Interface-free material, preparation method thereof and material processing equipment
By using strong pulsed photon beams to form a diffusion layer in the composite material, the interfacial thermal defects and thermal residual stress problems in the composite material are solved, the fatigue resistance and service life are improved, and the side effects of high-temperature treatment are avoided.
Patent Information
- Application Number
- CN202411171450.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Due to thermal defects and thermal residual stress on the material interface in composite materials, the fatigue resistance and service life are reduced, and the prior art methods are limited in effect and have great side effects.
A strong pulsed photon beam is used to irradiate the surface of the sublayer of the composite material to form a diffusion layer, reducing lattice defects and residual stresses at the interface, and improving the microstructure of the material.
Significantly reduce residual stress at the interface of composite materials, improve fatigue resistance and service life, and avoid new thermal defects introduced by high-temperature treatment.
Smart Images

Figure CN119036879A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of material manufacturing, and in particular to a non-interface material and a preparation method thereof, and material processing equipment. Background Art
[0002] Composite materials usually have a layer of material as the base material and another layer or multiple layers of material as reinforcement composited on the base material. This multi-layer material composite method allows the various materials to complement each other in performance, thereby producing a synergistic effect, making the overall performance of the composite material excellent.
[0003] Since composite materials are generally manufactured by thermal processing, there are thermal defects and thermal residual stresses in the materials, especially at the interfaces of the materials. It can be said that thermal defects and thermal residual stresses exist in almost all composite materials. For example, for composite materials composed of a substrate and a film layer (such as a coating, plating or hot melt cladding, etc.) formed on the surface of the substrate, due to the large difference in the physical and chemical properties (such as chemical compatibility, thermal expansion coefficient and Young's modulus, etc.) between the substrate material and the film layer material, lattice defects and residual stresses are easily generated at the interface between the substrate and the film layer. Lattice defects and residual stresses will affect the thermal and mechanical properties of composite materials, and are also the main causes of fatigue failure of composite materials.
[0004] At present, in order to reduce lattice defects and residual stress, commonly used technical means include heat treatment, vibration, shot peening, etc., but these technical means have limited effects and large side effects (such as introducing new thermal defects or destroying the surface morphology). Summary of the invention
[0005] In view of this, the embodiments of the present application provide an interface-free material and a preparation method thereof, and a material processing device to solve at least one problem existing in the background technology.
[0006] In a first aspect, an embodiment of the present application provides a method for preparing a non-interface material, the preparation method comprising:
[0007] Providing an initial multi-layer composite material, the initial multi-layer composite material comprising a first sub-layer to an nth sub-layer stacked in sequence, wherein n is greater than or equal to 2;
[0008] The surface of the first sublayer is irradiated with an intense pulsed photon beam, and the generated energy wave is transmitted through the first sublayer to the interface between the i-1th sublayer and the i-th sublayer, so as to form diffusion layers at the interfaces of adjacent sublayers from the first sublayer to the i-th sublayer, respectively, where i is greater than or equal to 2 and less than or equal to n;
[0009] In the case where the material of the i-1th sublayer is the first material and the material of the i-th sublayer is the second material, the diffusion layer located at the interface between the i-1th sublayer and the i-th sublayer is a diffusion layer formed by mutual diffusion of atoms and / or molecules of the first material and the second material; the thickness of the diffusion layer is 10 -7 m~10 -6 m;
[0010] There is a first incident angle between the incident direction of the intense pulsed photon beam and the plane where the first sublayer is located, and the first incident angle is greater than 0° and less than or equal to 90°.
[0011] In conjunction with the first aspect of the present application, in an optional implementation manner, the first incident angle ranges from 30° to 90°.
[0012] In conjunction with the first aspect of the present application, in an optional implementation manner, the energy source of the intense pulsed photon beam is an ultrashort pulse laser, and the width of a single pulse of the intense pulsed photon beam is 10 -15 s~10 -9 s.
[0013] In conjunction with the first aspect of the present application, in an optional implementation manner, the method further includes:
[0014] The surface of the nth sublayer is irradiated with an intense pulsed photon beam, and the generated energy wave is transmitted through the nth sublayer to the interface between the jth sublayer and the j+1th sublayer, so as to form diffusion layers at the interfaces of adjacent sublayers between the nth sublayer and the jth sublayer, wherein j is greater than or equal to 1 and less than n; the thickness of the diffusion layer is 10 -7 m~10 -6 m;
[0015] There is a second incident angle between the incident direction of the intense pulsed photon beam and the plane where the nth sublayer is located, and the second incident angle is greater than 0° and less than or equal to 90°.
[0016] In conjunction with the first aspect of the present application, in an optional embodiment, at least one of the first sublayer to the (i-1)th sublayer comprises a non-transparent material, and the thickness of the at least one sublayer is less than or equal to 10 -3 m.
[0017] In combination with the first aspect of the present application, in an optional embodiment, adjacent sublayers in the initial multilayer composite material are connected by at least one of a welding process, a hot pressing process, a deposition process, a spraying process, an electroplating process or an additive manufacturing process.
[0018] In conjunction with the first aspect of the present application, in an optional embodiment, an initial diffusion layer is provided between adjacent sub-layers in the initial multi-layer composite material, and the thickness of the initial diffusion layer is 10 -10 m~10 -7 m.
[0019] In a second aspect, an embodiment of the present application provides an interface-free material, wherein the interface-free material is prepared using the method for preparing the interface-free material as described in the first aspect.
[0020] In a third aspect, the present application provides another interface-free material, including:
[0021] A first sublayer to an nth sublayer stacked sequentially, wherein n is greater than or equal to 2;
[0022] at least one diffusion layer located at the interface between the kth sublayer and the k+1th sublayer, where k is greater than or equal to 1 and less than n;
[0023] When the material of the kth sublayer is the first material and the material of the k+1th sublayer is the second material, the diffusion layer located at the interface between the kth sublayer and the k+1th sublayer is a diffusion layer formed by mutual diffusion of atoms and / or molecules of the first material and the second material;
[0024] The thickness of the diffusion layer is 10 -7 m~10 -6 m.
[0025] In a fourth aspect, an embodiment of the present application provides a material processing device, including:
[0026] A fixing mechanism, used to fix an initial multi-layer composite material to be processed, wherein the initial multi-layer composite material comprises a first sub-layer to an nth sub-layer stacked in sequence, wherein n is greater than or equal to 2;
[0027] An intense pulsed photon beam generator is used to generate an intense pulsed photon beam to execute the method for preparing the interface-free material as described in the first aspect.
[0028] The interface-free material and preparation method thereof, and material processing equipment provided in the embodiment of the present application include: providing an initial multilayer composite material, wherein the initial multilayer composite material includes a first sublayer to an nth sublayer stacked in sequence, wherein n is greater than or equal to 2; irradiating the surface of the first sublayer with an intense pulsed photon beam, and the generated energy wave is transmitted through the first sublayer to the interface between the i-1th sublayer and the i-th sublayer, so as to form diffusion layers at the interfaces of adjacent sublayers between the first sublayer and the i-th sublayer, wherein i is greater than or equal to 2 and less than or equal to n; in the case where the material of the i-1th sublayer is the first material and the material of the i-th sublayer is the second material, the diffusion layer located at the interface between the i-1th sublayer and the i-th sublayer is a diffusion layer formed by mutual diffusion of atoms and / or molecules of the first material and the second material; the thickness of the diffusion layer is 10 -7 m~10 -6 m; there is a first incident angle between the incident direction of the intense pulsed photon beam and the plane where the first sublayer is located, and the first incident angle is greater than 0° and less than or equal to 90°. In the embodiment of the present application, by using an intense pulsed photon beam to irradiate the surface of the first sublayer of the initial multilayer composite material, the generated energy wave is transmitted through the first sublayer to the interface between the i-1th sublayer and the i-th sublayer, so as to form a thickness of 10 -7 m~10 -6 The diffusion layer of m, because the diffusion layer located at the interface of adjacent sub-layers is formed by the mutual diffusion of atoms and / or molecules of the materials of the adjacent sub-layers, changes the microstructure of the interface of the adjacent sub-layers (defects are reduced and density is increased), which can improve the sudden change of thermal and mechanical properties of the material at the interface, and then significantly reduce the residual stress at the interface of the adjacent sub-layers, thereby improving the fatigue resistance and service life of the interface-free material. In addition, the energy wave passes through the sub-layer, causing atomic diffusion in the sub-layer, so that the microstructure in each sub-layer through which the energy wave passes changes (defects are reduced and density is increased), which can also further improve the fatigue resistance and service life of the interface-free material.
[0029] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0031] Figure 1 A schematic diagram of a process for preparing a non-interface material provided in an embodiment of the present application;
[0032] Figures 2 to 8 A schematic diagram of the cross-sectional structure of the interface-free material during the preparation process provided in an embodiment of the present application;
[0033] Fig. 9 A schematic diagram of the cross-sectional structure of the interface-free material provided in the application embodiment. DETAILED DESCRIPTION
[0034] The exemplary embodiments disclosed in the present application will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present application are shown in the accompanying drawings, it should be understood that the present application can be implemented in various forms and should not be limited by the specific embodiments described herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present application and to fully convey the scope disclosed in the present application to those skilled in the art.
[0035] In the following description, a large number of specific details are given to provide a more thorough understanding of the present application. However, it is obvious to those skilled in the art that the present application can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present application, some technical features known in the art are not described; that is, all features of the actual embodiments are not described here, and well-known functions and structures are not described in detail.
[0036] In the drawings, the sizes of layers, regions, elements and their relative sizes may be exaggerated for clarity. Like reference numerals denote like elements throughout.
[0037] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present application, the first element, component, region, layer or part discussed below can be represented as the second element, component, region, layer or part. And when the second element, component, region, layer or part is discussed, it does not indicate that the present application necessarily has the first element, component, region, layer or part.
[0038] Spatially relative terms such as "under", "beneath", "below", "under", "above", "above", etc., may be used here for convenience of description to describe the relationship between an element or feature shown in the figure and other elements or features. It should be understood that in addition to the orientation shown in the figure, the spatial relationship terms are intended to also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is turned over, then the elements or features described as "under other elements" or "under it" or "under it" will be oriented as "on" other elements or features. Therefore, the exemplary terms "under" and "under" may include both upper and lower orientations. The device can be oriented otherwise (rotated 90 degrees or other orientations) and the spatial descriptors used herein are interpreted accordingly.
[0039] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be limiting of the present application. When used herein, the singular forms "one", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.
[0040] In order to thoroughly understand the present application, detailed steps and detailed structures will be presented in the following description to illustrate the technical solution of the present application. The preferred embodiments of the present application are described in detail below, but in addition to these detailed descriptions, the present application may also have other implementation methods.
[0041] In composite materials, lattice defects and residual stresses tend to be concentrated at the interface between different material layers. For example, when other film layers are deposited on a substrate, on the one hand, due to the difference in lattice parameters between the film layer and the substrate, lattice mismatch will cause defects, so intrinsic stress is usually generated at the interface between the substrate and the film layer. On the other hand, due to the different physical properties of the substrate and the film layer, there are differences in the thermal properties (including thermal expansion coefficient) of the substrate and the film layer. When the temperature changes, thermal expansion will be restricted, so thermal stress is easily generated at the interface between the substrate and the film layer. The lattice defects and residual stresses on these interfaces play a decisive role in the thermal and mechanical properties of the composite material, which will lead to reduced fatigue resistance and service life of the composite material.
[0042] Based on this, an embodiment of the present application provides a method for preparing a non-interface material. Figure 1 A schematic diagram of a process for preparing a non-interface material provided in an embodiment of the present application; Figure 1As shown, the method includes:
[0043] Step S101, providing an initial multi-layer composite material, the initial multi-layer composite material comprising a first sub-layer to an nth sub-layer stacked in sequence, wherein n is greater than or equal to 2;
[0044] Step S102, irradiating the surface of the first sublayer with an intense pulsed photon beam, and the generated energy wave is transmitted through the first sublayer to the interface between the i-1th sublayer and the i-th sublayer, so as to form diffusion layers at the interfaces of adjacent sublayers between the first sublayer and the i-th sublayer, respectively, where i is greater than or equal to 2 and less than or equal to n; when the material of the i-1th sublayer is the first material and the material of the i-th sublayer is the second material, the diffusion layer located at the interface between the i-1th sublayer and the i-th sublayer is a diffusion layer formed by mutual diffusion of atoms and / or molecules of the first material and the second material; the thickness of the diffusion layer is 10 -7 m~10 -6 m; there is a first incident angle between the incident direction of the intense pulsed photon beam and the plane where the first sublayer is located, and the first incident angle is greater than 0° and less than or equal to 90°.
[0045] It can be understood that, through the above method, the surface of the first sublayer of the initial multilayer composite material is irradiated with an intense pulsed photon beam, and the generated energy wave is transmitted through the first sublayer to the interface between the i-1th sublayer and the i-th sublayer, so as to form a thickness of 10 -7 m~10 -6 The diffusion layer of m, because the diffusion layer located at the interface of adjacent sub-layers is formed by the mutual diffusion of atoms and / or molecules of the materials of the adjacent sub-layers, changes the microstructure of the interface of the adjacent sub-layers (defects are reduced and density is increased), which can improve the sudden change of thermal and mechanical properties at the interface, and then significantly reduce the residual stress at the interface of the adjacent sub-layers, thereby improving the fatigue resistance and service life of the interface-free material. In addition, the energy wave passes through the sub-layer, causing atomic diffusion in the sub-layer, so that the microstructure in each sub-layer through which the energy wave passes changes (defects are reduced and density is increased), which can also further improve the fatigue resistance and service life of the interface-free material.
[0046] It should be noted that in the embodiment of the present application, a diffusion layer is formed at the interface of adjacent sub-layers so that the original interface between the adjacent sub-layers disappears. Since the diffusion layer is formed by the mutual diffusion of material atoms and / or molecules of the adjacent sub-layers, and it is an atomic-level gradient diffusion, there is no obvious boundary of composition and structural changes between the diffusion layer and the adjacent sub-layers. Therefore, it can be considered that the interface between the diffusion layer and the adjacent sub-layer has disappeared both microscopically and macroscopically. Therefore, the prepared material is called an interface-free material.
[0047] Next, combine Figures 2 to 8 A preparation method of a non-interface material provided in an embodiment of the present application and its beneficial effects are further described in detail.
[0048] First, please refer to Figure 2 , performing step S101, providing an initial multilayer composite material 10, the initial multilayer composite material 10 comprising a first sublayer 101 to an nth sublayer 106 stacked in sequence, wherein n is greater than or equal to 2.
[0049] In the embodiment of the present application, the material of each sublayer in the initial multilayer composite material 10 may be the same or different, and the thickness of each sublayer may be the same or different. The material of each sublayer may include metal and / or non-metal, respectively, for example. In some specific embodiments, the material of each sublayer may include at least one of ceramic, metal or diamond, etc. For example, when n=2, the first sublayer 101 and the second sublayer may be a metal-ceramic composite material, a metal-metal composite material, a metal-diamond composite material, a ceramic-ceramic composite material or a ceramic-diamond composite material, etc. When n=3, the first sublayer 101, the second sublayer and the third sublayer may be, for example, a metal-ceramic-metal composite material, a metal-metal-ceramic composite material, a metal-ceramic-ceramic composite material, a metal-ceramic-diamond composite material or a metal-diamond-ceramic composite material, etc.
[0050] In some embodiments, adjacent sublayers in the initial multilayer composite material 10 can be connected by at least one of a welding process, a hot pressing process (e.g., vacuum hot pressing), a deposition process (e.g., chemical vapor deposition, physical vapor deposition, or atomic layer vapor deposition), a spraying process (e.g., cold spraying or hot spraying), an electroplating process, or an additive manufacturing process (e.g., electron beam 3D printing, laser 3D printing, cladding, or sintering).
[0051] As mentioned above, in the initial multilayer composite material 10, residual stress is easily concentrated at the interface between different sub-layers. When adjacent sub-layers are made of the same material, the adjacent sub-layers may have different morphologies, such as different crystal phases. For example, taking high-temperature additive manufacturing materials as an example, when adjacent layers are made of the same material, due to the different temperatures of different layers during the preparation process, the crystal phases of adjacent layers at the interface are different, which in turn leads to thermal residual stress concentration.
[0052] In some embodiments, adjacent sub-layers in the initial multi-layer composite material 10 may be connected by a physical method, wherein the surface roughness of the connecting surfaces of the adjacent sub-layers is less than 10 μm.
[0053] In the embodiment of the present application, when the surface roughness of the connecting surfaces of adjacent sub-layers is less than 10 μm, the connecting surfaces of adjacent sub-layers are smooth enough so that the adjacent sub-layers can be well combined together by physical means. Exemplarily, the transparent material or translucent material and the non-transparent material and the transparent material and the translucent material can be physically connected to form the initial multi-layer composite material 10, so that the initial multi-layer composite material 10 can be processed by the above-mentioned preparation method of the interface-free material.
[0054] Next, please refer to Figure 3 and Figure 4 , execute step S102, irradiate the surface of the first sublayer 101 with an intense pulsed photon beam (such as Figure 3 The generated energy wave is transmitted through the first sub-layer 101 to the interface between the i-1th sub-layer 102 and the i-th sub-layer 103, so as to form diffusion layers 20 at the interfaces of adjacent sub-layers between the first sub-layer 101 and the i-th sub-layer 103 (see Figure 4 ), where i is greater than or equal to 2 and less than or equal to n; in the case where the material of the i-1th sublayer 102 is the first material and the material of the i-th sublayer 103 is the second material, the diffusion layer 20 located at the interface between the i-1th sublayer 102 and the i-th sublayer 103 is a diffusion layer formed by the mutual diffusion of atoms and / or molecules of the first material and the second material; the thickness of the diffusion layer 20 is 10 -7 m~10 -6 m; there is a first incident angle α between the incident direction of the intense pulsed photon beam and the plane where the first sublayer 101 is located, and the first incident angle α is greater than 0° and less than or equal to 90°.
[0055] The first sublayer 101 may include a top surface and a bottom surface opposite to the top surface, wherein the top surface is the side irradiated by the intense pulsed photon beam, and ignoring the flatness of the top surface and the bottom surface, the surface where the top surface and the bottom surface of the first sublayer 101 are located, or strictly speaking, the center plane in the thickness direction of the first sublayer 101, is determined as the plane where the first sublayer 101 is located.
[0056] In the embodiment of the present application, an intense pulsed photon beam is used to irradiate the surface of the first sublayer 101 of the initial multilayer composite material 10, and the generated energy wave is transmitted through the first sublayer 101 to the interface between the i-1 sublayer 102 and the i-th sublayer 103, so as to form diffusion layers 20 at the adjacent sublayer interfaces between the first sublayer 101 and the i-th sublayer 103. Since the diffusion layer 20 located at the adjacent sublayer interface is formed by the mutual diffusion of material atoms and / or molecules of the adjacent sublayers, the lattice in the adjacent sublayer material will be filled and ordered during the formation of the diffusion layer 20, thereby reducing the lattice defects (such as vacancies) in the diffusion layer 20 and the sublayer materials on both sides of the diffusion layer 20, and optimizing the interface microstructure of the adjacent sublayers. The sudden change of thermal and mechanical properties at the interface can be improved, so that the residual stress at the adjacent sublayer interface can be significantly reduced, thereby improving the fatigue resistance and service life of the interface-free material. In addition, since the energy wave passes through the sublayer, atomic diffusion occurs in the sublayer, so that the microstructure of each sublayer through which the energy wave passes is optimized. After the microstructure of the corresponding sublayer is optimized, the fatigue resistance and service life of the interface-free material can be further improved.
[0057] In the embodiment of the present application, an intense pulsed photon beam irradiates the surface of the first sublayer 101, and interacts with the atoms and / or molecules on the surface of the first sublayer 101 to generate energy waves, such as ultrasonic waves. In the process of the energy wave being transmitted through the first sublayer 101 to the interface between the i-1 sublayer 102 and the i-th sublayer 103, the atoms and / or molecules inside the sublayer material and at the interface are displaced or diffused. This process is a physical process. Compared with the usual high-temperature treatment of composite materials (such as annealing), the diffusion layer 20 in the present application can be regarded as a diffusion layer 20 bonded by room-temperature diffusion bonds. The room-temperature diffusion bonds here can be understood as, at room temperature, under the action of energy, the atoms and / or molecules in the materials of adjacent sublayers diffuse with each other to form new molecular orbitals. Therefore, the problem of high-temperature treatment easily introducing new thermal residual stresses into the composite material can be avoided. Moreover, the thickness range of the diffusion layer 20 bonded by room-temperature diffusion bonds is 10 -7 m~10 -6 m, which can better improve the mutation of thermal and mechanical properties at the interface, and thus can better improve the thermal and mechanical properties of the prepared interface-free materials.
[0058] In the embodiment of the present application, an intense pulsed photon beam is used to irradiate the surface of the first sublayer 101. By changing the relative position between the energy source of the intense pulsed photon beam and the initial multilayer composite material 10, the interfaces between adjacent sublayers in the initial multilayer composite material 10 can be easily and comprehensively processed, thereby better ensuring the thermal and mechanical properties of the prepared interface-free material.
[0059] It should be noted that Figure 4 The diffusion layer 20 between the i-1st sublayer 102 and the i-th sublayer 103 is exemplarily shown in FIG. It can be understood that in the first sublayer 101 to the i-1st sublayer 102, the diffusion layer 20 is formed at the interface of the adjacent sublayers, and the specific material and structure of the diffusion layer 20 are related to the material of the adjacent sublayer. In addition, Figure 4 The case where i is less than n is exemplarily shown in FIG. 1 . When i is equal to n, it can be understood that in the obtained interface-free material, a diffusion layer 20 is formed between every two adjacent sub-layers.
[0060] The larger the first incident angle α between the incident direction of the intense pulsed photon beam and the plane where the first sublayer 101 is located, the more concentrated the irradiation energy is, and the higher the efficiency of the irradiation treatment is. Therefore, in some embodiments, the first incident angle α can range from 30° to 90°, for example, 45°, 60°, 75° or 80°. In this way, the utilization efficiency of the energy of the intense pulsed photon beam can be improved. In a specific embodiment, the first incident angle α can be 90°, so that the utilization efficiency of the energy of the intense pulsed photon beam can be higher.
[0061] In some embodiments, the energy source of the intense pulsed photon beam may be an ultrashort pulse laser, and the width of a single pulse of the intense pulsed photon beam is 10 -15 s~10 -9 s.
[0062] The width of a single pulse of an intense pulsed photon beam is 10 -15 s~10 -9 s, the total energy can be controlled by the irradiation frequency, etc., so that the diffusion layer 20 with room temperature diffusion bonds can be formed well. It can be understood that in actual preparation, the energy of the intense pulsed photon beam can be selected in combination with the physical properties of the sub-layer material itself (dielectric constant or melting point, etc.), as well as parameters such as the sub-layer interface and the internal performance of the sub-layer.
[0063] In some embodiments, at least one of the first to i-1th sublayers includes a non-transparent material, and the thickness of the at least one sublayer may be less than or equal to 10 -3 m.
[0064] In the embodiment of the present application, the thickness of the sublayer including the non-transparent material in the first sublayer 101 to the (i-1)th sublayer 102 is less than or equal to 10 -3 m, the selection range of the energy source of the intense pulsed photon beam can be made wider. It can be understood that if one of the first to i-1th sublayers includes a non-transparent material, the thickness of the sublayer including the non-transparent material is less than or equal to 10 -3m, if multiple sub-layers from the first sub-layer to the (i-1)th sub-layer include non-transparent materials, the total thickness of the multiple sub-layers including non-transparent materials is less than or equal to 10 -3 m, so that the energy source of the intense pulsed photon beam can be selected more conveniently so that when the intense pulsed photon beam is used to irradiate the surface of the first sublayer 101, it is ensured that the generated energy wave can be smoothly transmitted through the first sublayer 101 to the interface between the i-1 sublayer 102 and the i sublayer 103.
[0065] In some embodiments, please refer to Figure 5 and Figure 6 The method for preparing the interface-free material may further include: irradiating the surface of the nth sublayer 106 with an intense pulsed photon beam (eg Figure 5 The generated energy wave is transmitted through the nth sublayer 106 to the interface between the jth sublayer 104 and the j+1th sublayer 105, so as to form diffusion layers 20 at the adjacent sublayer interfaces between the nth sublayer 106 and the jth sublayer 104 (see Figure 6 ), where j is greater than or equal to 1 and less than n; the thickness of the diffusion layer 20 is 10 -7 m~10 -6 m;
[0066] There is a second incident angle β between the incident direction of the intense pulsed photon beam and the plane where the n-th sublayer 106 is located, and the second incident angle β is greater than 0° and less than or equal to 90°.
[0067] In the embodiment of the present application, an intense pulsed photon beam can be used to irradiate the surfaces of the first sublayer 101 and the nth sublayer 106 respectively to form a diffusion layer 20 at the interface between the target adjacent sublayers, so that the initial multilayer material can be processed more flexibly. In actual preparation, the surface of the first sublayer 101 can be irradiated first, and then the surface of the nth sublayer 106 can be irradiated, or the surface of the nth sublayer 106 can be irradiated first, and then the surface of the first sublayer 101 can be irradiated, or the surfaces of the first sublayer 101 and the nth sublayer 106 can be irradiated at the same time. In some specific embodiments, for a composite material formed by a transparent material and a non-transparent material, an intense pulsed photon beam can be selected to irradiate the surface of the transparent material, so that the controllability and treatment effect of the irradiation treatment can be better.
[0068] It should be noted that Figure 6The diffusion layer 20 between the j-th sublayer 104 and the j+1-th sublayer 105 is exemplarily shown. It can be understood that in the j+1-th sublayer 105 to the n-th sublayer 106, the diffusion layer 20 is formed at the interface of the adjacent sublayers. The formation process of the diffusion layer 20 and the material and structure of the diffusion layer 20 here can be understood by referring to the formation process of the diffusion layer 20 and the material and structure of the diffusion layer 20 in the aforementioned embodiment, and will not be repeated here.
[0069] It also needs to be explained. Figure 5 What is shown is the case where j is greater than i. In some other embodiments of the present application, the case where j is less than or equal to i is not excluded.
[0070] In some specific embodiments, the second incident angle β may be in the range of 30° to 90°, for example, 45°, 60°, 75° or 80°. In this way, the utilization efficiency of the energy of the intense pulsed photon beam can be improved. In a specific embodiment, the second incident angle β may be 90°, so that the utilization efficiency of the energy of the intense pulsed photon beam can be higher.
[0071] In some specific embodiments, at least one of the nth sublayer 106 to the jth sublayer 104 comprises a non-transparent material, and the thickness of at least one sublayer is less than or equal to 10 -3 m, so that the energy source of the intense pulsed photon beam can be selected more conveniently so that when the intense pulsed photon beam is used to irradiate the surface of the n-th sublayer 106, it is ensured that the generated energy wave can be smoothly transmitted through the n-th sublayer 106 to the interface between the j-th sublayer 104 and the j+1-th sublayer 105.
[0072] It should be noted that the non-transparent material described in the embodiments of the present application includes a material that has a certain blocking effect on photon beams.
[0073] In some embodiments, Figure 7 As shown, there may be an initial diffusion layer 30 between adjacent sub-layers in the initial multi-layer composite material 10, and the thickness of the initial diffusion layer 30 is 10 -10 m~10 -7 m.
[0074] Figure 7 Taking n=2 as an example, in the initial multilayer composite material 10 formed by the existing process, the first sublayer 101 and the nth sublayer 106 have a certain wettability, and the initial diffusion layer 30 can be formed, but the thickness of the initial diffusion layer 30 is 10 -10 m~10 -7m, the initial diffusion layer 30 is usually obtained after thermal processing, so there are many thermal defects in the initial diffusion layer 30, the lattice arrangement is disordered, and the residual stress is large. The embodiment of the present application can be based on the initial diffusion layer 30, and the surface of the first sub-layer 101 is irradiated to cause the atoms and / or lattices of the initial diffusion layer 30 and the nearby sub-layer materials to vibrate, displace, diffuse and rearrange, thereby forming Figure 8 The diffusion layer 20 is shown.
[0075] The residual stress in the interface-free material and the corresponding initial multilayer composite material prepared in the embodiment of the present application was tested by X-ray diffraction (XRD). The diffraction peak shift effect at different ψ angles is related to the change of the interplanar spacing d. The basis for calculating the stress value is sin 2 The partial derivative of ψ with respect to d. The test results are shown in Table 1, wherein the interface-free material is obtained by processing the corresponding initial multilayer composite material using the preparation method of the interface-free material in the present application, and the initial multilayer composite material corresponding to the interface-free material is a substrate plus a coating, wherein the material of the substrate is cobalt-containing carbide (WC), and the coating is TiCN and Al2O3 prepared by a chemical vapor deposition process and sequentially stacked on the substrate.
[0076] It can be seen from the data in Table 1 that the residual stress of the interface-free material prepared by the embodiment of the present application is significantly reduced compared to the residual stress in the corresponding initial multilayer composite material, which can effectively improve the fatigue resistance and service life of the interface-free material.
[0077] Table 1
[0078]
[0079] Based on this, an embodiment of the present application provides an interface-free material, which is prepared using the steps in the method for preparing the interface-free material provided in any of the aforementioned embodiments.
[0080] Based on this, the present application embodiment provides another interface-free material, such as Fig. 9 As shown, the non-interface materials include:
[0081] A first sublayer 101 to an nth sublayer 106 stacked in sequence, wherein n is greater than or equal to 2;
[0082] at least one diffusion layer 20 located at the interface between the kth sublayer 107 and the k+1th sublayer 108 , where k is greater than or equal to 1 and less than n;
[0083] When the material of the kth sublayer 107 is the first material and the material of the k+1th sublayer 108 is the second material, the diffusion layer 20 located at the interface between the kth sublayer 107 and the k+1th sublayer 108 is a diffusion layer 20 formed by mutual diffusion of atoms and / or molecules of the first material and the second material;
[0084] The thickness of the diffusion layer 20 is 10 -7 m~10 -6 m.
[0085] In the embodiment of the present application, the diffusion layer 20 located at the interface between the kth sublayer 107 and the k+1th sublayer 108 is formed by mutual diffusion of atoms and / or molecules of the first material and the second material. During the diffusion process, the lattices in the adjacent sublayer materials are supplemented and ordered, so that the lattice defects (such as vacancies) in the diffusion layer 20 and the sublayer materials near the diffusion layer 20 are reduced and the microstructure of the interface between the adjacent sublayers is optimized. The thickness of the diffusion layer 20 is 10 -7 m~10 -6 m, can better improve the sudden change of thermal and mechanical properties at the interface, so that the residual stress at the interface of adjacent sub-layers can be significantly reduced, thereby improving the fatigue resistance and service life of the non-interface material. In addition, the diffusion layer 20 in the embodiment of the present application can be located at the interface between any one or more pairs of adjacent sub-layers in the non-interface material.
[0086] The non-interface material in the embodiment of the present application may be, for example, a composite material.
[0087] Based on this, an embodiment of the present application provides a material processing device, including:
[0088] A fixing mechanism, used for fixing an initial multi-layer composite material to be processed, wherein the initial multi-layer composite material comprises a first sub-layer to an nth sub-layer stacked in sequence, wherein n is greater than or equal to 2;
[0089] An intense pulsed photon beam generator is used to generate an intense pulsed photon beam to execute the method for preparing the interface-free material provided in any of the aforementioned embodiments.
[0090] In some embodiments, the material processing equipment may further include: a first moving mechanism, configured to drive the fixing mechanism to move so as to adjust the position of the initial multi-layer composite material.
[0091] Exemplarily, the first motion mechanism can drive the fixed mechanism to move, so that the intense pulsed photon beam generated by the intense pulsed photon beam generating device can irradiate the surface of the first sublayer and / or the nth sublayer of the initial multi-layer composite material to be processed, and the intense pulsed photon beam can irradiate the surface of the first sublayer and / or the nth sublayer along a preset trajectory. For the case where the surface of the first sublayer and / or the nth sublayer is a two-dimensional plane or a three-dimensional plane, irradiation treatment can be conveniently performed. Furthermore, the first motion mechanism can also drive the fixed mechanism to move to adjust the incident angle of the intense pulsed photon beam incident on the surface of the first sublayer and / or the nth sublayer. The incident angle here can be the angle between the incident direction of the intense pulsed photon beam and the plane where the first sublayer and / or the nth sublayer is located.
[0092] In some embodiments, the material processing equipment may further include: a second motion mechanism, used to drive the intense pulsed photon beam generating device to move so as to adjust the emission direction of the intense pulsed photon beam.
[0093] Exemplarily, the second motion mechanism can drive the intense pulsed photon beam generator to move, so that the intense pulsed photon beam generated by the intense pulsed photon beam generator can irradiate the surface of the first sublayer and / or the nth sublayer of the initial multi-layer composite material to be processed, and the intense pulsed photon beam can irradiate the surface of the first sublayer and / or the nth sublayer along a preset trajectory. The situation where the surface of the first sublayer and / or the nth sublayer is a two-dimensional plane or a three-dimensional plane can be easily handled. Furthermore, the second motion mechanism can also drive the fixed mechanism to move to adjust the incident angle of the intense pulsed photon beam incident on the surface of the first sublayer and / or the nth sublayer. The incident angle here can be the angle between the incident direction of the intense pulsed photon beam and the plane where the first sublayer and / or the nth sublayer is located.
[0094] In some embodiments, the material processing equipment may further include: a transmission and transformation device for changing the spot shape and transmission path of the intense pulsed photon beam, so as to more conveniently and flexibly control the energy and incident angle of the intense pulsed photon beam incident on the surface of the first sublayer and / or the nth sublayer of the initial multi-layer composite material to be processed.
[0095] It can be understood that in some other embodiments of the present application, the positions of the intense pulsed photon beam generating device and the fixing mechanism as well as the intense pulsed photon beam spot shape and the transmission path can be adjusted in coordination with the first motion mechanism, the second motion mechanism and the conduction and transformation device to achieve more flexible control of the intense pulsed photon beam irradiation to the surface of the first sublayer and / or the nth sublayer of the initial multi-layer composite material to be processed.
[0096] It should be noted that the interface-free material embodiment provided in this application, the interface-free material preparation method embodiment, and the material processing equipment embodiment belong to the same concept; the technical features in the technical solutions recorded in each embodiment can be arbitrarily combined without conflict. However, it should be further noted that the interface-free material provided in the embodiment of this application, the combination of its various technical features can already solve the technical problem to be solved by this application; therefore, the interface-free material provided in the embodiment of this application may not be limited by the interface-free material preparation method provided in the embodiment of this application, and any interface-free material prepared by the interface-free material preparation method provided in the embodiment of this application is within the scope of protection of this application.
[0097] It should be understood that the above embodiments are exemplary and are not intended to include all possible implementations included in the claims. Various modifications and changes may be made on the basis of the above embodiments without departing from the scope of the present disclosure. Similarly, the various technical features of the above embodiments may be arbitrarily combined to form other embodiments of the present application that may not be explicitly described. Therefore, the above embodiments only express several implementations of the present application and do not limit the scope of protection of the patent of this application.
Claims
1. A method for preparing a non-interface material, characterized in that: The method comprises: Providing an initial multi-layer composite material, the initial multi-layer composite material comprising a first sub-layer to an nth sub-layer stacked in sequence, wherein n is greater than or equal to 2; The surface of the first sublayer is irradiated with an intense pulsed photon beam, and the generated energy wave is transmitted through the first sublayer to the interface between the i-1th sublayer and the i-th sublayer, so as to form diffusion layers at the interfaces of adjacent sublayers from the first sublayer to the i-th sublayer, respectively, where i is greater than or equal to 2 and less than or equal to n; In the case where the material of the i-1th sublayer is the first material and the material of the i-th sublayer is the second material, the diffusion layer located at the interface between the i-1th sublayer and the i-th sublayer is a diffusion layer formed by mutual diffusion of atoms and / or molecules of the first material and the second material; the thickness of the diffusion layer is 10 -7 m~10 -6 m; There is a first incident angle between the incident direction of the intense pulsed photon beam and the plane where the first sublayer is located, and the first incident angle is greater than 0° and less than or equal to 90°.
2. The method for preparing the interface-free material according to claim 1, characterized in that: The first incident angle ranges from 30° to 90°.
3. The method for preparing the interface-free material according to claim 1, characterized in that: The energy source of the intense pulsed photon beam is an ultrashort pulse laser, and the width of a single pulse of the intense pulsed photon beam is 10 -15 s~10 -9 s.
4. The method for preparing the interface-free material according to claim 1, characterized in that: The method further comprises: The surface of the nth sublayer is irradiated with an intense pulsed photon beam, and the generated energy wave is transmitted through the nth sublayer to the interface between the jth sublayer and the j+1th sublayer, so as to form diffusion layers at the interfaces of adjacent sublayers between the nth sublayer and the jth sublayer, wherein j is greater than or equal to 1 and less than n; the thickness of the diffusion layer is 10 -7 m~10 -6 m; There is a second incident angle between the incident direction of the intense pulsed photon beam and the plane where the nth sublayer is located, and the second incident angle is greater than 0° and less than or equal to 90°.
5. The method for preparing the interface-free material according to any one of claims 1 to 4, characterized in that: At least one of the first to the (i-1)th sublayers comprises a non-transparent material, and a thickness of the at least one sublayer is less than or equal to 10 -3 m.
6. The method for preparing the interface-free material according to any one of claims 1 to 4, characterized in that: Adjacent sub-layers in the initial multi-layer composite material are connected by at least one of a welding process, a hot pressing process, a deposition process, a spraying process, an electroplating process or an additive manufacturing process; Alternatively, adjacent sub-layers in the initial multi-layer composite material are connected by a physical method, wherein the surface roughness of the connecting surfaces of the adjacent sub-layers is less than 10 μm.
7. The method for preparing the interface-free material according to claim 6, characterized in that: There is an initial diffusion layer between adjacent sub-layers in the initial multi-layer composite material, and the thickness of the initial diffusion layer is 10 -10 m~10 -7 m.
8. A non-interface material, characterized in that: The interface-free material is prepared by the method for preparing the interface-free material according to any one of claims 1 to 7.
9. A non-interface material, characterized in that: include: A first sublayer to an nth sublayer stacked sequentially, wherein n is greater than or equal to 2; at least one diffusion layer located at the interface between the kth sublayer and the k+1th sublayer, where k is greater than or equal to 1 and less than n; When the material of the kth sublayer is the first material and the material of the k+1th sublayer is the second material, the diffusion layer located at the interface between the kth sublayer and the k+1th sublayer is a diffusion layer formed by mutual diffusion of atoms and / or molecules of the first material and the second material; The thickness of the diffusion layer is 10 -7 m~10 -6 m.
10. A material processing equipment, characterized in that: include: A fixing mechanism, used to fix an initial multi-layer composite material to be processed, wherein the initial multi-layer composite material comprises a first sub-layer to an nth sub-layer stacked in sequence, wherein n is greater than or equal to 2; An intense pulsed photon beam generator is used to generate an intense pulsed photon beam to execute the method for preparing the interface-free material according to any one of claims 1 to 7.
Citation Information
Patent Citations
Preparation method of metal-inorganic composite material
CN110193664A
Laser cladding equipment
CN213232496U
Pulsed electron beam joining of materials
US5599468A