3D printing method for high-strength unfired mortar building component with traditional styles and features
By using powder materials of silicon carbide, lime and gelled materials in 3D printing technology, combined with jet printing and constant temperature and humidity treatment, the problem of material strength and interlayer bonding of traditional building components is solved, achieving high strength and low strength Cost and efficient manufacturing process are in line with the concept of sustainable development.
Patent Information
- Application Number
- CN202411227281.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-01
AI Technical Summary
The existing 3D printing technology faces challenges such as insufficient material strength and durability, interlayer bonding problems, and post-processing complexity in the manufacturing of traditional architectural components, resulting in increased manufacturing costs and time.
The powder material is prepared by mixing silicon carbide, lime, reinforcement and gelling materials in a specified proportion. The powder material is constructed layer by layer by layer by layer by spraying printer sprays, combined with computer-aided design and constant temperature and humidity box treatment, and realize high-strength traditional style buildings. member.
It realizes high-strength and low-cost 3D printed components, reduces energy consumption, improves material utilization, meets green and clean production requirements, and improves production efficiency.
Smart Images

Figure CN118876187A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of 3D printing, and in particular, relates to a 3D printing method for high-strength unfired mortar-sand traditional style building components. Background Art
[0002] With the continuous advancement of science and technology, 3D printing technology has demonstrated its unique advantages in many fields. 3D printing technology, also known as additive manufacturing technology, is a manufacturing method that constructs three-dimensional entities by adding materials layer by layer. Compared with traditional subtractive manufacturing, 3D printing technology has the advantages of high design flexibility, high material utilization, and short production cycle. In the field of architecture, the application of 3D printing technology is particularly eye-catching. Traditional methods of manufacturing building components often require a lot of manpower and time, and the manufacturing process is even more challenging for components with complex shapes. The emergence of 3D printing technology has made it possible to quickly manufacture complex components, especially for the manufacture of traditional architectural components.
[0003] Traditional methods of manufacturing architectural components usually rely on hand carving or mold casting, which are not only time-consuming and labor-intensive, but also difficult to reproduce complex structures and fine details. 3D printing technology, with its advantages of high design freedom, high material utilization, and high printing accuracy, provides a new solution for the manufacture of components with complex geometries and internal structures. Existing 3D printing technology still faces some challenges when applied to the manufacture of architectural components with traditional style. First, the strength and durability of most 3D printed building materials have not yet reached the level of traditional building materials. Secondly, the problem of interlayer bonding during the printing process is still a technical problem that affects the overall performance of the component. In addition, the post-printing post-processing process is complicated, which increases the manufacturing cost and time. Therefore, it is necessary to develop a 3D printing method suitable for the manufacture of architectural components with traditional style as soon as possible.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a 3D printing method for high-strength, unfired mortar-free traditional-style building components, thereby solving the problems raised in the above-mentioned background technology.
[0006] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is: A 3D printing method for high-strength non-fired mortar traditional style building components, comprising the following steps: Step 1: Use computer-aided design software to design a three-dimensional model and generate a model file; Step 2: Import the generated model file into the 3D printer, use the printer's built-in slicing software to slice the model layer by layer to generate a two-dimensional printing path; Step 3: Evenly mix silicon carbide, lime, reinforcing material and cementitious material in a specified mass ratio to prepare a powder material; Step 4: Spread the prepared powder material evenly on the printing platform, and then spray the printer spray on the powder material according to the printing path for molding; Step 5: During the printing process, repeat the process of laying powder and spraying printer spray in step 4, building layer by layer until a complete three-dimensional component is formed; Step 6: After the printing process is completed, the printed component is retained together with the printing platform in the printing chamber, and the printing chamber is heated to solidify the printed component; Step 7: After curing, take the component out of the printing chamber, remove the uncured powder on the surface of the component, and obtain a preliminary 3D printed component; Step 8: Place the component after removing the powder in a constant temperature and humidity chamber for curing until the set curing time is reached. After the curing time is reached, the final 3D printed component is obtained.
[0007] Optionally, in step 3, the powder material is obtained by uniformly mixing silicon carbide, lime, reinforcing material and cementitious material in a mass ratio of 3:1.5:0.15 to 0.2:1.
[0008] Optionally, when spraying printer spray on the powder material in step 4, 0.25 to 1 portion of printer spray is sprayed for every portion of powder material used.
[0009] Optionally, when the component is cured in step 6, the temperature of the printing chamber is 40-60°C.
[0010] Optionally, in step 8, the temperature of the constant temperature and humidity chamber is 20° C. to 25° C. and the humidity is 60% to 70%, and the curing time is 24 hours.
[0011] Optionally, the silicon carbide is industrial green silicon carbide with a particle size of 10 to 200 meshes.
[0012] Optionally, the reinforcing material is short-cut mullite fiber with a diameter of 5-20 µm and a length of 3-10 mm.
[0013] Optionally, the cementitious material is at least one of high alumina cement, sulphoaluminate cement, magnesium phosphate cement and geopolymer.
[0014] Optionally, the printer spray is at least one of water glass, silica sol, aluminum sol, and aluminum phosphate sol.
[0015] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art. Of course, any product implementing the present invention does not necessarily need to achieve all the advantages described below at the same time: The 3D printing method of the present invention has significant advantages. There is no need to consider the rheology and thixotropy of the printing material. The printer spray is directly sprayed on the powder material, which effectively solves the problem of material non-flow or easy collapse in the traditional method; the mixed material can harden quickly and has high strength after hardening. Each layer of material has little deformation during the stacking process, and the layers are tightly bonded to each other, showing excellent stacking performance and high inter-layer strength, reducing the anisotropy of the component; in addition, the printed component is quickly solidified in the printing chamber, and a firing-free process is adopted, which greatly saves energy, meets the requirements of green and clean production, improves production efficiency, and reduces manufacturing costs. At the same time, the unsolidified powder on the surface of the component can be recycled, which greatly improves the utilization rate of the material, reduces waste, and conforms to the concept of sustainable development.
[0016] The specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The drawings described below are only some embodiments. For those skilled in the art, other drawings can be obtained based on these drawings without creative work. In the drawings: Figure 1 This is a schematic diagram of printed traditional architectural components.
[0018] It should be noted that these drawings and textual descriptions are not intended to limit the conceptual scope of the present invention in any way, but are intended to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION
[0019] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0020] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0021] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0022] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0023] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0024] See also Figure 1 As shown, in this embodiment, a 3D printing method for high-strength non-fired mortar-sand traditional style building components is provided, comprising the following steps: Step 1: Use computer-aided design software to design a three-dimensional model and generate a model file; Step 2: Import the generated model file into the 3D printer, use the printer's built-in slicing software to slice the model layer by layer to generate a two-dimensional printing path; Step 3: Evenly mix silicon carbide, lime, reinforcing material and cementitious material in a specified mass ratio to prepare a powder material; Step 4: Spread the prepared powder material evenly on the printing platform, and then spray the printer spray on the powder material according to the printing path for molding; Step 5: During the printing process, repeat the process of laying powder and spraying printer spray in step 4, building layer by layer until a complete three-dimensional component is formed; Step 6: After the printing process is completed, the printed component is retained together with the printing platform in the printing chamber, and the printing chamber is heated to solidify the printed component; Step 7: After curing, take the component out of the printing chamber, remove the uncured powder on the surface of the component, and obtain a preliminary 3D printed component; Step 8: Place the component after removing the powder in a constant temperature and humidity chamber for curing until the set curing time is reached. After the curing time is reached, the final 3D printed component is obtained.
[0025] In some embodiments of the present invention, the powder material in step 3 is obtained by uniformly mixing silicon carbide, lime, reinforcing material and cementitious material in a mass ratio of 3:1.5:0.15 to 0.2:1.
[0026] According to a 3D printing method for a high-strength, unfired mortar traditional style building component according to claim 1, it is characterized in that when the printer spray is sprayed on the powder material in step 4, 0.25 to 1 part of the printer spray is sprayed for every 1 part of the powder material used.
[0027] In some embodiments of the present invention, when the component is cured in step 6, the temperature of the printing chamber is 40-60°C.
[0028] In some embodiments of the present invention, the temperature of the constant temperature and humidity chamber in step 8 is 20° C. to 25° C. and the humidity is 60% to 70%, and the curing time is 24 hours.
[0029] In some embodiments of the present invention, the silicon carbide is industrial green silicon carbide with a particle size of 300 mesh.
[0030] In some embodiments of the present invention, the reinforcing material is short-cut mullite fiber with a diameter of 20 μm and a length of 3 mm.
[0031] In some embodiments of the present invention, the cementitious material is at least one of high alumina cement, sulphoaluminate cement, magnesium phosphate cement, and geopolymer.
[0032] In some embodiments of the present invention, the printer spray is at least one of water glass, silica sol, aluminum sol, and aluminum phosphate sol.
[0033] The present invention will now be further described in detail with reference to embodiments.
[0034] It should be noted that all raw materials in the examples of the present invention were obtained through commercial sources.
[0035] The model files in the following embodiments are STL format files.
[0036] Example 1: 3 kg of silicon carbide, 1.5 kg of lime, 0.15 kg of short-cut mullite fiber, and 1 kg of high-alumina cement are weighed, and the specific steps of 3D printing are as follows: Step S11: Design a three-dimensional model of a traditional architectural component using computer design software, determine the geometric parameters of the model, and generate a model file in STL format; Step S12: Import the model file in STL format into the 3D printer, and use the built-in slicing software of the printer to slice the model layer by layer to generate a two-dimensional printing path.
[0037] Step S13: mixing silicon carbide, lime, short-cut mullite fiber and high-alumina cement uniformly to prepare a powder material; Step S14: Lay the configured powder material on the printing platform of the 3D printer, and then spray 0.25 parts of silica sol on 1 part of the powder material according to the mass ratio along the printing path to print and shape it layer by layer.
[0038] Step S15: During the printing process, the process of spreading powder and spraying printer spray in step 4 is repeated, and the structure is constructed layer by layer until a complete three-dimensional component is formed.
[0039] Step S16: After the printing process is completed, the printed component is retained together with the printing platform in the printing chamber, and then the printing chamber is heated to 40° C. to solidify the printed component; Step S17: After curing, the component is taken out from the printing chamber, and the uncured powder on the surface of the component is removed to obtain a preliminary 3D printed component; Step S18: Place the component after removing the powder in a constant temperature and humidity chamber at a temperature of 20° C. and a humidity of 60% for curing for 24 hours. After the curing time is up, the final 3D printed component is obtained.
[0040] Example 2: 3 kg of silicon carbide, 1.5 kg of lime, 0.15 kg of short-cut mullite fiber, and 1 kg of sulphoaluminate cement were weighed, and the specific steps of 3D printing were as follows: Step S21: Design a three-dimensional model of a traditional architectural component using computer design software, determine the geometric parameters of the model, and generate a model file in STL format; Step S22: Import the model file in STL format into the 3D printer, and use the built-in slicing software of the printer to slice the model layer by layer to generate a two-dimensional printing path.
[0041] Step S23: mixing silicon carbide, lime, short-cut mullite fiber and sulphoaluminate cement uniformly to prepare a powder material; Step S24: Lay the configured powder material on the printing platform of the 3D printer, and then spray 0.5 parts of aluminum sol on 1 part of the powder material according to the mass ratio along the printing path to print and shape it layer by layer.
[0042] Step S25: During the printing process, the process of spreading powder and spraying printer spray in step 4 is repeated, and the structure is constructed layer by layer until a complete three-dimensional component is formed.
[0043] Step S26: After the printing process is completed, the printed component is retained together with the printing platform in the printing chamber, and then the printing chamber is heated to 45° C. to solidify the printed component; Step S27: After curing, the component is taken out from the printing chamber, and the uncured powder on the surface of the component is removed to obtain a preliminary 3D printed component; Step S28: Place the component after removing the powder in a constant temperature and humidity chamber at a temperature of 20° C. and a humidity of 60% for curing for 24 hours. After the curing time is up, the final 3D printed component is obtained.
[0044] Example 3: 3 kg of silicon carbide, 1.5 kg of lime, 0.15 kg of short-cut mullite fiber, and 1 kg of magnesium phosphate cement were weighed, and the specific steps of 3D printing were as follows: Step S31: Design a three-dimensional model of a traditional architectural component using computer design software, determine the geometric parameters of the model, and generate a model file in STL format; Step S32: Import the model file in STL format into the 3D printer, and use the built-in slicing software of the printer to slice the model layer by layer to generate a two-dimensional printing path.
[0045] Step S33: mixing silicon carbide, lime, short-cut mullite fiber and magnesium phosphate cement uniformly to prepare a powder material; Step S34: Lay the configured powder material on the printing platform of the 3D printer, and then spray 0.75 parts of aluminum phosphate sol on 1 part of the powder material according to the mass ratio along the printing path to print and shape it layer by layer.
[0046] Step S35: During the printing process, the process of spreading powder and spraying printer spray in step 4 is repeated, and the structure is constructed layer by layer until a complete three-dimensional component is formed.
[0047] Step S36: After the printing process is completed, the printed component is retained together with the printing platform in the printing chamber, and then the printing chamber is heated to 50° C. to solidify the printed component; Step S37: After curing, the component is taken out from the printing chamber, and the uncured powder on the surface of the component is removed to obtain a preliminary 3D printed component; Step S38: Place the component after the powder is removed into a constant temperature and humidity chamber at a temperature of 20° C. and a humidity of 60% for curing for 24 hours. After the curing time is up, the final 3D printed component is obtained.
[0048] Example 4: 3 kg of silicon carbide, 1.5 kg of lime, 0.15 kg of short-cut mullite fiber, and 1 kg of geopolymer were weighed, and the specific steps of 3D printing were as follows: Step S41: Design a three-dimensional model of a traditional architectural component using computer design software, determine the geometric parameters of the model, and generate a model file in STL format; Step S42: Import the model file in STL format into the 3D printer, and use the built-in slicing software of the printer to slice the model layer by layer to generate a two-dimensional printing path.
[0049] Step S43: mixing silicon carbide, lime, short-cut mullite fiber and geopolymer uniformly to prepare a powder material; Step S44: Lay the configured powder material on the printing platform of the 3D printer, and then spray 1 part of water glass on 1 part of the powder material according to the mass ratio along the printing path to print and shape it layer by layer.
[0050] Step S45: During the printing process, the process of spreading powder and spraying printer spray in step 4 is repeated, and the structure is constructed layer by layer until a complete three-dimensional component is formed.
[0051] Step S46: After the printing process is completed, the printed component is retained together with the printing platform in the printing chamber, and then the printing chamber is heated to 55° C. to solidify the printed component; Step S47: After curing, the component is taken out from the printing chamber, and the uncured powder on the surface of the component is removed to obtain a preliminary 3D printed component; Step S48: Place the component after removing the powder in a constant temperature and humidity chamber at a temperature of 20° C. and a humidity of 60% for curing for 24 hours. After the curing time is up, the final 3D printed component is obtained.
[0052] Example 5: 3 kg of silicon carbide, 1.5 kg of lime, 0.2 kg of short-cut mullite fiber, and 1 kg of high-alumina cement were weighed, and the specific steps of 3D printing were as follows: Step S51: Design a three-dimensional model of a traditional architectural component using computer design software, determine the geometric parameters of the model, and generate a model file in STL format; Step S52: Import the model file in STL format into the 3D printer, and use the built-in slicing software of the printer to slice the model layer by layer to generate a two-dimensional printing path.
[0053] Step S53: mixing silicon carbide, lime, short-cut mullite fiber and high-alumina cement uniformly to prepare a powder material; Step S54: Lay the configured powder material on the printing platform of the 3D printer, and then spray one part of silica sol on one part of the powder material according to the mass ratio along the printing path to print and shape it layer by layer.
[0054] Step S55: During the printing process, the process of spreading powder and spraying printer spray in step 4 is repeated, and the structure is constructed layer by layer until a complete three-dimensional component is formed.
[0055] Step S56: After the printing process is completed, the printed component is retained together with the printing platform in the printing chamber, and then the printing chamber is heated to 60° C. to solidify the printed component; Step S57: After curing, the component is taken out from the printing chamber, and the uncured powder on the surface of the component is removed to obtain a preliminary 3D printed component; Step S58: Place the component after removing the powder in a constant temperature and humidity chamber at a temperature of 20° C. and a humidity of 60% for curing for 24 hours. After the curing time is up, the final 3D printed component is obtained.
[0056] Comparative Example 1: In Example 1, high alumina cement was replaced with ordinary Portland cement.
[0057] Comparative Example 2: In Example 1, silicon carbide was removed.
[0058] Comparative Example 3: In Example 1, the lime was removed.
[0059] Comparative Example 4: In Example 1, the chopped mullite fibers were removed.
[0060] Comparative Example 5: In Example 1, step S14 is omitted, and the material is directly naturally cured and cured at room temperature.
[0061] Related performance tests: The processing characteristics and construction performances provided by the above Examples 1 to 5 and Comparative Examples 1 to 5 are shown in Table 1.
[0062] Table 1 Comparison results of examples and comparative examples 1 day compressive strength (MPa) 28-day compressive strength (MPa) Example 1 23 64 Example 2 26 66 Example 3 34 75 Example 4 32 71 Example 5 21 59 Comparative Example 1 17 46 Comparative Example 2 22 57 Comparative Example 3 20 59 Comparative Example 4 19 60 Comparative Example 5 18 61 From the test results in the above table, it can be seen that Examples 1-5 exhibit relatively high 1-day and 28-day compressive strengths, especially Examples 3 and 4, which exhibit the highest 28-day compressive strengths (75 MPa and 71 MPa), indicating that their material ratios and process designs have significant effects in improving the early and long-term strength of the materials.
[0063] The 1-day and 28-day compressive strengths of all comparative examples are lower than those of the examples, which indicates that replacing the cementitious material and removing certain materials will have a negative impact on the material properties.
[0064] The compressive strength of Comparative Example 1 decreased significantly, especially the 28-day compressive strength, which was only 46 MPa, indicating that ordinary Portland cement could not provide the same strength instead of high alumina cement.
[0065] The removal of silicon carbide in Comparative Example 2 resulted in a decrease in the 28-day compressive strength to 57 MPa, indicating the importance of silicon carbide in enhancing the strength of the material.
[0066] After removing the lime, the 28-day compressive strength of Comparative Example 3 is 59 MPa, which is slightly higher than that of Comparative Example 2, indicating that the lime has some contribution to the material properties.
[0067] The compressive strength of Comparative Example 4 after removing the short-cut mullite fibers is 60 MPa, indicating the enhancing effect of the fibers on the crack resistance and toughness of the material.
[0068] In Comparative Example 5, in which heating curing is omitted and natural curing is adopted, the compressive strengths at 1 day and 28 days are 18 MPa and 61 MPa, respectively, indicating that natural curing is not sufficient to quickly form a high-strength structure.
[0069] The present invention ensures that the material has excellent fluidity during the 3D printing process by using silicon carbide, lime, short-cut mullite fiber and gelling material. This fluidity enables the powder material to be evenly spread and filled, avoiding the phenomenon of material accumulation or unevenness during the printing process.
[0070] The stability and consistency of the materials during the printing process are ensured, and the blockage of the print head and the errors during the printing process are reduced. Cementitious materials such as high-alumina cement provide sufficient bonding force, so that the printed layers can be firmly combined, ensuring that the printed components are highly accurate and have clear edges. Secondly, the present invention adopts a firing-free process, which does not require a traditional sintering process, reduces pollution to the environment, and meets the requirements of green environmental protection. In addition, the selection of harmless and recyclable materials helps to reduce carbon footprint, which is in line with the concept of sustainable development. Moreover, since no high-temperature sintering and complex post-processing processes are required, the present invention greatly reduces energy consumption compared to traditional manufacturing methods. The printing process only requires moderate heating to achieve rapid curing, which further reduces energy consumption and makes the entire production process more economical and efficient. Finally, the use of reinforcing materials such as silicon carbide and short-cut mullite fibers of the present invention greatly improves the compressive strength and flexural strength of the components. According to the test results, the 28-day compressive strength can reach up to 75 MPa, indicating that this material combination can meet the needs of high-strength building components and is suitable for load-bearing structure applications.
[0071] The present invention is not limited to the above-mentioned embodiments. Anyone should be aware that any structural changes made under the enlightenment of the present invention, and any technical solutions that are the same or similar to the present invention, fall within the protection scope of the present invention. The technology, shape, and structural parts not described in detail in the present invention are all well-known technologies.
Claims
1. A 3D printing method for high-strength unfired mortar-sand traditional style building components, characterized in that: The following steps are involved: Step 1: Use computer-aided design software to design a three-dimensional model and generate a model file; Step 2: Import the generated model file into the 3D printer, use the printer's built-in slicing software to slice the model layer by layer to generate a two-dimensional printing path; Step 3: Evenly mix silicon carbide, lime, reinforcing material and cementitious material in a specified mass ratio to prepare a powder material; Step 4: Spread the prepared powder material evenly on the printing platform, and then spray the printer spray on the powder material according to the printing path for molding; Step 5: During the printing process, repeat the process of laying powder and spraying printer spray in step 4, building layer by layer until a complete three-dimensional component is formed; Step 6: After the printing process is completed, the printed component is retained together with the printing platform in the printing chamber, and the printing chamber is heated to solidify the printed component; Step 7: After curing, take the component out of the printing chamber, remove the uncured powder on the surface of the component, and obtain a preliminary 3D printed component; Step 8: Place the component after removing the powder in a constant temperature and humidity chamber for curing until the set curing time is reached. After the curing time is reached, the final 3D printed component is obtained.
2. The 3D printing method of a high-strength, unburned mortar-sand traditional style building component according to claim 1 is characterized in that: In step 3, the powder material is obtained by uniformly mixing silicon carbide, lime, reinforcing material and cementitious material in a mass ratio of 3:1.5:0.15-0.2:
1.
3. The 3D printing method of a high-strength, unburned mortar-sand traditional style building component according to claim 1, characterized in that: When spraying the printer spray on the powder material in step 4, spray 0.25 to 1 part of the printer spray for every 1 part of the powder material used.
4. The 3D printing method of a high-strength non-fired mortar traditional style building component according to claim 1 is characterized in that: When the component is cured in step 6, the temperature of the printing chamber is 40~60℃.
5. The 3D printing method of a high-strength, unfired mortar-sand traditional style building component according to claim 1, characterized in that: In step 8, the temperature of the constant temperature and humidity chamber is 20° C. to 25° C. and the humidity is 60% to 70%, and the curing time is 24 hours.
6. The 3D printing method of a high-strength, unfired mortar-sand traditional style building component according to claim 1, characterized in that: The silicon carbide is industrial green silicon carbide with a particle size of 10-200 meshes.
7. The 3D printing method of a high-strength, unfired mortar-sand traditional style building component according to claim 1, characterized in that: The reinforcing material is short-cut mullite fiber with a diameter of 5-20 μm and a length of 3-10 mm.
8. The 3D printing method of a high-strength, unfired mortar-sand traditional style building component according to claim 1, characterized in that: The cementitious material is at least one of high alumina cement, sulphoaluminate cement, magnesium phosphate cement and geopolymer.
9. The 3D printing method of a high-strength, unfired mortar-sand traditional style building component according to claim 1, characterized in that: The printer spray is at least one of water glass, silica sol, aluminum sol and aluminum phosphate sol.
Citation Information
Cited By
3D printing lightweight high-strength low-carbon cement-based material and preparation method thereof
CN119320261A