Preparation method of CeO2-coated MnO2 composite material
CeO2@MnO2 composite material prepared by deposition method improves catalytic performance by using strong interaction between components, solving the problems of insufficient catalytic performance and poor environmental adaptability in the prior art, and achieving efficient removal and stability of water pollutants recycle use.
Patent Information
- Application Number
- CN202411303652.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-03
AI Technical Summary
CeO2@MnO2 composite materials lack strong interactions, resulting in insufficient catalytic performance, low adsorption and degradation efficiency of pollutants, and a great impact on pH value and ions in water, limiting their application under different water quality conditions, resulting in unstable treatment effect and Costs increase.
CeO2@MnO2 composite material was prepared by deposition method, and CeO2 nanorods were prepared by hydrothermal method and co-precipitation method, and mixed with persulfate to promote strong interactions between components to improve catalytic performance.
It has achieved significant improvement in catalytic performance, is widely used in the removal of various pollutants, improves degradation efficiency, and has a small impact on pH value and ions in water. It is suitable for water pollution control in various environments, and is used in multiple cycles. Maintain good results afterwards.
Smart Images

Figure CN119056441A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water pollution control engineering, and in particular to a method for preparing a CeO2@MnO2 composite material. Background Art
[0003] At present, among the many methods for removing organic matter from water, such as photocatalysis, adsorption, and persulfate oxidation, persulfate advanced oxidation has the advantages of strong oxidation ability, wide applicable pH range, and high stability. This technology has universal applicability and is applicable to most organic pollutants. It can degrade pollutants into small molecular inorganic substances or CO2 and H2O in a short time to avoid secondary pollution. In the prior art, metals or metal oxides are often used as catalysts to degrade liquid phase organic pollutants. Among many materials, Mn-based materials are used for water pollution control due to their diverse valence states, environmental friendliness, and rich and extensive sources. Although MnO2 has good performance in activating PMS to oxidize pollutants, the activity of single-component materials is poor compared to that of multi-component materials (low degradation rate, long degradation time, low mineralization rate, etc.). In addition, researchers mainly focus on MnO2 to activate PMS, and rarely pay attention to PDS to oxidize pollutants. In order to further realize the practical applicability of Mn-based materials, it is very important to prepare Mn-based materials with good catalytic activity under both PMS and PDS.
[0004] Based on the oxidation mechanism, PMS / PDS is activated on the surface of the material to generate SO4 2·- , OH or 1 O2 and other active species oxidize pollutants. However, the lifespan of various free radicals is short (SO4 2·- The lifetime of OH is 20ns, 1The lifetime of O2 is 3μs). Therefore, close contact between pollutants, PMS / PDS, and catalytic materials can achieve deep catalytic oxidation of pollutants. In order to improve catalytic activity, researchers have adopted various methods to promote the rapid utilization of active species, such as adsorption-catalytic coupling or strong interaction between active components. For adsorption-catalytic coupling, some researchers use adsorbent materials to adsorb pollutants and then add PMS for oxidation, and some researchers couple oxides with adsorbent materials, and adsorption and catalysis are carried out simultaneously (ACS ES&T Water, 2020, 1(1): 145-156; Small, 2023, 19(50): 2303928.). For materials with strong interactions between active components, researchers prepared spinels and multi-component composite materials (Journal of hazardous materials, 2020, 381: 121209; Chemical Engineering Journal, 2019, 355: 448-456). Although some progress has been made in the research of Mn-based materials, no research on adsorption and in-situ degradation integrated materials has been reported.
[0005] However, CeO2@MnO2 composite materials do not have strong interactions, and their catalytic performance will be significantly insufficient, resulting in low efficiency in the adsorption and degradation of pollutants, prolonged treatment time, and affected water quality improvement effects. In addition, if it has a greater impact on pH values and common ions in water, it will limit its application under different water quality conditions, resulting in unstable treatment effects, and reducing the breadth and reliability of practical applications. At the same time, if the degradation effect of the composite material decreases significantly after multiple cycles of use, users will face higher replacement costs, affecting economic efficiency and sustainability, thereby reducing the attractiveness and market competitiveness of the technology. In response to the above problems, the inventors propose a method for preparing a CeO2@MnO2 composite material to solve the above problems. Summary of the invention
[0006] In order to solve the problems that CeO2@MnO2 lacks strong interaction, has poor environmental adaptability and poor recycling performance, which will lead to low catalytic efficiency, unstable treatment effect and increased overall cost, thereby limiting its application effect and sustainability in water pollution control; the purpose of the present invention is to provide a method for preparing a CeO2@MnO2 composite material.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solution: a method for preparing a CeO2@MnO2 composite material, comprising the following steps:
[0008] S1. Preparation of MnO2 nanorods: Preparation of MnO2 nanorods by hydrothermal method;
[0009] S2. Preparation of CeO2: Preparation of CeO2 by coprecipitation method;
[0010] S3, preparing CeO2@MnO2 series composite materials: preparing CeO2@MnO2 composite materials by a deposition method;
[0011] S4, preparing a mixture: mixing the CeO2@MnO2 composite material with persulfate;
[0012] S5. Degradation of organic pollutants: The mixture is dispersed in a water body containing organic pollutants to be treated for degradation to obtain degraded water.
[0013] Preferably, the mass ratio of CeO2 to MnO2 in the CeO2@MnO2 composite material in S3 is 0.1-4; the mass ratio of CeO2@MnO2 to persulfate in S4 is 0.1-5; and the amount of the mixture in S5 is 0.06-2.5 g / L.
[0014] Preferably, the calcination temperature required in the material preparation process is 400-600°C, the calcination time is 2-6h, and the calcination heating rate is 5°C / min; the alkaline precipitant includes ammonia water, potassium hydroxide, saturated aqueous solution of ammonium carbonate, ammonia water-ammonium carbonate buffer solution, potassium hydroxide-ammonium carbonate buffer solution; the cerium has a significant effect on the morphology and structure of MnO2 nanorods and the chemical environment of manganese during the nucleation process in an alkaline environment; the cerium nucleation temperature range is -5-60°C, and the nucleation precipitation time is 5-120min.
[0015] Preferably, the CeO2@MnO2 composite material and persulfate degrade organic pollutants, the particle size of the CeO2@MnO2 composite material is 100-400 mesh; the persulfate is any one of potassium persulfate, sodium persulfate, and potassium hydrogen persulfate, the reaction temperature of the CeO2@MnO2 composite material and persulfate to degrade organic pollutants is 10-30°C, and the degradation time is 60-180min; the pH value of the mixture of the CeO2@MnO2 composite material and persulfate to degrade organic pollutants is 3-9 after being dispersed in the water body containing organic pollutants to be treated; the organic pollutants in the organic pollutants degraded by the CeO2@MnO2 composite material and persulfate are any one of Congo red, tetracycline, and doxycycline.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] 1. The present invention obtains CeO2@MnO2 with excellent catalytic performance by using a deposition method. There is a strong interaction between the CeO2 and MnO2 components in the CeO2@MnO2 composite material, which promotes the in-situ coordinated adsorption and catalysis of pollutants and facilitates the interface transfer of electrons. Therefore, both static and dynamic systems can effectively oxidize organic pollutants in water bodies.
[0018] 2. The CeO2@MnO2 in the present invention is widely applicable to the removal of various pollutants and complex pollution, and has the characteristics of being less affected by pH value and other common ions in water, and is suitable for water pollution control in various environments;
[0019] 3. The CeO2@MnO2 in the present invention effectively solves the problems of low degradation rate and long degradation time of single-component (MnO2) materials, and still maintains a good pollutant degradation effect after multiple cycles. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 The degradation results of tetracycline in water by CeO2@MnO2 single components CeO2 and MnO2 of the present invention.
[0022] Figure 2 The degradation results of CeO2@MnO2 of the present invention on Congo red, tetracycline and doxycycline are compared.
[0023] Figure 3 Results of tetracycline degradation by CeO2@MnO2 at different pH values.
[0024] Figure 4 The results of the CeO2@MnO2 of the present invention degrading tetracycline in actual water bodies.
[0025] Figure 5 Comparison of cyclic test results of tetracycline degradation by CeO2@MnO2 of the present invention.
[0026] Figure 6 SEM results of CeO2, MnO2 and CeO2@MnO2 composites.
[0027] Figure 7 XRD results of CeO2, MnO2 and CeO2@MnO2 composites. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1: Figure 1-7 As shown, a method for preparing CeO2@MnO2 composite materials based on strong interaction between active components to promote pollutant adsorption catalysis and its activation of persulfate to degrade organic pollutants includes the following steps:
[0030] S1. Preparation of MnO2 nanorods: The hydrothermal method was used. Potassium permanganate and manganese acetate were first added to 32 mL of deionized water, and then 0.5 mL of nitric acid solution was added. After the reagents were fully dissolved, they were transferred to a hydrothermal reactor. The reactor was kept at 100°C for 24 hours and then naturally cooled to room temperature. The obtained material was washed and dried, and then placed in a muffle furnace. After being kept at 400°C for 4 hours, the nanorod MnO2 material was obtained.
[0031] Preparation of S2 and CeO2: Prepared by coprecipitation method, dissolve a certain amount of cerium nitrate in deionized water. After the cerium nitrate is completely dissolved, add ammonia water drop by drop until the pH value reaches 11, and then let it stand for 2 hours. After standing, wash the precipitate and then dry it. Then transfer the material to a muffle furnace for calcination, with a heating rate of 5℃ / min, and a holding temperature and time of 400℃ and 4h respectively. The obtained material is CeO2.
[0032] S3. Preparation of CeO2@MnO2 series composite materials: The method is consistent with the preparation method of pure CeO2. The only difference is that MnO2 is first ultrasonically dispersed in deionized water.
[0033] S4. Add 100 mg of CeO2@MnO2 and 80 mg of sodium persulfate into 100 mL of 20 mg / L tetracycline solution in sequence; 95.18% of tetracycline can be removed after 180 min of reaction at 20°C.
[0034] Embodiment 2:
[0035] A method for preparing CeO2@MnO2 composite materials based on strong interaction between active components to promote pollutant adsorption catalysis and study on their activation of persulfate to degrade organic pollutants includes the following steps:
[0036] S1. Preparation of MnO2 nanorods: The hydrothermal method was used. Potassium permanganate and manganese acetate were first added to 32 mL of deionized water, and then 0.5 mL of nitric acid solution was added. After the reagents were fully dissolved, they were transferred to a hydrothermal reactor. The reactor was kept at 100°C for 24 hours and then naturally cooled to room temperature. The obtained material was washed and dried, and then placed in a muffle furnace. After being kept at 400°C for 4 hours, the nanorod MnO2 material was obtained.
[0037] Preparation of S2 and CeO2: Prepared by coprecipitation method, dissolve a certain amount of cerium nitrate in deionized water. After the cerium nitrate is completely dissolved, add ammonia water drop by drop until the pH value reaches 11, and then let it stand for 2 hours. After standing, wash the precipitate and then dry it. Then transfer the material to a muffle furnace for calcination, with a heating rate of 5℃ / min, and a holding temperature and time of 400℃ and 4h respectively. The obtained material is CeO2.
[0038] S3. Preparation of CeO2@MnO2 series composite materials: The method is consistent with the preparation method of pure CeO2. The only difference is that MnO2 is first ultrasonically dispersed in deionized water, and the obtained suspension is aged at 0℃ for 60min.
[0039] S4. 80 mg CeO2@MnO2 and 60 mg potassium persulfate were added to 100 mL of 20 mg / L tetracycline aqueous solution to degrade tetracycline in situ; the tetracycline was degraded at 25°C for 180 min to obtain an aqueous solution in which tetracycline was completely degraded. The removal rate was calculated to be 94.17%.
[0040] The aqueous solution contains anions such as chloride ions and nitrate ions.
[0041] Embodiment 3:
[0042] A method for preparing CeO2@MnO2 composite materials based on strong interaction between active components to promote pollutant adsorption catalysis and study on their activation of persulfate to degrade organic pollutants includes the following steps:
[0043] S1. Preparation of MnO2 nanorods: The hydrothermal method was used. Potassium permanganate and manganese acetate were first added to 32 mL of deionized water, and then 0.5 mL of nitric acid solution was added. After the reagents were fully dissolved, they were transferred to a hydrothermal reactor. The reactor was kept at 100°C for 24 hours and then naturally cooled to room temperature. The obtained material was washed and dried, and then placed in a muffle furnace. After being kept at 400°C for 4 hours, the nanorod MnO2 material was obtained.
[0044] Preparation of S2 and CeO2: Prepared by coprecipitation method, a certain amount of cerium nitrate is dissolved in deionized water. After the cerium nitrate is completely dissolved, add ammonia-ammonium carbonate buffer solution drop by drop until the pH value reaches 11, and then let it stand for 2 hours. After standing, wash the precipitate and then dry it. Then transfer the material to a muffle furnace for calcination, with a heating rate of 5℃ / min, and the insulation temperature and time are 400℃ and 4h respectively. The obtained material is CeO2.
[0045] Preparation of S3, CeO2@MnO2 series composite materials: The method is consistent with the preparation method of pure CeO2, with two differences. First, MnO2 is first ultrasonically dispersed in deionized water, and second, the Chen Hua temperature is 5°C and the Chen Hua standing time is 30 min.
[0046] S4. 100mg CeO2@MnO2 and 80mg sodium persulfate were added to 100mL of 20mg / L tetracycline in Zhanhe River water to degrade tetracycline in situ; degraded at 23℃ for 180min to obtain actual wastewater (Zhanhe River, Baiguishan Reservoir) with good degradation effects of tetracycline and Congo red. The removal rates were calculated to be 80.05% for tetracycline and 94.72% for Congo red.
[0047] In order to further study the effect of CeO2@MnO2 composite materials and persulfate on degrading organic pollutants, the following experiments were conducted.
[0048] 1. Degradation effect on tetracycline
[0049] The method of Example 1 was used as the test group, and the same method as in Example 1 was used as the control group 1 except that CeO2@MnO2 was not added and CeO2 was added. The other steps were the same as in Example 1 as the control group 1. The same method as in Example 1 was used as the control group 2 except that CeO2@MnO2 was not added and MnO2 was added. 2 mL of the suspension was taken at 1 min, 3 min, 5 min, 10 min, 20 min, and 30 min respectively, and its absorbance was tested on a spectrophotometer after filtering with a 0.45 um filter head. The removal rate was calculated after conversion. The results are as follows Figure 1 shown.
[0050] from Figure 1 It can be seen from the results that the degradation effects of single-component CeO2 and single-component MnO2 on tetracycline are lower than the degradation effect of CeO2@MnO2 material used in Example 1 of the present invention on tetracycline, indicating that CeO2@MnO2 can effectively improve the degradation effect of tetracycline. Figure 1It can be seen that when the reaction was carried out for 60 minutes, the concentration of tetracycline tended to be stable, indicating that the degradation was basically completed. It can be seen that CeO2@MnO2 can significantly shorten the degradation time and improve the degradation effect, indicating that the strong interaction between the components of the composite material can promote the deep catalytic oxidation of pollutants.
[0051] 2. Degradation effect on different organic pollutants
[0052] The method in Example 1 was used to degrade Congo red, tetracycline, and doxycycline, respectively. 2 mL of the suspension was taken at 1 min, 3 min, 5 min, 10 min, 20 min, and 30 min, respectively. After filtering through a 0.45 um filter head, the absorbance was tested on a spectrophotometer. The removal rate was calculated after conversion. The results are as follows: Figure 2 shown.
[0053] from Figure 2 The results show that CeO2@MnO2 composite materials have good catalytic activity for tetracycline, doxycycline and Congo red. After 60 minutes, the concentrations of Congo red, tetracycline and doxycycline all tend to be stable, indicating that the degradation process is basically completed. It can be seen that CeO2@MnO2 is widely used in the degradation of many common antibiotics and dyes.
[0054] 4. Effect of different pH values on the degradation of CeO2@MnO2
[0055] The method in Example 1 was used to measure the effect of tetracycline degradation at pH values of 3, 5, and 9, respectively. 2 mL of the suspension was taken at 1 min, 3 min, 5 min, 10 min, 20 min, and 30 min, respectively. After filtering with a 0.45 um filter head, the absorbance was tested on a spectrophotometer. The removal rate was calculated after conversion. Figure 3 shown.
[0056] from Figure 3 From the results, it can be seen that pH has a certain influence on the degradation effect, but the influence is small. Whether under acidic or alkaline conditions, CeO2@MnO2 can maintain good catalytic activity for the removal rate of tetracycline.
[0057] 5. Degradation effect of tetracycline in actual water
[0058] Exploring the removal of organic matter in actual wastewater is crucial for the practical application of catalytic materials. The situation in actual water bodies is relatively complex and there are many influencing factors. In order to explore the degradation effect of the CeO2@MnO2 material on tetracycline in actual water bodies, the method in Example 1 was adopted, and tap water, Zhanhe River water, Baigui Lake water, and tail water from the sewage treatment plant were selected as water sources. 2 mL of the suspension was taken at 1 min, 3 min, 5 min, 10 min, 20 min, and 30 min, respectively. After filtering with a 0.45 um filter head, its absorbance was tested on a spectrophotometer, and its removal rate was calculated after conversion. The results are as follows: Figure 4 shown.
[0059] from Figure 4 The results show that compared with deionized water, the removal rate of tetracycline by CeO2@MnO2 in actual wastewater is slightly lower, and its reduced activity may be related to the presence of anions, cations and pollutants in the actual water body. Although the degradation effect has decreased, after 180 minutes of reaction, CeO2@MnO2 can still maintain relatively good catalytic activity in various water media environments.
[0060] 6. Degradation effect of CeO2@MnO2 in dynamic experiment
[0061] In practical applications, the actual water body does not exist in a static form, but flows at a certain flow rate. In order to explore the degradation effect of the CeO2@MnO2 material in the dynamic experiment and intuitively display the purification efficiency of pollutants, 500mL of Congo red with a concentration of 20mg / L was placed in beaker 1. Another beaker was configured with a PMS solution with a concentration of 0.8g / L. Congo red and PMS were allowed to contact the catalytic material in a homemade reactor at a rate of 1.5mL / min. After 300 minutes of reaction, the material can degrade 98.62% of Congo red in water in the dynamic experiment, indicating that the material has good practical application value and application prospects.
[0062] 7. Comparison of the test results of CeO2@MnO2 degradation of tetracycline cycle:
[0063] The method in Example 1 was used to degrade tetracycline 1, 2, 3, 4, and 5 times, respectively. 2 mL of the suspension was taken at 1 min, 3 min, 5 min, 10 min, 20 min, and 30 min, respectively. After filtering with a 0.45 um filter head, the absorbance was tested on a spectrophotometer, and the removal rate was calculated after conversion. The results are as follows: Figure 5 shown.
[0064] from Figure 5 It can be seen from the results that after multiple degradations, the degradation effect of the CeO2@MnO2 material on tetracycline has not been significantly reduced, indicating that the material has good cyclic stability and can be reused.
[0065] 8. Morphology and structure analysis of CeO2@MnO2 series composite materials
[0066] Figure 6 The SEM results of CeO2@MnO2 composite materials show that the nucleation of Ce in an alkaline environment affects the morphology of MnO2 nanorods, indicating that there is an interaction between Ce and Mn in the composite material. Figure 7 The XRD results of the series of materials show that the alkaline environment and secondary calcination have a significant effect on the crystallinity of MnO2. Combined with the activity results, it can be seen that the strong interaction among the composite components is conducive to the adsorption of pollutants, while promoting electron transfer and the generation of active oxygen species, which is conducive to the in-situ degradation of adsorbed pollutants, achieving in-situ coordinated adsorption and catalysis of pollutants.
[0067] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing a CeO2@MnO2 composite material, characterized in that: The following steps are involved: S1. Preparation of MnO2 nanorods: Preparation of MnO2 nanorods by hydrothermal method; S2. Preparation of CeO2: Preparation of CeO2 by coprecipitation method; S3, preparing CeO2@MnO2 series composite materials: preparing CeO2@MnO2 composite materials by a deposition method; S4, preparing a mixture: mixing the CeO2@MnO2 composite material with persulfate; S5. Degradation of organic pollutants: The mixture is dispersed in a water body containing organic pollutants to be treated for degradation to obtain degraded water.
2. The method for preparing a CeO2@MnO2 composite material according to claim 1, characterized in that: The mass ratio of CeO2 to MnO2 in the CeO2@MnO2 composite material in S3 is 0.1-4; The mass ratio of CeO2@MnO2 to persulfate in S4 is 0.1-5; The dosage of the mixture in S5 is 0.06-2.5 g / L.
3. The method for preparing a CeO2@MnO2 composite material according to claim 1, characterized in that: The material preparation process requires a calcination temperature of 400-600° C., a calcination time of 2-6 hours, and a calcination heating rate of 5° C. / min.
4. The method for preparing a CeO2@MnO2 composite material according to claim 1, characterized in that: The alkaline precipitant includes ammonia water, potassium hydroxide, saturated aqueous solution of ammonium carbonate, ammonia water-ammonium carbonate buffer solution, potassium hydroxide-ammonium carbonate buffer solution.
5. The method for preparing a CeO2@MnO2 composite material according to claim 1, characterized in that: The cerium has a significant influence on the morphology and structure of the MnO2 nanorods and the chemical environment of manganese during the nucleation process in an alkaline environment.
6. The method for preparing a CeO2@MnO2 composite material according to claim 5, characterized in that: The cerium nucleation temperature ranges from -5 to 60°C, and the nucleation precipitation time ranges from 5 to 120 minutes.
7. The method for preparing a CeO2@MnO2 composite material according to claim 1, characterized in that: The CeO2@MnO2 composite material and persulfate degrade organic pollutants, and the particle size of the CeO2@MnO2 composite material is 100-400 meshes.
8. The method for preparing a CeO2@MnO2 composite material according to claim 7, characterized in that: The persulfate is any one of potassium persulfate, sodium persulfate and potassium hydrogen persulfate. The temperature of the reaction of the CeO2@MnO2 composite material and the persulfate for degrading organic pollutants is 10 to 30° C., and the degradation time is 60 to 180 minutes.
9. The method for preparing a CeO2@MnO2 composite material according to claim 7, characterized in that: The pH value of the mixture of the CeO2@MnO2 composite material and the persulfate for degrading organic pollutants is 3-9 after being dispersed in the water body containing organic pollutants to be treated.
10. The method for preparing a CeO2@MnO2 composite material according to claim 7, characterized in that: The organic pollutants degraded by the CeO2@MnO2 composite material and persulfate are any one or more of Congo red, tetracycline and doxycycline.
Citation Information
Cited By
Water body purification material and preparation method thereof
CN119680532A
A water purification material and its preparation method
CN119680532B