Composite copper foil for embedded thin-film resistor and preparation method and application thereof
By sputtering a resistive layer on the carrier dielectric layer and forming a conductive copper layer, a composite copper foil with stable block resistance and flexibility characteristics was prepared, which solved the problem of integrating flexible circuit boards and embedded resistor technology in PCB manufacturing, and realized Further miniaturization and flexibility of electronic products are improved.
Patent Information
- Application Number
- CN202411203134.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The lack of copper foil products in existing PCB manufacturing that integrates flexible circuit board technology with embedded resistor capacitor technology, limiting the further development of electronic products.
The composite copper foil that forms a composite structure is prepared by sputtering resistive layers on both sides of the carrier dielectric layer and forming a conductive copper layer on the resistive layer. Composite copper foil for embedded film resistance with good comprehensive performance.
The stable block resistance performance of composite copper foil and the bendable folding characteristics of the flexible circuit board are realized, which reduces the surface space requirements of the circuit board and reduces the inductive anti-interference between the resistance soldering points.
Smart Images

Figure CN119008147A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic materials, and in particular relates to a composite copper foil for an embedded thin-film resistor and a preparation method and application thereof. Background Art
[0002] Thinness and portability have become an important development direction for consumer electronic products. The thinness and lightness of electronic products requires the configuration of sufficient electronic components in a limited internal space, and the use of embedded resistor and capacitor technology can well meet this demand. Portable electronic products usually use flexible circuit board technology, which can help reduce the overall size and weight of electronic equipment, and can adapt to a variety of bending and folding requirements. As a mature technology, flexible circuit boards are widely used in electronic products, such as foldable mobile phones; and embedded resistor and capacitor technology has also been used in some high-end electronic product equipment fields in recent years. In the PCB manufacturing industry, there are currently no copper foil products that integrate flexible circuit board technology and embedded resistor and capacitor technology. Processing these two technologies into composite copper foil through an integrated production method is expected to further accelerate the miniaturization of electronic products. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a composite copper foil for embedded thin-film resistors, a preparation method and an application thereof. The composite copper foil has good comprehensive performance and surface roughness, and has a stable square resistance, can be used for the manufacture of flexible embedded thin-film resistor PCBs, and has good application prospects.
[0004] The present invention provides a composite copper foil for embedded thin-film resistors. The composite copper foil is formed by sputtering resistor layers on both sides of a carrier dielectric layer and then forming a conductive copper layer on the resistor layer to form a composite structure of a first conductive copper layer, a first resistor layer, a carrier dielectric layer, a second resistor layer and a second conductive copper layer.
[0005] Preferably, the carrier medium layer is a polyimide film, and the thickness of the film is between 5-50 μm.
[0006] Preferably, the composition of the resistance layer includes a single metal selected from the group consisting of nickel, chromium, platinum, palladium, and titanium, or an alloy consisting of two or more elements selected from the group consisting of nickel, chromium, platinum, palladium, titanium, silicon, phosphorus, and aluminum. For example, it may be a nickel-chromium (NiCr) alloy or a nickel-phosphorus (NiP) alloy having low electrical conductivity, or a chromium-silicon (Cr-Si) alloy having high resistivity.
[0007] Preferably, the thickness of the resistor layer is 0.05-2.0 μm, and the metal element content of the resistor layer is ≥70wt%, and the non-metal element content is between 0wt% and 30wt%.
[0008] Furthermore, the composite copper foil has a tensile strength of >300 MPa, an elongation after fracture of >4%, a wettability of >38 mN / m, and a coating adhesion of >2.0 N / mm.
[0009] Furthermore, the final surface roughness spd of the composite copper foil is between 13900-59000 1 / mm 2 , spc is between 15-6501 / mm, sdr is between 5%-200%, and Rq is between 0.2-4.0μm.
[0010] Furthermore, the composite copper foil has a stable sheet resistance, the sheet resistance is 5-250Ω / □, and the embedded resistance value deviation does not exceed ±5%.
[0011] The present invention also provides a method for preparing a composite copper foil for an embedded thin-film resistor, comprising the following steps:
[0012] (1) firstly pre-treating the carrier medium layer by plasma, so as to activate the surface of the carrier medium layer while cleaning the surface of the carrier medium layer;
[0013] (2) forming a resistor layer on the surface of the pretreated carrier dielectric layer by vacuum sputtering, and depositing a chromium layer or a titanium layer as a base layer before sputtering the resistor layer;
[0014] (3) vacuum sputtering a seed copper layer on the resistor layer. Sputtering the seed copper layer is an important step in realizing the metallization of the carrier dielectric layer-resistor layer composite material matrix, which provides a conductive foundation for subsequent electroplating.
[0015] (4) thickening the copper layer by electroplating copper;
[0016] (5) The copper layer is subjected to a nodular treatment to ensure that the composite copper foil has sufficient bonding strength when pressed with the dielectric material;
[0017] (6) Electrochemically deposit an anti-oxidation layer to obtain a composite copper foil for embedded thin-film resistors. Metallic copper easily reacts chemically with water vapor and carbon dioxide in the air, causing oxidation and discoloration of the copper foil. Anti-oxidation treatment of the surface of the carrier medium-resistance layer-conductive copper layer composite material can effectively improve the weather resistance and performance stability of the composite material.
[0018] Preferably, the pretreatment in step (1) makes the surface roughness of the carrier medium layer Ra≥0.08 μm.
[0019] Preferably, the surface roughness Ra of the resistor layer in step (2) is between 0.04 μm and 0.4 μm.
[0020] Preferably, the thickness of the seed copper layer in step (3) is between 50-100 nm; and the thickness of the copper layer after thickening in step (4) is between 12-35 μm.
[0021] Preferably, the tumor treatment in step (5) includes a roughening treatment and a curing treatment.
[0022] Furthermore, the current density of the roughening treatment is 5-20A / dm 2 The roughening treatment time is 15-18s; the current density of the curing treatment is 4-10A / dm 2 , the curing time is 5-12s.
[0023] Furthermore, the roughening solution used in the roughening treatment contains 5-15 g / L of Cu 2+ , 100-150g / L H2SO4, the roughening liquid temperature is 20-30°C; the curing liquid used in the curing treatment contains 55-60g / L Cu 2+ , 90-120g / L H2SO4, solidification liquid temperature 45-60℃.
[0024] Preferably, the anti-oxidation layer in step (6) is metal chromium or carboxybenzotriazole, and the thickness of the anti-oxidation layer is less than 3 nm.
[0025] The invention also provides an application of the composite copper foil for an embedded thin-film resistor in the manufacture of the embedded resistor.
[0026] The steps include:
[0027] (1) pre-pressing the first conductive copper layer of the composite copper foil and the prepreg;
[0028] (2) laminating a first photoresist on the outer surface of the second conductive copper layer;
[0029] (3) exposing and molding the first photoresist to define the width of the embedded resistor and developing the first photoresist;
[0030] (4) etching away the second conductive copper layer and the second resistor layer at the developed portion;
[0031] (5) removing the first photoresist on the outer surface of the second conductive copper layer to obtain a conductive circuit pattern;
[0032] (6) laminating a second photoresist on the outer surface of the second conductive copper layer;
[0033] (7) exposing and molding the second photoresist to define the length of the embedded resistor, and developing the second photoresist;
[0034] (8) etching away the second conductive copper layer at the developed portion to expose the second resistor layer;
[0035] (9) removing the second photoresist on the outer surface of the second conductive copper layer to complete the preparation of the embedded resistor in the second resistor layer.
[0036] (10) Peel off the prepreg sheet and repeat the above steps to complete the preparation of the embedded resistor of the first resistor layer.
[0037] Preferably, the bonding force after pre-pressing in step (1) is between 0.3 N / mm and 1.0 N / mm.
[0038] Preferably, the etching in step (4) uses an acidic etching solution, or a combination of an alkaline etching solution for etching the copper layer and an acidic etching solution for etching the resistor layer.
[0039] Preferably, in step (3) and step (7), etching compensation must be performed on the width and length of the embedded resistor.
[0040] Furthermore, the stripping of step (10) is specifically as follows: the second conductive copper layer of the prepared embedded resistor is pressed with the prepreg at high temperature, and the first conductive copper layer is mechanically separated from the prepreg.
[0041] Furthermore, the temperature of the high-temperature pressing is greater than 170° C., the pressing time is greater than 2 hours, and the bonding strength at room temperature after pressing is greater than 0.9 N / mm.
[0042] Furthermore, before the first conductive copper layer is mechanically separated from the prepreg laminate, a preheating treatment is performed, with the treatment temperature being less than 150° C. and the treatment time being less than 30 min.
[0043] Beneficial Effects
[0044] The composite copper foil of the present invention not only has the bendable and foldable characteristics of the flexible copper-clad laminate, but also combines the embedded resistor production technology. The composite copper foil of the present invention is used to produce flexible circuit boards, and a large number of passive resistor devices can be buried inside the circuit board, further saving the surface space of the circuit board, and greatly reducing the inductive interference between the resistor welding points. Compared with the traditional surface mounted resistor rigid circuit board, the flexible embedded thin film resistor PCB produced by the composite copper foil of the present invention has the advantages of both the flexibility of the flexible circuit board and the stability of the embedded resistor.
[0045] The present invention provides a method for preparing a composite copper foil, which can flexibly sputter alloy resistor layers of different combinations on a dielectric layer, and the resistivity and square resistance of the resistor layer can be flexibly adjusted. The copper layer is thickened by combining sputtering and electroplating, which greatly improves production efficiency. The present invention also provides an application method of a composite copper foil in the manufacture of embedded resistors. Compared with the method of using an organic solvent to separate the buried resistor copper foil in patent document CN105695993A, this method uses an integrated processing technology, does not require the use of an organic solvent to remove the PI dielectric layer, retains the bendability of the composite copper foil, and PI is used as a support layer to provide a completeness guarantee for subsequent flexible circuit board processing. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 It is a schematic diagram of the structure of the composite copper foil of the present invention;
[0047] Figure 2 To prepare the schematic diagram of embedded resistor;
[0048] 11-First conductive copper layer
[0049] 12-First resistance layer
[0050] 21-Second conductive copper layer
[0051] 22- Second resistance layer
[0052] 31-PI film
[0053] 32-Pad
[0054] 33-Signal Line
[0055] 34-Embedded Resistor
[0056] 35- Ground layer. DETAILED DESCRIPTION
[0057] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0058] Example 1
[0059] like Figure 1 As shown, this embodiment provides a composite copper foil for embedded thin-film resistors. The composite copper foil is formed by sputtering a resistor layer on both sides of a carrier dielectric layer and then forming a conductive copper layer on the resistor layer to form a composite structure of a first conductive copper layer, a first resistor layer, a carrier dielectric layer, a second resistor layer, and a second conductive copper layer.
[0060] The specific production process is as follows:
[0061] S1.PI film pretreatment
[0062] The 5μm thick PI film was unrolled and run into the vacuum coating equipment, and the film surface was pretreated with oxygen plasma under vacuum conditions. The parameters during the plasma pretreatment process are as follows:
[0063] Vacuum degree: 0.0035Torr;
[0064] Plasma source: oxygen;
[0065] Power: 1000W;
[0066] Time: 100s.
[0067] S2. Sputtering base
[0068] Before vacuum sputtering the resistor layer of the PI film, in order to enhance the bonding force between the resistor layer and the PI film, a certain thickness of chromium or titanium layer needs to be deposited on the surface of the PI film as a primer layer. The parameters during the primer layer deposition process are as follows:
[0069] Target material: titanium metal (purity: 99.997%);
[0070] Vacuum degree: 0.003Torr;
[0071] Carrier gas: argon;
[0072] Power: 3000W;
[0073] Time: 500s;
[0074] Sputtering method: double-sided synchronous sputtering.
[0075] S3. Double-sided sputtered resistor layer
[0076] The resistor layer is deposited on the surface of the sputtered PI film by magnetron sputtering. The parameters during the resistor layer deposition process are as follows:
[0077] Target: Ni-Cr alloy target (Ni 55-75at.%, Cr 25-45at.%);
[0078] Vacuum degree: 0.003Torr;
[0079] Sputtering power: 5000W;
[0080] Sputtering time: 15min;
[0081] Sputtering method: double-sided synchronous sputtering.
[0082] S4. Sputtering of seed copper layer
[0083] The conductivity of the PI film surface decreases significantly after the resistor layer is sputtered, and it needs to be metallized to provide a conductive substrate for subsequent electrochemical deposition. Therefore, after the base layer and resistor layer are sputtered on the PI film surface, the seed copper layer is deposited to enhance the conductivity of the substrate. The parameters during the seed copper layer sputtering process are as follows:
[0084] Target material: metal copper target (purity: 99.997%);
[0085] Vacuum degree: 0.0025Torr;
[0086] Sputtering power: 4000W;
[0087] Sputtering time: 10min;
[0088] Sputtering method: double-sided synchronous sputtering.
[0089] S5. Electrodeposition thickening copper layer
[0090] The deposition rate of vacuum sputtering is relatively low. In order to improve production efficiency, electrochemical deposition is used to thicken the copper layer. The parameters in the electrochemical copper deposition process are as follows:
[0091] Copper pyrophosphate concentration: 150g / L;
[0092] pH = 11;
[0093] Additive A (potassium selenite) concentration: 12 mg / L;
[0094] Additive B (2-mercaptobenzothiazole) concentration: 0.003 mg / L;
[0095] Electrolyte temperature: 50°C;
[0096] Electrolyte flow rate: 4.5m 3 / h;
[0097] Electrodeposition method: pulse electrodeposition;
[0098] Duty cycle: 33%;
[0099] Frequency: 1000Hz;
[0100] Average current density: 800A / m 2 ;
[0101] Electrodeposition time: 60s.
[0102] S6. Tumor treatment
[0103] Roughening treatment: 11g / L Cu 2+, 120g / L H2SO4, temperature 28℃, current density 8A / dm 2 , processing time 15s;
[0104] Curing treatment: 55g / L Cu 2+ , 100g / L H2SO4, temperature 50℃, current density 6A / dm 2 , processing time 8s.
[0105] S7. Anti-oxidation treatment
[0106] Metallic copper has active chemical properties and is prone to chemical reactions with water vapor and carbon dioxide in the air, which causes a certain degree of oxidation of the copper foil, which in turn has an adverse effect on the performance of the composite copper foil. Therefore, the composite copper foil needs to be treated with anti-oxidation to improve its weather resistance and performance stability. The parameters during the anti-oxidation treatment are as follows:
[0107] Antioxidant: carboxybenzotriazole (BTA);
[0108] Antioxidant concentration: 1.0wt.%;
[0109] Treatment method: roller coating;
[0110] Processing temperature: 25℃;
[0111] Processing time: 5s;
[0112] Drying temperature: 150℃.
[0113] The parameters of the composite copper foil for the final embedded thin film resistor are shown in Table 1.
[0114] Example 2
[0115] The difference between this embodiment and embodiment 1 is that the thickness of the resistor layer is adjusted. The parameters in the resistor layer deposition process are as follows:
[0116] Target: Ni-Cr alloy target (Ni 55-75at%, Cr 25-45at%);
[0117] Vacuum degree: 0.003Torr;
[0118] Sputtering power: 5000W;
[0119] Sputtering time: 150min;
[0120] Sputtering method: double-sided synchronous sputtering.
[0121] Example 3
[0122] The difference between this embodiment and embodiment 1 is that the composition of the resistance layer and the vacuum coating process parameters are adjusted. The parameters in the resistance layer deposition process are as follows:
[0123] Target: Cr-Si alloy target (Cr 68-76at.%, Si 24-32at.%);
[0124] Vacuum degree: 0.0028Torr;
[0125] Sputtering power: 12000W;
[0126] Sputtering time: 20min;
[0127] Sputtering method: double-sided synchronous sputtering.
[0128] Example 4
[0129] The difference between this embodiment and embodiment 1 is that the thickness of the base layer is adjusted. The parameters during the deposition of the base layer are as follows:
[0130] Target material: titanium metal (purity: 99.997%);
[0131] Vacuum degree: 2.5*10 -5 Torr;
[0132] Carrier gas: argon;
[0133] Power: 3000W;
[0134] Time: 1000s;
[0135] Sputtering method: double-sided synchronous sputtering.
[0136] Example 5
[0137] The difference between this embodiment and embodiment 1 is that the composition of the base layer is adjusted. The parameters during the deposition of the base layer are as follows:
[0138] Target material: metal Cr target (purity: 99.99%);
[0139] Vacuum degree: 2*10 -5 Torr;
[0140] Carrier gas: argon;
[0141] Sputtering power: 4500W;
[0142] Sputtering time: 750s;
[0143] Sputtering method: double-sided synchronous sputtering.
[0144] Example 6
[0145] The difference between this embodiment and embodiment 1 is that the thickness of the conductive copper layer is adjusted. The parameters in the electrochemical copper deposition process are as follows:
[0146] Copper pyrophosphate concentration: 150g / L;
[0147] pH = 11;
[0148] Additive A (potassium selenite) concentration: 12 mg / L;
[0149] Additive B (2-mercaptobenzothiazole) concentration: 0.003 mg / L;
[0150] Electrolyte temperature: 50°C;
[0151] Electrolyte flow rate: 4.5m 3 / h;
[0152] Electrodeposition method: pulse electrodeposition;
[0153] Duty cycle: 33%;
[0154] Frequency: 1000Hz;
[0155] Average current density: 800A / m 2 ;
[0156] Electrodeposition time: 117s.
[0157] Example 7
[0158] The difference between this embodiment and embodiment 1 is that the thickness of the seed copper layer is adjusted. The parameters during the sputtering process of the seed copper layer are as follows:
[0159] Target material: metal copper target (purity: 99.997%);
[0160] Vacuum degree: 0.0025Torr;
[0161] Sputtering power: 4000W;
[0162] Sputtering time: 14min 18s;
[0163] Sputtering method: double-sided synchronous sputtering.
[0164] Example 8
[0165] The difference between this embodiment and embodiment 1 is that the parameters in the electrochemical copper plating thickening process are adjusted. The parameters in the electrochemical copper plating thickening process are as follows:
[0166] Copper pyrophosphate concentration: 150g / L;
[0167] pH value: 11;
[0168] Additive A (potassium selenite) concentration: 12 mg / L;
[0169] Additive B (2-mercaptobenzothiazole) concentration: 0.003 mg / L
[0170] Electrolyte temperature: 50°C;
[0171] Electrolyte flow rate: 4.5m 3 / h;
[0172] Electrodeposition method: pulse electrodeposition;
[0173] Duty cycle: 25%;
[0174] Frequency: 2000Hz;
[0175] Current density: 750A / m 2 ;
[0176] Electrodeposition time: 60s.
[0177] Example 9
[0178] The difference between this embodiment and embodiment 1 is that the parameters in the electrochemical copper deposition thickening process are adjusted. The parameters in the electrochemical deposition thickening process are as follows:
[0179] Copper pyrophosphate concentration: 150g / L;
[0180] pH: 11;
[0181] Additive A (potassium selenite) concentration: 12 mg / L;
[0182] Additive B (2-mercaptobenzothiazole) concentration: 0mg / L
[0183] Electrolyte temperature: 50°C;
[0184] Electrolyte flow rate: 4.5m 3 / h;
[0185] Electrodeposition method: DC electrodeposition;
[0186] Current density: 2400A / m 2 ;
[0187] Electrodeposition time: 60s.
[0188] Example 10
[0189] The difference between this embodiment and embodiment 1 is that the thickness of the PI film is adjusted from 5 μm to 25 μm.
[0190] Embodiment 11
[0191] The difference between this embodiment and embodiment 1 is that the thickness of the PI film is adjusted from 5 μm to 50 μm.
[0192] In order to more intuitively compare the effects of samples produced in different embodiments, the present invention summarizes the performance of samples in different embodiments. By comparing the data in Table 1, it can be found that: (1) the square resistance of the composite copper foil is significantly different for materials with different compositions of the resistor layer. The better the conductivity of the alloy layer, the smaller the square resistance of the product; (2) the square resistance deviation of the resistor layer with different thickness is significantly different; (3) the adhesion of the coating is significantly different due to the different thickness of the seed copper layer or the base layer; (4) the elongation of the composite copper foil is significantly different due to the different thickness of the PI film; (5) the surface roughness is significantly different due to the different parameters of the electrochemical copper deposition.
[0193] Table 1 Comparison of implementation effects of different embodiments
[0194]
[0195]
[0196] Example 12
[0197] like Figure 2 As shown, this embodiment provides an application of a composite copper foil for an embedded thin-film resistor in the manufacture of an embedded resistor, comprising the following steps:
[0198] (1) Pre-pressing the first conductive copper layer of the composite copper foil prepared in Example 1 with the prepreg, with a bonding force between 0.3 N / mm and 1.0 N / mm;
[0199] (2) laminating a first photoresist on the outer surface of the second conductive copper layer;
[0200] (3) exposing and molding the first photoresist to define the width of the embedded resistor and developing the first photoresist;
[0201] (4) etching away the second conductive copper layer and the second resistor layer at the developed portion;
[0202] (5) removing the first photoresist on the outer surface of the second conductive copper layer to obtain a conductive circuit pattern;
[0203] (6) laminating a second photoresist on the outer surface of the second conductive copper layer;
[0204] (7) exposing and molding the second photoresist to define the length of the embedded resistor, and developing the second photoresist;
[0205] (8) etching away the second conductive copper layer at the developed portion to expose the second resistor layer;
[0206] (9) removing the second photoresist on the outer surface of the second conductive copper layer to complete the preparation of the embedded resistor in the second resistor layer.
[0207] (10) The second conductive copper layer of the prepared embedded resistor is subjected to high-temperature pressing with the semi-cured sheet (the temperature of the high-temperature pressing is greater than 170°C, the pressing time is greater than 2h, and the bonding strength at room temperature after pressing is greater than 0.9N / mm), and the first conductive copper layer is mechanically separated from the pre-pressed semi-cured sheet. Before the mechanical separation, a preheating treatment is performed, the treatment temperature is less than 150°C, and the treatment time is less than 30min. The above steps are repeated to complete the preparation of the embedded resistor of the first resistor layer.
[0208] Furthermore, the etching in step (4) uses an acidic etching solution, or a combination of an alkaline etching solution for etching the copper layer and an acidic etching solution for etching the resistor layer.
[0209] Furthermore, in the steps (3) and (7), etching compensation must be performed on the width and length of the embedded resistor.
[0210] After the preparation of the embedded resistor of the first resistor layer or the second resistor layer is completed, the conductive pattern of the embedded resistor is tested for resistance using a resistance tester, and the length and width of the resistor pattern are tested using a metallographic microscope, and the size of the square resistance is finally calculated. When the square resistance design value is below 200Ω / □, the actual square resistance is within 2.5% of the design value, and when the square resistance design value is 200Ω / □ and above, the actual square resistance is within ±4% of the design value.
[0211] Finally, it should be emphasized that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A composite copper foil for embedded thin film resistor, characterized in that: The composite copper foil is formed by sputtering resistance layers on both sides of a carrier dielectric layer and then forming a conductive copper layer on the resistance layer to form a composite structure of a first conductive copper layer, a first resistance layer, a carrier dielectric layer, a second resistance layer and a second conductive copper layer.
2. The composite copper foil according to claim 1, characterized in that: The carrier medium layer is a polyimide film, and the thickness of the film is between 5-50 μm.
3. The composite copper foil according to claim 1, characterized in that: The resistor layer comprises a single metal selected from the group consisting of nickel, chromium, platinum, palladium and titanium, or an alloy consisting of two or more elements selected from the group consisting of nickel, chromium, platinum, palladium, titanium, silicon, phosphorus and aluminum.
4. The composite copper foil according to claim 1, characterized in that: The thickness of the resistor layer is 0.05-2.0 μm, and the metal element content of the resistor layer is ≥70wt%, and the non-metal element content is between 0wt% and 30wt%.
5. A method for preparing a composite copper foil for an embedded thin film resistor, comprising the following steps: (1) firstly pre-treating the carrier medium layer by plasma; (2) forming a resistor layer on the surface of the pretreated carrier dielectric layer by vacuum sputtering, and depositing a chromium layer or a titanium layer as a base layer before sputtering the resistor layer; (3) vacuum sputtering a seed copper layer on the resistor layer; (4) thickening the copper layer by electroplating copper; (5) treating the copper layer with tumor; (6) Electrochemically deposit an anti-oxidation layer to obtain a composite copper foil for embedded thin-film resistors.
6. The preparation method according to claim 5, characterized in that: The thickness of the seed copper layer in step (3) is between 50-100 nm; the thickness of the copper layer after thickening in step (4) is between 12-35 μm.
7. The preparation method according to claim 5, characterized in that: The nodularization treatment in step (5) includes a roughening treatment and a curing treatment.
8. The preparation method according to claim 5, characterized in that: The anti-oxidation layer in step (6) is metal chromium or carboxybenzotriazole, and the thickness of the anti-oxidation layer is less than 3 nm.
9. Use of the composite copper foil for embedded thin-film resistors as claimed in claim 1 in the manufacture of embedded resistors.
10. The use according to claim 9, characterized in that: The steps include: (1) pre-pressing the first conductive copper layer of the composite copper foil and the prepreg; (2) laminating a first photoresist on the outer surface of the second conductive copper layer; (3) exposing and molding the first photoresist to define the width of the embedded resistor and developing the first photoresist; (4) etching away the second conductive copper layer and the second resistor layer at the developed portion; (5) removing the first photoresist on the outer surface of the second conductive copper layer to obtain a conductive circuit pattern; (6) laminating a second photoresist on the outer surface of the second conductive copper layer; (7) exposing and molding the second photoresist to define the length of the embedded resistor, and developing the second photoresist; (8) etching away the second conductive copper layer at the developed portion to expose the second resistor layer; (9) removing the second photoresist on the outer surface of the second conductive copper layer to complete the preparation of the second resistor layer embedded resistor; (10) peeling off the prepreg sheet that was pre-laminated, and repeating the above steps to complete the preparation of the first resistor layer embedded resistor.
Citation Information
Patent Citations
Preparation method of embedded resistance material
CN102324294A
Polyimide metal-coated thin film with transition combination layer and preparing method of thin film
CN105463376A
Copper foil resistor and circuit board structure having the same
CN110246639A
Composite metal foil and circuit board
CN114554686A
Production process of embedded resistance copper foil and product thereof
CN116056344A
Cited By
Embedded resistor structure and preparation method and application thereof
CN120907684A