Self-repairing anticorrosive paint and preparation method thereof

By using 2-mercaptobenzimidazole intercalated magnesium-aluminum hydrotalcite and 8-hydroxyquinoline intercalated montmorillonite as fillers in self-healing anticorrosion coatings, and optimizing the proportions with epoxy resin, the controlled release of corrosion inhibitors and the ionic stimulation response of the coating is achieved, which solves the problems of short anticorrosion cycle and high repair cost, and improves the anticorrosion performance and service life of the coating.

CN120505021APending Publication Date: 2025-08-19JIANGSU YEJIAN ZINC IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510792888.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-13
Publication Date
2025-08-19

AI Technical Summary

Technical Problem

The release of corrosion inhibitors in existing self-repair anticorrosion coatings is uncontrolled, resulting in a short anti-corrosion cycle of the coating and cannot be repaired multiple times. Traditional repair measures consume manpower and material resources and have high economic costs.

Method used

2-mercaptobenzimidazole intercalated magnesium-aluminum hydrotalcite and 8-hydroxyquinoline intercalated montmorillonium were used as fillers, and the release of corrosion inhibitors was controlled using its ion stimulation response characteristics, and combined with the optimized ratio of bisphenol A-type epoxy resin and fillers, self-healing anticorrosion coatings were prepared.

Benefits of technology

It improves the corrosion cycle and protective performance of the coating, extends the service life, reduces the repair cost, and enhances the density and water resistance of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005448924380000101
    Figure BDA0005448924380000101
  • Figure BDA0005448924380000102
    Figure BDA0005448924380000102
Patent Text Reader

Abstract

The invention relates to the field of anticorrosive coatings, and particularly discloses a self-repairing anticorrosive coating and a preparation method thereof. The self-repairing anticorrosive coating comprises the following raw materials: 100 parts of bisphenol A epoxy resin, 35-40 parts of butyl acetate, 1-5 parts of a filler, 45-55 parts of a polyamide curing agent, 1-2 parts of a wetting dispersant and 2-5 parts of an auxiliary agent, wherein the filler comprises 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite and 8-hydroxyquinoline intercalated montmorillonite in a weight ratio of (0.5-2.0): 1. The 2-mercaptobenzimidazole intercalated magnesium-aluminum hydrotalcite and the 8-hydroxyquinoline intercalated montmorillonite are added into the anticorrosive coating, the anticorrosive coating with better corrosion resistance is prepared by utilizing the synergistic effect of the 2-mercaptobenzimidazole intercalated magnesium-aluminum hydrotalcite and the 8-hydroxyquinoline intercalated montmorillonite, and the anticorrosive coating also has ion stimulation response self-repairing performance, so that release of a corrosion inhibitor in the coating is effectively controlled, and the service life of the coating is prolonged. The anti-corrosion period and the protection performance of the coating are improved, and the service life of the anti-corrosion coating is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of anti-corrosion coatings, and more specifically, to a self-repairing anti-corrosion coating and a preparation method thereof. Background Art

[0002] With the development of various industries, the use of metal materials has increased, and the resulting corrosion problems have become increasingly serious. To extend the service life of materials, people have adopted a variety of protective measures, mainly including cathodic protection and anti-corrosion coatings. Among them, anti-corrosion coatings are one of the most common and effective measures used in corrosion protection. Their protective mechanism is to provide a barrier to isolate metal materials from corrosive environments and corrosive media. Currently, a large amount of research is aimed at developing stronger and more durable corrosion-resistant coatings, and improving the corrosion resistance of coatings by adding functional fillers.

[0003] However, during the practical application of anti-corrosion coatings, cracks inevitably develop due to environmental and stress-induced damage, severely compromising the coating's barrier properties. Damage primarily includes localized scratches or delamination, stress-related macroscopic cracks, and environmental factors (including UV rays, heat, oxygen, moisture, and ions). These are the primary causes of macroscopic degradation of the coating's protective and aesthetic properties. If not promptly and effectively repaired, these damages create pathways for the rapid ingress of corrosive media, ultimately leading to premature failure and a gradual loss of protective capabilities, significantly shortening the coating's lifespan. Furthermore, these coating damages often present several repair challenges. First, internal coating damage, including bubbles, microcracks, and delamination generated during the curing process, is difficult to detect macroscopically, requiring specialized equipment for inspection. If undetected, it can lead to localized corrosion and severely shorten the material's service life. Second, macroscopic damage caused by stress-induced damage typically requires manual repair or coating replacement. These two are currently the most prevalent forms of damage, and their repair often incurs significant financial costs and consumes significant human and material resources. To mitigate the economic losses caused by coating damage and improve the coating's corrosion protection lifespan and performance, researchers have introduced the concept of self-healing into coatings, resulting in the development of self-healing coatings. These coatings effectively utilize their inherent functional properties and changes in material properties caused by environmental stimuli to restore or even enhance the coating's corrosion resistance with minimal human intervention.

[0004] Existing self-healing anti-corrosion coatings generally fall into two categories, depending on their self-healing mechanisms: externally added corrosion inhibitors or repair agents, which are released when the coating is damaged to protect the damaged area and achieve self-healing. However, the corrosion inhibitors or repair agents loaded into the micro / nano containers are released even when the coating is intact, significantly reducing the lifespan of the self-healing coating. Furthermore, due to the limited amount of corrosion inhibitors, these self-healing coatings cannot complete multiple repairs. Summary of the Invention

[0005] In order to solve the above technical problems, the present application provides a self-repairing anti-corrosion coating and a preparation method thereof.

[0006] In the first aspect, the present application provides a self-repairing anti-corrosion coating, which adopts the following technical solution: A self-repairing anti-corrosion coating, the raw materials used include the following components in parts by weight: 100 parts of bisphenol A epoxy resin; 35-40 parts of butyl acetate; 1-5 parts of filler; 45-55 parts of polyamide curing agent; 1-2 parts of wetting and dispersing agent; 2-5 parts of additives; The filler comprises 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite and 8-hydroxyquinoline intercalated montmorillonite in a weight ratio of (0.5-2.0):1.

[0007] By adopting the above-mentioned technical scheme, the 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite of the present application has ion stimulation response characteristics, and the anions in the environment can cause the 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite to undergo ion exchange, thereby promoting the release of the interlayer corrosion inhibitor 2-mercaptobenzimidazole, and the release amount of 2-mercaptobenzimidazole increases with the increase of anion concentration. Adding it to the anti-corrosion coating can not only make the cured anti-corrosion coating have better corrosion resistance, but also make the coating have ion stimulation response self-repairing properties, effectively control the release of the corrosion inhibitor in the coating, improve the anti-corrosion cycle and protective performance of the coating, and extend the service life of the anti-corrosion coating.

[0008] In addition, the 8-hydroxyquinoline intercalated montmorillonite of the present application uses montmorillonite as a carrier and 8-hydroxyquinoline as a corrosion inhibitor, which can play a synergistic role with 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite in the anti-corrosion coating, further hindering the penetration of the anti-corrosion medium and effectively promoting the improvement of the anti-corrosion performance of the self-repairing anti-corrosion coating.

[0009] At the same time, the present invention controls the ratio of bisphenol A epoxy resin to filler, allowing the filler to fully enhance the anticorrosive performance of the anticorrosive coating. If the filler dosage is too low, the anticorrosive performance of the coating will only be slightly improved; if the filler dosage is too high, the filler will not be fully dispersed in the anticorrosive coating, resulting in agglomeration in the cured anticorrosive coating, which may lead to premature failure of the anticorrosive coating.

[0010] Preferably, the weight ratio of the bisphenol A epoxy resin to the filler is 100:(2.5-3.5).

[0011] By adopting the above-mentioned technical solution, the present application further optimizes the ratio between bisphenol A epoxy resin and filler, thereby further improving the effect of the filler on improving the anti-corrosion performance of the coating, reducing the possibility of filler agglomeration in the anti-corrosion coating, and further improving the anti-corrosion performance of the anti-corrosion coating, thereby extending the service life of the anti-corrosion coating.

[0012] Preferably, the filler comprises 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite and 8-hydroxyquinoline intercalated montmorillonite in a weight ratio of (1.5-2.0):1.

[0013] By adopting the above technical solution, the present application further optimizes the ratio between 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite and 8-hydroxyquinoline intercalated montmorillonite, thereby further improving the density of the anti-corrosion coating, further enhancing the barrier effect on the anti-corrosion medium, thereby improving the water resistance of the coating and extending the service life of the coating.

[0014] Preferably, the 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite is prepared by the following method: a. calcining the carbonate-intercalated magnesium-aluminum hydrotalcite under the protection of an inert gas and cooling it to room temperature to obtain a bimetallic oxide; b. Under the protection of an inert gas, stirring the 2-mercaptobenzimidazole anion solution and the bimetallic oxide at a temperature of 55-65° C. for 24-26 hours, wherein the molar ratio of 2-mercaptobenzimidazole to the bimetallic oxide is (2.5-3.5):1; c. Centrifuge the product obtained in step b at a rotation speed of 5500-6500 rpm for 3-5 min, then wash, dry and grind the precipitate to obtain 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite.

[0015] Preferably, the calcination temperature is 450-550° C. and the calcination time is 3-5 hours.

[0016] Preferably, the preparation process of the 2-mercaptobenzimidazole anion solution is specifically as follows: 2-mercaptobenzimidazole is added to boiling deionized water to obtain a solution with a concentration of 0.08-0.12 mol / L, and then NaOH equivalent to 2-mercaptobenzimidazole is added to anionize it, and the pH value of the system is adjusted to 11 to obtain a 2-mercaptobenzimidazole anion solution.

[0017] By adopting the above technical solution, the present application first calcines the carbonate-intercalated magnesium-aluminum hydrotalcite under the protection of an inert gas to obtain a bimetallic oxide, which facilitates the subsequent insertion of 2-mercaptobenzimidazole anions. Then, under certain temperature and molar ratio conditions, the 2-mercaptobenzimidazole anion solution is stirred with the bimetallic oxide, so that the 2-mercaptobenzimidazole anions can be effectively inserted into the magnesium-aluminum hydrotalcite. Finally, through centrifugation at a certain speed, washing, drying and grinding, a high-quality 2-mercaptobenzimidazole-intercalated magnesium-aluminum hydrotalcite can be obtained.

[0018] Preferably, the 8-hydroxyquinoline intercalated montmorillonite is prepared by the following method: The montmorillonite is dissolved in a solvent, and 8-hydroxyquinoline is added and mixed evenly, wherein the weight ratio of 8-hydroxyquinoline to montmorillonite is 1:(9-10), and then vacuum is applied and maintained for 4-5 hours, and then washed, centrifuged, cleaned, and dried to obtain 8-hydroxyquinoline intercalated montmorillonite.

[0019] Preferably, the montmorillonite is modified by the following method: Montmorillonite is dispersed in deionized water and magnetically stirred for 24-26 hours to obtain solution A, octadecylamine and hydrochloric acid are magnetically stirred for 30-35 minutes to obtain solution B with a pH value of 3-4, solution A and solution B are mixed and reacted at a temperature of 75-85°C for 22-26 hours, wherein the weight ratio of montmorillonite to octadecylamine is 1:(0.25-0.35), and then centrifuged and filtered until the filtrate is tested with a 0.1 mol / L AgNO3 solution without white precipitate, and then dried and ground to obtain modified montmorillonite.

[0020] By adopting the above technical solution, the present invention uses octadecylamine to modify montmorillonite, and the head NH3 + It enters the interlayer of montmorillonite through ion exchange, and the subsequent alkyl chain also enters the same interlayer, expanding the layered structure and increasing the interlayer spacing, which is conducive to the subsequent corrosion inhibitor 8-hydroxyquinoline entering the interlayer of montmorillonite. The organic amine between the layers is conducive to its compatibility with organic phases such as bisphenol A epoxy resin, thereby further improving the effect of 8-hydroxyquinoline intercalated montmorillonite on the anti-corrosion coating, and further improving the anti-corrosion performance of the anti-corrosion coating.

[0021] In a second aspect, the present application provides a method for preparing a self-repairing anti-corrosion coating, which adopts the following technical solution: A method for preparing a self-repairing anti-corrosion coating comprises the following steps: S1, mixing 100 parts by weight of bisphenol A epoxy resin and 30-33 parts by weight of butyl acetate to obtain a bisphenol A epoxy resin dilution; S2, mixing 1-5 parts by weight of filler, 5-7 parts by weight of butyl acetate and 1-2 parts by weight of a wetting and dispersing agent and ultrasonically dispersing for 5-10 minutes; S3. Mix the bisphenol A epoxy resin dilution and the product obtained in step S2, add 45-55 parts by weight of a polyamide curing agent, and continue stirring until the system is uniform and transparent. Add 2-5 parts by weight of an auxiliary agent and mix evenly to obtain a self-repairing anti-corrosion coating.

[0022] Through the above technical solution, the preparation method of the present application has simple steps, is easy to operate, and the raw materials used are easily available, which is suitable for large-scale industrial production.

[0023] In summary, this application has the following beneficial technical effects: 1. The anti-corrosion coating of the present application incorporates 2-mercaptobenzimidazole-intercalated magnesium-aluminum hydrotalcite and 8-hydroxyquinoline-intercalated montmorillonite. Utilizing the synergistic effect of the two, an anti-corrosion coating with excellent anti-corrosion performance is produced. Furthermore, the anti-corrosion coating also exhibits ion stimulation-responsive self-repairing properties, effectively controlling the release of corrosion inhibitors in the coating, thereby improving the anti-corrosion cycle and protective performance of the coating and extending the service life of the anti-corrosion coating. 2. The present application modifies the montmorillonite in the 8-hydroxyquinoline intercalated montmorillonite, which not only facilitates the insertion of the corrosion inhibitor 8-hydroxyquinoline into the montmorillonite interlayers, but also improves the compatibility between the 8-hydroxyquinoline intercalated montmorillonite and the bisphenol A epoxy resin, thereby enhancing the reinforcing effect of the 8-hydroxyquinoline intercalated montmorillonite on the anti-corrosion coating; 3. The preparation method of the anti-corrosion coating of the present application has simple steps, is easy to operate, and the raw materials used are easily available, making it suitable for large-scale industrial production. DETAILED DESCRIPTION

[0024] The present application is further described in detail below with reference to the embodiments.

[0025] Material Source Unless otherwise specified, the raw materials used in this application are commercially available products.

[0026] The bisphenol A epoxy resin of the present application has a model number of E44, a bonding strength of 1.55 MPa, a melting point of 115-120° C., and a flash point of 252° C.

[0027] The polyamide curing agent of the present application has a model of 650, an amine value of 80-220 mgKOH / g, a viscosity (40°C) of 1000-10000 mPa·s, a molecular weight of 600-1100, and a density (40°C) of 0.97-0.99 g / cm 3 .

[0028] The wetting and dispersing agent of the present application is a commonly used wetting and dispersing agent in the art. In a specific embodiment of the present application, the model of the wetting and dispersing agent is SN-5060, the main component of which is acrylate, and the pH is 7-9.

[0029] The additives of the present application include a leveling agent and a defoaming agent, both of which can be added in an amount commonly used in the art. In a specific embodiment of the present application, the weight ratio of the leveling agent to the defoaming agent is 0.2:0.8. The leveling agent and the defoaming agent are both commonly used leveling agents and defoaming agents in the art. In a specific embodiment of the present application, the model of the leveling agent is BYK-306 and the model of the defoaming agent is BYK-1748.

[0030] Preparation Example 1.1 2-Mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite was prepared by the following method: a. Under nitrogen protection, the carbonate-intercalated magnesium-aluminum hydrotalcite was calcined at 450°C for 5 hours and cooled to room temperature to obtain a bimetallic oxide; b. Adding 2-mercaptobenzimidazole to boiling deionized water to obtain a solution with a concentration of 0.08 mol / L, then adding NaOH in an amount equivalent to the 2-mercaptobenzimidazole to anionize the solution, and adjusting the pH of the system to 11 to obtain a 2-mercaptobenzimidazole anion solution; under the protection of nitrogen, stirring the 2-mercaptobenzimidazole anion solution and the bimetallic oxide at a temperature of 55° C. for 26 hours, wherein the molar ratio of 2-mercaptobenzimidazole to the bimetallic oxide is 2.5:1; c. The product obtained in step b was centrifuged at a speed of 5500 rpm for 5 min, and then the precipitate was washed with boiled deionized water and centrifuged twice, vacuum-dried at a temperature of 60° C. for 24 h, and ground to obtain 2-mercaptobenzimidazole-intercalated magnesium aluminum hydrotalcite.

[0031] Preparation Example 1.2 2-Mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite was prepared by the following method: a. Under nitrogen protection, the carbonate-intercalated magnesium-aluminum hydrotalcite was calcined at 550°C for 3 hours and cooled to room temperature to obtain a bimetallic oxide; b. Adding 2-mercaptobenzimidazole to boiling deionized water to obtain a solution with a concentration of 0.12 mol / L, then adding NaOH in an amount equivalent to the 2-mercaptobenzimidazole to anionize the solution, and adjusting the pH of the system to 11 to obtain a 2-mercaptobenzimidazole anion solution; under the protection of nitrogen, stirring the 2-mercaptobenzimidazole anion solution and the bimetallic oxide at 65° C. for 24 hours, wherein the molar ratio of 2-mercaptobenzimidazole to the bimetallic oxide is 3.5:1; c. The product obtained in step b was centrifuged at 6500 rpm for 3 min, and the precipitate was washed with boiled deionized water and centrifuged twice, dried in vacuo at 60° C. for 24 h, and ground to obtain 2-mercaptobenzimidazole-intercalated magnesium aluminum hydrotalcite.

[0032] Preparation Example 2.1 8-Hydroxyquinoline intercalated montmorillonite was prepared by the following method: The montmorillonite was dissolved in a solvent (the weight ratio of acetone and water was 1:1), and 8-hydroxyquinoline was added and mixed and stirred evenly. The weight ratio of 8-hydroxyquinoline to montmorillonite was 1:9. The mixture was then vacuumed and maintained for 4 hours. The mixture was then washed twice with deionized water, centrifuged, washed once with ethanol, and vacuum dried at 60°C for 24 hours to obtain 8-hydroxyquinoline intercalated montmorillonite.

[0033] Preparation Example 2.2 8-Hydroxyquinoline intercalated montmorillonite was prepared by the following method: The montmorillonite was dissolved in a solvent (the weight ratio of acetone and water was 1:1), and 8-hydroxyquinoline was added and mixed and stirred evenly, the weight ratio of 8-hydroxyquinoline to montmorillonite was 1:10, and then vacuumed and maintained for 5 hours, and then washed twice with deionized water, centrifuged, washed once with ethanol, and vacuum dried at 60°C for 24 hours to obtain 8-hydroxyquinoline intercalated montmorillonite.

[0034] Preparation Example 2.3 The difference from Preparation Example 2.2 is that: before dissolving montmorillonite in the solvent, it is first modified. The specific process is: montmorillonite is dispersed in deionized water and magnetically stirred for 24 hours to obtain solution A, octadecylamine and hydrochloric acid are magnetically stirred for 30 minutes to obtain solution B with a pH value of 3, solution A and solution B are mixed and reacted at a temperature of 75°C for 26 hours, wherein the weight ratio of montmorillonite to octadecylamine is 1:0.25, and then centrifuged three times until the filtrate is tested with a 0.1 mol / L AgNO3 solution without white precipitate, and then dried at a temperature of 60°C for 24 hours and ground to obtain modified montmorillonite.

[0035] Preparation Example 2.4 The difference from Preparation Example 2.2 is that: before dissolving montmorillonite in the solvent, it is first modified. The specific process is: montmorillonite is dispersed in deionized water and magnetically stirred for 26 hours to obtain solution A, octadecylamine and hydrochloric acid are magnetically stirred for 35 minutes to obtain solution B with a pH value of 4, solution A and solution B are mixed and reacted at a temperature of 85°C for 22 hours, wherein the weight ratio of montmorillonite to octadecylamine is 1:0.35, and then centrifuged three times until the filtrate is tested with a 0.1 mol / L AgNO3 solution without white precipitate, and then dried at a temperature of 60°C for 24 hours and ground to obtain modified montmorillonite.

[0036] Example 1.1 A method for preparing a self-repairing anti-corrosion coating comprises the following steps: S1, 100kg bisphenol A type epoxy resin and 30kg butyl acetate are mixed to obtain a bisphenol A type epoxy resin dilution; S2, 1 kg of filler, 5 kg of butyl acetate and 1 kg of wetting and dispersing agent were mixed and ultrasonically dispersed for 5 min; The filler comprises 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite prepared in Preparation Example 1.1 and 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.1 in a weight ratio of 0.5:1. The amount of 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite is 0.33 kg, and the amount of 8-hydroxyquinoline intercalated montmorillonite is 0.67 kg. S3. Mix the bisphenol A epoxy resin dilution and the result of step S2, add 45 kg of polyamide curing agent and continue stirring until the system is uniform and transparent, add 2 kg of additives (0.4 kg of leveling agent and 1.6 kg of defoaming agent) and mix evenly to obtain a self-repairing anti-corrosion coating.

[0037] Example 1.2 A method for preparing a self-repairing anti-corrosion coating comprises the following steps: S1, 100kg bisphenol A type epoxy resin and 33kg butyl acetate are mixed to obtain a bisphenol A type epoxy resin dilution; S2, 1 kg of filler, 7 kg of butyl acetate and 2 kg of wetting and dispersing agent were mixed and ultrasonically dispersed for 10 min; The filler comprises 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite prepared in Preparation Example 1.2 and 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.2 in a weight ratio of 0.5:1, the amount of 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite used is 0.33 kg, and the amount of 8-hydroxyquinoline intercalated montmorillonite used is 0.67 kg; S3. Mix the bisphenol A epoxy resin dilution and the result of step S2, add 55 kg of polyamide curing agent and continue stirring until the system is uniform and transparent, add 5 kg of additives (1 kg of leveling agent, 4 kg of defoaming agent) and mix evenly to obtain a self-repairing anti-corrosion coating.

[0038] Example 2.1 A method for preparing a self-repairing anti-corrosion coating, which differs from Example 1.2 in that: in step S2, the amount of filler used is 2.5 kg, and the rest is the same as Example 1.2; wherein, the filler includes 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite prepared in Preparation Example 1.2 and 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.2 in a weight ratio of 0.5:1, the amount of 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite used is 0.83 kg, and the amount of 8-hydroxyquinoline intercalated montmorillonite used is 1.67 kg.

[0039] Example 2.2 A method for preparing a self-repairing anti-corrosion coating, which differs from Example 1.2 in that: in step S2, the amount of filler used is 3 kg, and the rest is the same as Example 1.2; wherein, the filler includes 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite prepared in Preparation Example 1.2 and 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.2 in a weight ratio of 0.5:1, the amount of 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite used is 1 kg, and the amount of 8-hydroxyquinoline intercalated montmorillonite used is 2 kg.

[0040] Example 2.3 A method for preparing a self-repairing anti-corrosion coating, which differs from Example 1.2 in that: in step S2, the amount of filler used is 3.5 kg, and the rest is the same as Example 1.2; wherein, the filler includes 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite prepared in Preparation Example 1.2 and 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.2 in a weight ratio of 0.5:1, the amount of 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite used is 1.17 kg, and the amount of 8-hydroxyquinoline intercalated montmorillonite used is 2.33 kg.

[0041] Example 2.4 A method for preparing a self-repairing anti-corrosion coating, which differs from Example 1.2 in that: in step S2, the amount of filler used is 5 kg, and the rest is the same as Example 1.2; wherein, the filler includes 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite prepared in Preparation Example 1.2 and 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.2 in a weight ratio of 0.5:1, the amount of 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite used is 1.67 kg, and the amount of 8-hydroxyquinoline intercalated montmorillonite used is 3.33 kg.

[0042] Example 3.1 A method for preparing a self-repairing anti-corrosion coating, which differs from Example 2.2 in that: 3 kg of filler includes 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite prepared in Preparation Example 1.2 and 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.2 in a weight ratio of 1:1, the amount of 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite used is 1.5 kg, the amount of 8-hydroxyquinoline intercalated montmorillonite used is 1.5 kg, and the rest is the same as Example 2.2.

[0043] Example 3.2 A method for preparing a self-repairing anti-corrosion coating, which differs from Example 2.2 in that: 3 kg of filler includes 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite prepared in Preparation Example 1.2 and 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.2 in a weight ratio of 1.5:1, the amount of 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite used is 1.8 kg, the amount of 8-hydroxyquinoline intercalated montmorillonite used is 1.2 kg, and the rest is the same as Example 2.2.

[0044] Example 3.3 A method for preparing a self-repairing anti-corrosion coating, which differs from Example 2.2 in that: 3 kg of filler includes 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite prepared in Preparation Example 1.2 and 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.2 in a weight ratio of 2:1, the amount of 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite used is 2 kg, the amount of 8-hydroxyquinoline intercalated montmorillonite used is 1 kg, and the rest is the same as Example 2.2.

[0045] Example 4.1 A method for preparing a self-repairing anti-corrosion coating, which differs from Example 2.2 in that the 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.2 is replaced by the 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.3, and the rest is the same as Example 2.2.

[0046] Example 4.2 A method for preparing a self-repairing anti-corrosion coating, which differs from Example 2.2 in that the 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.2 is replaced by the 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.4, and the rest is the same as Example 2.2.

[0047] Comparative Example 1.1 The difference from Example 2.2 is that only the 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite prepared in Preparation Example 1.2 is used as the filler, and the rest is the same as Example 2.2.

[0048] Comparative Example 1.2 The difference from Example 2.2 is that only the 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.2 is used as the filler, and the rest is the same as Example 2.2.

[0049] Comparative Example 2.1 The difference from Example 2.2 is that: 3 kg of filler includes 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite prepared in Preparation Example 1.2 and 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.2 in a weight ratio of 0.2:1, the amount of 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite used is 0.5 kg, the amount of 8-hydroxyquinoline intercalated montmorillonite used is 2.5 kg, and the rest is the same as Example 2.2.

[0050] Comparative Example 2.2 The difference from Example 2.2 is that: 3 kg of filler includes 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite prepared in Preparation Example 1.2 and 8-hydroxyquinoline intercalated montmorillonite prepared in Preparation Example 2.2 in a weight ratio of 3:1, the amount of 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite used is 2.25 kg, the amount of 8-hydroxyquinoline intercalated montmorillonite used is 0.75 kg, and the rest is the same as Example 2.2.

[0051] Performance testing First, a low-carbon steel plate with a size of 120 mm × 50 mm × 1 mm was used as the substrate, and coarse and fine grinding was performed with 400-mesh and 1200-mesh sandpapers, and surface impurities and oil stains were washed away with anhydrous ethanol. After drying, the anti-corrosion coatings prepared in the above embodiments and comparative examples were applied to the steel plate surface with a coating rod with a specification of 150 μm. The coatings were cured in an oven at 100°C for 1 hour to obtain coating samples, and the thickness of the coating samples was controlled at 60 ± 5 μm. Then, the prepared coating samples were subjected to relevant performance tests.

[0052] 1. Mechanical Properties: Adhesion tests were conducted on coating samples according to GB / T 5210-2006. For cured coatings of the same thickness, a test ingot was applied to the coating surface with adhesive. After the adhesive cured, the ingot was pulled away from the coating surface using a pull-off tester. The tensile force required to break the attachment between the coating and the substrate was measured, which was the dry adhesion. The coating samples were soaked in a 3.5 wt% NaCl solution for 7 days, then removed. The moisture on the coating surface was wiped off, and the wet adhesion of the coating was measured using the above method. The adhesion failure rate (η) of the coating was calculated as follows: η = (dry adhesion - wet adhesion) / dry adhesion × 100%. The results are recorded in Table 1.

[0053] 2. Anti-corrosion performance: The anti-corrosion performance of the coating was tested by electrochemical testing. The electrochemical test used a traditional three-electrode system, in which a carbon steel electrode was used as the working electrode, a saturated calomel electrode (SCE) was used as the reference electrode, and a platinum sheet (1×1 cm 2) is the counter electrode, and the EIS spectrum of the test coating after being immersed in 3.5wt% NaCl aqueous solution for 10 days, the EIS test frequency is 10 5 Hz-10 -2 Hz, the disturbance signal voltage relative to the open circuit potential (OCP) is 10mV, and the test results are fitted using ZSimpWin software. Since among these electrochemical parameters, the total resistance R total It is an important parameter that reflects the failure of the coating during immersion in the corrosive medium. Therefore, the total resistance R total Recorded in Table 1.

[0054] 3. Self-repairing performance: Use a utility knife to make an artificial scratch of about 2 cm on the coating surface, and ensure that the scratch penetrates the substrate. Then soak the coating in a 3.5wt% NaCl aqueous solution. After 12 hours, perform an electrochemical test on the damaged coating according to the above method, and measure the total resistance R total Recorded in Table 1.

[0055] Table 1 In order to verify the ion stimulation response self-repairing performance of the anti-corrosion coating prepared in this application, the coating sample corresponding to the anti-corrosion coating prepared in Example 2.2 was scratched with a utility knife with a length of about 2 cm on the coating surface, and the scratch was ensured to penetrate the substrate. The coating was then immersed in NaCl aqueous solution of different concentrations for 10 h and then subjected to EIS testing. The EIS data were fitted and the low-frequency impedance modulus |Z| of the coating system was calculated. 0.01Hz The changes with the concentration of NaCl aqueous solution are recorded in Table 2.

[0056] Table 2 As can be seen from Table 1, the adhesion failure rate of the anti-corrosion coating formed by curing in Examples 1.1-1.2 of the present application was 27.38-28.21% after being immersed in a 3.5wt% NaCl solution for 7 days. After being immersed in a 3.5wt% NaCl solution for 10 days, the Log|R total | is 8.5Ω. After artificial scratching and immersion in 3.5wt% NaCl aqueous solution for 12h, R total 5.51×10 5 -5.53×10 5 Ω·cm 2, the test data show that the anticorrosive coatings prepared in Examples 1.1-1.2 of the present application have good water resistance, low adhesion failure rate after immersion, and good corrosion resistance and self-repair performance. At the same time, combined with Table 2, it can be seen that the low-frequency impedance modulus of the anticorrosive coatings prepared in Examples 1-2 of the present application changes with the change of the concentration of the NaCl solution. At a higher concentration of the NaCl solution, the anticorrosive coating can perform ion exchange faster, release the corrosion inhibitor anions, and capture Cl - The experimental data show that the anti-corrosion coating prepared in Examples 1-2 of the present application has ion stimulation response self-repairing properties and has high anti-corrosion performance in 7.5wt% NaCl solution.

[0057] The difference between Examples 2.1-2.4 and Example 1.2 lies in the different amounts of filler used. As can be seen from Table 1, with the increase in the amount of filler used, the adhesion failure rate shows a trend of first decreasing and then increasing, and the total resistance shows a trend of first increasing and then decreasing. The test data show that with the increase in the amount of filler added, the mechanical properties and corrosion resistance of the coating are enhanced to a certain extent. However, when the amount of filler added is too high, agglomeration will occur in the coating, which in turn reduces the various properties of the coating.

[0058] The difference between Examples 3.1-3.3 and Example 2.2 is that the ratio between 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite and 8-hydroxyquinoline intercalated montmorillonite in the filler is different. It can be seen from Table 1 that with the increase in the proportion of 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite, the adhesion failure rate of the coating decreases and the total resistance increases. The experimental data show that by further optimizing the ratio between 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite and 8-hydroxyquinoline intercalated montmorillonite, the mechanical properties, corrosion resistance and self-healing properties of the coating can be further improved.

[0059] The difference between Examples 4.1-4.2 and Example 2.2 is that the montmorillonite in the 8-hydroxyquinoline intercalated montmorillonite is modified. As can be seen from Table 1, the adhesion failure rate of Examples 4.1-4.2 is lower than that of Example 2.2, and the total resistance is higher than that of Example 2.2. The experimental data show that by modifying the montmorillonite, the reinforcing effect of the 8-hydroxyquinoline intercalated montmorillonite on the coating can be further improved, thereby further improving the mechanical properties, corrosion resistance, and self-healing properties of the coating.

[0060] The difference between Comparative Examples 1.1-1.2 and Example 2.2 is that only one of 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite and 8-hydroxyquinoline intercalated montmorillonite is used as a filler. As can be seen from Table 1, the adhesion failure rate of Comparative Examples 1.1-1.2 is higher than that of Example 2.2, and the total resistance is lower than that of Example 2.2. The experimental data show that the present application mixes 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite and 8-hydroxyquinoline intercalated montmorillonite, which can exert a synergistic effect between the two, thereby improving the mechanical properties, corrosion resistance and self-healing properties of the coating.

[0061] Comparative Examples 2.1-2.2 differ from Example 2.2 in that only 2-mercaptobenzimidazole-intercalated magnesium-aluminum hydrotalcite is used, and the proportion of the filler is too low or too high. As can be seen from Table 1, the adhesion failure rate of Comparative Example 2.1 is higher than that of Example 2.2, and the total resistance is lower than that of Example 2.2. Test data show that if the amount of 2-mercaptobenzimidazole-intercalated magnesium-aluminum hydrotalcite is too low, the mechanical properties, corrosion resistance, and self-healing properties of the coating will be reduced. Although the adhesion failure rate of Comparative Example 2.2 is lower than that of Example 2.2 and the total resistance is higher than that of Example 2.2, all properties have shown a downward trend compared to Example 3.3. Test data show that if the proportion of 2-mercaptobenzimidazole-intercalated magnesium-aluminum hydrotalcite in the filler is too high, the various properties of the coating will be reduced.

[0062] The embodiments of this specific implementation method are all preferred embodiments of the present application and are not intended to limit the scope of protection of the present application. Therefore, any equivalent changes made based on the structure, shape, and principle of the present application should be included in the scope of protection of the present application.

Claims

1. A self-repairing anti-corrosion coating, characterized in that: The raw materials used include the following components in parts by weight: 100 parts of bisphenol A epoxy resin; 35-40 parts of butyl acetate; 1-5 parts of filler; 45-55 parts of polyamide curing agent; 1-2 parts of wetting and dispersing agent; 2-5 parts of additives; The filler comprises 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite and 8-hydroxyquinoline intercalated montmorillonite in a weight ratio of (0.5-2.0):

1.

2. A self-repairing anti-corrosion coating according to claim 1, characterized in that: The weight ratio of the bisphenol A epoxy resin to the filler is 100:(2.5-3.5).

3. The self-repairing anti-corrosion coating according to claim 1, characterized in that: The filler comprises 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite and 8-hydroxyquinoline intercalated montmorillonite in a weight ratio of (1.5-2.0):

1.

4. The self-repairing anti-corrosion coating according to claim 1, characterized in that: The 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite is prepared by the following method: a. calcining the carbonate-intercalated magnesium-aluminum hydrotalcite under the protection of an inert gas and cooling it to room temperature to obtain a bimetallic oxide; b. Under the protection of inert gas, stir the 2-mercaptobenzimidazole anion solution and the bimetallic oxide at a temperature of 55-65°C for 24-26 hours, wherein the molar ratio of 2-mercaptobenzimidazole to bimetallic oxide is (2.5-3.5):1; c. Centrifuge the product obtained in step b at a rotation speed of 5500-6500 rpm for 3-5 min, then wash, dry and grind the precipitate to obtain 2-mercaptobenzimidazole intercalated magnesium aluminum hydrotalcite.

5. The self-repairing anti-corrosion coating according to claim 4, characterized in that: The calcination temperature is 450-550° C. and the calcination time is 3-5 hours.

6. The self-repairing anti-corrosion coating according to claim 4, characterized in that: The preparation process of the 2-mercaptobenzimidazole anion solution is specifically as follows: 2-mercaptobenzimidazole is added to boiling deionized water to obtain a solution with a concentration of 0.08-0.12 mol / L, then NaOH is added in an amount equivalent to 2-mercaptobenzimidazole to anionize it, and the pH value of the system is adjusted to 11 to obtain the 2-mercaptobenzimidazole anion solution.

7. The self-repairing anti-corrosion coating according to claim 1, characterized in that: The 8-hydroxyquinoline intercalated montmorillonite is prepared by the following method: The montmorillonite is dissolved in a solvent, and 8-hydroxyquinoline is added and mixed and stirred evenly, the weight ratio of 8-hydroxyquinoline to montmorillonite is 1: (9-10), and then vacuumed and maintained for 4-5 hours, and then washed, centrifuged, cleaned, and dried to obtain 8-hydroxyquinoline intercalated montmorillonite.

8. The self-repairing anti-corrosion coating according to claim 7, characterized in that: The montmorillonite is modified by the following method: Montmorillonite is dispersed in deionized water and magnetically stirred for 24-26 hours to obtain solution A. Octadecylamine and hydrochloric acid are magnetically stirred for 30-35 minutes to obtain solution B with a pH value of 3-4. Solution A and solution B are mixed and reacted at a temperature of 75-85°C for 22-26 hours, wherein the weight ratio of montmorillonite to octadecylamine is 1:(0.25-0.35). The mixture is then centrifuged and filtered until the filtrate is tested for no white precipitate by using a 0.1 mol / L AgNO3 solution. The mixture is then dried and ground to obtain modified montmorillonite.

9. A method for preparing the self-repairing anti-corrosion coating according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, mixing 100 parts by weight of bisphenol A epoxy resin and 30-33 parts by weight of butyl acetate to obtain a bisphenol A epoxy resin dilution; S2, mixing 1-5 parts by weight of filler, 5-7 parts by weight of butyl acetate and 1-2 parts by weight of a wetting and dispersing agent and ultrasonically dispersing for 5-10 minutes; S3. Mix the bisphenol A epoxy resin dilution and the product obtained in step S2, add 45-55 parts by weight of a polyamide curing agent, and continue stirring until the system is uniform and transparent. Add 2-5 parts by weight of an auxiliary agent and mix evenly to obtain a self-repairing anti-corrosion coating.