Preparation method of metal catalyst based on hydroquinoline-imine coordination and high-performance polyolefin elastomer synthesized by metal catalyst

By preparing hydrogenated quinoline-imine-based titanium zirconium hafnium catalyst, the problems of reduced catalytic activity and molecular weight at high temperatures were solved, enabling the efficient synthesis of high-performance polyolefin elastomers suitable for high-temperature solution polymerization.

CN121064240APending Publication Date: 2025-12-05QINGDAO UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510739838.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-04
Publication Date
2025-12-05

AI Technical Summary

Technical Problem

Existing polyolefin catalysts exhibit reduced catalytic activity and lower molecular weight of the resulting polymers at high temperatures, making it difficult to meet the requirements of high-temperature solution polymerization. Furthermore, imine-amine type metal catalysts have shortcomings in terms of high-temperature resistance and synthesis cost.

Method used

Hydrogenated quinoline-imine ligands are generated by condensation of 1,2,3,4-tetrahydroquinoline-8-carboxaldehyde and various anilines under acidic conditions, and then reacted with MMe4 (M=Ti, Zr or Hf) to prepare a hydrogenated quinoline-imine titanium zirconium hafnium catalyst. When used in conjunction with a co-catalyst, it is suitable for high-temperature solution polymerization.

Benefits of technology

The prepared hydrogenated quinoline-imine-based titanium zirconium hafnium catalyst exhibits excellent catalytic activity and α-olefin selectivity at high temperatures, enabling the synthesis of high molecular weight polyolefin elastomers, and is suitable for the production of high-performance polyolefin materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0005434344330000031
    Figure BDA0005434344330000031
  • Figure BDA0005434344330000032
    Figure BDA0005434344330000032
Patent Text Reader

Abstract

According to the invention, a series of novel hydroquinoline-imino ligands are directly synthesized through amine-aldehyde condensation between 1, 2, 3, 4-tetrahydroquinoline-8-formaldehyde and various anilines under the catalysis of p-TsOH. Next, the obtained ligand and MMe4 (M = Ti, Zr or Hf) obtained through in-situ synthesis are subjected to a one-pot reaction to obtain the hydrogenated quinoline-imino coordinated titanium zirconium hafnium catalyst, and the hydrogenated quinoline-imino coordinated titanium zirconium hafnium catalyst is high in yield and has great economic benefits. The application of the obtained hydrogenated quinoline-imino coordinated titanium zirconium hafnium catalyst in the synthesis of polyolefin elastomers finds that the molecular weight and alpha-olefin insertion rate of the obtained polymer can be effectively improved by changing substituent groups on the catalyst structure. The hydroquinoline-imino coordinated titanium-zirconium-hafnium catalyst disclosed by the invention has the advantages of simple synthesis, easily available raw materials and high product yield. In the presence of a cocatalyst, the catalyst shows excellent activity (3.32 * 10 < 8 > g (POE). Mol <-1 > (Hf). H <-1 >) and alpha-olefin selectivity (the insertion rate reaches 38.4 mol%), and a high-molecular-weight polyolefin elastomer (POE) (the polymer molecular weight Mw reaches 3020 kg.mol <-1 >) is prepared. In addition, the hydrogenated quinoline-imino coordinated titanium zirconium hafnium catalyst also shows excellent high temperature resistance (higher than 200 DEG C), is suitable for high-temperature solution polymerization, and can be used for preparing high-performance polyolefin elastomers. In addition, the hydrogenated quinoline-imino coordinated titanium zirconium hafnium catalyst disclosed by the invention still shows an excellent catalytic effect in ethylene homopolymerization. Therefore, the invention has originality, and provides a new direction for the development of the field of polyolefin materials.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to the preparation of olefin coordination polymerization metal catalysts and their use in the field of olefin polymerization. BACKGROUND

[0002] In recent years, the production capacity and application of polyolefin materials have been rising. Polyethylene (PE), polypropylene (PP), and ethylene / alpha-olefin copolymers, etc. polyolefin materials are widely used in daily necessities, military products, from toys, sports equipment to automobiles, aircraft, rockets, etc. various fields due to their light weight, high mechanical strength, impact resistance, good processability and other advantages. With the continuous development of society, the application range of polyolefin materials continues to expand. However, in this development process, a single polyolefin material cannot meet the diversified needs. Therefore, high-performance polyolefin materials such as ultrahigh molecular weight polyethylene, polyolefin elastomer, etc. have emerged. Among them, polyolefin elastomer (POE) is a kind of ethylene-based random copolymer with high alpha-olefin content (usually more than 20 wt. %), which is copolymerized by ethylene and 1-octene, 1-hexene or 1-butene. It is a kind of high-performance polyolefin with excellent mechanical and elastic properties, which has attracted much attention in the automotive industry and the photovoltaic field. Generally speaking, polyolefin elastomer is synthesized by solution polymerization technology, which can more efficiently synthesize the product and better control the polymer microstructure, thereby obtaining a material with more excellent performance. Solution polymerization is best carried out at high temperature (usually more than 120℃) to prevent the polymer from precipitating during polymerization. In addition, high-temperature solution polymerization can reduce viscosity, increase product yield, and thus reduce cost. However, these limitations pose great challenges to the catalysts used in catalytic olefin polymerization, because as the polymerization temperature increases, the activity of the polyolefin catalyst for catalytic olefin polymerization and the molecular weight (M w s) of the generated polymer usually decrease. Therefore, it is necessary to develop homogeneous metal catalysts with better catalytic performance at high temperature.

[0003] To this end, metallocene and constrained geometry catalysts (CGC) were designed and synthesized by researchers worldwide and successfully used in the commercial production of POE in the early 1990s (Chem. Rev. 1998, 98, 2587-2598). In addition, a variety of non-metallocene transition metal catalysts have also gradually developed. Among them, the imine-amine type metal catalyst was first discovered by Dow Chemical (Organometallics 2007, 26, 3896-3899), and the imine ligand can be easily obtained from the market, and the resulting metal catalyst has high activity and can achieve the regulation of α-olefin content. However, this kind of imine-amine metal catalyst performs poorly in terms of high temperature resistance. Subsequently, the imine-based complex designed by introducing a six-membered ring into the ligand structure has better thermal stability, but the ligand itself is prone to isomerization under the induction of acid, which brings inconvenience to synthesis (Organometallics 2011, 30, 1695-1709). Kloin et al. successfully improved the high temperature resistance of the catalyst by introducing a quinoline structure into the catalyst skeleton (Organometallics 2012, 31, 6244-6251), and obtained a series of polyolefin catalysts with different catalytic properties by changing the substituents on the catalyst structure. Although the amine-quinoline ligand can provide the metal catalyst with good high temperature resistance and copolymerization performance, it has an undeniable disadvantage that an expensive Pd catalyst is used to catalyze the coupling reaction in the synthesis of the ligand, which makes it have an undeniable disadvantage in large-scale production.

[0004] In the present application, a series of new hydrogenated quinoline-imine ligands are directly synthesized by p-TsOH-catalyzed amine aldehyde condensation between 1,2,3,4-tetrahydroquinoline-8-carboxaldehyde and various anilines. Next, the hydrogenated quinoline-imine ligands are reacted with MMe4 (M = Ti, Zr or Hf) synthesized in situ by one-pot method to obtain hydrogenated quinoline-imine ligated titanium, zirconium and hafnium catalysts, which have high yield and are very economical. The hydrogenated quinoline-imine titanium, zirconium and hafnium catalysts obtained are used in the synthesis of polyolefin elastomers, and it is found that by changing the substituents on the catalyst structure, the molecular weight and α-olefin insertion rate of the obtained polymer can be effectively improved. The hydrogenated quinoline-imine titanium, zirconium and hafnium catalysts reported in the present application have the advantages of simple synthesis, easy availability of raw materials and high product yield. In the presence of a cocatalyst, the catalyst exhibits excellent activity (3.32 × 10 8 g (POE) · mol -1 (Hf) · h -1 ), α-olefin selectivity (insertion rate of 38.4 mol%), and preparation of high molecular weight polyolefin elastomer POE (polymer molecular weight Mw of 3020 kg · mol -1). In addition, the hydrogenated quinoline-imino titanium zirconium hafnium catalyst reported by the present application also exhibits excellent high-temperature resistance (greater than 200℃), is suitable for high-temperature solution polymerization, and can be used to prepare high-performance polyolefin elastomers. Therefore, the present application has originality and provides a new direction for the development of the polyolefin material field. SUMMARY

[0005] The purpose of the present application is to provide a hydrogenated quinoline-imino titanium zirconium hafnium catalyst and its application in the preparation of polyolefin elastomers.

[0006] The present application provides a hydrogenated quinoline-imino titanium zirconium hafnium catalyst represented by formula (I):

[0007]

[0008] wherein M is selected from titanium, zirconium, and hafnium; R 1 is selected from methyl, ethyl, hydrogen, isopropyl, chlorine, and fluorine; R 2 is selected from methyl, ethyl, hydrogen, isopropyl, chlorine, and fluorine; R 3 is selected from methyl, methoxy, hydrogen, and tert-butyl.

[0009] Preferably, the metal compound of the present application is selected from any one of the metal catalysts represented by formula (II):

[0010]

[0011] The present application provides a preparation method of the above-mentioned hydrogenated quinoline-imino titanium zirconium hafnium catalyst, comprising the following steps:

[0012] Under a nitrogen atmosphere, the metal salt MCl4 is dissolved in 20-80 mL of anhydrous solvent, 4.0-5.0 molar equivalents of methyl magnesium bromide are added, and the reaction is carried out at low temperature under nitrogen protection for 2 hours, after which 1 molar equivalent of hydrogenated quinoline imine ligand is added and the reaction is carried out for 5 hours; after the reaction is completed, the solvent is removed under reduced pressure, and the resulting product is extracted with a good solvent to obtain the hydrogenated quinoline-imino titanium zirconium hafnium catalyst.

[0013] In the above preparation method, the anhydrous solvent is selected from toluene, n-hexane, xylene, and benzene; and the good solvent is selected from n-hexane, toluene, pentane, heptane, and cyclohexane.

[0014] In the above preparation method, the metal salt MCl4 is selected from one of TiCl4, ZrCl4, and HfCl4.

[0015] The present application also provides the application of the above-mentioned hydrogenated quinoline-imino titanium zirconium hafnium catalyst in the catalysis of olefin polymerization.

[0016] In the above application, the olefin monomer is one or more of ethylene, propylene, 1-butene, styrene, 1-hexene, norbornene, and 1-octene.

[0017] The hydrogenated quinoline-imido titanium zirconium hafnium catalyst needs to be catalyzed with a cocatalyst, which is one or more of trifluorophenyl boron, triphenyl carbonium tetrakis (pentafluorophenyl) borate, N, N-dimethyl aniline tetrakis (pentafluorophenyl) borate, aluminoxane, alkyl aluminum and chlorinated alkyl aluminum. The aluminoxane is methyl aluminoxane, ethyl aluminoxane or isobutyl aluminoxane; the alkyl aluminum is trimethyl aluminum, triethyl aluminum, triisobutyl aluminum or tri-n-hexyl aluminum; and the chlorinated alkyl aluminum is monochlorodiethyl aluminum, hemi-monochlorodiethyl aluminum or ethyl aluminum dichloride.

[0018] In the above polymerization reaction, the polymerization temperature is 0-200℃, the polymerization pressure is 0.1-5 MPa, and the polymerization solvent is one or more of n-hexane, heptane, pentane and toluene.

[0019] The application provides preparation of a hydrogenated quinoline-imido titanium zirconium hafnium metal catalyst and application of the catalyst in catalyzing olefin polymerization. The hydrogenated quinoline-imido titanium zirconium hafnium metal catalyst reported in the application has the advantages of simple synthesis, easy availability of raw materials, high product yield, high catalytic activity (the highest activity can reach 3.32 x 10 8 g (PE) · mol -1 (Hf) · h -1 ) and good copolymerization performance (1-octene insertion rate can reach 38.4 mol%), and is especially suitable for high-temperature solution polymerization for preparing high-quality and high-performance polyolefin materials. The metal catalyst provided in the application has original innovation and can promote development of a high-end polyolefin chemical industry in China. BRIEF DESCRIPTION OF DRAWINGS

[0020] Figure 1 is NMR hydrogen spectrum of catalyst C1 in Example 1.

[0021] Figure 2 NMR hydrogen spectrum of catalyst C2 in Example 2.

[0022] Figure 3 High-temperature GPC spectrum of a polyolefin elastomer POE with a molecular weight of 2120 kg·mol -1 in Example 23.

[0023] Figure 4 High-temperature GPC spectrum of a polyolefin elastomer POE with a molecular weight of 1840 kg·mol -1 in Example 28.

[0024] Figure 5 NMR carbon spectrum of a polyolefin elastomer POE with a 1-octene insertion rate of 13.6% in Example 33.

[0025] Figure 6NMR carbon spectrum of the polyolefin elastomer POE with 1-octene insertion rate of 30.6% in Example 22.

[0026] Figure 7 NMR carbon spectrum of the polyolefin elastomer POE with 1-octene insertion rate of 36.4% in Example 21.

[0027] Figure 8 Crystal pattern of catalyst C1. DETAILED DESCRIPTION

[0028] The present application is further illustrated by the following examples without being limited thereto. The examples of the present application can enable a person skilled in the art to have a more comprehensive understanding of the present application.

[0029] The experimental methods used in the following examples are conventional methods unless otherwise specified.

[0030] The raw materials and reagents used in the following examples are commercially available unless otherwise specified.

[0031] The ligand precursor 1,2,3,4-tetrahydroquinoline-8-carboxaldehyde in the present application is synthesized according to the literature method (Synthesis 2021, 53, 4689–4699; Tetrahedron 2005, 61, 2631). As shown in (III), the hydrogenated quinoline-imine ligand C1-L-C3-L is prepared by a simple amine-aldehyde condensation reaction under acidic conditions.

[0032]

[0033] The present application is described below with specific examples.

[0034] Example 1, preparation of catalyst C1

[0035] 2,6-diisopropylaniline (1.78 g, 10.0 mmol), 1,2,3,4-tetrahydroquinoline-8-carboxaldehyde (1.60 g, 10.0 mmol), p-toluenesulfonic acid (30 mg, 0.174 mmol) were weighed and dissolved in 50 mL of ethanol, and stirred at 90°C under nitrogen atmosphere for 12 hours. After the mixture was cooled to room temperature, the solvent was removed by a rotary evaporator, and then recrystallized with an appropriate amount of methanol to obtain yellow solid C1-L (2.86 g, yield 89%). 1H NMR (400 MHz, CDC13): δ 9.19 (s, 1H), 8.19 (s, 1H), 7.19-7.14 (m, 2H), 7.13-7.06 (m, 2H), 7.01 (d, J = 7.4 Hz, 1H), 6.55 (t, J = 7.4 Hz, 1H), 3.50 (t, J = 5.5 Hz, 1H), 3.02 (hept, J = 6.8 Hz, 2H), 2.86 (t, J = 6.3 Hz, 2H), 1.99 (p, J = 6.1 Hz, 2H), 1.18 (d, J = 6.9 Hz, 13H). 13 C NMR (100 MHz, CDC13): δ 165.51, 149.26, 147.01, 138.37, 132.78, 132.02, 124.24, 123.16, 121.54, 115.46, 113.68, 41.11, 28.05, 27.76, 23.77, 20.96 ppm. Anal. Calcd for C 22 H 28 N2: C, 82.45; H, 8.81; N, 8.74. Found: C, 82.26; H, 8.83; N, 8.69.

[0036] HfCl4(0.352 g, 1.1 mmol) was weighed, 10 mL of anhydrous toluene was added, and 1.6 mL / 4.8 mmol of methyl magnesium bromide solution (3M) was slowly added at -40°C (acetonitrile-liquid nitrogen bath) and stirred for 2 hours. Then ligand C1-L (0.32 g / 1 mmol) was added, and the reaction was continued for 2 hours at -40°C in the dark and for 5 hours at room temperature. After the reaction was completed, the solvent was removed, toluene was added for extraction, and filtration was performed to obtain the product 0.41 g with a yield of 75%. 1 H NMR (400 MHz, CDC13): δ 9.19 (s, 1H), 8.19 (s, 1H), 7.19-7.14 (m, 2H), 7.13-7.06 (m, 2H), 7.01 (d, J = 7.4 Hz, 1H), 6.55 (t, J = 7.4 Hz, 1H), 3.50 (t, J = 5.5 Hz, 1H), 3.02 (hept, J = 6.8 Hz, 2H), 2.86 (t, J = 6.3 Hz, 2H), 1.99 (p, J = 6.1 Hz, 2H), 1.18 (d, J = 6.9 Hz, 13H). 13C NMR (400 MHz, C6D6): δ 169.56, 153.97, 152.64, 140.55, 135.86, 135.15, 127.02, 125.23, 123.96, 120.64, 115.94, 60.71, 42.09, 29.48, 28.33, 25.40, 22.58, 20.82 ppm. Anal. Calcd for C 25 H 36 HfN2: C, 55.29; H, 6.68; Hf, 32.87; N, 5.16. Found: C, 55.21; H, 6.70; Hf, 32.76; N, 5.21.

[0037] Example 2, Preparation of Catalyst C2

[0038] A mixture of 2,6-dimethylaniline (1.22 g, 10.0 mmol), 1,2,3,4-tetrahydroquinoline-8-carboxaldehyde (1.60 g, 10.0 mmol), p-toluenesulfonic acid (30 mg, 0.174 mmol) was dissolved in 50 mL of ethanol and stirred at 90 °C under nitrogen atmosphere for 12 hours. The mixture was cooled to room temperature and the solvent was removed by rotary evaporator, then recrystallized with proper amount of methanol to give yellow solid C2-L (2.33 g, yield 88%). 1 H NMR (400 MHz, CDC13): δ 8.14 (q, J = 1.4 Hz, 1H), 7.17 (t, J = 7.1 Hz, 1H), 6.95 (d, J = 7.2 Hz, 2H), 6.82 - 6.76 (m, 1H), 6.03 (dd, J = 8.1, 1.6 Hz, 1H), 5.96 (dd, J = 7.6, 1.4 Hz, 0H), 3.33 (t, J = 6.5 Hz, 0H), 3.01 - 2.89 (m, 1H), 2.88 - 2.81 (m, 0H), 2.77 (dt, J = 5.9, 3.0 Hz, 1H), 2.25 (s, 6H), 1.73 - 1.60 (m, 4H). 13 C NMR (100 MHz, CDC13): δ 151.73, 147.90, 135.76, 134.33, 131.89, 131.14, 126.93, 126.30, 126.11, 54.32, 45.25, 37.27, 28.81, 24.22, 18.00 ppm. Anal. Calcd for C 18 H 20 N2: C, 81.78; H, 7.63; N, 10.60. Found: C, 81.72; H, 7.53; N, 10.64.

[0039] HfCI3(0.256 g, 1.1 mmol) was weighed out, 10 mL of dry toluene was added, 1.6 mL / 4.8 mmol of methyl magnesium bromide solution (3 M) was slowly added at -40°C (acetonitrile-liquid nitrogen bath), and stirring was performed for 2 hours. Thereafter, ligand C2-L (0.27 g / 1 mmol) was added, and stirring was performed for two hours at -40°C in the dark, and the reaction was continued for 5 hours after the temperature was returned to room temperature. After the reaction was completed, the solvent was removed, toluene was added for extraction, and filtration was performed to obtain the product (0.42 g, yield 85%). 1 H NMR (400 MHz, C6D6): δ 7.10 (t, J = 7.3 Hz, 1H), 6.74 (d, J = 7.3 Hz, 2H), 6.72–6.68 (m, 1H), 6.63 (q, J = 1.4 Hz, 1H), 6.21 (s, 1H), 6.04–6.00 (m, 2H), 3.40–3.35 (m, 1H), 2.99 (dd, J = 6.2, 3.5 Hz, 1H), 2.98–2.95 (m, 1H), 2.95–2.92 (m, 1H), 2.10 (s, 6H), 1.93 (s, 9H), 1.83–1.69 (m, 3H), 1.62 (dd, J = 10.3, 8.6 Hz, 1H) ppm. 13 C NMR (400 MHz, C6D6): δ 209.14, 154.51, 137.64, 136.19, 134.38, 133.55, 129.88, 128.91, 127.04, 124.41, 56.07, 49.67, 37.48, 29.42, 23.10, 20.15, 18.16, 18.13, 18.11 ppm. Anal. Calcd for C 21 H 28 HfN2: C, 51.58; H, 6.18; Hf, 36.50; N, 5.73. Found: C, 51.62; H, 6.03; Hf, 36.51; N, 5.71.

[0040] Example 3, Preparation of Catalyst C3

[0041] 2,4,6-Trimethylaniline (1.35 g, 10.0 mmol), 1,2,3,4-tetrahydroquinoline-8- carboxaldehyde (1.60 g, 10.0 mmol), and p-toluenesulfonic acid (30 mg, 0.174 mmol) were dissolved in 50 mL of ethanol, and stirring was performed at 90°C under a nitrogen atmosphere for 12 hours. After the mixture was cooled to room temperature, the solvent was removed using a rotary evaporator, and recrystallization was performed by adding an appropriate amount of methanol to obtain yellow solid C3-L (2.21 g, yield 79%). 1H NMR (400 MHz, CDC13): δ 8.14 (q, J = 1.3 Hz, 1H), 6.90 (s, 2H), 6.79 (dd, J = 7.2, 2.8 Hz, 1H), 6.03 (dd, J = 8.1, 1.6 Hz, 1H), 5.99 - 5.91 (m, 0H), 3.37 - 3.30 (m, 0H), 3.01 - 2.89 (m, 1H), 2.88 - 2.80 (m, 0H), 2.77 (dt, J = 5.9, 3.0 Hz, 1H), 2.27 (s, 3H), 2.19 (s, 7H), 1.73 - 1.60 (m, 2H). 13 C NMR (100 MHz, CDC13): δ 149.21, 147.58, 135.76, 133.82, 131.89, 131.27, 131.14, 130.12, 126.11, 54.32, 45.25, 37.67, 28.81, 24.22, 20.75, 18.27 ppm. Anal. Calcd for C 19 H 22 N2: C, 81.97; H, 7.97; N, 10.06. Found: C, 81.86; H, 7.93; N, 10.01.

[0042] H NMR (400 MHz, CDC13): δ 8.14 (q, J = 1.3 Hz, 1H), 6.90 (s, 2H), 6.79 (dd, J = 7.2, 2.8 Hz, 1H), 6.03 (dd, J = 8.1, 1.6 Hz, 1H), 5.99 - 5.91 (m, 0H), 3.37 - 3.30 (m, 0H), 3.01 - 2.89 (m, 1H), 2.88 - 2.80 (m, 0H), 2.77 (dt, J = 5.9, 3.0 Hz, 1H), 2.27 (s, 3H), 2.19 (s, 7H), 1.73 - 1.60 (m, 2H). 1 H NMR (400 MHz, CDC13): δ 8.14 (q, J = 1.3 Hz, 1H), 6.90 (s, 2H), 6.79 (dd, J = 7.2, 2.8 Hz, 1H), 6.03 (dd, J = 8.1, 1.6 Hz, 1H), 5.99 - 5.91 (m, 0H), 3.37 - 3.30 (m, 0H), 3.01 - 2.89 (m, 1H), 2.88 - 2.80 (m, 0H), 2.77 (dt, J = 5.9, 3.0 Hz, 1H), 2.27 (s, 3H), 2.19 (s, 7H), 1.73 - 1.60 (m, 2H). 13C NMR (400 MHz, C6D6) δ 151.78, 137.33, 136.09, 134.67, 134.38, 133.55, 130.46, 129.88, 124.41, 56.07, 49.67, 37.48, 29.42, 23.10, 20.88, 20.53, 18.16, 18.13, 18.11 ppm. Anal. Calcd for C 22 H 30 HfN2: C, 52.53; H, 6.41; Hf, 35.48; N, 5.57. Found: C, 52.42; H, 6.44; Hf, 35.39; N, 5.62.

[0043] Example 4, Preparation of Catalyst C4

[0044] Under nitrogen protection, to a solution of ligand C1-L (1.43 g, 4.30 mmol, 8 mL hexanes) was added Ti(NMe2)4(1.39 g, 4.70 mmol) via syringe under nitrogen. The reaction mixture was stirred at 65 °C for 24 h to give a yellow suspension. The suspension was filtered at room temperature, the residue was washed with 2 mL hexanes and dried under reduced pressure to give a yellow powder (1.80 g, 3.60 mmol, 83% yield). To a solution of the yellow powder from the previous step (1.53 g, 3.00 mmol) in 50 mL of toluene was slowly added Me2SiCl2(2.15 g, 16.7 mmol) via syringe at 0 °C. The reaction mixture was stirred at room temperature overnight. The solvent was removed from the reaction mixture under reduced pressure. The residue was washed with 20 mL of hexanes to give a red powder (1.26 g, 2.64 mmol, 88% yield). To the red powder (0.63 g, 1.30 mmol) suspended in 50 mL of toluene was added 2 mL (6.0 mmol) of 3 M methylmagnesium bromide in ether at -40 °C to give a black suspension. The reaction mixture was stirred at room temperature for 3 h. The solvent was removed from the reaction mixture under reduced pressure. To the residue was added 80 mL of hexanes. After stirring at room temperature for 5 min, the suspension was filtered. The filtrate was concentrated and filtered to give a yellow powder product (0.43 g, 1.10 mmol, 80% yield). 1H NMR (400 MHz, C6D6): δ 7.26 (t, J = 7.6 Hz, 1H), 7.04 (d, J = 7.7 Hz, 2H), 6.73 (dd, J = 7.2, 1.4 Hz, 1H), 6.59 (d, J = 2.9 Hz, 1H), 6.22 (s, 1H), 6.07 - 5.93 (m, 2H), 3.34 - 3.29 (m, 1H), 3.05 - 2.98 (m, 2H), 2.98 - 2.93 (m, 1H), 2.93 - 2.77 (m, 2H), 1.76 - 1.58 (m, 4H), 1.29 (d, J = 6.2 Hz, 6H), 1.24 (d, J = 6.0 Hz, 6H), 1.00 (s, 9H) ppm. 13 C NMR (400 MHz, C6D6): δ 143.32, 141.39, 133.86, 133.45, 131.48, 129.73, 127.75, 124.81, 124.41, 55.88, 49.70, 43.00, 37.56, 29.61, 29.41, 23.55, 23.20, 19.42 ppm. Anal. Calcd for C 25 H 36 N2Ti: C, 72.45; H, 9.24; N, 6.76; Ti, 11.55 Found: C, 72.38; H, 9.26; N, 6.71; Ti, 11.58.

[0045] Example 5, Preparation of catalyst C5

[0046] Zirconium tetrachloride (0.256 g, 1.1 mmol) was weighed, 10 mL of dry toluene was added, and 1.6 mL / 4.8 mmol of methyl magnesium bromide solution (3M) was slowly added at -40°C (acetonitrile-liquid nitrogen bath) and stirred for 2 hours. Then ligand C1-L (0.32 g / 1 mmol) was added and stirred for two hours at -40°C in the dark, and the reaction was continued for 5 hours after returning to room temperature. After the reaction was completed, the solvent was removed, toluene was added for extraction, filtered, and the product 0.33 g was obtained with a yield of 72%. 1H NMR (400 MHz, C6D6) δ 7.26 (t, J = 7.6 Hz, 1H), 7.02 (d, J = 7.6 Hz, 2H), 6.80 - 6.70 (m, 1H), 6.59 (d, J = 1.2 Hz, 1H), 6.01 (dd, J = 6.7, 3.4 Hz, 2H), 5.96 (s, 1H), 3.26 (d, J = 9.4 Hz, 1H), 3.08 - 2.70 (m, 5H), 1.78 - 1.61 (m, 4H), 1.29 (d, J = 6.2 Hz, 6H), 1.24 (d, J = 6.0 Hz, 6H), 1.08 (s, 9H) ppm. 13 C NMR (400 MHz, C6D6): δ 151.32, 143.78, 134.52, 133.49, 131.48, 129.91, 127.75, 124.87, 124.41, 55.89, 49.62, 37.64, 29.62, 29.41, 23.55, 23.05, 19.37 ppm. Anal. Calcd for C 25 H 36 N2Zr: C, 65.59; H, 8.37; N, 6.12; Zr, 19.93. Found: C, 65.52; H, 8.38; N, 6.06; Zr, 19.97.

[0047] Example 6, ethylene polymerization catalyzed by C1

[0048] A 350 mL glass reactor equipped with a magnetic stirrer was used for the polymerization. In a glove box, 2 μmol of catalyst C1, 2.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate and 100 μmol of methylaluminoxane were weighed. The glass reactor was connected to the polymerization line and 50 mL of toluene was added to it. The temperature was raised to 50 °C and ethylene gas was continuously fed to maintain the reaction pressure at 5 atm. After 2 min, 30 mL of ethanol was added to the reactor under nitrogen atmosphere. After cooling, the reaction solution was poured into a large amount of ethanol to precipitate, and the final polymer was obtained by filtration and drying. Polymerization activity: 10800 kg·mol -1 (Hf)·h -1 , polymer Mw = 1220 kg·mol -1 , Mw / Mn = 2.1.

[0049] Example 7, ethylene polymerization catalyzed by C1

[0050] A 100 mL steel reactor equipped with a magnet was used for the polymerization, 50 mL of toluene was injected with a syringe, the reactor content was heated to 160°C, the reactor was saturated with 1 MPa of ethylene. In a glove box, 2 μmol of catalyst C1, 100 μmol of methylaluminoxane, 2.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate were dissolved in toluene and transferred to the catalyst storage tube with a syringe, and were pressurized into the reactor with nitrogen (more than 1 MPa), the reaction pressure was maintained at 1 MPa by continuous ethylene gas flow during the polymerization. After reaching the set reaction time of 2 min, 2 mL of ethanol were pressurized into the reactor under nitrogen (more than 1 MPa), the reactor was cooled and vented, the content of the reactor was poured into a large amount of ethanol, the polymer precipitated, was filtered, washed with a small amount of ethanol and finally dried under vacuum overnight. The polymer was weighed. Polymerization activity: 78000 kg-mol -1 (Hf) h -1 Polymer Mw = 1760 kg-mol -1 Mw / Mn = 2.0.

[0051] Example 8, ethylene polymerization with catalyst C1

[0052] The polymerization was carried out as in example 6, the polymerization temperature was 80°C. Polymerization activity: 65000 kg-mol -1 (Hf) h -1 Polymer Mw = 1640 kg-mol -1 Mw / Mn = 2.1.

[0053] Example 9, ethylene polymerization with catalyst C1

[0054] The polymerization was carried out as in example 6, the polymerization temperature was 100°C. Polymerization activity: 110000 kg-mol -1 (Hf) h -1 Polymer Mw = 1830 kg-mol -1 Mw / Mn = 2.3.

[0055] Example 10, ethylene polymerization with catalyst C1

[0056] The polymerization was carried out as in example 6, the polymerization temperature was 140°C. Polymerization activity: 198000 kg-mol -1 (Hf) h -1 Polymer Mw = 2160 kg-mol -1 Mw / Mn = 2.2.

[0057] Example 11, ethylene polymerization with catalyst C1

[0058] The polymerization was carried out under the same conditions as in Example 6, except that the polymerization temperature was 160°C. Polymerization activity: 332000 kg-mol -1 (Hf) - h -1 The polymer Mw = 2780 kg-mol -1 Mw / Mn = 2.3.

[0059] Example 12, Polymerization of ethylene catalyzed by Cl

[0060] The polymerization was carried out under the same conditions as in Example 6, except that the polymerization temperature was 180°C. Polymerization activity: 311000 kg-mol -1 (Hf) - h -1 The polymer Mw = 2820 kg-mol -1 Mw / Mn = 2.4.

[0061] Example 13, Polymerization of ethylene catalyzed by Cl

[0062] The polymerization was carried out under the same conditions as in Example 6, except that the polymerization temperature was 200°C. Polymerization activity: 274000 kg-mol -1 (Hf) - h -1 The polymer Mw = 2160 kg-mol -1 Mw / Mn = 2.3.

[0063] Example 14, Polymerization of ethylene catalyzed by Cl

[0064] A 350 mL glass reactor equipped with a magnetic stirrer was used for the polymerization. In a glove box, 2 μmol of catalyst Cl and 1000 μmol of methylaluminoxane were weighed. The glass reactor was connected to the polymerization line, and 50 mL of toluene was added to the reactor, which was heated to 120°C. Ethylene gas was continuously introduced into the reactor to maintain the pressure at 5 atm during the polymerization. After 2 min, 30 mL of ethanol was added to the reactor under a nitrogen atmosphere. After cooling, the reaction solution was poured into a large amount of ethanol to precipitate the polymer, which was filtered and dried. Polymerization activity: 82000 kg-mol -1 (Hf) - h -1 The polymer Mw = 102 kg-mol -1 Mw / Mn = 2.2.

[0065] Example 15, Polymerization of ethylene catalyzed by Cl

[0066] A 350 mL glass reactor equipped with a magnetic stirrer was used for the polymerization. In a glove box, 2 μmol of catalyst C1, 2.2 μmol of triphenylphosphonium tetrafluoroborate and methylaluminoxane were weighed. The glass reactor was connected to the polymerization line and, after the temperature was raised to 120°C, 50 mL of toluene was added. During the polymerization, ethylene was continuously fed to maintain the reaction pressure at 5 atm. After 2 min of reaction, 30 mL of ethanol was added to the reactor under a nitrogen atmosphere. After cooling, the reaction solution was poured into a large amount of ethanol to precipitate the polymer, which was filtered and dried. Polymerization activity: 104000 kg-mol -1 (Hf) • h -1 Polymer Mw = 2180 kg-mol -1 Mw / Mn = 2.4.

[0067] Example 16, Polymerization of ethylene catalyzed by C1

[0068] A 350 mL glass reactor equipped with a magnetic stirrer was used for the polymerization. In a glove box, 2 μmol of catalyst C1, 2.2 μmol of N,N-dimethylanilinium tetrafluoroborate and methylaluminoxane were weighed. The glass reactor was connected to the polymerization line and, after the temperature was raised to 120°C, 50 mL of toluene was added. During the polymerization, ethylene was continuously fed to maintain the reaction pressure at 5 atm. After 2 min of reaction, 30 mL of ethanol was added to the reactor under a nitrogen atmosphere. After cooling, the reaction solution was poured into a large amount of ethanol to precipitate the polymer, which was filtered and dried. Polymerization activity: 69000 kg-mol -1 (Hf) • h -1 Polymer Mw = 249 kg-mol -1 Mw / Mn = 2.2.

[0069] Example 17, Polymerization of ethylene catalyzed by C2

[0070] The polymerization was carried out under the same conditions as in Example 6, using C2 as catalyst. Polymerization activity: 311000 kg-mol -1 (Hf) • h -1 Polymer Mw = 3340 kg-mol -1 Mw / Mn = 2.0.

[0071] Example 18, Polymerization of ethylene catalyzed by C3

[0072] The polymerization was carried out under the same conditions as in Example 6, using C3 as catalyst. Polymerization activity: 276000 kg-mol -1 (Hf) • h -1 Polymer Mw = 4760 kg-mol -1 Mw / Mn = 2.1.

[0073] Example 19, C4 catalyzed ethylene polymerization

[0074] The polymerization was carried out under the same conditions as in Example 6 using catalyst C4. Polymerization activity: 233000 kg-mol -1 (Hf) - h -1 . Polymer Mw = 2890 kg-mol -1 , Mw / Mn = 2.2.

[0075] Example 20, C5 catalyzed ethylene polymerization

[0076] The polymerization was carried out under the same conditions as in Example 6 using catalyst C5. Polymerization activity: 289000 kg-mol -1 (Ti) - h -1 . Polymer Mw = 4690 kg-mol -1 , Mw / Mn = 2.1.

[0077] Example 21, CI catalyzed ethylene / 1-octene copolymerization

[0078] A 350 mL glass reactor equipped with a magnetic stirrer was used for the polymerization. In a glove box, 2 μmol of catalyst CI, 2.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate and 100 μmol of methylaluminoxane were weighed. The glass reactor was then attached to the polymerization line and 26.6 mL of toluene and 23.4 mL of 1-octene were added to the reactor. The temperature was raised to 160°C and ethylene gas was continuously fed to maintain the pressure at 5 atm. After 2 min of reaction, 30 mL of ethanol was added to the reactor under nitrogen atmosphere. After cooling, the reaction solution was poured into a large amount of ethanol to precipitate the polymer. The final polymer was obtained by filtration and drying. Polymerization activity: 121000 kg-mol -1 (Hf) - h -1 . Polymer Mw = 1240 kg-mol -1 , Mw / Mn = 2.3, 1-octene content in the copolymer 36.4 mol%.

[0079] Example 22, CI catalyzed ethylene / 1-octene copolymerization

[0080] The polymerization was carried out under the same conditions as in Example 21 using 34.4 mL of toluene and 15.6 mL of 1-octene. Polymerization activity: 154000 kg-mol -1 (Hf) - h -1 . Polymer Mw = 1780 kg-mol -1 , Mw / Mn = 2.1, 1-octene content in the copolymer 30.6 mol%.

[0081] Example 23: C1-catalyzed copolymerization of ethylene / 1-octene

[0082] The polymerization process and reaction conditions were the same as in Example 21, using 42.2 mL of toluene and 7.8 mL of 1-octene. Polymerization activity: 24800 kg·mol⁻¹ -1 (Hf)·h -1 Polymer Mw = 2120 kg·mol -1 Mw / Mn = 2.3, and the copolymer contains 22.3 mol% 1-octene.

[0083] Example 24: C1-catalyzed copolymerization of ethylene / 1-octene

[0084] A 100 mL steel reactor equipped with a magnetic inductor was used for the polymerization reaction. A mixture of 26.6 mL toluene and 23.4 mL 1-octene (total 50 mL) was injected using a syringe. The reactor contents were heated to 120 °C, and the reactor was saturated with ethylene at 1 MPa. In a glove box, 2 μmol of catalyst C1, 100 μmol of methylaluminoxane, and 2.2 μmol of triphenylcarbontetra(pentafluorophenyl)borate were added, dissolved in toluene, and transferred to a catalyst storage tube via a syringe. Nitrogen gas (above 1 MPa) was then pressurized into the reactor. During polymerization, the reaction pressure was maintained at 1 MPa by continuously introducing ethylene gas. After the set reaction time of 2 minutes, 2 mL of ethanol was pressurized into the reactor under nitrogen (above 1 MPa). After the reactor cooled and the atmosphere was vented, the contents were poured into a large volume of ethanol, causing polymer precipitation. The polymer was obtained by filtration, washed with a small amount of ethanol, and finally vacuum dried overnight and weighed. Polymerization activity: 172000 kg·mol⁻¹ -1 (Hf)·h -1 Polymer Mw = 2360 kg·mol -1 Mw / Mn = 2.2, and the content of 1-octene in the copolymer is 28.2 mol%.

[0085] Example 25: C1-catalyzed copolymerization of ethylene / 1-octene

[0086] The polymerization process and conditions were the same as in Example 24, with a polymerization pressure of 2 MPa. Polymerization activity: 221000 kg·mol⁻¹ -1 (Hf)·h -1 Polymer Mw = 2630 kg·mol -1 Mw / Mn = 2.1, and the copolymer contains 24.5 mol% 1-octene.

[0087] Example 26: C1-catalyzed copolymerization of ethylene / 1-octene

[0088] The polymerization was carried out under the same conditions as in Example 24, and the polymerization pressure was 3 MPa. Polymerization activity: 248000 kg-mol -1 (Hf) - h -1 The polymer Mw = 2830 kg-mol -1 Mw / Mn = 2.4, and the content of 1-octene in the copolymer was 15.8 mol%.

[0089] Example 27, copolymerization of ethylene / 1-octene catalyzed by Cl

[0090] The polymerization was carried out under the same conditions as in Example 24, and the polymerization pressure was 4 MPa. Polymerization activity: 296000 kg-mol -1 (Hf) - h -1 The polymer Mw = 3020 kg-mol -1 Mw / Mn = 2.3, and the content of 1-octene in the copolymer was 10.2 mol%.

[0091] Example 28, copolymerization of ethylene / 1-octene catalyzed by Cl

[0092] The polymerization was carried out under the same conditions as in Example 21, and the temperature selected was 180°C. Polymerization activity: 108000 kg-mol -1 (Hf) - h -1 The polymer Mw = 1840 kg-mol -1 Mw / Mn = 2.2, and the content of 1-octene in the copolymer was 27.4 mol%.

[0093] Example 29, copolymerization of ethylene / 1-octene catalyzed by Cl

[0094] The polymerization was carried out under the same conditions as in Example 21, and the temperature selected was 200°C. Polymerization activity: 96000 kg-mol -1 (Hf) - h -1 The polymer Mw = 1590 kg-mol -1 Mw / Mn = 2.3, and the content of 1-octene in the copolymer was 22.6 mol%.

[0095] Example 30, copolymerization of ethylene / 1-octene catalyzed by C2

[0096] The polymerization was carried out under the same conditions as in Example 21, and the catalyst used was C2. Polymerization activity: 129000 kg-mol -1 (Hf) - h -1 The polymer Mw = 1430 kg-mol -1 Mw / Mn = 2.2, and the content of 1-octene in the copolymer was 29.3 mol%.

[0097] Example 31, C3 catalyzed ethylene / 1-octene copolymerization

[0098] The polymerization was carried out in a 350 mL glass reactor equipped with a magnetic stirrer. In a glove box, 2 μmol of catalyst C3, 2.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate and 100 μmol of methylaluminoxane were weighed. Then the glass reactor was attached to the polymerization line and 31.6 mL of toluene and 18.4 mL of 1-octene were added. The reaction was started by continuously bubbling ethylene gas into the reactor to maintain a pressure of 5 atm. After 2 min of reaction, 30 mL of ethanol was added to the reactor under a nitrogen atmosphere. After cooling, the reaction solution was poured into a large amount of ethanol to precipitate the polymer. The final polymer was obtained by filtration and drying. Polymerization activity: 113000 kg-mol -1 (Hf) h -1 The polymer Mw = 1860 kg-mol -1 Mw / Mn = 2.3, and the content of 1-octene in the copolymer was 38.4 mol%.

[0099] Example 32, C4 catalyzed ethylene / 1-octene copolymerization

[0100] The polymerization was carried out in a 350 mL glass reactor equipped with a magnetic stirrer. In a glove box, 2 μmol of catalyst C4, 2.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate and 100 μmol of methylaluminoxane were weighed. Then the glass reactor was attached to the polymerization line and 31.6 mL of toluene and 18.4 mL of 1-octene were added. The reaction was started by continuously bubbling ethylene gas into the reactor to maintain a pressure of 5 atm. After 2 min of reaction, 30 mL of ethanol was added to the reactor under a nitrogen atmosphere. After cooling, the reaction solution was poured into a large amount of ethanol to precipitate the polymer. The final polymer was obtained by filtration and drying. Polymerization activity: 142000 kg-mol -1 (Hf) h -1 The polymer Mw = 1420 kg-mol -1 Mw / Mn = 2.3, and the content of 1-octene in the copolymer was 21.9 mol%.

[0101] Example 33, C5 catalyzed ethylene / 1-octene copolymerization

[0102] The polymerization was carried out in a 350 mL glass reactor equipped with a magnetic stirrer. In a glove box, 2 μmol of catalyst C5, 2.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate and 100 μmol of methylaluminoxane were weighed. Then the glass reactor was attached to the polymerization line and 31.6 mL of toluene and 18.4 mL of 1-octene were added. The reaction was started by continuously bubbling ethylene gas into the reactor to maintain a pressure of 5 atm. After 2 min of reaction, 30 mL of ethanol was added to the reactor under a nitrogen atmosphere. After cooling, the reaction solution was poured into a large amount of ethanol to precipitate the polymer. The final polymer was obtained by filtration and drying. Polymerization activity: 163000 kg-mol -1 (Hf) h -1 The polymer Mw = 1280 kg-mol -1 Mw / Mn = 2.2, and the content of 1-octene in the copolymer was 13.6 mol%.

[0103] Example 34, C1 catalyzed ethylene / 1-hexene copolymerization

[0104] The polymerization was carried out in a 350 mL glass reactor equipped with a magnetic stirrer. In a glove box, 2 μmol of catalyst C1, 2.2 μmol of triphenylcarbenium tetrakis(pentafluorophenyl)borate and 100 μmol of methylaluminoxane were weighed. Then the glass reactor was attached to the polymerization line and 31.6 mL of toluene and 18.4 mL of 1-hexene were added. The reaction was started by continuously bubbling ethylene gas into the reactor to maintain a pressure of 5 atm. After 2 min of reaction, 30 mL of ethanol was added to the reactor under a nitrogen atmosphere. After cooling, the reaction solution was poured into a large amount of ethanol to precipitate the polymer. The final polymer was obtained by filtration and drying. Polymerization activity: 145000 kg-mol -1 (Hf) h -1 The polymer Mw = 1360 kg-mol -1 Mw / Mn = 2.0, and the content of 1-hexene in the copolymer was 33.5 mol%.

Claims

1. A hydrogenated quinoline-imido titanium zirconium hafnium metal catalyst, having a structure as shown in formula (I): wherein M is selected from titanium, zirconium, hafnium; R 1 selected from methyl, ethyl, hydrogen, isopropyl, chloro, fluoro; R 2 selected from methyl, ethyl, hydrogen, isopropyl, chloro, fluoro; R 3 selected from methyl, methoxy, hydrogen, t-butyl.

2. A method for preparing the hydrogenated quinoline-imido titanium zirconium hafnium metal catalyst of claim 1, comprising the following steps: dissolving a metal salt MCl4 in 20-80 mL of anhydrous solvent under a nitrogen atmosphere, adding 4.0-5.0 molar equivalents of methyl magnesium bromide, reacting at low temperature under nitrogen protection for 2 hours, and then adding 1 molar equivalent of hydrogenated quinoline imine ligand and reacting for 5 hours; after the reaction is completed, removing the solvent under reduced pressure, extracting with a good solvent, and obtaining the hydrogenated quinoline-imido titanium zirconium hafnium catalyst of claim 1.

3. The method of claim 2, wherein: The anhydrous solvent is selected from toluene, n-hexane, xylene, and benzene; the good solvent is selected from n-hexane, toluene, pentane, heptane, and cyclohexane.

4. The method of claim 2, wherein: The metal salt MCl4 is selected from one of TiCl4, ZrCl4, and HfCl4.

5. A process for the polymerization of olefins, characterized in that: The catalyst used is the hydrogenated quinoline-imido titanium zirconium hafnium catalyst of claim 1.

6. The method of claim 5, wherein: The olefin monomer is one or more of ethylene, propylene, 1-butene, styrene, 1-hexene, norbornene, and 1-octene.

7. The method of claim 5, wherein: The hydrogenated quinoline-imido titanium zirconium hafnium catalyst needs to be combined with a cocatalyst for catalysis, and the cocatalyst is one or more of tri(pentafluorophenyl)boron, triphenylcarbenium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, aluminoxane, alkylaluminum, and chlorinated alkylaluminum.

8. The method of claim 7, wherein: The aluminoxane is methylaluminoxane, ethylaluminoxane, or isobutylaluminoxane; the alkylaluminum is trimethylaluminum, triethylaluminum, triisobutylaluminum, or tri-n-hexylaluminum; and the chlorinated alkylaluminum is dichlorodiethylaluminum, sesqui-dichlorodiethylaluminum, or dichloroethylaluminum.

9. The method of claim 5, wherein: The polymerization temperature is 0-200°C, the polymerization pressure is 0.1-5 MPa, and the solvent used for polymerization is one or more of n-hexane, n-heptane, n-pentane, and toluene.