ratio, thereby making the obtained polymer contain four active groups: cyano, cyano, amino and carboxyl.
[0027] In the polymerized monomers of the polymer, the molar percentage of the alkenyl nitrile monomer is 1-50%, for example, it can be 2%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40% or 45%; the molar percentage of the hydroxyl-containing acrylate monomer is 1-50%, for example, it can be 2%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40% or 45%; the molar percentage of the acrylamide monomer is 1-20%, for example, For example, it can be 2%, 3%, 5%, 7%, 9%, 10%, 11%, 13%, 15%, 17% or 19%; the molar percentage of the olefinic carboxylic acid monomer is 1-40%, for example, it can be 2%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35% or 38%, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the said range.
[0028] Preferably, the alkenyl nitrile monomer includes any one of acrylonitrile, methacrylonitrile and crotononitrile, or a combination of at least two of them.
[0029] Preferably, the hydroxyl-containing acrylic ester monomer includes any one of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, and hydroxybutyl methacrylate, or a combination of at least two thereof.
[0030] Preferably, the acrylamide monomers include acrylamide and / or methacrylamide.
[0031] Preferably, the alkenyl carboxylic acid monomer includes any one of acrylic acid, methacrylic acid, and crotonic acid, or a combination of at least two of them.
[0032] In a second aspect, the present invention provides a method for preparing the polymer-coated material as described in the first aspect, wherein the preparation method comprises method A or method B;
[0033] The method A comprises: mixing a polymer solution with a conductive material to obtain the polymer coating material;
[0034] The method B comprises: mixing a polymer monomer solution of a polymer with a conductive material and then performing a polymerization reaction to obtain the polymer coating material.
[0035] The preparation methods provided by the present invention include two categories: in method A, a polymer is first obtained, and then the polymer solution is mixed evenly with a conductive material to obtain the polymer-coated material. In method B, a polymerization monomer solution of the polymer is mixed evenly with a conductive material, and then a polymerization reaction is carried out to obtain the polymer-coated material. In method B, since the polymerization reaction is carried out in the presence of a conductive material, the polymer obtained by polymerization can be better coated on the surface of the conductive material.
[0036] Preferably, in method A, the method for preparing the polymer comprises: subjecting a polymerizable monomer to a polymerization reaction in the presence of an initiator to obtain the polymer.
[0037] Preferably, in method A, the initiator comprises a water-soluble azo initiator and / or a persulfate.
[0038] Preferably, in method A, the initiator is selected from any one of ammonium persulfate, potassium persulfate or sodium persulfate, or a combination of at least two thereof.
[0039] Preferably, in method A, based on the mass of the polymerized monomer as 100%, the mass of the initiator is 0.05-5%, for example, it can be 0.08%, 0.1%, 0.3%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0040] Preferably, in method A, the polymerization reaction is carried out in the presence of a solvent, and the solvent preferably comprises water.
[0041] Preferably, in method A, the polymerization reaction temperature is 60-100°C, for example, it can be 62°C, 65°C, 68°C, 70°C, 72°C, 75°C, 78°C, 80°C, 82°C, 85°C, 88°C, 90°C, 92°C, 95°C or 98°C, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0042] Preferably, in method A, the polymerization reaction time is 0.5-12 h, for example, it can be 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h or 11 h, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0043] Preferably, in method A, the solvent of the polymer solution comprises water.
[0044] Preferably, method B comprises: mixing a polymerization monomer solution of a polymer with a conductive material, and then performing a polymerization reaction in the presence of an initiator to obtain the polymer coating material.
[0045] Preferably, in method B, the solvent of the polymerization monomer solution includes water.
[0046] Preferably, in method B, the initiator comprises a water-soluble azo initiator and / or a persulfate, and further preferably comprises any one of ammonium persulfate, potassium persulfate or sodium persulfate, or a combination of at least two thereof.
[0047] Preferably, in method B, based on the mass of the polymerized monomer as 100%, the mass of the initiator is 0.05-5%, for example, it can be 0.08%, 0.1%, 0.3%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0048] Preferably, in method B, the polymerization reaction temperature is 60-100°C, for example, it can be 62°C, 65°C, 68°C, 70°C, 72°C, 75°C, 78°C, 80°C, 82°C, 85°C, 88°C, 90°C, 92°C, 95°C or 98°C, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0049] Preferably, in method B, the polymerization reaction time is 0.5-12 h, for example, it can be 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h or 11 h, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0050] In method A and method B, the polymerizable monomers include a combination of alkenyl nitrile monomers, hydroxyl-containing acrylate monomers, acrylamide monomers and alkenyl carboxylic acid monomers; preferably, the polymerizable monomers include the following components in molar percentage: 1-50% alkenyl nitrile monomers, 1-50% hydroxyl-containing acrylate monomers, 1-20% acrylamide monomers, and 1-40% alkenyl carboxylic acid monomers.
[0051] In a third aspect, the present invention provides a use of the polymer coating material as described in the first aspect in a negative electrode active material.
[0052] Preferably, the polymer coating material is used as a negative electrode active material modifier in the negative electrode active material.
[0053] In a fourth aspect, the present invention provides a modified negative electrode active material, comprising a negative electrode active material and a coating layer disposed on the surface of the negative electrode active material; the raw material of the coating layer is the polymer coating material as described in the first aspect.
[0054] Preferably, the negative electrode active material comprises a carbon-based material and / or a silicon-based material.
[0055] Preferably, the carbon-based material includes any one of graphite, carbon black, carbon nanotubes, carbon fibers, mesocarbon microbeads, and petroleum coke, or a combination of at least two thereof.
[0056] Preferably, the silicon-based material includes any one of nano silicon, micro silicon, porous silicon, amorphous silicon, silicon oxide, or a combination of at least two thereof.
[0057] Preferably, based on the mass of the negative electrode active material as 100%, the mass of the polymer coating material is 1-10%, for example, it can be 2%, 3%, 4%, 5%, 6%, 7%, 8% or 9%, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0058] In the present invention, the mass of the polymer coating material is the total mass of the polymer and the conductive material, and the polymer is calculated based on the solid content, excluding any solvent / dispersant, etc.
[0059] As a preferred technical solution of the present invention, in the modified negative electrode active material, the mass of the polymer coating material is 1-10%, based on the mass of the negative electrode active material as 100%, and a uniform and stable polymer-conductive material hybrid coating layer is formed on the surface of the negative electrode active material, so that the obtained modified negative electrode active material has good hydrophilicity, is easy to be evenly dispersed in the negative electrode slurry, shortens the slurrying time, and improves the wettability of the negative electrode plate to the electrolyte, shortens the liquid absorption time of the negative electrode plate, and improves the liquid absorption efficiency; at the same time, the polymer-conductive material hybrid coating layer formed can effectively inhibit the volume expansion of the negative electrode active material in the cycle, significantly improves the structural stability and cycle performance of the material, and has good conductive properties. If the mass of the polymer coating material is too small, it cannot form an effective coating, nor can it inhibit the volume expansion of the negative electrode active material; if the mass of the polymer coating material is too large, the thickness of the formed coating structure is too high, which will increase the impedance of the modified negative electrode active material, and deteriorate the conductivity and rate performance.
[0060] Preferably, the modified negative electrode active material is prepared by the following method, which comprises: mixing the negative electrode active material with a polymer coating material dispersion to obtain a slurry; and drying the slurry to obtain the modified negative electrode active material.
[0061] Preferably, the solvent of the polymer coating material dispersion includes water.
[0062] Preferably, the drying method is spray drying.
[0063] Preferably, the inlet temperature of the spray drying is 200-300°C, for example, it can be 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C or 290°C, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0064] Preferably, the outlet temperature of the spray drying is 100-200°C, for example, it can be 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C or 190°C, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0065] Preferably, the spray drying pressure is 0.2-0.8 MPa, for example, it can be 0.25 MPa, 0.30 MPa, 0.35 MPa, 0.40 MPa, 0.45 MPa, 0.50 MPa, 0.55 MPa, 0.60 MPa, 0.65 MPa, 0.70 MPa or 0.75 MPa, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0066] Preferably, the feed rate of the slurry in the spray drying is 5-15 mL / min, for example, it can be 6 mL / min, 7 mL / min, 8 mL / min, 9 mL / min, 10 mL / min, 11 mL / min, 12 mL / min, 13 mL / min or 14 mL / min, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0067] As a preferred technical solution of the present invention, in the preparation process of the modified negative electrode active material, the negative electrode active material and the polymer coating material dispersion are first mixed evenly to obtain a slurry; the slurry is spray-dried, and the process is accompanied by high-temperature heat treatment (inlet temperature is 200-300°C, outlet temperature is 100-200°C) to allow the hydroxyl group and the amino group / carboxyl group to undergo a thermal cross-linking reaction, so that the coating layer on the surface of the modified negative electrode active material has hydrophilicity and also has good water resistance and coating stability based on the thermal cross-linking reaction. The coating layer will not fall off during the preparation process of the negative electrode slurry, and can play a role in improving hydrophilicity and inhibiting volume expansion in a long-lasting and stable manner.
[0068] In a fifth aspect, the present invention provides a negative electrode material composition, which includes the modified negative electrode active material as described in the fourth aspect.
[0069] Preferably, the negative electrode material composition comprises a combination of a modified negative electrode active material, a conductive agent, a binder and optionally a thickener.
[0070] Preferably, based on 100 parts by mass of the modified negative electrode active material, the mass of the conductive agent is 0.1-5.0 parts, for example, it can be 0.1 parts, 0.3 parts, 0.5 parts, 0.7 parts, 0.9 parts, 1.0 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2.0 parts, 2.2 parts, 2.5 parts, 2.8 parts, 3.0 parts, 3.2 parts, 3.5 parts, 3.8 parts, 4.0 parts, 4.2 parts, 4.5 parts or 4.8 parts, as well as specific point values between the above points. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0071] Preferably, the binder comprises styrene butadiene rubber (SBR).
[0072] Preferably, based on 100 parts by mass of the modified negative electrode active material, the mass of the binder is 0.1-5.0 parts, for example, it can be 0.1 parts, 0.3 parts, 0.5 parts, 0.7 parts, 0.9 parts, 1.0 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2.0 parts, 2.2 parts, 2.5 parts, 2.8 parts, 3.0 parts, 3.2 parts, 3.5 parts, 3.8 parts, 4.0 parts, 4.2 parts, 4.5 parts or 4.8 parts, as well as specific point values between the above points. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0073] Preferably, the thickener comprises sodium carboxymethylcellulose (CMC).
[0074] Preferably, based on 100 parts by mass of the modified negative electrode active material, the mass of the thickener is 0.1-3.0 parts, for example, it can be 0.1 parts, 0.3 parts, 0.5 parts, 0.7 parts, 0.9 parts, 1.0 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2.0 parts, 2.2 parts, 2.5 parts or 2.8 parts, as well as specific point values between the above point values. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0075] In a sixth aspect, the present invention provides a negative electrode plate, comprising a current collector and a coating disposed on the current collector, wherein the material of the coating comprises the negative electrode material composition as described in the fifth aspect.
[0076] In a seventh aspect, the present invention provides an electrochemical energy storage device, comprising at least one of the polymer coating material as described in the first aspect, the modified negative electrode active material as described in the fourth aspect, the negative electrode material composition as described in the fifth aspect, and the negative electrode plate as described in the sixth aspect.
[0077] Preferably, the electrochemical energy storage device comprises any one of a lithium ion battery, a sodium ion battery, a supercapacitor, a fuel cell or a solar cell, and a lithium ion battery is more preferred.
[0078] Compared with the prior art, the present invention has the following beneficial effects:
[0079] (1) The polymer coating material provided by the present invention has excellent hydrophilicity and conductivity through the design of the polymer containing active groups and its compounding with the conductive material. It can be used as a modifier for negative electrode active materials. On the one hand, it improves the hydrophilicity of the negative electrode active material, improves its dispersion performance in the negative electrode slurry, shortens the slurrying time, improves the production efficiency of the negative electrode slurry, and improves the wettability and liquid absorption efficiency of the negative electrode plate to the electrolyte; on the other hand, the polymer coating material can form a stable and reliable coating layer on the surface of the negative electrode active material, effectively inhibits the volume expansion of the negative electrode active material, avoids the impedance degradation caused by the coating, and improves the conductive performance.
[0080] (2) In the modified negative electrode active material provided by the present invention, the polymer coating material can form a stable polymer-conductive material hybrid coating layer on the surface of the negative electrode active material, so that the modified negative electrode active material has excellent hydrophilicity and dispersibility, cycle performance, conductivity and rate performance, thereby improving the production efficiency of lithium-ion batteries and the cycle performance of lithium-ion batteries.
[0081] (3) The present invention uses the component design and optimization of the polymer coating material to enable the modified negative electrode active material to be used in negative electrode plates and lithium-ion batteries. The negative electrode plates have good wettability to the electrolyte, which significantly improves the liquid absorption efficiency of the negative electrode plates and the production efficiency of the liquid injection process. At the same time, the coating layer on the surface of the negative electrode active material can effectively inhibit the volume expansion of the negative electrode active material without causing impedance degradation, so that the modified negative electrode active material has excellent cycle stability and conductivity, which significantly improves the cycle performance of the lithium-ion battery. DETAILED DESCRIPTION
[0082] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0083] As used herein, the terms "comprises," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0084] "Optionally" or "either" means that the subsequently described matter or event can or cannot occur, and that the description includes instances where the event occurs and instances where it does not.
[0085] The indefinite articles "a" and "an" before the elements or components of the present invention have no limitation on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the quantity obviously refers to the singular form only.
[0086] The terms "one embodiment", "some embodiments", "exemplarily", "specific examples" or "some examples" described in the present invention mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this document, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.
[0087] Moreover, the technical features involved in various embodiments of the present invention can be combined with each other as long as they do not conflict with each other.
[0088] In the following specific embodiments of the present invention, the conductive materials and polymerized monomers used are commercially available products; wherein the specific sources of the conductive materials are as follows:
[0089] Conductive carbon black (SP): brand name is arbon F-200GS, purchased from ASAHI CARBON CO LTD, Japan;
[0090] Polythiophene: brand name Solar3, purchased from Shanghai Kaishefeng Industrial Co., Ltd.;
[0091] Carbon fiber: brand VGCF-H, purchased from Showa Denko, Japan;
[0092] Carbon nanotubes: brand CN301C3, purchased from Kolon, South Korea;
[0093] Graphene: Brand TA-001A, purchased from Shenzhen Turing Evolution Technology Co., Ltd.
[0094] Ketjen black: brand EC-300J, purchased from Lion of Japan.
[0095] Example 1
[0096] This embodiment provides a polymer coating material and a preparation method thereof, and a modified negative electrode active material using the polymer coating material.
[0097] Specifically, the polymer coating material includes a combination of conductive carbon black (SP) and a polymer, wherein the mass percentage of SP is 20%; the active groups of the polymer include a combination of cyano, hydroxyl, amino and carboxyl groups, and the polymerized monomers thereof include, by molar percentage, 20% acrylonitrile, 40% hydroxyethyl acrylate, 15% acrylamide and 25% acrylic acid.
[0098] The preparation method of the polymer coating material is as follows: 0.2 mol acrylonitrile, 0.4 mol hydroxyethyl acrylate, 0.15 mol acrylamide, 0.25 mol acrylic acid, ammonium persulfate (0.86 g, the mass of which is 1% of the total mass of the four monomers), SP (21.4 g, the mass of SP is 25% of the total mass of the four monomers) and 400 mL of deionized water are mixed evenly, and a polymerization reaction is carried out at 85° C. for 5 hours to obtain the polymer coating material.
[0099] A modified negative electrode active material, comprising a negative electrode active material (artificial graphite) and a coating layer disposed on the surface of the negative electrode active material, wherein the raw material of the coating layer is the polymer coating material provided in this embodiment; the preparation method is as follows:
[0100] By mass, 5 parts of polymer coating material (in terms of solid content) were dispersed in 100 parts of water, and 95 parts of artificial graphite were added under stirring at 1000 rpm, and stirred for 30 minutes to fully mix to obtain slurry; the slurry was spray dried, and the parameters were set as follows: inlet temperature was 250°C, outlet temperature was 150°C, feed rate was 10 mL / min, and air pressure was 0.5 MPa. After the spraying was completed, the collected particles were the modified negative electrode active material.
[0101] Example 2
[0102] This embodiment provides a polymer coating material and a preparation method thereof, and a modified negative electrode active material using the polymer coating material.
[0103] Specifically, the polymer coating material includes a combination of conductive carbon black (SP) and a polymer, wherein the mass percentage of SP is 25%; the active groups of the polymer include a combination of cyano, hydroxyl, amino and carboxyl groups, and the polymerized monomers include, by molar percentage, 20% acrylonitrile, 40% hydroxyethyl acrylate, 10% acrylamide, and 30% acrylic acid.
[0104] The preparation method of the polymer coating material is as follows: 0.2 mol of acrylonitrile, 0.4 mol of hydroxyethyl acrylate, 0.1 mol of acrylamide, 0.3 mol of acrylic acid, ammonium persulfate (0.86 g, which is 1% of the total mass of the four monomers) and 400 mL of deionized water are mixed evenly, and a polymerization reaction is carried out at 85° C. for 5 hours to obtain a polymer solution; the polymer solution is mixed with 8.6 g of SP2 so that the mass ratio of the polymer to the SP is 3:1, and the mixture is mixed evenly to obtain the polymer coating material.
[0105] A modified negative electrode active material, comprising a negative electrode active material (silicon dioxide) and a coating layer disposed on the surface of the negative electrode active material, wherein the raw material of the coating layer is the polymer coating material provided in this embodiment; the preparation method is as follows:
[0106] By mass, 5 parts of polymer coating material (in terms of solid content) were dispersed in 100 parts of water, and 95 parts of silicon oxide were added under stirring at 1000 rpm, and stirred for 30 minutes to fully mix to obtain slurry; the slurry was spray dried, and the parameters were set as follows: inlet temperature was 250°C, outlet temperature was 150°C, feed rate was 10 mL / min, and air pressure was 0.5 MPa. After the spraying was completed, the collected particles were the modified negative electrode active material.
[0107] Example 3-15
[0108] A polymer coating material and a preparation method thereof, and a modified negative electrode active material using the polymer coating material, which differs from Example 1 only in that the components and amounts in the polymer coating material are different, as shown in Table 1; wherein "content (%)" represents the mass percentage of the conductive material in the polymer coating material; "mol%" represents the molar percentage of the monomer in the polymerized monomer. The preparation methods of the polymer coating materials and the preparation methods of the modified negative electrode active materials provided in Examples 3-15 are the same as those in Example 1.
[0109] Table 1
[0110]
[0111]
[0112] In Table 1, “--” represents that the component does not exist.
[0113] Comparative Example 1
[0114] This comparative example provides a polymer coating material and a preparation method thereof, and a modified negative electrode active material using the polymer coating material. The only difference between the polymer coating material and Example 1 is that the active group of the polymer does not contain hydroxyl groups, and the polymerized monomers include, by mole percentage, 20% acrylonitrile, 40% ethyl acrylate, 15% acrylamide, and 25% acrylic acid; the other components, amounts, and preparation methods of the polymer coating material are the same as those in Example 1.
[0115] A modified negative electrode active material, which differs from the modified negative electrode active material in Example 1 only in that the polymer coating material provided in this comparative example is used as the raw material of the coating layer; other components, amounts and preparation methods of the modified negative electrode active material are the same as those in Example 1.
[0116] Comparative Example 2
[0117] This comparative example provides a polymer coating material and a preparation method thereof, and a modified negative electrode active material using the polymer coating material. The only difference between the polymer coating material and Example 1 is that the active group of the polymer does not contain a cyano group, and the polymerized monomers include, by mole percentage, 20% methyl acrylate, 40% hydroxyethyl acrylate, 15% acrylamide, and 25% acrylic acid; the other components, amounts, and preparation method of the polymer coating material are the same as those in Example 1.
[0118] A modified negative electrode active material, which differs from the modified negative electrode active material in Example 1 only in that the polymer coating material provided in this comparative example is used as the raw material of the coating layer; other components, amounts and preparation methods of the modified negative electrode active material are the same as those in Example 1.
[0119] Comparative Example 3
[0120] This comparative example provides a polymer coating material and a preparation method thereof, and a modified negative electrode active material using the polymer coating material. The only difference between the polymer coating material and Example 1 is that the active group of the polymer does not contain carboxyl groups and amino groups, and the polymerized monomers include, by molar percentage, 20% acrylonitrile, 40% hydroxyethyl acrylate, and 40% methyl acrylate; the other components, amounts, and preparation methods of the polymer coating material are the same as those in Example 1.
[0121] A modified negative electrode active material, which differs from the modified negative electrode active material in Example 1 only in that the polymer coating material provided in this comparative example is used as the raw material of the coating layer; other components, amounts and preparation methods of the modified negative electrode active material are the same as those in Example 1.
[0122] Comparative Example 4
[0123] This comparative example is unmodified artificial graphite.
[0124] Comparative Example 5
[0125] This comparative example is unmodified silicon dioxide.
[0126] Application Example 1-15, Comparative Application Example 1-5
[0127] A negative electrode plate comprises a current collector (Cu foil) and a coating disposed on the current collector, wherein the material of the coating is a negative electrode material composition; the negative electrode material composition comprises a negative electrode active material, a conductive agent (conductive carbon black, SP), a binder (styrene-butadiene rubber, SBR) and a thickener (sodium carboxymethyl cellulose, CMC) in a mass ratio of 95:1.0:2.5:1.5; wherein the negative electrode active material is the modified negative electrode active material provided in Examples 1-15 and Comparative Examples 1-5, respectively.
[0128] Preparation of the negative electrode sheet: The negative electrode active material, SP, SBR and CMC were mixed in a mass ratio of 95:1.0:2.5:1.5, added into deionized water at a solid content of 40wt% and stirred to make a uniform negative electrode slurry, which was passed through a 100-mesh sieve and then coated on a negative electrode current collector Cu foil, dried, and rolled using a roller at a speed of 10×10 4 The negative electrode sheet is obtained by rolling with a unit length load of N / m.
[0129] A lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the negative electrode sheet is the aforementioned negative electrode sheet; the preparation method of the lithium-ion battery is as follows:
[0130] (1) Preparation of positive electrode sheet: The positive electrode active material (lithium iron phosphate), conductive agent (conductive carbon black) and binder (polyvinylidene fluoride, PVDF) were mixed in a mass ratio of 95.5:2.0:2.5, added to NMP at a ratio of 50 wt% solid content, and stirred to make a uniform positive electrode slurry. After passing through a 100 mesh sieve, the slurry was coated on the positive electrode current collector Al foil, dried, and rolled using a roller at a speed of 10×10 4 The positive electrode sheet is obtained by rolling with a unit length load of N / m.
[0131] (2) Preparation of negative electrode sheet: as described above;
[0132] (3) Diaphragm: PE porous polymer film (Shenzhen Xingyuan Material Technology Co., Ltd.) was used as the diaphragm;
[0133] (4) Assembly of lithium-ion batteries: The positive electrode sheet, the separator, and the negative electrode sheet are wound in order to obtain a battery cell; the battery cell is packaged with an aluminum-plastic film, baked to remove water, and then injected with an electrolyte. After vacuum packaging, storage, formation, secondary sealing, shaping and other processes, the lithium-ion battery is obtained.
[0134] Performance Testing:
[0135] (1) Fineness of negative electrode slurry
[0136] During the preparation of the negative electrode slurry, the fineness (μm) of the negative electrode active material after dispersion for 10 minutes was tested. The lower the fineness measured at 10 minutes, the better the dispersion performance of the negative electrode active material.
[0137] (2) Liquid absorption performance of negative electrode
[0138] 1 mL of electrolyte DMC was dripped onto the negative electrode to be tested. The timing started from the moment when the electrolyte DMC contacted the electrode and ended when the electrolyte was completely absorbed by the electrode. The electrode absorption time was recorded, as shown in Table 2.
[0139] (3) Normal temperature cycle performance
[0140] The prepared lithium-ion battery was charged to 4.2V at a constant current of 0.33C, then charged to a cutoff current of 0.02C at a constant voltage, and discharged to 2.5V at 0.33C; left for 5 minutes, charged to 4.2V at a constant current of 0.33C, then charged to a cutoff current of 0.02C at a constant voltage, and discharged to 2.5V at 0.33C, thus performing initial adjustment.
[0141] At 25°C, the initially adjusted lithium-ion battery is charged to 4.2V at a constant current of 0.5C, then charged to a cut-off current of 0.02C at a constant voltage, left for 5 minutes, and then discharged to 2.5V at a constant current of 1C, left for 5 minutes, and the first cycle discharge capacity is measured; after 100 cycles of charge / discharge, the 100th cycle discharge capacity is measured, and the 100th cycle capacity retention rate is calculated using the following formula:
[0142] The capacity retention rate after 100 cycles (%) = 100% × 100th cycle discharge capacity / first cycle discharge capacity.
[0143] (4) Rate performance
[0144] At 25°C, the initially adjusted lithium-ion battery was charged to 4.2V at 0.5C constant current, then charged to a cutoff current of 0.02C at constant voltage, left for 5 minutes, then discharged to 2.5V at 1C constant current, left for 5 minutes, and the 1C discharge capacity was measured. Then, it was charged to 4.2V at 0.5C constant current, then charged to a cutoff current of 0.02C at constant voltage, left for 5 minutes, then discharged to 2.5V at 3C constant current, left for 5 minutes, and the discharge capacity at 3C rate was measured.
[0145] 3C capacity retention rate (%) = 100% × 3C discharge capacity / 1C discharge capacity.
[0146] The test results are shown in Table 2.
[0147] Table 2
[0148]
[0149]
[0150] Combined with the performance test data in Table 2, it can be seen that compared with the negative electrode sheets and lithium-ion batteries prepared using conventional negative electrode active materials in Comparative Examples 4 and 5 (Comparative Example 4: artificial graphite; Comparative Example 5: silicon dioxide), the polymer coating material provided by Examples 1-7 of the present invention is used as a negative electrode active material modifier, so that the prepared modified negative electrode active material has good hydrophilicity and dispersibility, and a fineness of 20-22 μm can be achieved after dispersion for 10 minutes, which can shorten the pulping time, improve the wettability and liquid absorption efficiency of the negative electrode sheet to the electrolyte, and make the liquid absorption time 21-32s. At the same time, the volume expansion of the negative electrode active material in the modified negative electrode active material is effectively suppressed, and while having excellent structural stability and cycle performance, the conductivity and rate performance of the material can also be improved, so that the capacity retention rate of the lithium ion battery containing the carbon-based modified negative electrode active material (artificial graphite, Examples 1, 3-7) after 100 cycles at room temperature is ≥96.1%, and the 3C rate performance is ≥85.0%; the capacity retention rate of the lithium ion battery containing the silicon-based modified negative electrode active material (silicon dioxide, Example 2) after 100 cycles at room temperature is ≥90%, and the 3C rate performance is ≥82.0%.
[0151] In the present invention, by designing a polymer containing active groups and compounding it with a conductive material, the polymer coating material is coated on the surface of the negative electrode active material to form a stable polymer-conductive material hybrid coating layer, so that the modified negative electrode active material has good hydrophilicity and dispersibility, and the introduction of cyano groups makes the polymer and the negative electrode active material have good adhesion, and the hydroxyl group and the amino group and / or carboxyl group can undergo a thermal cross-linking reaction to form a stable coating layer with good water resistance on the surface of the negative electrode active material, inhibiting the volume expansion of the negative electrode active material during the charge and discharge process, and the coating layer will not fall off during the preparation of the slurry; at the same time, because the coating layer contains a conductive material, the impedance degradation caused by the coating is avoided, so that the modified negative electrode active material has excellent cycle performance, conductivity and rate performance. Combined with the effect data of Examples 1-15, it can be seen that by adjusting the component ratio of the conductive material and the polymer and the type and ratio of the active groups in the polymer, the cycle performance and rate performance of the modified negative electrode active material and the lithium ion battery containing it can be controlled and optimized. If the proportion of cyano groups in the polymer is too low (Example 8), the adhesion between the polymer and the negative electrode active material is reduced, and the stability of the coating layer is insufficient, affecting the cycle performance; if the proportion of cyano groups in the polymer is too high (Example 9), it will affect the hydrophilicity of the modified negative electrode active material, resulting in a prolonged liquid absorption time of the negative electrode sheet. If the proportion of hydroxyl groups in the polymer is too high and the proportion of carboxyl and amino groups of strong hydrophilic groups is too low (Example 10), or the proportion of hydroxyl groups in the polymer is too low and the proportion of carboxyl and amino groups of strong hydrophilic groups is too high (Example 11), it will lead to insufficient cross-linking of hydroxyl groups with carboxyl and amino groups during coating, and partial detachment of the coating layer occurs during the preparation of the negative electrode slurry, affecting the cycle performance. If the amount of conductive material used is small (Example 14), the improvement effect on the conductive properties of the modified negative electrode active material is not obvious, resulting in a slightly lower rate performance of the battery; if the amount of conductive material used is too much (Example 15), it will affect the coating effect of the coating layer on the negative electrode active material and the inhibitory effect on the volume expansion of the negative electrode active material, resulting in a decrease in the cycle performance.
[0152] The polymer of Comparative Example 1 does not contain hydroxyl groups, and the polymer of Comparative Example 3 does not contain carboxyl groups and amino groups, resulting in insufficient hydrophilicity of the modified negative electrode active material, slow liquid absorption rate of the negative electrode plate, and the polymer coating material cannot be thermally cross-linked, resulting in low stability of the coating layer, which falls off during the preparation of the negative electrode slurry, and therefore cannot inhibit volume expansion and pulverization, resulting in poor cycle performance; the polymer of Comparative Example 2 does not contain cyanide groups. Although the hydrophilicity of the modified negative electrode active material is acceptable, due to insufficient adhesion between the polymer and the negative electrode active material, the coating layer is unstable and the cycle performance is poor.
[0153] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the polymer coating material and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A polymer coating material, characterized in that: The polymer coating material comprises a combination of a polymer and a conductive material; the polymer contains active groups, the active groups comprise a combination of a cyano group, a hydroxyl group and a strong hydrophilic group, and the strong hydrophilic group comprises an amino group and / or a carboxyl group.
2. The polymer coating material according to claim 1, characterized in that: The polymer is coated on the surface of the conductive material; Preferably, the mass percentage of the conductive material in the polymer coating material is 1-60%; Preferably, the conductive material includes any one of polythiophene, polypyrrole, polyaniline, carbon black, carbon nanotubes, carbon fibers, graphene, graphite, Ketjen black, and acetylene black, or a combination of at least two thereof.
3. The polymer coating material according to claim 1 or 2, characterized in that: The active groups include a combination of cyano, hydroxyl, amino and carboxyl groups; Preferably, the molar percentage of cyano groups in the active groups is 1-50%; Preferably, the molar percentage of hydroxyl groups in the active groups is 1-50%; Preferably, the molar percentage of amino groups in the active groups is 1-20%; Preferably, the molar percentage of carboxyl groups in the active groups is 1-40%.
4. The polymer coating material according to any one of claims 1 to 3, characterized in that: The polymerizable monomers of the polymer include a combination of alkenyl nitrile monomers, hydroxyl-containing acrylate monomers, acrylamide monomers and alkenyl carboxylic acid monomers; Preferably, the polymerizable monomers include the following components in terms of molar percentage: 1-50% of alkenyl nitrile monomers, 1-50% of hydroxyl-containing acrylate monomers, 1-20% of acrylamide monomers, and 1-40% of alkenyl carboxylic acid monomers; Preferably, the alkenyl nitrile monomer includes any one of acrylonitrile, methacrylonitrile, and crotononitrile, or a combination of at least two thereof; Preferably, the hydroxyl-containing acrylic ester monomer includes any one of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, and hydroxybutyl methacrylate, or a combination of at least two thereof; Preferably, the acrylamide monomers include acrylamide and / or methacrylamide; Preferably, the alkenyl carboxylic acid monomer includes any one of acrylic acid, methacrylic acid, and crotonic acid, or a combination of at least two of them.
5. A method for preparing a polymer coating material according to any one of claims 1 to 4, characterized in that: The preparation method includes method A or method B; The method A comprises: mixing a polymer solution with a conductive material to obtain the polymer coating material; The method B comprises: mixing a polymer monomer solution of a polymer with a conductive material and then performing a polymerization reaction to obtain the polymer coating material.
6. A modified negative electrode active material, characterized in that: The modified negative electrode active material comprises a negative electrode active material and a coating layer disposed on the surface of the negative electrode active material; the raw material of the coating layer is the polymer coating material according to any one of claims 1 to 4; Preferably, the negative electrode active material comprises a carbon-based material and / or a silicon-based material; Preferably, the carbon-based material includes any one of graphite, carbon black, carbon nanotubes, carbon fibers, mesocarbon microbeads, and petroleum coke, or a combination of at least two thereof; Preferably, the silicon-based material includes any one of nano silicon, micro silicon, porous silicon, amorphous silicon, silicon oxide, or a combination of at least two thereof; Preferably, based on 100% of the mass of the negative electrode active material, the mass of the polymer coating material is 1-10%.
7. The modified negative electrode active material according to claim 6, characterized in that: The modified negative electrode active material is prepared by the following method, which includes: mixing the negative electrode active material with a polymer coating material dispersion to obtain a slurry; drying the slurry to obtain the modified negative electrode active material; Preferably, the drying method is spray drying; Preferably, the inlet temperature of the spray drying is 200-300°C; Preferably, the outlet temperature of the spray drying is 100-200°C; Preferably, the spray drying pressure is 0.2-0.8 MPa; Preferably, the feed rate of the slurry in the spray drying is 5-15 mL / min.
8. A negative electrode material composition, characterized in that: The negative electrode material composition comprises the modified negative electrode active material according to claim 6 or 7; Preferably, the negative electrode material composition comprises a combination of a modified negative electrode active material, a conductive agent, a binder and optionally a thickener.
9. A negative electrode plate, characterized in that: The negative electrode plate comprises a current collector and a coating disposed on the current collector, and the material of the coating comprises the negative electrode material composition as claimed in claim 8.
10. An electrochemical energy storage device, characterized in that: The electrochemical energy storage device comprises at least one of the polymer coating material according to any one of claims 1 to 4, the modified negative electrode active material according to claim 6 or 7, the negative electrode material composition according to claim 8, and the negative electrode sheet according to claim 9; Preferably, the electrochemical energy storage device comprises any one of a lithium ion battery, a sodium ion battery, a supercapacitor, a fuel cell or a solar cell, and a lithium ion battery is more preferred.
Citation Information
Cited By
Carbon nanotube conductive binder and synthesis and application thereof
CN119752405A
Modified conductive agent, manufacturing method thereof, all-solid-state battery and preparation method of all-solid-state battery
CN120878848A
Graphite material, negative plate, battery and electric device
CN121237838A
A graphite material, a negative electrode, a battery, and an electrical device.
CN121237838B
Graphite material, negative electrode sheet, battery, and electrical device
WO2026194755A1