Gas diffusion layer and preparation method and application thereof
By spraying hydrophilic reagents on the hydrophobic microporous layer and using ultrasonic spray technology, the problem of gas transport obstruction under high current density is solved, the performance of the membrane electrode and the drainage and gas conduction capacity of the gas diffusion layer are improved, and the gas diffusion layer is realized Excellent performance under high electrical density conditions.
Patent Information
- Application Number
- CN202410830421.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-25
AI Technical Summary
In the prior art, gas diffusion layers containing hydrophobic coatings under high current densities have the problem of hindered gas transport, especially the problems of water flooding and poor transmission of reactant gases under high current density conditions.
Use atomization technology to spray hydrophilic reagents composed of dioctyl sodium sulfonate, ethyl acetate or polyethylene glycol on the hydrophobic microporous layer, combined with ultrasonic spray technology to optimize the hydrophilic reagents The composition and spraying amount are used to reduce the surface energy of the catalytic layer and the microporous layer, and achieve uniform distribution of gas on the surface of the catalytic layer and drainage and gas conduction.
Under the condition of high electrical density, it can significantly improve the performance of membrane electrodes, reduce ohmic impedance, improve electron transmission capabilities, avoid obstruction of gas transportation, and maintain the wetting and water management effects of proton exchange membranes.
Smart Images

Figure CN118841578A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of membrane electrode technology, and in particular to a gas diffusion layer and a preparation method and application thereof. Background Art
[0002] Proton exchange membrane fuel cells (PEMFC) have the advantages of high energy conversion efficiency, fast low-temperature start-up, and zero emissions. They can be used for transportation and fixed power sources and are recognized as the ultimate energy source in the 21st century. The gas diffusion layer (GDL) is one of the key materials of proton exchange membrane fuel cells, playing the role of "gas-water-electricity-heat" conduction. Specifically, it is mainly responsible for: conducting electrons between the catalyst layer and the bipolar plate, efficiently transporting gases to the catalyst layer, maintaining the wetness of the proton exchange membrane, and effective water management.
[0003] The gas diffusion layer (GDL) is usually composed of a base layer and a microporous layer. The microporous layer is generally prepared by mixing conductive carbon powder and a hydrophobic agent in a certain proportion into a uniform slurry, and then treating it on the base layer of the gas diffusion layer by scraping or spraying. After high-temperature treatment, the microporous layer has the effect of reducing the contact resistance between the base layer and the catalyst layer, improving the pore structure, and forming the effect of redistribution of generated water and reaction gas. Although the GDL containing a hydrophobic coating can ensure the hydration of the proton exchange membrane at low current density, the transport of water will cause an increase in capillary pressure and hinder gas transport. This disadvantage is particularly significant at high current density. Summary of the invention
[0004] The invention provides a gas diffusion layer and a preparation method and application thereof, which are used to solve the defect of the gas diffusion layer containing a hydrophobic coating under high current density in the prior art that gas transport is blocked.
[0005] The present invention provides a method for preparing a gas diffusion layer, comprising: A hydrophilic reagent mainly composed of sodium dioctyl sulfosuccinate, substance A and water is sprayed on the hydrophobic microporous layer by an atomization process; the substance A is ethyl acetate and / or polyethylene glycol; The hydrophobic microporous layer is obtained by calcining a hydrophobic base layer containing microporous layer slurry.
[0006] The sodium dioctyl sulfosuccinate in the present invention has a CAS number of 577-11-7, also known as Surfactant.
[0007] Generally speaking, with regard to the distribution of hydrophilic and hydrophobic areas on the surface of the gas diffusion layer, under high current density conditions, the hydrophobic structure can to a certain extent prevent the generated water from accumulating on the surface of the catalyst layer, resulting in a reduction in active sites and a decrease in performance due to flooding, while preventing the accumulated water from causing the reaction gas to be unable to be transmitted to the surface of the catalyst layer in a timely manner; under low current density and high temperature conditions, the hydrophilic structure retains a certain amount of moisture, promotes the mass transfer of protons in the exchange membrane, and improves the performance of the membrane electrode.
[0008] The present invention optimizes the composition of the hydrophilic reagent and finds that when sodium dioctyl sulfosuccinate, the substance A and deionized water are used in combination, the membrane electrode performance can be significantly improved under high electric density conditions. Moreover, compared with other hydrophilic reagents, such as polyvinyl alcohol, N-vinyl formamide, etc., the present invention utilizes a low surface hydrophilic reagent to reduce the surface energy between the catalyst layer and the microporous layer, promote the uniform distribution of gas on the surface of the catalyst layer, and cooperate with the hydrophilic and hydrophobic effects to achieve excellent drainage and gas conduction of the gas diffusion layer under high electric density conditions, reduce ohmic impedance, and improve the ability of electron transmission.
[0009] According to the method for preparing the gas diffusion layer provided by the present invention, the hydrophilic reagent is composed of sodium dioctyl sulfosuccinate, substance A and water; Preferably, the mass proportion of sodium dioctyl sulfosuccinate in the hydrophilic reagent is 8-12%, and the mass ratio of substance A to water is 0.5-2:8.5-7.
[0010] According to the preparation method of the gas diffusion layer provided by the present invention, the carbon loading on the hydrophobic base layer after calcination is 1-2 mg / cm 2 .
[0011] According to the method for preparing the gas diffusion layer provided by the present invention, the preparation of the hydrophobic base layer comprises: immersing the carbon material in a dispersion containing a hydrophobic agent B so that the carbon material adsorbs the hydrophobic agent B, and then calcining; Preferably, the mass percentage of the hydrophobic agent B on the hydrophobic base layer after calcination is 5 to 10%; Preferably, the carbon material includes carbon paper and carbon cloth; Preferably, the hydrophobic agent B is one or a combination of two or more of polytetrafluoroethylene (PTFE), fluorinated ethylene propylene (FEP), and polyvinylidene fluoride (PVDF).
[0012] Generally, the dispersion containing the hydrophobic agent B is prepared by mixing the hydrophobic agent B with water, and the mass concentration is 5-10%.
[0013] During the soaking, the carbon material may contain the hydrophobic agent B that meets the requirements through multiple soaking.
[0014] According to the method for preparing the gas diffusion layer provided by the present invention, the microporous layer slurry is mainly composed of a conductive agent, a hydrophobic agent C and a solvent.
[0015] Preferably, the conductive agent is carbon powder, such as carbon black 50, carbon black 100, Li400, Li435, XC72, etc.
[0016] Preferably, the hydrophobic agent C is one or a combination of two or more of polytetrafluoroethylene (PTFE), fluorinated ethylene propylene (FEP), and polyvinylidene fluoride (PVDF).
[0017] The hydrophobic agent C in the microporous layer slurry and the hydrophobic agent B on the hydrophobic base layer may be the same or different, and are preferably the same type of hydrophobic agent.
[0018] Preferably, the solvent includes alcohol and water; more preferably, the alcohol includes one or a combination of two or more of ethanol, isopropanol, glycerol, and ethylene glycol.
[0019] According to the method for preparing the gas diffusion layer provided by the present invention, the mass ratio of the conductive agent to the hydrophobic agent C is 70-75:40-45; the mass percentage of the conductive agent in the microporous layer slurry is 10-15%.
[0020] According to the method for preparing the gas diffusion layer provided by the present invention, the spraying process includes: ultrasonic spraying.
[0021] Ultrasonic atomization is used to break up small droplets of low surface hydrophilic reagents, which can promote the uniform distribution of the solution in the gaps of the microporous layer without causing excessive hydrophilicity of the microporous layer to affect the removal of generated water under high electrical density conditions. At the same time, ultrasonic atomization has minimal impact on the microporous layer structure.
[0022] According to the method for preparing the gas diffusion layer provided by the present invention, the method comprises: The carbon paper is immersed in a dispersion containing a hydrophobic agent B to allow it to absorb the hydrophobic agent B, and then sintered at 350 to 400° C. for 30 to 60 minutes to obtain a hydrophobic carbon paper substrate layer; A microporous layer slurry containing carbon powder, a hydrophobic agent C and a solvent is sprayed on the hydrophobic carbon paper base layer, and then sintered at 350 to 400° C. for 30 to 60 minutes to obtain a gas diffusion layer containing a hydrophobic microporous layer; during spraying, the carbon loading on the gas diffusion layer can be controlled by controlling the spraying parameters to meet the requirements of the present invention.
[0023] The hydrophilic reagent is sprayed on the side of the gas diffusion layer where the hydrophobic microporous layer is located by ultrasonic spraying, and the propulsion speed is 3-10 ml / h. According to the projected area of the hydrophobic microporous layer, the spraying amount of the hydrophilic reagent is less than 1 ml / cm 2, and obtain the gas diffusion layer.
[0024] When the ultrasonic spray process is used, the gas diffusion layer with different hydrophilic area ratios can be prepared by changing the propulsion speed of the injection pump.
[0025] The present invention also provides a gas diffusion layer, which is prepared by the method for preparing the gas diffusion layer as described above.
[0026] The present invention also provides a membrane electrode, comprising the gas diffusion layer as described above.
[0027] The gas diffusion layer provided by the present invention and its preparation method and application, by optimizing the composition of the hydrophilic reagent, found that when sodium dioctyl sulfosuccinate, the substance A and deionized water are used in combination, the membrane electrode performance is significantly improved under high electric density conditions. Moreover, compared with other hydrophilic reagents, such as polyvinyl alcohol, N-vinyl formamide, etc., the present invention utilizes a low surface hydrophilic reagent to reduce the surface energy between the catalyst layer and the microporous layer, promote the uniform distribution of gas on the surface of the catalyst layer, and cooperate with the hydrophilic and hydrophobic effects to achieve excellent drainage and gas conduction under high electric density conditions. The ohmic impedance is reduced and the electron transmission capacity is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 These are the membrane electrode performance test results of Comparative Examples 1 to 3 provided by the present invention. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Combine the following Figure 1 The gas diffusion layer of the present invention and its preparation method and application are described.
[0032] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.
[0033] The carbon powder in the present invention is American Cabot Carbon Black XC-72.
[0034] Example 1
[0035] A method for preparing a gas diffusion layer, the steps of which are as follows: (1) Take a 6 cm × 6 cm carbon paper, dry it, and weigh it.
[0036] (2) The dried carbon paper was immersed in a polytetrafluoroethylene (PTFE) dispersion (the solvent was water) with a mass content of 10%, and sintered at 360° C. for 30 min to obtain a hydrophobic carbon paper substrate layer with a PTFE mass percentage of 8%.
[0037] (3) 72 mg of carbon powder, 420 mg of a 10% polytetrafluoroethylene (PTFE) suspension (the solvent is water), 10 g of deionized water and 20 g of isopropanol were mixed and ultrasonically treated for 2 h to obtain an MPL slurry.
[0038] The MPL slurry was sprayed on the hydrophobic carbon paper substrate obtained in step (2), and sintered in a muffle furnace at 360° C. for 60 min to obtain a gas diffusion layer containing a hydrophobic microporous layer. The carbon loading on the gas diffusion layer was 2.0 mg / cm 2 .
[0039] (4) The surfactant, ethyl acetate and deionized water were mixed in a mass ratio of 1:1:8 to obtain a low surface hydrophilicity reagent.
[0040] The gas diffusion layer obtained in step (3) is placed on a heater, and the low surface hydrophilic reagent is sprayed on the side of the gas diffusion layer where the MPL slurry is located by a jet pump and an ultrasonic atomizer. The propulsion speed is 5 ml / h. According to the projected area of the hydrophobic microporous layer, the spraying amount of the hydrophilic reagent is 0.3 ml / cm 2 , and obtain a gas diffusion layer.
[0041] Example 2
[0042] A method for preparing a gas diffusion layer, wherein the steps are substantially the same as those in Example 1, except that the spraying rate is 0.1 ml / cm 2 .
[0043] Example 3
[0044] A method for preparing a gas diffusion layer, wherein the steps are substantially the same as those in Example 1, except that the spraying rate is 0.5 ml / cm 2 .
[0045] Example 4
[0046] A method for preparing a gas diffusion layer, wherein the steps are substantially the same as those of Example 1, except that ethyl acetate is replaced by polyethylene glycol.
[0047] Example 5
[0048] A method for preparing a gas diffusion layer, wherein the steps are substantially the same as those of Example 4, except that the spraying rate is 0.1 ml / cm 2 .
[0049] Example 6
[0050] A method for preparing a gas diffusion layer, wherein the steps are substantially the same as those of Example 4, except that the spraying rate is 0.5 ml / cm 2 .
[0051] Comparative Example 1
[0052] A method for preparing a gas diffusion layer, wherein the steps are substantially the same as those of Example 1, except that: Step (3) obtains a carbon loading of 1.0 mg / cm 2 The gas diffusion layer is directly used as the gas diffusion layer (ie, step (4) is not performed).
[0053] Comparative Example 2
[0054] A method for preparing a gas diffusion layer, wherein the steps are substantially the same as those of Comparative Example 1, except that: Step (3) obtains a carbon loading of 1.5 mg / cm 2 of the gas diffusion layer.
[0055] Comparative Example 3
[0056] A method for preparing a gas diffusion layer, wherein the steps are substantially the same as those of Comparative Example 1, except that: Step (3) obtains a carbon loading of 2.0 mg / cm 2 of the gas diffusion layer.
[0057] Comparative Example 4
[0058] A method for preparing a gas diffusion layer, wherein the steps are substantially the same as those of Example 1, except that ethyl acetate is replaced by polyacrylic acid.
[0059] Comparative Example 5
[0060] A method for preparing a gas diffusion layer, wherein the steps are substantially the same as those of Comparative Example 4, except that: Step (3) obtains a carbon loading of 1.0 mg / cm 2 of the gas diffusion layer.
[0061] Comparative Example 6
[0062] A method for preparing a gas diffusion layer, wherein the steps are substantially the same as those of Comparative Example 4, except that: Step (3) obtains a carbon loading of 1.5 mg / cm 2 of the gas diffusion layer.
[0063] The gas diffusion layers prepared in the embodiments and comparative examples were tested using the following test methods: Commercial CCM was used to test the gas diffusion layer prepared above under the same conditions (humidity An: 50%-Cn50%) on 850e.
[0064] The test results are as follows:
[0065] From Comparative Examples 1 to 3, it can be seen that under the same current density conditions, the membrane electrode power increases with the increase of carbon loading. This is because: the carbon loading can change the pore size distribution of the microporous layer. As the carbon loading increases, the pore size decreases and the capillary force increases, which can optimize the drainage performance under high current density conditions. From Comparative Examples 1 and 2, at 1A / cm 2 Under the condition of high current density, the power density decreases and the peak power shifts. This shows that under high current density operation conditions, when transporting water, the capillary pressure increases, which also leads to the obstruction of gas transport and affects the performance of the membrane electrode. Therefore, it is necessary to propose a method that can improve the function of the membrane electrode and promote the peak power to move towards high current density.
[0066] From Comparative Examples 4 to 6, it can be seen that after using the hydrophilic reagent polyacrylic acid, under the same electrical density conditions, the membrane electrode power is improved compared with Comparative Examples 1 to 3, and the peak power is shifted backward, which shows that the hydrophilic and hydrophobic synergistic surface has a promoting effect on gas conduction without affecting drainage. At the same time, from Comparative Examples 4 to 6, it can be seen that for low surface hydrophilic reagents containing film-forming agent polyacrylic acid, the carbon loading also affects the performance of the membrane electrode, and the greater the loading, the better the performance.
[0067] By comparison with Examples 1 to 3, based on the above process conditions, after the film-forming agent polyacrylic acid replaced the hydrophilic reagent ethyl acetate, the overall performance of the membrane electrode was improved under high current density conditions. This is because the presence of ester groups in ethyl acetate affects the surface hydrophilic effect, which can achieve water retention without affecting the drainage effect of the carbon microporous layer.
[0068] Comparing with Examples 4 to 6, when ethyl acetate is replaced with polyethylene glycol, a low surface hydrophilic agent, the performance is slightly decreased, but is better than that of polyacrylic acid.
[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a gas diffusion layer, characterized in that: include: A hydrophilic reagent mainly composed of sodium dioctyl sulfosuccinate, substance A and water is sprayed on the hydrophobic microporous layer by an atomization process; the substance A is ethyl acetate and / or polyethylene glycol; The hydrophobic microporous layer is obtained by calcining a hydrophobic base layer containing microporous layer slurry.
2. The method for preparing a gas diffusion layer according to claim 1, characterized in that: The hydrophilic agent is composed of sodium dioctyl sulfosuccinate, substance A and water; Preferably, the mass proportion of sodium dioctyl sulfosuccinate in the hydrophilic reagent is 8-12%, and the mass ratio of substance A to water is 0.5-2:8.5-7.
3. The method for preparing a gas diffusion layer according to claim 1 or 2, characterized in that: The carbon loading on the hydrophobic substrate after calcination is 1-2 mg / cm 2 .
4. The method for preparing a gas diffusion layer according to any one of claims 1 to 3, characterized in that: The preparation of the hydrophobic base layer comprises: immersing the carbon material in a dispersion containing a hydrophobic agent B to make it absorb the hydrophobic agent B, and then calcining; preferably, the mass percentage of the hydrophobic agent B on the hydrophobic base layer after calcination is 5-10%; Preferably, the carbon material includes carbon paper and carbon cloth; Preferably, the hydrophobic agent B is one or a combination of two or more of polytetrafluoroethylene, fluorinated ethylene propylene, and polyvinylidene fluoride.
5. The method for preparing a gas diffusion layer according to any one of claims 1 to 4, characterized in that: The microporous layer slurry is mainly composed of a conductive agent, a hydrophobic agent C and a solvent; Preferably, the conductive agent is carbon powder; Preferably, the hydrophobic agent C is one or a combination of two or more of polytetrafluoroethylene, fluorinated ethylene propylene, and polyvinylidene fluoride; Preferably, the solvent includes alcohol and water; more preferably, the alcohol includes one or a combination of two or more of ethanol, isopropanol, glycerol, and ethylene glycol.
6. The method for preparing a gas diffusion layer according to claim 5, characterized in that: The mass ratio of the conductive agent to the hydrophobic agent C is 70-75:40-45; the mass percentage of the conductive agent in the microporous layer slurry is 10-15%.
7. The method for preparing a gas diffusion layer according to any one of claims 1 to 6, characterized in that: The spraying process includes: ultrasonic spraying.
8. The method for preparing a gas diffusion layer according to any one of claims 1 to 7, characterized in that: The preparation method comprises: The carbon paper is immersed in a dispersion containing a hydrophobic agent B to allow it to absorb the hydrophobic agent B, and then sintered at 350 to 400° C. for 30 to 60 minutes to obtain a hydrophobic carbon paper substrate layer; Spraying a microporous layer slurry containing carbon powder, a hydrophobic agent C and a solvent onto the hydrophobic carbon paper substrate layer, and then sintering at 350-400° C. for 30-60 minutes to obtain a gas diffusion layer containing a hydrophobic microporous layer; The hydrophilic reagent is sprayed on the side of the gas diffusion layer where the hydrophobic microporous layer is located by ultrasonic spraying, and the propulsion speed is 3-10 ml / h. According to the projected area of the hydrophobic microporous layer, the spraying amount of the hydrophilic reagent is less than 1 ml / cm 2 , and obtain the gas diffusion layer.
9. A gas diffusion layer, characterized in that: The gas diffusion layer is prepared by the method for preparing the gas diffusion layer according to any one of claims 1 to 8.
10. A membrane electrode, characterized in that: Comprising the gas diffusion layer as claimed in claim 9.
Citation Information
Cited By
Preparation process of highly graphitized fuel cell microporous layer with hierarchical pore structure and gradient wetting performance
CN119419288A
Preparation process of highly graphitized fuel cell microporous layer with hierarchical pore structure and gradient wetting performance
CN119419288B