Stripe composite structure fluorescent material as well as preparation method and application thereof
By using striped composite structure fluorescent materials in white LED/LD light sources, alternately arranging red and green fluorescent films on yellow fluorescent ceramics, the problem of insufficient red and green light in fluorescent ceramics is solved, and high color rendering index and high Full spectrum illumination efficiency and improves the thermal conductivity and preparation cost-effectiveness of the material.
Patent Information
- Application Number
- CN202411093843.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Due to the lack of green and red components in fluorescent ceramics, the existing white LED/LD light sources have low color rendering index and low luminous efficiency, making full spectrum illumination impossible.
Using striped composite structure fluorescent materials, red and green fluorescent films are alternately arranged on the main structure of yellow fluorescent ceramics. They are prepared by solid phase reaction method and low-temperature sintering technology to ensure the equal width and thickness distribution of red and green fluorescent films, and make up for the fluorescent ceramics. The problem of insufficient red and green light.
Achieve high color rendering index and high luminous efficiency white LED/LD lighting, with a color rendering index of 86-96, a color temperature of 3000-6000K, a luminous efficiency of 140-180lm/W, and the material has excellent thermal conductivity and low cost preparation Craft.
Smart Images

Figure CN118930329A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of inorganic luminescent materials, and in particular to a composite fluorescent material with high color rendering index, high light efficiency and high thermal conductivity for white light LED / LD and a preparation method thereof. Background Art
[0002] Against the backdrop of increasingly serious global issues such as energy crisis, climate warming, and ecological pollution, solid-state lighting technology based on semiconductor chips is considered to be a new generation of green solid-state lighting sources in the 21st century due to its significant advantages such as energy saving, high reliability, long service life, high luminous efficiency, and green environmental protection. With the rapid development of the solid-state lighting industry, a new lighting method, "full-spectrum lighting", is emerging with each passing day. The emission spectrum of "full-spectrum lighting" is similar to the spectrum of sunlight, with light of all wavelengths in the visible light region of the human eye, and can truly and effectively restore the original color of the illuminated object. However, the current mainstream implementation scheme of white light LED / LD light sources is still blue light LED / LD excitation of garnet-type YAG:Ce yellow fluorescent materials. The green and red components are missing in the emission spectrum of YAG:Ce yellow fluorescent materials, so white light LED / LD light sources face the problems of low color rendering index, high color temperature, and low light color quality, making it difficult to achieve full-spectrum lighting.
[0003] At present, the main methods used by researchers to regulate the spectrum of YAG:Ce fluorescent ceramics are: ① Co-doping luminescent ions (Journal of Materials Chemistry C, 2020, 8(13): 4329-4337.), such as Cr 3+ , Pr 3+ , Mn 2+ 、Sm 3+ However, the red light supplemented by this scheme is limited, and there is energy transfer between the co-doped luminescent ions, thereby reducing the luminescence efficiency; ② By stacking YAG:Ce fluorescent ceramics with fluorescent ceramics with red light emission (Optics Express, 2023, 31(15): 24914-24925.), however, this scheme will severely limit the luminescence efficiency of each emission layer, and lacks the cyan part, and the cost is relatively high; ③ Adjust the chemical composition of the matrix (CN111393166A), by replacing the octahedral A1 lattice with the rare earth element Sc, Gd 3+ Ion-substituted dodecahedron Y 3+ Although ions effectively solve the problem of insufficient cyan light in fluorescent ceramics, the red light component is insufficient and full-spectrum lighting cannot be achieved.
[0004] Chinese invention patent CN113979739A arranges multiple fluorescent ceramics alternately on a plane to form a composite fluorescent ceramic, which is placed vertically on the excitation surface of a light-emitting chip to obtain a light-emitting device. After being excited by the same light-emitting chip, the composite fluorescent ceramic can obtain light of different colors, and the light of different colors is combined into a uniform white light. Since the spot of laser illumination is small, the composite fluorescent ceramic is only suitable for white light LED illumination. In addition, the composite fluorescent ceramic lacks a green light layer, cannot achieve full-spectrum illumination, and has a high production cost.
[0005] In summary, fluorescent ceramics for white light LED / LD cannot achieve full spectrum emission, and have problems such as low color rendering index, low luminous efficiency, and re-absorption. Therefore, it is urgent to develop composite fluorescent materials that can solve the above problems. Summary of the invention
[0006] In order to solve the above problems, the present invention provides a stripe composite structure fluorescent material and its preparation method and application. The stripe composite structure fluorescent material is used as a high-quality luminescent fluorescent material for white light LED / LD for white light LED / LD lighting. The structural composite fluorescent material can effectively solve the problems of low light color quality and low luminous efficiency of ceramics, and the whole preparation process is simple, the process is stable and controllable, and the cost is low.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] A striped composite structure fluorescent material, comprising a yellow fluorescent ceramic main structure and a layer of red and green fluorescent films of equal width and thickness coated on the upper surface of the yellow fluorescent ceramic main structure, the thickness of the yellow fluorescent ceramic is 1-1.8 mm, the thickness of the red and green fluorescent films are both 50-60 μm, and the width of the red and green fluorescent glass films are both 1-1.5 mm.
[0009] The chemical composition of the yellow fluorescent ceramic main structure is (Y 1-x Ce x )3Al5O 12 , 0.001≤x≤0.01; the chemical composition of the red fluorescent film is (Sr,Ca)AlSiN3:Eu 2+ ; The chemical composition of the green fluorescent film is β-SiAlON:Eu 2+ .
[0010] The yellow fluorescent ceramic is garnet ceramic (Y 1-x Ce x )3Al5O 12 Center 3+The ion concentration is 0.2 at%-1.0 at%, and the weight ratio of the green phosphor in the green fluorescent film to the red phosphor in the red fluorescent film is (1-5):1, preferably (1-2):1.
[0011] The raw material phosphor used in the red fluorescent film is (Sr,Ca)AlSiN3:Eu 2+ , particle size is 200nm-250nm; the raw material phosphor used in the green fluorescent film is β-SiAlON:Eu 2+ The particle size is 200nm-250nm.
[0012] The present invention also provides a method for preparing the stripe composite structure fluorescent material, using a solid phase reaction method combined with vacuum sintering technology to prepare yellow fluorescent ceramics (Y 1-x Ce x )3Al5O 12 The fluorescent ceramic sheet is YAG:Ce fluorescent ceramic, and then the slurry of red and green fluorescent films is coated on the surface of the yellow fluorescent ceramic by a scraper, and the striped composite structure fluorescent material is prepared by low temperature sintering technology, which specifically includes the following steps:
[0013] (1) YAG:Ce fluorescent ceramics were prepared by solid phase reaction technology;
[0014] (2) After coating the gel-state red and green fluorescent glass films on the YAG:Ce fluorescent ceramics through a mold, a striped composite structure fluorescent material is obtained by low-temperature sintering technology.
[0015] Furthermore, the preparation method of the YAG:Ce fluorescent ceramic in step (1) is as follows:
[0016] ① According to the chemical stoichiometric formula (Y 1-x Ce x )3Al5O 12 , 0.001≤x≤0.01, accurately weigh the required powder raw materials, wherein the powder raw materials are Al2O3, Y2O3 and CeO2, and then place them in a nylon ball mill for planetary ball milling for 15-25h, wherein the ball milling speed is set to 200r / min, the ball milling beads are Al2O3 balls, and the ball milling medium is anhydrous ethanol. The slurry after ball milling is poured into an evaporating dish and placed in an 80℃ electric blast drying oven for drying for 24h, and then passed through a 200-mesh sieve 5 times to obtain a mixed powder;
[0017] ② The mixed powder is placed in a stainless steel mold with a diameter of 22 mm, and a unidirectional pressure is applied to it by a press to make it into a green billet with a certain strength, wherein the applied pressure is 20 MPa, and the holding time is 5 min. After the dry pressed green billet is packaged, it is placed in a cold isostatic press for cold isostatic pressing, and the holding pressure is 300 MPa, and the holding time is 300 s. The obtained green billet is calcined in an air atmosphere in a muffle furnace at 800-900 ° C for 10 h to remove impurities;
[0018] ③ Place the impurity-removed blank in a vacuum tungsten wire furnace at 1765℃ and 5×10 -4 After sintering for 10 h under a vacuum degree of 0.03 Pa, the ceramic was annealed in an air atmosphere at 1450° C. for 10 h. The annealed ceramic was double-sided polished to 1 mm to obtain YAG:Ce fluorescent ceramic.
[0019] Furthermore, the preparation method of the stripe composite structure fluorescent material in step (2) is as follows:
[0020] ① Using an analytical balance to accurately weigh the required powder raw materials according to the chemical stoichiometric formula 38SiO2-40B2O3-4ZnO-4Na2O-3Al2O3-1Li2O (mol%), wherein the powder raw materials are SiO2, B2O3, ZnO, Na2O, Al2O3 and Li2O, and then fully grind them in an agate mortar, pour the ground mixed powder into an alumina crucible and sinter in a high-temperature furnace at 1300°C for 2h to obtain a molten liquid, pour it into a copper mold and cool it to obtain a precursor glass block, and finally grind the precursor glass block into powder and pass it through a 100-mesh sieve to obtain a precursor glass powder;
[0021] ② Mix the precursor glass powder with commercial (Sr,Ca)AlSiN3:Eu 2+ The red fluorescent glass film slurry is obtained by mixing the red fluorescent powder and the organic binder, and the precursor glass powder is mixed with the commercial (Sr, Ca)AlSiN3:Eu 2+ The total mass of the red phosphor is 0.5g. The composition of the organic binder is: 0.15g ethyl cellulose, 150μL pinene alcohol, 300μL ethyl acetate. The precursor glass powder is mixed with commercial β-SiAlON:Eu 2+ Green fluorescent powder is mixed with organic binder to obtain green fluorescent glass film slurry, and the precursor glass powder is mixed with commercial β-SiAlON:Eu 2+ Based on the total mass of the green phosphor being 0.5 g, the composition of the organic binder is: 0.15 g ethyl cellulose, 150 μL pinene alcohol, and 300 μL ethyl acetate; the weight ratio of the green phosphor to the precursor glass powder is 3:1, and the weight ratio of the green phosphor to the red phosphor is (1-5):1.
[0022] Furthermore, β-SiAlON:Eu2+ Green phosphor and (Sr,Ca)AlSiN3:Eu 2+ The weight ratio of the red phosphor is 1: 1, 2: 1, 3: 1, 4: 1, 5: 1. Preferably, the green fluorescent glass film contains 0.125 g of glass powder and 0.375 g of green phosphor, and the red fluorescent glass film contains 0.125-0.425 g of glass powder and 0.075-0.375 g of red phosphor.
[0023] ③ Place the 3D printed mold on the YAG:Ce fluorescent ceramic sheet and fix it on the glass substrate with tape, scrape the red fluorescent glass film slurry on the YAG:Ce ceramic sheet through the 3D printed mold with a scraper, dry it in a 150℃ electric blast drying oven for 3 hours, then translate the 3D printed mold on the YAG:Ce fluorescent ceramic sheet by a red fluorescent film width, and fix it on the glass substrate again, scrape the green fluorescent glass film slurry on the YAG:Ce ceramic sheet through the 3D printed mold with a scraper, and dry it in a 150℃ electric blast drying oven for 3 hours; the obtained composite fluorescent material is sintered to obtain a striped composite structure fluorescent material;
[0024] Furthermore, the sintering procedure is: keep warm at 120℃-130℃ for 0.5h-1h, keep warm at 400℃-450℃ for 0.5h-1h, and after the heat preservation, cool the sample to room temperature in an argon atmosphere.
[0025] The present invention also provides the application of the striped composite structure fluorescent material in the field of fluorescence conversion white light LED / LD lighting, characterized in that: when it is applied to a white light LED lighting device, the excitation source is a blue light LED chip; when it is applied to a white light LD lighting device, the excitation source is a blue light LD chip.
[0026] Furthermore, under the excitation of a 450-460nm blue light LED / LD chip, the first layer of YAG:Ce fluorescent ceramic main structure emits yellow light, and the second layer of red and green fluorescent glass films emit red light and green light respectively, and mix with the unabsorbed blue light to form white light, effectively avoiding the reabsorption of red and green light materials. The obtained white light LED / LD has a color temperature of 3000-6000K, a color rendering index of 86-94, and a luminous efficiency of 140-180lm / W.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) The present invention effectively avoids the photon reabsorption effect caused by stacking red and green fluorescent materials or mixing multi-color fluorescent films by using a structure in which red and green light stripe films are alternately arranged on a YAG:Ce ceramic sheet, thereby mediating the "luminosity-chromaticity contradiction" to a certain extent. At the same time, the composite fluorescent material prepared by this structure can improve the heat transfer process, thereby effectively avoiding the heat accumulation phenomenon under high-power LD; the β-SiAlON:Eu coated in this structure 2+ Under the excitation of 450-460nm blue light LED / LD, the fluorescent glass film can emit green fluorescence with a central wavelength of 520-530nm, which effectively improves the green valley effect in white light LED / laser lighting. In addition, (Sr,Ca)AlSiN3:Eu 2+ When excited by 450-460nm blue light LED / LD, the fluorescent glass film can emit red fluorescence with a central wavelength of 625-635nm, making up for the problem of insufficient red light of YAG:Ce fluorescent material.
[0029] (2) When excited by a 450-460nm blue light LED / LD chip, the stripe composite structure fluorescent material of the present invention emits yellow light, red light and green light respectively, which are mixed with the unabsorbed blue light to obtain high-quality white light, thereby achieving full-spectrum white light LED / LD lighting with a color rendering index of 86-96 and a color temperature of 3000-6000K.
[0030] (3) The present invention adopts low temperature sintering technology to realize the integrated molding of three fluorescent materials. Since YAG:Ce fluorescent ceramics have excellent thermal conductivity, YAG:Ce fluorescent ceramics are used as the main structure, and the coating of striped fluorescent glass film has little effect on it. Therefore, the composite fluorescent material has excellent thermal conductivity, and the thermal conductivity is 7-9Wm -1 K -1 .
[0031] (4) The present invention provides a method for preparing a composite structure fluorescent material containing stripes. The fluorescent glass film prepared by the method has controllable thickness, simple process and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 This is a physical picture of the stripe composite structure fluorescent material of the present invention.
[0034] Figure 2 It is a schematic diagram of the structure of the stripe composite structure fluorescent material of the present invention.
[0035] Figure 3 It is a schematic diagram of the structure of the red and green fluorescent films of the stripe composite structure fluorescent material of the present invention.
[0036] Figure 4 A 3D printing mold for preparing striped red and green fluorescent films in the present invention (left - model image, right - actual image).
[0037] Figure 5 This is the XRD spectrum of the green fluorescent film and the red fluorescent film in the striped composite fluorescent material prepared in Example 2 of the present invention.
[0038] Figure 6 This is a cross-sectional microstructure SEM image of the striped composite fluorescent material of Example 2 of the present invention (area 1: green fluorescent film, area 2: YAG:Ce fluorescent ceramic).
[0039] Figure 7 This is a temperature-dependent emission spectrum diagram of the striped composite fluorescent material according to Example 2 of the present invention.
[0040] Figure 8 This is a comparison chart of thermal conductivity of the YAG:Ce fluorescent ceramic and the stripe composite structure fluorescent material prepared in Example 2 of the present invention.
[0041] Fig. 9 This is the electroluminescence spectrum of the stripe composite structure fluorescent material prepared in Example 2 of the present invention under the excitation of a blue light LED.
[0042] Fig.10 This is the electroluminescence spectrum of the stripe composite structure fluorescent material prepared in Example 2 of the present invention under the excitation of blue light LD.
[0043] In the figure, 1 is the main structure of yellow fluorescent ceramic, 2 is the red fluorescent film, 3 is the green fluorescent film; DETAILED DESCRIPTION
[0044] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. The raw materials used in the following examples are all commercially available products with a purity greater than 99.9%. (Sr,Ca)AlSiN3:Eu 2+ and β-SiAlON:Eu 2+ The particle size is between 200nm-250nm. The particle size of the glass matrix is between 50nm-150nm.
[0045] Example 1
[0046] In this embodiment, the stripe composite structure fluorescent material is as follows Figure 1-2As shown, the striped composite structure fluorescent material is composed of a yellow fluorescent ceramic main structure 1 and a layer of red fluorescent film 3 and green fluorescent film 2 which are alternately arranged and have equal width and height and are coated on the upper surface of the yellow fluorescent ceramic main structure. The yellow fluorescent ceramic main structure is YAG:Ce fluorescent ceramic, and the chemical composition is (Y 0.998 Ce 0.002 )3Al5O 12 The chemical composition of the red fluorescent film is (Sr,Ca)AlSiN3:Eu 2+ ; The chemical composition of the green fluorescent film is β-SiAlON:Eu 2+ .
[0047] In this embodiment, the thickness of the yellow fluorescent ceramic main structure is 1 mm, the thickness of the red and green fluorescent films are both 50 μm, and the width of the red and green fluorescent glass films are both 1 mm.
[0048] The preparation method of the stripe composite structure fluorescent material in this embodiment is as follows:
[0049] (1) According to the stoichiometric formula (Y 0.998 Ce 0.002 )3Al5O 12 The required powder raw materials are accurately weighed, wherein the powder raw materials are Al2O3, Y2O3 and CeO2, and then placed in a nylon ball mill for planetary ball milling for 16 hours, wherein the ball milling speed is set to 200r / min, the ball milling beads are Al2O3 balls, and the ball milling medium is anhydrous ethanol. The ball-milled slurry is poured into an evaporating dish and placed in an 80℃ electric blast drying oven for drying for 24 hours, and then passed through a 200-mesh sieve 5 times. The mixed powder is placed in a stainless steel mold with a diameter of 22mm, and a unidirectional pressure is applied to it by a press to make it a blank with a certain strength, wherein the applied pressure is 20Mpa and the holding time is 5min. After the dry-pressed blank is packaged, it is placed in a cold isostatic press for cold isostatic pressing (holding pressure is 300Mpa, holding time is 300s), and the obtained blank is calcined in a muffle furnace for 10 hours in an air atmosphere at 800℃ to remove impurities. The blank was placed in a vacuum tungsten furnace at 5 × 10 -4 After sintering at 1765°C × 10h under a vacuum degree of 1.5 Pa, the ceramic was annealed in an air atmosphere at 1450°C × 10h. The annealed ceramic was double-sided polished to 1 mm to obtain YAG:Ce fluorescent ceramic.
[0050] (2) Accurately weigh the required powder raw materials according to the chemical stoichiometric formula 38SiO2-40B2O3-4ZnO-4Na2O-3Al2O3-1Li2O (mol%), where the powder raw materials are SiO2, B2O3, ZnO, Na2O, Al2O3 and Li2O, and then grind them thoroughly in an agate mortar. Pour the ground mixed powder into an alumina crucible and sinter it in a high-temperature furnace at 1300°C for 2 hours. Then pour the molten liquid into a copper mold and cool it. Finally, grind the precursor glass block into powder and pass it through a 100-mesh sieve to obtain the precursor glass powder. Mix 0.125g of the precursor glass powder with 0.375g of commercial red phosphor (Sr,Ca)AlSiN3:Eu 2+ and an organic binder consisting of 0.15 g ethyl cellulose, 150 μL pinene alcohol, and 300 μL ethyl acetate was mixed to obtain a red fluorescent glass film slurry; 0.125 g precursor glass powder was mixed with 0.375 g commercial green fluorescent powder β-SiAlON:Eu 2+ and an organic binder consisting of 1 mL of pine alcohol, 3 mL of ethyl acetate and 1 g of ethyl cellulose is mixed to obtain a green fluorescent glass film slurry;
[0051] (3) Place the 3D printed mold on the YAG:Ce fluorescent ceramic sheet and fix it on the glass substrate with tape. The 3D printed mold structure is as follows: Figure 4 As shown, the 3D printing mold uses a plastic plate with rectangular holes at equal intervals, the interval is 1mm, and the width of the rectangular holes is 1mm. The red fluorescent glass film slurry is scraped on the YAG:Ce ceramic sheet through the 3D printing mold with a scraper thickness of 50-60μm, and dried in a 150℃ electric blast drying oven for 3 hours. Then, the 3D printing mold on the YAG:Ce fluorescent ceramic sheet is translated by a red fluorescent film width and fixed on the glass substrate again. The slurry of the green fluorescent glass film is scraped on the YAG:Ce ceramic sheet through the 3D printing mold with a scraper thickness of 50-60μm, and dried in a 150℃ electric blast drying oven for 3 hours; the obtained composite fluorescent material is sintered to obtain a striped composite structure fluorescent material, and the sintering procedure is: keep warm at 120℃ for 40min, keep warm at 400℃ for 1h, and after the insulation, the sample is cooled to room temperature in an argon atmosphere to obtain a striped composite structure fluorescent material, and its thermal conductivity is 7Wm -1 K -1 .
[0052] The obtained stripe composite structure fluorescent material was packaged with a 460nm blue light LED chip to obtain a white light source with a correlated color temperature of 3184K, a color rendering index of 93.1, color coordinates (0.3345, 0.3326), and a luminous efficiency of 142.1lm / W; and packaged with a 460nm blue light LD chip to obtain a white light source with a correlated color temperature of 4569K, a color rendering index of 90, color coordinates (0.3376, 0.3311), and a luminous efficiency of 172.4lm / W.
[0053] Example 2
[0054] In this embodiment, the chemical composition of the yellow fluorescent ceramic main structure YAG:Ce fluorescent ceramic is (Y 0.996 Ce 0.004 )3Al5O 12 The weight ratio of the green phosphor in the green fluorescent film to the red phosphor in the red fluorescent film is 2: 1. The thickness of the yellow fluorescent ceramic main structure of this embodiment is 1 mm, the thickness of the red and green fluorescent films are both 50 μm, and the width of the red and green fluorescent glass films are both 1 mm.
[0055] The preparation method of red and green fluorescent glass film slurry is as follows: 0.3125g of precursor glass powder and 0.1875g of commercial red phosphor (Sr, Ca)AlSiN3:Eu 2+ and an organic binder consisting of 1 mL of pine alcohol, 3 mL of ethyl acetate, and 1 g of ethyl cellulose was mixed to obtain a red fluorescent glass film slurry; 0.125 g of precursor glass powder and 0.375 g of commercial green fluorescent powder β-SiAlON:Eu were mixed. 2+ and an organic binder consisting of 1 mL of pine alcohol, 3 mL of ethyl acetate and 1 g of ethyl cellulose is mixed to obtain a green fluorescent glass film slurry;
[0056] Other implementation steps are the same as those in Example 1.
[0057] The stripe composite structure fluorescent material prepared in this embodiment has a thermal conductivity of 8Wm -1 K -1 .
[0058] The obtained composite fluorescent material was packaged with a 460nm blue light LED chip to obtain a white light source with a correlated color temperature of 3911K, a color rendering index of 94, color coordinates (0.3336, 0.3312), and a luminous efficiency of 145.8lm / W; and packaged with a 460nm blue light LD chip to obtain a white light source with a correlated color temperature of 4861K, a color rendering index of 91.4, color coordinates (0.3354, 0.3309), and a luminous efficiency of 171.8lm / W.
[0059] Figure 6This is a SEM image of the microstructure at the interface of the red and green fluorescent glass films in the striped composite fluorescent material of Example 2. From the SEM cross-sectional image, it can be seen that the fluorescent glass film is closely attached to the YAG:Ce fluorescent ceramic and has good film-forming properties. Figure 7 This is the temperature-dependent emission spectrum of the striped composite fluorescent material in Example 2. Figure 7 It can be seen that with the increase of temperature, the luminous intensity of the composite fluorescent material decreases slightly, and can still maintain 66% at 473K, which has good thermal stability.
[0060] Example 3
[0061] In this embodiment, the chemical composition of the yellow fluorescent ceramic main structure YAG:Ce fluorescent ceramic is (Y 0.994 Ce 0.006 )3Al5O 12 The weight ratio of the green phosphor in the green phosphor film to the red phosphor in the red phosphor film is 3:1.
[0062] The preparation method of red and green fluorescent glass film slurry is as follows: 0.375g of precursor glass powder and 0.125g of commercial red fluorescent powder (Sr, Ca)AlSiN3:Eu 2+ and an organic binder consisting of 0.15 g ethyl cellulose, 150 μL pinene alcohol, and 300 μL ethyl acetate was mixed to obtain a red fluorescent glass film slurry; 0.125 g precursor glass powder was mixed with 0.375 g commercial green fluorescent powder β-SiAlON:Eu 2+ and an organic binder consisting of 1 mL of pine alcohol, 3 mL of ethyl acetate and 1 g of ethyl cellulose is mixed to obtain a green fluorescent glass film slurry;
[0063] Other implementation steps are the same as those in Example 1.
[0064] The stripe composite structure fluorescent material prepared in this embodiment has a thermal conductivity of 9Wm -1 K -1 .
[0065] The obtained composite fluorescent material was packaged with a 460nm blue light LED chip to obtain a white light source with a correlated color temperature of 4111K, a color rendering index of 92, color coordinates (0.3357, 0.3338), and a luminous efficiency of 139.6lm / W; and packaged with a 460nm blue light LD chip to obtain a white light source with a correlated color temperature of 4334K, a color rendering index of 89.9, color coordinates (0.3369, 0.3321), and a luminous efficiency of 168.6lm / W.
[0066] Example 4
[0067] In this embodiment, the chemical composition of the yellow fluorescent ceramic main structure YAG:Ce fluorescent ceramic is (Y 0.992 Ce 0.008 )3Al5O 12 The weight ratio of the green phosphor in the green phosphor film to the red phosphor in the red phosphor film is 4:1.
[0068] The preparation method of red and green fluorescent glass film slurry is as follows: 0.4062g of precursor glass powder and 0.0938g of commercial red phosphor (Sr, Ca)AlSiN3:Eu 2+ and an organic binder consisting of 0.15 g ethyl cellulose, 150 μL pinene alcohol, and 300 μL ethyl acetate was mixed to obtain a red fluorescent glass film slurry; 0.125 g precursor glass powder was mixed with 0.375 g commercial green fluorescent powder β-SiAlON:Eu 2+ and an organic binder consisting of 1 mL of pine alcohol, 3 mL of ethyl acetate and 1 g of ethyl cellulose is mixed to obtain a green fluorescent glass film slurry;
[0069] Other implementation steps are the same as those in Example 1.
[0070] The stripe composite structure fluorescent material prepared in this embodiment has a thermal conductivity of 7.5 Wm -1 K -1 .
[0071] The obtained composite fluorescent material was packaged with a 460nm blue light LED chip to obtain a white light source with a correlated color temperature of 4700K, a color rendering index of 91.2, color coordinates (0.3381, 0.3354), and a luminous efficiency of 136.7lm / W; and packaged with a 460nm blue light LD chip to obtain a white light source with a correlated color temperature of 5283K, a color rendering index of 88.6, color coordinates (0.3379, 0.3345), and a luminous efficiency of 162.1lm / W.
[0072] Example 5
[0073] In this embodiment, the chemical composition of the yellow fluorescent ceramic main structure YAG:Ce fluorescent ceramic is (Y 0.990 Ce 0.010 )3Al5O 12 The weight ratio of the green phosphor in the green phosphor film to the red phosphor in the red phosphor film is 5:1.
[0074] The preparation method of red and green fluorescent glass film slurry is as follows: 0.425g of precursor glass powder and 0.075g of commercial red phosphor (Sr, Ca)AlSiN3:Eu 2+and an organic binder consisting of 0.15 g ethyl cellulose, 150 μL pinene alcohol, and 300 μL ethyl acetate was mixed to obtain a red fluorescent glass film slurry; 0.125 g precursor glass powder was mixed with 0.375 g commercial green fluorescent powder β-SiAlON:Eu 2+ and an organic binder consisting of 1 mL of pine alcohol, 3 mL of ethyl acetate and 1 g of ethyl cellulose is mixed to obtain a green fluorescent glass film slurry;
[0075] Other implementation steps are the same as those in Example 1.
[0076] The stripe composite structure fluorescent material prepared in this embodiment has a thermal conductivity of 8.5 Wm -1 K -1 .
[0077] The obtained composite fluorescent material was packaged with a 460nm blue LED chip to obtain a white light source with a correlated color temperature of 5144K, a color rendering index of 90.1, color coordinates (0.3421, 0.3391), and a luminous efficiency of 132.5lm / W; and packaged with a 460nm blue LD chip to obtain a white light source with a correlated color temperature of 4534K, a color rendering index of 86.9, color coordinates (0.3421, 0.3397), and a luminous efficiency of 159.8lm / W. The performance tests of the white light LEDs of Examples 1-5 are shown in Table 1.
[0078] Table 1 White light LED performance test results of Examples 1-5
[0079]
[0080] It can be seen from Table 1 that by changing the mass ratio of red and green phosphors, the red-green-blue light ratio in the electroluminescent spectrum of the composite fluorescent material can be effectively controlled, thereby achieving high-quality luminescence. When the mass ratio of red and green phosphors is 1:2, the light color quality of the composite fluorescent material is the best.
[0081] Embodiment 6-10
[0082] On the basis of Example 2, under the premise of keeping the total area of the red and green fluorescent films unchanged, only the widths of the red and green fluorescent films are adjusted to 1.1, 1.2, 1.3, 1.4, and 1.5 mm, and the other implementations are the same as Example 2. The performance tests of white light LEDs of Examples 6-10 are shown in Table 2.
[0083] Table 2 White light LED performance test results of Examples 6-10
[0084]
[0085] It can be seen from Table 2 that as the width of the red and green fluorescent glass films increases, the number of gaps between the red and green films decreases, thereby relatively increasing the area of the red and green films. Therefore, as the width of the fluorescent glass film increases, the luminous efficiency, color rendering index and color temperature increase accordingly.
[0086] Examples 11-14
[0087] On the basis of Example 2, only the thickness of the YAG:Ce fluorescent ceramic is adjusted to 1.2, 1.4, 1.6, and 1.8 mm, and the other implementations are the same as Example 2. The performance tests of the white light LEDs of Examples 11-14 are shown in Table 3.
[0088] Table 3 White light LED performance test results of Examples 6-10
[0089]
[0090] It can be seen from Table 3 that as the thickness of the YAG:Ce fluorescent ceramic increases, the luminous efficiency of the composite fluorescent material increases, and the color rendering index and color temperature decrease.
[0091] Comparative Examples 1-5
[0092] On the basis of Example 1, only the thickness of the red and green fluorescent films are adjusted to 60-70, 70-80, 80-90, 100-110, 120-130 μm, and the other implementations are the same as Example 1. The performance tests of the white light LEDs of Comparative Examples 1-5 are shown in Table 4.
[0093] Table 4 Comparative Examples 1-5 White Light LED Performance Test Results
[0094]
[0095] It can be seen from Table 4 that as the thickness of the red and green fluorescent glass films increases, the overall fluorescent material increases, and thus the luminous efficiency increases accordingly. However, as the thickness increases, the red-green-blue ratio in the electroluminescent spectrum of the composite fluorescent material becomes unbalanced, and thus the color rendering index shows a downward trend.
[0096] Comparative Example 6
[0097] The ceramic material prepared by the method of Chinese invention patent CN113979739A has a luminous efficiency of 102 lm / W and a color rendering index of 74 under the excitation of a blue light LED. The performance tests of the white light LEDs of Examples 1-10 and Comparative Examples 1-6 are shown in Table 5.
[0098] Table 5 White light LED performance test results of Examples 1-10 and Comparative Examples 1-6
[0099]
[0100]
[0101] It can be seen from Table 5 that the striped composite structure fluorescent material provided by the present invention effectively avoids the photon reabsorption effect caused by the stacking of red and green fluorescent materials or the mixing of multi-color fluorescent films, thereby mediating the "luminosity-chromaticity contradiction" to a certain extent. At the same time, the composite fluorescent material prepared by this structure can improve the heat transfer process, thereby effectively avoiding the heat accumulation phenomenon under high-power LD; the red and green fluorescent glass films coated on YAG:Ce fluorescent ceramics under this structure effectively improve the green valley effect in white light LED / laser lighting and make up for the problem of insufficient red light of YAG:Ce fluorescent materials, thereby achieving high-quality luminescence. Compared with the prior art, the composite fluorescent material of the present invention has excellent optical and thermal properties, and because the spot area of the blue light LD is ≤2mm 2 The width of the film prepared by the technology adopted in the present invention can reach 1 mm, so it can be used in white light LED / LD lighting at the same time.
[0102] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered within the protection scope of the present invention.
Claims
1. A stripe composite structure fluorescent material, characterized in that: The striped composite structure fluorescent material consists of a yellow fluorescent ceramic main structure and a layer of red and green fluorescent films of equal width and thickness coated on the upper surface of the yellow fluorescent ceramic main structure. The thickness of the yellow fluorescent ceramic is 1-1.8 mm, wherein the thickness of the red and green fluorescent films is 50-60 μm, and the width of the red and green fluorescent glass films is 1-1.5 mm.
2. The stripe composite structure fluorescent material according to claim 1, characterized in that: The chemical composition of the yellow fluorescent ceramic main structure is (Y 1-x Ce x )3Al5O 12 , 0.001≤x≤0.01; the chemical composition of the red fluorescent film is (Sr,Ca)AlSiN3:Eu 2+ ; The chemical composition of the green fluorescent film is 𝜷-SiAlON:Eu 2+ .
3. The stripe composite structure fluorescent material according to claim 2, characterized in that: The yellow fluorescent ceramic is garnet ceramic (Y 1-x Ce x )3Al5O 12 Center 3+ The ion concentration is 0.2 at%-1.0 at%, and the weight ratio of the green phosphor in the green fluorescent film to the red phosphor in the red fluorescent film is (1-5):
1.
4. The stripe composite structure fluorescent material according to claim 1, characterized in that: The raw material phosphor used in the red fluorescent film is (Sr,Ca)AlSiN3:Eu 2+ , particle size is 200nm-250nm; the raw material phosphor used for green fluorescent film is 𝜷-SiAlON:Eu 2+ The particle size is 200nm-250nm.
5. The method for preparing the stripe composite structure fluorescent material according to any one of claims 1 to 4, characterized in that: Preparation of yellow fluorescent ceramics (Y 1-x Ce x )3Al5O 12 The fluorescent ceramic sheet is YAG:Ce fluorescent ceramic, and then the slurry of red and green fluorescent films is coated on the surface of the yellow fluorescent ceramic by a scraper, and the striped composite structure fluorescent material is prepared by low temperature sintering technology, which specifically includes the following steps: (1) Preparation of YAG:Ce fluorescent ceramics using solid phase reaction technology; (2) After coating the gel-state red and green fluorescent glass films on the YAG:Ce fluorescent ceramics through a mold, a striped composite structure fluorescent material is obtained by low-temperature sintering technology.
6. The method for preparing the stripe composite structure fluorescent material according to claim 5, characterized in that: The preparation method of the YAG:Ce fluorescent ceramic in step (1) is as follows: ① According to the stoichiometric formula (Y 1-x Ce x )3Al5O 12 , 0.001≤x≤0.01, accurately weigh the required powder raw materials, wherein the powder raw materials are Al2O3, Y2O3 and CeO2, and then place them in a nylon ball mill for planetary ball milling for 15-25h, wherein the ball milling speed is set to 200r / min, the ball milling beads are Al2O3 balls, and the ball milling medium is anhydrous ethanol. The slurry after ball milling is poured into an evaporating dish and placed in an 80℃ electric blast drying oven for drying for 24h, and then passed through a 200-mesh sieve 5 times to obtain a mixed powder; ② The mixed powder is placed in a stainless steel mold with a diameter of 22 mm, and a unidirectional pressure is applied to it by a press to make it into a green billet with a certain strength, wherein the applied pressure is 20 Mpa, and the holding time is 5 min. After the dry pressed green billet is packaged, it is placed in a cold isostatic press for cold isostatic pressing, and the holding pressure is 300 Mpa, and the holding time is 300 s. The obtained green billet is calcined in an air atmosphere in a muffle furnace at 800-900 ° C for 10 h to remove impurities; ③ Place the cleaned blank in a vacuum tungsten wire furnace at 1765°C and 5×10 -4 After sintering for 10 h under a vacuum degree of 1.5 Pa, the ceramic was annealed in an air atmosphere at 1450°C for 10 h. The annealed ceramic was double-sided polished to 1 mm to obtain YAG:Ce fluorescent ceramic.
7. The method for preparing the stripe composite structure fluorescent material according to claim 5, characterized in that: The method for preparing the stripe composite structure fluorescent material in step (2) is as follows: ① Use an analytical balance to accurately weigh the required powder raw materials according to the chemical stoichiometric formula 38SiO2-40B2O3-4ZnO-4Na2O-3Al2O3-1Li2O (mol%), where the powder raw materials are SiO2, B2O3, ZnO, Na2O, Al2O3 and Li2O, and then fully grind them in an agate mortar, pour the ground mixed powder into an alumina crucible and sinter in a high-temperature furnace at 1300°C for 2 hours to obtain a molten liquid, pour it into a copper mold and cool it to obtain a precursor glass block, and finally grind the precursor glass block into powder and pass it through a 100-mesh sieve to obtain a precursor glass powder; ② Mix the precursor glass powder with commercial (Sr,Ca)AlSiN3:Eu 2+ The red fluorescent glass film slurry is obtained by mixing the red fluorescent powder and the organic binder, and the precursor glass powder is mixed with the commercial (Sr, Ca)AlSiN3:Eu 2+ The total mass of the phosphor is 0.5g, and the composition of the organic binder is: 0.15g ethyl cellulose, 150μL pinene alcohol, 300μL ethyl acetate; the precursor glass powder is mixed with commercial 𝜷-SiAlON:Eu 2+ Green fluorescent glass film slurry is obtained by mixing green fluorescent powder with organic binder, and the precursor glass powder is mixed with commercial 𝜷-SiAlON:Eu 2+ The total mass of the green phosphor is 0.5 g, and the composition of the organic binder is: 0.15 g ethyl cellulose, 150 μL pinene alcohol, and 300 μL ethyl acetate; wherein the weight ratio of the green phosphor to the precursor glass powder is 3:1, and the weight ratio of the green phosphor to the red phosphor is (1-5):1; ③ Place the 3D printed mold on the YAG:Ce fluorescent ceramic sheet and fix it on the glass substrate with tape, use a scraper to scrape the red fluorescent glass film slurry onto the YAG:Ce ceramic sheet through the 3D printed mold, and dry it in a 150 °C electric blast drying oven for 3 hours, then translate the 3D printed mold on the YAG:Ce fluorescent ceramic sheet by the width of a red fluorescent film, and fix it on the glass substrate again, and use a scraper to scrape the green fluorescent glass film slurry onto the YAG:Ce ceramic sheet through the 3D printed mold, and dry it in a 150 °C electric blast drying oven for 3 hours; the obtained composite fluorescent material is sintered to obtain a striped composite structure fluorescent material.
8. The method for preparing the stripe composite structure fluorescent material according to claim 5 or 7, characterized in that: The sintering procedure is: at 120 o C-130 o In the C stage, keep warm for 0.5h-1h at 400 o C-450 o In stage C, the sample is kept warm for 0.5h-1h. After the heat preservation, the sample is cooled to room temperature in an argon atmosphere.
9. The stripe composite structure fluorescent material according to claims 1-4 is used in the field of fluorescence conversion white light LED / LD lighting, characterized in that: When it is applied to a white light LED lighting device, the excitation source is a blue light LED chip; when it is applied to a white light LD lighting device, the excitation source is a blue light LD chip.
10. The use according to claim 9, characterized in that: Under the excitation of 450-460 nm blue light LED / LD chip, the obtained white light LED / LD has a color temperature of 3000-6000K, a color rendering index of 86-94, and a luminous efficiency of 140-180lm / W.
Citation Information
Patent Citations
Complex phase ceramic array for laser illumination, preparation method of complex phase ceramic array and light source device
CN109896843A
Cyan fluorescent glass, preparation method thereof and full-spectrum LED device thereof
CN111003933A
Composite fluorescent ceramic, preparation method and light-emitting
CN113979739A
Composite fluorescent ceramic for white light LD illumination and preparation method thereof
CN115490508A
High-color-rendering-index and high-luminous-efficiency fluorescence conversion composite material for laser illumination and preparation method thereof
CN117342866A
Cited By
LED packaging structure and preparation method thereof
CN122340975A