Analysis method for packaging substrate after reliability test
After the reliability test of the package substrate, the method of determining the failure area, light transmission observation, slice and micromorphic observation is solved, and the problem of low success rate of bHAST failure analysis in the prior art is achieved, and a higher success rate and faster analysis aging is achieved.
Patent Information
- Application Number
- CN202510183844.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-02-18
- Publication Date
- 2025-06-10
AI Technical Summary
In the prior art, the success rate of bHAST failure analysis is too low to meet the testing needs when mass production of packaged substrates.
By determining the failure area of the sample, light-transmitting observation is performed to determine the ion migration position, sectioning is obtained, and micromorphic observation is performed on the cross-sectional area to determine the cause of failure.
It effectively improves the success rate of bHAST failure analysis, simplifies the analysis steps, shortens the analysis timeliness, and meets the needs of factory operations.
Smart Images

Figure CN120121614A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing, and particularly to an analysis method after reliability testing of a packaging substrate. Background Art
[0002] With the progress of technology and the development of the electronics industry, the technology of packaging substrates (Substrate, abbreviated as SUB) is also constantly improving, and the performance requirements for packaging substrates are gradually increasing. Among them, the reliability of the packaging substrate is one of the key factors to ensure its stable operation. In the prior art, the methods for reliability testing of packaging substrates include but are not limited to H3TRB (High Temperature and High Humidity Reverse Bias), bHAST (Bias Highly Accelerated Stress Test), TCT (Temperature Cycling Test), etc.
[0003] Among them, bHAST is an important means to evaluate packaging substrates. If bHAST fails, the true cause of failure analyzed at this time can be used to guide process improvement to improve the qualification rate and reliability of the final product. In the prior art, the success rate of failure analysis for a single sample is about twenty percent. Such a success rate cannot meet the test requirements when mass-producing packaging substrates. Summary of the Invention
[0004] An embodiment of the present invention provides an analysis method after reliability testing of a packaging substrate to solve the problem of too low success rate of bHAST failure analysis in the prior art.
[0005] In a first aspect of the present invention, an analysis method after reliability testing of a packaging substrate is provided, including: Determine the failure area of the sample; Perform light transmission observation on the failure area to determine the ion migration position in the failure area; Slice the sample to obtain the cross-sectional area of the ion migration position; Perform microscopic morphology observation on the cross-sectional area to determine the failure cause of the sample.
[0006] In a possible design, after performing microscopic morphology observation on the cross-sectional area to determine the failure cause of the sample, the method further includes: Perform elemental analysis on the failure area to determine whether there are abnormal elements in the failure area.
[0007] In a possible design, after slicing the sample to obtain the cross-sectional area of the ion migration position, the method further includes: Analyzing the cross-sectional area to obtain the cross-sectional state of the ion migration position.
[0008] In a possible design, determining the failure area of the sample includes: Performing thermal imaging analysis on the sample to determine the failure area of the sample.
[0009] In a possible design, after determining the failure area of the sample and before observing the failure area through light transmission to determine the ion migration position of the failure area, the method further includes: Observing the appearance of the sample to obtain the abnormal area on the surface of the sample.
[0010] In a possible design, after observing the appearance of the sample to obtain the abnormal area on the surface of the sample and before observing the failure area through light transmission to determine the ion migration position of the failure area, the method further includes: Performing planar grinding on the sample to gradually confirm the failure morphology of the sample.
[0011] In a possible design, before performing thermal imaging analysis on the sample to determine the failure area of the sample, the method further includes: Placing the sample into a high-accelerated stress test (bHAST) chamber; Performing electrical testing on the sample located in the bHAST chamber; Taking out the sample from the bHAST chamber.
[0012] In a possible design, observing the failure area through light transmission to determine the ion migration position of the failure area includes: Observing the ion migration dendrite morphology connecting the positive and negative electrodes with the inner layer length of the sample; Determining the ion migration position of the failure area through the ion migration dendrite morphology.
[0013] In a possible design, observing the ion migration dendrite morphology connecting the positive and negative electrodes with the inner layer length of the sample includes: Observing the ion migration dendrite morphology with a width of 2 to 3 microns in the inner layer of the sample and connecting the positive and negative ions.
[0014] In a possible design, observing the ion migration dendrite morphology connecting the positive and negative electrodes with the inner layer length of the sample includes: The sample is inspected with green light using a 3D microscope to determine the morphology of the ion migration dendrites connecting the positive and negative electrodes at the inner layer length of the sample.
[0015] For the analysis method after the reliability test of the above-mentioned packaging substrate, after the failure area of the sample is determined in the present invention, by observing the light transmission of the failure area, the ion migration position in the failure area is determined. Then, the sample is sliced to obtain the cross-sectional area of the ion migration position. Finally, the micro-morphology of the cross-sectional area is observed to determine the failure cause of the sample. Compared with the resolution of observing the internal state of the sample by X-ray diffraction after determining the failure area in the prior art, by observing the light transmission of the failure area in the present invention to identify the ion migration state, not only can more accurate results be observed, but also the ability of slicing, positioning and grinding in subsequent steps can be improved, thereby effectively improving the success rate of bHAST failure analysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for the description of the embodiments of the present invention will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For those of ordinary skill in the art, without creative efforts, other drawings can be obtained based on these drawings.
[0017] Figure 1 It is a flowchart of a reliability test method for a packaging substrate in an embodiment of the present invention. DETAILED DESCRIPTION OF THE EMBODIMENTS
[0018] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the drawings in the embodiments of the present invention. Obviously, the described embodiments are some, but not all, of the embodiments of the present invention. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present invention without creative efforts fall within the protection scope of the present invention.
[0019] As a core material for chip packaging, the reliability of the packaging substrate is a key factor for its long-term stable operation. Therefore, comprehensive reliability testing and evaluation of the packaging substrate are indispensable technical points. In the prior art, testing techniques such as bHAST are usually used to evaluate the stability and reliability of the performance of the packaging substrate. bHAST refers to high-accelerated stress testing under temperature and humidity bias. It subjects the packaging substrate samples to high temperature and high humidity conditions while also under bias voltage, with the aim of accelerating the corrosion of the samples. Then, the samples are taken out of the bHAST test chamber for failure analysis. This failure analysis can identify the true cause of the failure of the samples, and then improve the production process based on the true cause of the failure, thereby further improving its production process. Thus, it can be seen the importance of bHAST failure analysis for the packaging substrate process.
[0020] A chip is a very complex system, and the defects and failure causes generated during its packaging process are also very complex. Therefore, when analyzing packaging failures, it is necessary to analyze the possible failure causes step by step from multiple perspectives. To address the above problems, the present invention optimizes the original step sequence and content of bHAST failure analysis in the prior art to improve the overall analysis efficiency and accuracy, so as to meet the operation requirements of the factory. The optimization result is the reliability testing method for the packaging substrate provided by the present invention, as Figure 1 shown, which specifically includes the following steps: S10: Determine the failure area of the sample.
[0021] Among them, the failure area includes but is not limited to performance failure area, device failure area, packaging defect area, etc. Exemplarily, in this embodiment, the failure criterion for the sample can be that the insulation resistance value is less than .
[0022] It should be noted that in this embodiment, the failure area of the sample is preferentially locked. Compared with the prior art where the sample is first subjected to electrical testing (electricity refers to the positive or negative charge carried by the charge), and then the failure area of the sample is locked. This embodiment essentially optimizes the step of electrical testing. Therefore, without waiting for the sample to return to normal temperature and pressure, the ion migration position of the failure area can be directly determined through the subsequent step S20. This simplifies the overall failure analysis steps, thereby improving the efficiency of failure analysis.
[0023] S20: Conduct a light-transmitting observation on the failure area to determine the ion migration position of the failure area.
[0024] Among them, ion migration refers to the state where metals on the circuit board such as copper, silver, tin, etc. are ionized under certain conditions and migrate through the insulating layer to the other pole under the action of an electric field, resulting in a decrease in insulation performance.
[0025] It should be noted that in this embodiment, the electrical testing and X-ray diffraction in the existing failure analysis are substantially optimized. Instead, the ion migration state of the sample is determined through light transmission analysis. This simplifies the steps of the entire failure analysis and further improves the efficiency of failure analysis.
[0026] S30: Slice the sample to obtain the cross-sectional area of the ion migration position.
[0027] It should be noted that in the existing failure analysis steps, X-ray diffraction judges the internal state of the sample by analyzing the diffraction pattern inside the sample. In this embodiment, step S20 obtains the ion migration state of the sample in the failure area, and step S30 performs slicing analysis to further observe the cross-sectional area of the ion migration state position. Compared with the existing X-ray diffraction observation method, the method of S20-S30 in this embodiment is more accurate and detailed, effectively improving the accuracy and success rate of failure analysis.
[0028] S40: Observe the microtopography of the cross-sectional area to determine the failure cause of the sample.
[0029] Among them, the microtopography observation is to perform high-magnification observation on the surface, fracture or cross-section of the sample through an optical microscope or a scanning electron microscope.
[0030] It should be noted that compared with the resolution of observing the internal state of the sample through X-ray diffraction after determining the failure area in the prior art, the present invention identifies the ion migration state through light transmission observation of the failure area, which can not only observe more accurate results, but also improve the ability of slicing, positioning and grinding in subsequent steps, thus effectively improving the success rate of bHAST failure analysis.
[0031] In one embodiment, as Figure 1 shown, after step S40, that is, after observing the microtopography of the cross-sectional area to determine the failure cause of the sample, the method further includes the following steps: S41: Perform elemental analysis on the failure area to determine whether there are abnormal elements in the failure area.
[0032] Among them, elemental analysis (EA, full name: Elemental analysis) is a chemical step or a series of steps to determine the elemental composition of a sample. Elemental analysis can be qualitative analysis or quantitative analysis, which is not limited here. Elemental analysis includes but is not limited to combustion method, mass spectrometry, gravimetric analysis, electromagnetic spectrum method, etc. Abnormal elements include but are not limited to elements caused by external or internal environmental pollution.
[0033] It should be noted that the abnormal elements for determining the failure region can further accurately judge the cause of sample failure, so as to improve the success rate of failure analysis.
[0034] In one embodiment, after step S30, that is, after slicing the sample to obtain the cross-sectional area of the ion migration position, the method further includes the following steps: S31: Analyze the cross-sectional area to obtain the cross-sectional state of the ion migration position.
[0035] Among them, the cross-sectional state refers to the ion migration state on the cross-section of the sliced failure region.
[0036] It should be noted that analyzing the cross-sectional area after slicing can more accurately comprehensively analyze the ion migration state of the failure region, so as to improve the accuracy and success rate of failure analysis.
[0037] In one embodiment, in step S10, that is, when determining the failure region of the sample, it specifically includes the following steps: S11: Perform thermal imaging analysis on the sample to determine the failure region of the sample.
[0038] Among them, thermal imaging, that is, long-wave infrared imaging, is used to record the self-infrared radiation of an object when it is heated, and can transform the thermal image of the scene radiation into a visible two-dimensional image.
[0039] It should be noted that performing thermal imaging analysis on the sample to determine its failure region. In the original failure analysis, this step was the third step to be executed. In this embodiment, step S11 is essentially the first step to be executed. This is because in the original steps, the electrical test of the sample needs to be performed at room temperature, so it takes a certain amount of time to adjust the state of the sample to room temperature and normal pressure. After the appearance and electrical tests of the sample, thermal imaging analysis can be performed on the sample. And this embodiment simplifies the electrical test, so there is no need to wait for the sample to return to room temperature before performing thermal imaging analysis on it. This effectively improves the speed of sample analysis, thereby further improving the timeliness of failure analysis.
[0040] In one embodiment, after step S10, that is, after determining the failure region of the sample and before observing the ion migration position of the failure region through light transmission, the method further includes the following steps: S50: Observe the appearance of the sample to obtain the abnormal region on the surface of the sample.
[0041] Among them, by way of example, the abnormal region includes but is not limited to the substrate contamination region, the chip bonding and curing region, etc.
[0042] It should be noted that by observing the abnormal area on the surface of the sample, the cause of the sample abnormality can be more accurately comprehensively analyzed, so as to improve the accuracy and success rate of failure analysis.
[0043] In one embodiment, in step S50, that is, after observing the appearance of the sample and obtaining the abnormal area on the surface of the sample, before performing a light transmission observation on the failure area to determine the ion migration position of the failure area, the method further includes the following steps: S51: Perform planar grinding on the sample and layer by layer confirm the failure morphology of the sample.
[0044] Among them, the failure morphology includes but is not limited to collision failure morphology, board bending failure morphology, and failure morphology with unclear board-level stress, etc.
[0045] It should be noted that the planar grinding step in this embodiment is substantially before the light transmission observation step of step S20. Therefore, in this embodiment, it is preferably to perform a light transmission observation on the area where no sample failure morphology is observed after planar grinding, rather than performing a light transmission observation on the entire sample. This can further improve the speed of failure analysis, thereby improving the timeliness of failure analysis.
[0046] In one embodiment, before step S11, that is, before performing thermal imaging analysis on the sample to determine the failure area of the sample, the method further includes the following steps: S61: Place the sample in a highly accelerated stress test bHAST test chamber.
[0047] S62: Perform an electrical test on the sample located in the bHAST test chamber.
[0048] S63: Take out the sample from the bHAST test chamber.
[0049] Among them, the bHAST test chamber refers to a test chamber that allows the packaged substrate to withstand conditions such as high temperature, high humidity, and bias voltage, and its purpose is to accelerate the corrosion of the packaged substrate. This test chamber can adjust the environment such as temperature and pressure.
[0050] It should be noted that this embodiment essentially occurs before failure analysis, that is, before the failed sample is taken out of the bHAST test chamber. This step essentially places the electrical test in step 2 of the existing failure analysis into the bHAST test chamber. Since the electrical test needs to be carried out at room temperature, and the existing failure analysis is carried out after the package substrate is taken out of the test chamber, it takes a long time for the package substrate to return to room temperature and normal pressure. In this embodiment, the electrical test is placed in the bHAST test chamber, and the test chamber can quickly restore the temperature and pressure from the high-temperature bias in the experiment to room temperature and normal pressure. Therefore, this embodiment essentially does not need to wait for a long time and can complete the electrical test more quickly.
[0051] In addition, since the electrical test that originally needed to be carried out at room temperature is adjusted to be carried out in the bHAST test chamber, after the sample is taken out of the bHAST test chamber, the next test can be directly carried out, saving a large amount of waiting time in the middle, thus effectively improving the efficiency of failure analysis.
[0052] In one embodiment, in step S20, that is, observing the failed area through light transmission to determine the ion migration position of the failed area, specifically includes the following steps: S21: Observe the morphology of the ion migration dendrites connecting the positive and negative electrodes in the inner layer length of the sample.
[0053] S22: Determine the ion migration position of the failed area through the morphology of the ion migration dendrites.
[0054] Among them, dendrites are crystals that develop in the form of electrically branched trees.
[0055] It should be noted that steps S21 - S22 determine a more accurate ion migration position by observing the morphology of the ion migration dendrites connecting the positive and negative electrodes in the inner layer length of the sample, improving the subsequent slice positioning and grinding ability, and further effectively improving the success rate of bHAST analysis.
[0056] In one embodiment, in step S21, that is, observing the morphology of the ion migration dendrites connecting the positive and negative electrodes in the inner layer length of the sample, specifically includes the following steps: S211: Observe the morphology of the ion migration dendrites with a width of 2 to 3 microns in the inner layer of the sample and connecting positive and negative ions.
[0057] It should be noted that accurately observing the morphology of the ion migration dendrites with a width of 2 - 3 microns in the inner layer of the sample can further accurately determine the ion migration position, further improve the slice positioning and grinding ability, and more effectively improve the success rate of bHAST analysis.
[0058] In one embodiment, in step S21, that is, observing the morphology of the ion migration dendrites connecting the positive and negative electrodes of the inner layer of the sample, specifically includes the following steps: S212: Use a microscope to perform a green light inspection on the sample to determine the morphology of the ion migration dendrites connecting the positive and negative electrodes of the inner layer of the sample. The microscope includes but is not limited to a polarized light microscope, an inverted microscope, etc. In this embodiment, it is preferably to perform a green light inspection on the sample through a 3D microscope.
[0059] It should be noted that performing a green light inspection on the sample through a microscope can more accurately obtain the morphology of the ion migration dendrites, thereby more accurately obtaining the ion migration position, and further improving the slicing and positioning grinding ability, so as to better improve the success rate of bHAST analysis.
[0060] It can be seen that in the embodiment provided by the present invention, after determining the failure area of the sample, by observing the light transmission of the failure area, the ion migration position of the failure area is determined. Then, the sample is sliced to obtain the cross-sectional area of the ion migration position. Finally, the microscopic morphology of the cross-sectional area is observed to determine the failure cause of the sample. Compared with the resolution of observing the internal state of the sample through X-ray diffraction after determining the failure area in the prior art, the present invention observes the ion migration state through the light transmission observation of the failure area, which can not only observe more accurate results, but also improve the slicing and positioning grinding ability in the subsequent steps, thus effectively improving the success rate of bHAST failure analysis. In one embodiment, an analysis method after reliability testing of a packaging substrate is provided, including the following 7 steps, and the comparison with the 8 steps before optimization is shown in the following table: It can be seen that in the embodiment of the present invention, the analysis method is optimized to seven steps, and by reasonably using the bHAST test chamber, the analysis time is shortened by nearly 60%. Then, through planar grinding, light transmission observation, and slicing analysis, the success rate of bHAST failure analysis is further increased to 70%. Therefore, compared with the prior art, the present invention shortens the analysis time from 7.5 hours per sample to 3 hours per sample, and the analysis success rate is increased from the existing 20% to 90%, greatly improving the efficiency and success rate of failure analysis, meeting the needs of factory operation, and enabling the results of failure analysis to more effectively promote the improvement of product manufacturing processes.
[0061] It should be understood that the magnitudes of the sequence numbers of the steps in the above embodiments do not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation to the implementation process of the embodiments of the present invention.
[0062] Those skilled in the art can clearly understand that, for the convenience and conciseness of description, only the above division of each functional unit and module is used as an example. In actual applications, the above functions can be allocated to different functional units and modules according to needs, that is, the internal structure of the device can be divided into different functional units or modules to complete all or part of the functions described above.
[0063] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it; although the present invention has been described in detail with reference to the foregoing embodiments, those of ordinary skill in the art should understand that they can still modify the technical solutions recorded in the foregoing embodiments, or perform equivalent replacements on some of the technical features; and these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be included in the protection scope of the present invention.
Claims
1. A method for analyzing a package substrate after reliability testing, characterized in that: include: Determine the failure area of the sample; Observe the failure area through light transmission to determine the ion migration position of the failure area; Slicing the sample to obtain a cross-sectional area of the ion migration position; The cross-sectional area is subjected to microscopic morphological observation to determine the failure cause of the sample.
2. The analysis method after reliability testing according to claim 1, characterized in that: After observing the microscopic morphology of the cross-sectional area and determining the failure cause of the sample, the method further comprises: An element analysis is performed on the failure region to determine whether abnormal elements exist in the failure region.
3. The analysis method after reliability testing according to claim 1, characterized in that: After slicing the sample to obtain the cross-sectional area of the ion migration position, the method further includes: The cross-sectional area is analyzed to obtain the cross-sectional state of the ion migration position.
4. The analysis method after reliability testing according to claim 1, characterized in that: Determining the failure area of the sample includes: Perform thermal imaging analysis on the sample to determine the failure area of the sample.
5. The analysis method after reliability testing according to claim 1, characterized in that: After determining the failure area of the sample, observing the failure area through light, and before determining the ion migration position of the failure area, the method further includes: The appearance of the sample is observed to identify abnormal areas on the surface of the sample.
6. The analysis method after reliability testing according to claim 5, characterized in that: After observing the appearance of the sample and obtaining the abnormal area on the surface of the sample, and before observing the failure area through light and determining the ion migration position of the failure area, the method further includes: The sample is plane-ground to confirm the failure morphology of the sample layer by layer.
7. The analysis method after reliability testing according to claim 4, characterized in that: Before performing thermal imaging analysis on the sample to determine the failure area of the sample, the method further includes: The sample is placed in a highly accelerated stress test (bHAST) test box; Conducting electrical testing on the sample in the bHAST test chamber; The sample was removed from the bHAST test chamber.
8. The analysis method after reliability testing according to any one of claims 1 to 7, characterized in that: The step of observing the failure area through light to determine the ion migration position of the failure area includes: The ion migration dendrite morphology of the inner layer of the sample connecting the positive and negative electrodes was observed; The ion migration position of the failure area is determined by the ion migration dendrite morphology.
9. The analysis method after reliability testing according to claim 8, characterized in that: The observing of the ion migration dendrite morphology of the inner layer of the sample connecting the positive and negative electrodes includes: The sample observed had an inner layer with a width of 2 to 3 microns and an ion migration dendrite morphology with a length connecting positive and negative ions.
10. The analysis method after reliability testing according to claim 8, characterized in that: The ion migration dendrite morphology of the inner layer of the sample at the observation point connecting the positive and negative electrodes includes: The sample was inspected under green light using a 3D microscope to determine the morphology of ion migration dendrites connecting the positive and negative electrodes in the inner layer of the sample.