3D printing gel composite solid electrolyte and preparation method thereof
Preparation of gel composite solid electrolyte through 3D printing technology, solving the problem of solid electrolyte/electrode interface and manufacturing process complexity in lithium-ion batteries, realizing high energy density, safety and long-life lithium-ion batteries, improving the battery's machinery Strength and magnification performance.
Patent Information
- Application Number
- CN202410930316.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional liquid lithium-ion batteries have safety hazards, capacity attenuation, large volume and weight, limited use temperature and environmental pollution, and the solid electrolyte/electrode interface problems of solid-state batteries, complex manufacturing processes and high load positive electrode energy performance hinder their business. .
Use 3D printing technology to prepare gel composite solid electrolytes, coat the inner solid electrolyte through the outer gel electrolyte, and use polymer monomers and ionic liquids to form core-shell structures, improve mechanical strength and ion transfer efficiency, and reduce electrode/electrolyte interface impedance.
It significantly enhances the mechanical strength and cycle life of lithium-ion batteries, improves the rate performance and energy density of the battery, reduces costs, and improves the interface compatibility and stability of the electrode and electrolyte.
Smart Images

Figure CN118970162A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a 3D printed gel composite solid electrolyte and a preparation method thereof, and relates to the field of lithium ion batteries. Background Art
[0002] In recent years, the new energy market has flourished, and lithium-ion batteries have attracted particular attention. With the improvement of environmental awareness and the promotion of scientific and technological innovation, people's urgent demand for clean energy continues to grow, which has also led to the increasing global ownership of lithium-ion battery products. However, with this comes the increasing viscosity between lithium batteries and various application products, which in turn brings a series of challenges. Traditional liquid batteries have problems such as safety hazards, capacity attenuation, large volume and weight, limited operating temperature and environmental pollution. These shortcomings have gradually emerged and are approaching the upper limit of their development, and it is also difficult to meet the growing market demand.
[0003] Therefore, developing solid-state batteries with high safety and high energy density is the only way to promote market development. Solid-state batteries are considered to be the technical development direction of the next generation of new energy batteries. They have higher theoretical energy density and volume density, wider operating temperature range, simpler battery structure and better safety performance, meeting the performance requirements of the industry and market for products. In the development of solid-state battery technology, the interface problems of solid electrolyte / electrode, the cost problems caused by complex manufacturing processes, and the problems of high-load positive electrode energy performance are important bottlenecks that hinder the commercialization and large-scale application of solid-state batteries. Solid-state batteries replace traditional liquid electrolytes with solid electrolytes. The lack of "flow" characteristics means that there is insufficient wettability and tight bonding between the electrodes and the electrolyte. Not only does it seriously affect the transfer path and transfer efficiency of lithium ions, it will also greatly increase the interface impedance between the electrode and the electrolyte, affecting the battery cycle capacity, energy density and life.
[0004] The gel polymer electrolyte prepared by the in-situ polymerization process combines the advantages of solid electrolytes and liquid electrolytes. It not only effectively reduces the fluidity of the electrolyte and improves the safety of the battery, but also its excellent deformation ability allows it to adapt to the morphological characteristics of the electrode interface to achieve a close combination effect, ensuring the interface compatibility and stability of the solid-state battery. However, the physical strength of the gel polymer electrolyte is too low, and it is easily punctured by lithium dendrites, causing the battery to short-circuit. Due to the factors of the molding method, it cannot be improved through structural design. Developing a solid electrolyte with high ionic conductivity, low electrode / electrolyte solid-solid interface impedance, high mechanical strength and long life is the research focus of the development of solid-state batteries. Summary of the invention
[0005] In order to overcome the defects of the prior art, the present invention provides a 3D printed gel composite solid electrolyte and a preparation method thereof. The technical solution of the present invention is:
[0006] A 3D printed gel composite solid electrolyte comprises an outer layer gel electrolyte and an inner layer solid electrolyte located inside the outer layer gel electrolyte, wherein the precursor solution components of the outer layer gel electrolyte comprise the following components by weight ratio: 2 to 30 parts of outer layer polymer monomers, 1 to 3 parts of initiators and 69 to 89 parts of ionic liquids; the slurry components of the inner layer solid electrolyte comprise the following components by weight ratio: 50 to 95 parts of inner layer polymers, 0.1 to 10 parts of lithium salts, 5 to 40 parts of active fillers and organic solvents, wherein the mixture formed by the polymer, the lithium salt and the active fillers accounts for 5 to 40% by weight of the organic solvent.
[0007] The polymer monomer is pentaerythritol triacrylate, the initiator is azobisisobutyronitrile, the ionic liquid is an electrolyte solution of 0.1-2 mol / L, the solute in the electrolyte solution is a mixture of one or more of lithium bistrifluoromethanesulfonyl imide, lithium bisdifluorosulfonyl imide, lithium bisoxalatoborate, lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium tetrafluoroborate or lithium perchlorate in any proportion, and the solvent is a mixture of one or more of ethylene carbonate, diethyl carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate or ethyl methyl carbonate in any proportion.
[0008] The inner layer polymer is a mixture of one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polymethyl methacrylate, polyvinyl pyrrolidone, polyethylene oxide, polyethylene glycol or polyacrylonitrile in any proportion; the lithium salt is a mixture of one or more of lithium bis(trifluoromethanesulfonyl imide), lithium bis(difluorosulfonyl imide), lithium bis(oxalatoborate), lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium tetrafluoroborate or lithium perchlorate in any proportion; the active filler is a mixture of one or more of lithium titanium aluminum phosphate nanoparticles, lithium lanthanum zirconium oxide nanoparticles, lithium lanthanum titanium oxide nanoparticles or lithium lanthanum zirconium titanium oxide nanoparticles in any proportion; the organic solvent is a mixture of one or more of N-methylpyrrolidone, NN dimethylformamide, acetonitrile, tetrahydrofuran or acetone in any proportion.
[0009] A method for preparing the 3D printed gel composite solid electrolyte comprises the following steps:
[0010] (1) using a DIW printer to print the inner layer solid electrolyte slurry on a release paper substrate according to a preset model to obtain the 3D printed inner layer solid electrolyte;
[0011] (2) Weighing a solute and a solvent according to a ratio, placing them in a glass container, stirring and mixing, and obtaining a desired ionic liquid;
[0012] (3) weighing the outer layer polymer monomer, initiator and ionic liquid according to the ratio, and placing the outer layer polymer monomer and initiator raw materials into the prepared ionic liquid, mixing and stirring at a speed of 200 to 600 r / min for 10 to 40 minutes, and mixing them until they are transparent and uniform, to obtain a gel electrolyte precursor solution;
[0013] (4) dripping the gel electrolyte precursor solution onto both sides of the inner solid electrolyte, assembling the lithium ion battery with the positive and negative electrodes and standing at room temperature for 6 to 12 hours to allow the gel electrolyte precursor solution to completely infiltrate the inner solid electrolyte and the positive and negative electrodes;
[0014] (5) The assembled battery is placed in an oven at a temperature of 40 to 80 degrees Celsius for 2 to 8 hours to allow the initiator to initiate a polymerization reaction of the polymer monomer to form a 3D printed gel composite electrolyte.
[0015] Before the step (1), the method further comprises the following steps:
[0016] a) Use orcaslicer software to design the solid electrolyte model;
[0017] b) Set the model's print line width, line spacing, and print speed, slice the model according to its longitudinal size, and generate a G-code file executable by the printer;
[0018] c) preparing a solid electrolyte printing slurry;
[0019] d) Set the inner diameter of the printing needle, the feeding pressure and the heating temperature, transfer the printing slurry into the feeding tube and remove the air.
[0020] In the step c), specifically, lithium aluminum titanium phosphate and lithium bis(trifluoromethanesulfonyl imide) are added to N-methylpyrrolidone and stirred for 2-12 hours, and then polyvinylidene fluoride is added thereto and stirred for 12-24 hours.
[0021] In the step d), the inner diameter of the printing needle is 60-600um, the printing speed is 3-30mm / s, the feed pressure is 0.3-0.5MPa, the printing line width is 10-50um, the heating temperature is 30-80°C, the ambient temperature is 23°C, and the ambient dew point temperature is -45°C.
[0022] The preparation of the gel electrolyte precursor solution and the assembly of the lithium-ion battery are both carried out in a glove box, and the water partial pressure and oxygen partial pressure in the glove box are both less than 0.1 ppm.
[0023] A 3D printed gel composite solid electrolyte is prepared by the method for 3D printed gel composite solid electrolyte.
[0024] The advantages of the present invention are:
[0025] The gel composite electrolyte of the present invention has a typical core-shell structure. The solid electrolyte is made by three-dimensional model printing, has the characteristics of high strength and light weight, and serves as the skeleton structure of the ion transmission network. The gel electrolyte is formed by polymer monomers initiating polymerization and coated on the outer layer of the solid electrolyte. The raw materials of the present invention are widely available, low cost, and simple process. The structure, volume and mass of the electrolyte can be accurately controlled by structural design, the ion transfer efficiency can be improved, the mechanical strength of the gel composite electrolyte can be significantly enhanced, and the cycle life and rate performance of the quasi-solid-state battery can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the 3D printing gel composite solid electrolyte molding method of the present invention.
[0027] Figure 2 This is a graph of impedance data for lithium batteries obtained in Examples 1-3 of the present invention.
[0028] Figure 3 This is a data graph of room temperature ionic conductivity of lithium batteries obtained in Examples 1-3 of the present invention.
[0029] Figure 4 It is a rate performance data diagram of the lithium-ion solid-state batteries prepared in Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with specific embodiments, and the advantages and features of the present invention will become clearer as the description proceeds. However, these embodiments are exemplary only and do not constitute any limitation to the scope of the present invention. It should be understood by those skilled in the art that the details and forms of the technical solution of the present invention may be modified or replaced without departing from the spirit and scope of the present invention, but these modifications and replacements all fall within the scope of protection of the present invention.
[0031] Embodiment 1: A method for preparing a 3D printed gel composite solid electrolyte, specifically comprising the following steps:
[0032] Preparation of gel electrolyte precursor solution: The entire preparation process was carried out in a glove box filled with argon (H2O < 0.1ppm, O2 < 0.1ppm). Weigh 8.61g of lithium bis(trifluoromethanesulfonyl)imide, 15ml of ethylene carbonate and 15ml of diethyl carbonate, and prepare a 1mol / L electrolyte solution as an ionic liquid. Weigh pentaerythritol triacrylate, ionic liquid and azobisisobutyronitrile in a dry glass vial, with their mass proportions being 10%, 89% and 1% of the total mass respectively, and stir for 20 minutes to form a transparent and uniform precursor solution.
[0033] Preparation of solid electrolyte slurry: Weigh 2.5g of lithium aluminum titanium phosphate, 0.375g of lithium bis(trifluoromethanesulfonyl imide) and 23g of N-methylpyrrolidone, add lithium aluminum titanium phosphate and lithium bis(trifluoromethanesulfonyl imide) to N-methylpyrrolidone, and place in a dry glass vial and stir for 8 hours at a stirring rate of 450r / min. Then weigh 3.75g of polyvinylidene fluoride and add it, and transfer to a stainless steel stirring tank and stir for 12 hours, with the rotation speeds of 100r / min for 1 hour, 300r / min for 1 hour, and 600r / min for 10 hours to obtain a solid electrolyte slurry.
[0034] Solid electrolyte printing: The entire preparation process is carried out in a dry room with a temperature of 23°C and a dew point temperature of -45°C. Modeling is performed using orcaslicer, and the inner diameter of the printing needle is set to 210um, the printing speed is 10mm / s, the feed pressure is 0.45MPa, the printing line width is 20um, and the heating temperature is 60°C. The electrolyte slurry is transferred to the feed barrel for printing.
[0035] Preparation of 3D printed gel composite solid electrolyte: The entire preparation process was carried out in a glove box filled with argon (H2O < 0.1ppm, O2 < 0.1ppm). First, 40μL of gel electrolyte precursor solution was dripped onto a smooth glass slide, and then a 3D printed solid electrolyte was placed above the center of the solution. 40μL of precursor solution was dripped again, and a cover glass was used to cover it and pressurized and allowed to stand for 10 hours. It was then transferred to a heating table and set to 60 degrees Celsius for heating reaction for 3 hours to obtain a 3D printed gel composite solid electrolyte.
[0036] The prepared 3D printed gel composite solid electrolyte was combined with lithium metal sheets on both sides to form a pair of lithium button batteries, and the battery impedance test and ion conductivity test were carried out using Chenhua electrochemical workstation.
[0037] The measured impedance and ionic conductivity of the 3D printed gel composite solid electrolyte are shown in the attached figure. Figure 2 and attached Figure 3 As shown in the curve of Example 1, it can be seen that the 3D printed gel composite solid electrolyte has an extremely low interface impedance, and the ionic conductivity at room temperature can reach 2.8×10 -4 S cm -1 , with efficient lithium ion migration capability.
[0038] Furthermore, the prepared 3D printed gel composite solid electrolyte was combined with lithium iron phosphate positive electrode and lithium metal negative electrode to form a lithium ion button battery, and the battery rate performance test was carried out using a Xinwei battery test cabinet, with the current settings being 0.1C, 0.3C, 0.5C, 1C, 2C, and 0.1C respectively.
[0039] The measured rate performance of 3D printed gel composite solid electrolyte is shown in the attached figure. Figure 4 As shown in Example 1, it can be seen that the 3D printed gel composite solid electrolyte can not only effectively exert the capacity performance of the positive electrode material, but also the energy density at 0.1C current density can reach 160mAh·g -1 , and can still reach 130mAh·g at a current density of 1C at a high rate -1 The specific capacity can reach more than 100 at a current density of 2C. This shows that the 3D printed solid electrolyte skeleton enhances the structural firmness of the 3D printed gel composite solid electrolyte and improves its tolerance to large currents.
[0040] Example 2: Preparation of gel electrolyte precursor solution: The entire preparation process was carried out in a glove box filled with argon (H2O < 0.1ppm, O2 < 0.1ppm). Weigh 8.61g of lithium bis(trifluoromethanesulfonyl)imide, 15ml of ethylene carbonate and 15ml of diethyl carbonate, and prepare a 1mol / L electrolyte solution as an ionic liquid. Weigh pentaerythritol triacrylate, ionic liquid and azobisisobutyronitrile in a dry glass vial, with their mass proportions being 15%, 83% and 2% of the total mass respectively, and stir for 20 minutes to form a transparent and uniform precursor solution.
[0041] Preparation of solid electrolyte slurry: Weigh 2.5g of lithium aluminum titanium phosphate, 0.375g of lithium bis(trifluoromethanesulfonyl imide) and 23g of N-methylpyrrolidone, add lithium aluminum titanium phosphate and lithium bis(trifluoromethanesulfonyl imide) to N-methylpyrrolidone, and place in a dry glass vial and stir for 8 hours at a stirring rate of 450r / min. Then weigh 3.75g of polyvinylidene fluoride and add it, and transfer to a stainless steel stirring tank and stir for 12 hours, with the rotation speeds of 100r / min for 1 hour, 300r / min for 1 hour, and 600r / min for 10 hours to obtain a solid electrolyte slurry.
[0042] Solid electrolyte printing: The entire preparation process is carried out in a dry room with a temperature of 23°C and a dew point temperature of -45°C. Modeling is performed using orcaslicer, and the inner diameter of the printing needle is set to 210um, the printing speed is 10mm / s, the feed pressure is 0.45MPa, the printing line width is 20um, and the heating temperature is 60°C. The electrolyte slurry is transferred to the feed barrel for printing.
[0043] Preparation of 3D printed gel composite solid electrolyte: The entire preparation process was carried out in a glove box filled with argon (H2O < 0.1ppm, O2 < 0.1ppm). First, 40μL of gel electrolyte precursor solution was dripped onto a smooth glass slide, and then a 3D printed solid electrolyte was placed above the center of the solution. 40μL of precursor solution was dripped again, and a cover glass was used to cover it and pressurized and allowed to stand for 10 hours. It was then transferred to a heating table and set to 60 degrees Celsius for heating reaction for 3 hours to obtain a 3D printed gel composite solid electrolyte.
[0044] The prepared 3D printed gel composite solid electrolyte was combined with lithium metal sheets on both sides to form a pair of lithium button batteries, and the battery impedance test and ion conductivity test were carried out using Chenhua electrochemical workstation.
[0045] The impedance and ionic conductivity of the 3D printed gel composite solid electrolyte prepared in Example 2 were measured as shown in the attached figure. Figure 2 and attached Figure 3 As shown in the curve of Example 2, although the impedance is slightly increased compared with Example 1, the ionic conductivity of the 3D printed gel at room temperature can still reach 1.94×10 -4 S cm -1 , which can provide ion transmission channels and effectively assist the transfer of lithium ions.
[0046] Embodiment 3:
[0047] Preparation of gel electrolyte precursor solution: The entire preparation process was carried out in a glove box filled with argon (H2O < 0.1ppm, O2 < 0.1ppm). Weigh 8.61g of lithium bis(trifluoromethanesulfonyl)imide, 15ml of ethylene carbonate and 15ml of diethyl carbonate, and prepare a 1mol / L electrolyte solution as an ionic liquid. Weigh pentaerythritol triacrylate, ionic liquid and azobisisobutyronitrile in a dry glass vial, with their mass proportions being 10%, 89% and 1% of the total mass respectively, and stir for 20 minutes to form a transparent and uniform precursor solution.
[0048] Preparation of solid electrolyte slurry: Weigh 2g of lithium aluminum titanium phosphate, 0.3g of lithium bis(trifluoromethanesulfonyl imide) and 17g of N-methylpyrrolidone, add lithium aluminum titanium phosphate and lithium bis(trifluoromethanesulfonyl imide) to N-methylpyrrolidone, and place in a dry glass vial and stir for 8 hours at a stirring rate of 450r / min. Then weigh 2.7g of polyvinylidene fluoride and add it, and transfer to a stainless steel stirring tank and stir for 12 hours, with the speeds of 100r / min for 1 hour, 300r / min for 1 hour, and 600r / min for 10 hours to obtain a solid electrolyte slurry.
[0049] Solid electrolyte printing: The entire preparation process is carried out in a dry room with a temperature of 23°C and a dew point temperature of -45°C. Modeling is performed using orcaslicer, and the inner diameter of the printing needle is set to 210um, the printing speed is 10mm / s, the feed pressure is 0.45MPa, the printing line width is 20um, and the heating temperature is 60°C. The electrolyte slurry is transferred to the feed barrel for printing.
[0050] Preparation of 3D printed gel composite solid electrolyte: The entire preparation process was carried out in a glove box filled with argon (H2O < 0.1ppm, O2 < 0.1ppm). First, 40μL of gel electrolyte precursor solution was dripped onto a smooth glass slide, and then a 3D printed solid electrolyte was placed above the center of the solution. 40μL of precursor solution was dripped again, and a cover glass was used to cover it and pressurized and allowed to stand for 10 hours. It was then transferred to a heating table and set to 60 degrees Celsius for heating reaction for 3 hours to obtain a 3D printed gel composite solid electrolyte.
[0051] The prepared 3D printed gel composite solid electrolyte was combined with lithium metal sheets on both sides to form a pair of lithium button batteries, and the battery impedance test and ion conductivity test were carried out using Chenhua electrochemical workstation.
[0052] The impedance and ionic conductivity of the 3D printed gel composite solid electrolyte prepared in Example 3 are measured as shown in the attached figure. Figure 2 and attached Figure 3 As shown in the curve of Example 3, the ionic conductivity of the 3D printed gel at room temperature is 1.9×10 -4 S cm -1 .
[0053] Comparative Example 1:
[0054] Preparation of gel electrolyte precursor solution: The entire preparation process was carried out in a glove box filled with argon (H2O < 0.1ppm, O2 < 0.1ppm). Weigh 8.61g of lithium bis(trifluoromethanesulfonyl)imide, 15ml of ethylene carbonate and 15ml of diethyl carbonate, and prepare a 1mol / L electrolyte solution as an ionic liquid. Weigh pentaerythritol triacrylate, ionic liquid and azobisisobutyronitrile in a dry glass vial, with their mass proportions being 10%, 89% and 1% of the total mass respectively, and stir for 20 minutes to form a transparent and uniform precursor solution.
[0055] Preparation of gel electrolyte: The entire preparation process is carried out in a glove box filled with argon (H2O < 0.1ppm, O2 < 0.1ppm). First, 40μL of gel electrolyte precursor solution is dripped on a flat and smooth glass slide, and then a commercial PP diaphragm is placed above the center of the solution. 40μL of precursor solution is dripped again, covered with a cover glass and pressurized for 10 hours, transferred to a heating table and set to 60 degrees Celsius for heating reaction for 3 hours to obtain a gel electrolyte. The prepared gel electrolyte is combined with a lithium iron phosphate positive electrode and a lithium metal negative electrode to form a lithium-ion button battery. The battery rate performance is tested using a Xinwei battery test cabinet, and the current settings are 0.1C, 0.3C, 0.5C, 1C, 2C, and 0.1C, respectively. Figure 4 It can be seen from the comparison between the data of comparative example 1 and embodiment 1 that the solid electrolyte skeleton prepared by 3D printing in the inner layer can provide better tolerance at high current density. At high current density of 1C and 2C, the charging capacity of the battery using 3D printed gel composite solid electrolyte in embodiment 1 is 2 to 3 times the charging capacity of the conventional gel electrolyte battery in the comparative example. The specific capacity retention rate of the battery is greatly increased at high rates. It shows that the 3D printed gel composite solid electrolyte has excellent structural strength and stability, can withstand the impact of high current, and plays a very important role in improving the fast charging performance of the battery.
[0056] The 3D printed gel composite solid electrolyte of the present invention uses the 3D printed solid electrolyte as the mechanical skeleton of the composite electrolyte to ensure high strength under lightweight, improve the mechanical strength and structural stability of the composite electrolyte, prevent lithium dendrite puncture, and improve the cycle life. The gel polymer electrolyte is coated on the surface of the 3D printed solid electrolyte by in-situ polymerization and fills the mesopores, thereby improving the ionic conductivity of the composite electrolyte, improving the interface contact between the electrode / electrolyte, buffering the interface deformation caused by the volume expansion of the pole piece, and adaptively fitting.
[0057] 3D printed solid electrolyte skeletons can realize the configuration of complex structures through three-dimensional modeling design and printing, and the structural design is highly liberalized and high-precision. The method of skeleton support not only enhances the self-support of the composite electrolyte, but also improves the problem of gel electrolyte structure being restricted. And the molding process is simple and clear, which improves material utilization and reduces costs. The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field within the technical scope disclosed by the present invention, according to the technical solution and its inventive concept of the present invention, is equivalently replaced or changed, which should be covered within the protection scope of the present invention.
Claims
1. A 3D printed gel composite solid electrolyte, characterized in that: The invention comprises an outer layer gel electrolyte and an inner layer solid electrolyte located inside the outer layer gel electrolyte, wherein the precursor solution components of the outer layer gel electrolyte include the following components according to weight ratio: 2 to 30 parts of outer layer polymer monomer, 1 to 3 parts of initiator and 69 to 89 parts of ionic liquid; The slurry components of the inner layer solid electrolyte include the following components according to weight ratio: 50-95 parts of inner layer polymer, 0.1-10 parts of lithium salt, 5-40 parts of active filler and organic solvent, and the mixture formed by the polymer, lithium salt and active filler accounts for 5-40% of the weight of the organic solvent.
2. A 3D printed gel composite solid electrolyte according to claim 1, characterized in that: The polymer monomer is pentaerythritol triacrylate, the initiator is azobisisobutyronitrile, the ionic liquid is an electrolyte solution of 0.1-2 mol / L, the solute in the electrolyte solution is a mixture of one or more of lithium bistrifluoromethanesulfonyl imide, lithium bisdifluorosulfonyl imide, lithium bisoxalatoborate, lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium tetrafluoroborate or lithium perchlorate in any proportion, and the solvent is a mixture of one or more of ethylene carbonate, diethyl carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate or ethyl methyl carbonate in any proportion.
3. A 3D printed gel composite solid electrolyte according to claim 1, characterized in that: The inner layer polymer is a mixture of one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polymethyl methacrylate, polyvinyl pyrrolidone, polyethylene oxide, polyethylene glycol or polyacrylonitrile in any proportion; the lithium salt is a mixture of one or more of lithium bis(trifluoromethanesulfonyl imide), lithium bis(difluorosulfonyl imide), lithium bis(oxalatoborate), lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium tetrafluoroborate or lithium perchlorate in any proportion; the active filler is a mixture of one or more of lithium titanium aluminum phosphate nanoparticles, lithium lanthanum zirconium oxide nanoparticles, lithium lanthanum titanium oxide nanoparticles or lithium lanthanum zirconium titanium oxide nanoparticles in any proportion; the organic solvent is a mixture of one or more of N-methylpyrrolidone, NN dimethylformamide, acetonitrile, tetrahydrofuran or acetone in any proportion.
4. A method for preparing the 3D printed gel composite solid electrolyte according to any one of claims 2 to 3, characterized in that: The following steps are involved: (1) using a DIW printer to print the inner layer solid electrolyte slurry on a release paper substrate according to a preset model to obtain the 3D printed inner layer solid electrolyte; (2) Weighing a solute and a solvent according to a ratio, placing them in a glass container, stirring and mixing, and obtaining a desired ionic liquid; (3) weighing the outer layer polymer monomer, initiator and ionic liquid according to the ratio, and placing the outer layer polymer monomer and initiator raw materials into the prepared ionic liquid, mixing and stirring at a speed of 200 to 600 r / min for 10 to 40 minutes, and mixing them until they are transparent and uniform, to obtain a gel electrolyte precursor solution; (4) dripping the gel electrolyte precursor solution onto both sides of the inner solid electrolyte, assembling the lithium ion battery with the positive and negative electrodes and standing at room temperature for 6 to 12 hours to allow the gel electrolyte precursor solution to completely infiltrate the inner solid electrolyte and the positive and negative electrodes; (5) placing the assembled battery in an oven at a temperature of 40 to 80 degrees Celsius for 2 to 8 hours, so that the initiator triggers the polymerization reaction of the polymer monomer to form a 3D printed gel composite electrolyte.
5. The method for 3D printing gel composite solid electrolyte according to claim 4, characterized in that: Before the step (1), the method further comprises the following steps: a) Use orcaslicer software to design the solid electrolyte model; b) Set the model's print line width, line spacing, and print speed, slice the model according to its longitudinal size, and generate a G-code file executable by the printer; c) preparing a solid electrolyte printing slurry; d) Set the inner diameter of the printing needle, the feeding pressure and the heating temperature, transfer the printing slurry into the feeding tube and exhaust the air.
6. The method for 3D printing gel composite solid electrolyte according to claim 4, characterized in that: In the step c), specifically, lithium aluminum titanium phosphate and lithium bis(trifluoromethanesulfonyl imide) are added to N-methylpyrrolidone and stirred for 2-12 hours, and then polyvinylidene fluoride is added thereto and stirred for 12-24 hours.
7. The method for 3D printing gel composite solid electrolyte according to claim 4, characterized in that: In the step d), the inner diameter of the printing needle is 60-600um, the printing speed is 3-30mm / s, the feed pressure is 0.3-0.5MPa, the printing line width is 10-50um, the heating temperature is 30-80°C, the ambient temperature is 23°C, and the ambient dew point temperature is -45°C.
8. The method for 3D printing gel composite solid electrolyte according to claim 4, characterized in that: The preparation of the gel electrolyte precursor solution and the assembly of the lithium-ion battery are both carried out in a glove box, and the water partial pressure and oxygen partial pressure in the glove box are both less than 0.1 ppm.